WO2024195518A1 - ペレット混合物、電波吸収体、電波吸収物品および電波吸収体の製造方法 - Google Patents

ペレット混合物、電波吸収体、電波吸収物品および電波吸収体の製造方法 Download PDF

Info

Publication number
WO2024195518A1
WO2024195518A1 PCT/JP2024/008283 JP2024008283W WO2024195518A1 WO 2024195518 A1 WO2024195518 A1 WO 2024195518A1 JP 2024008283 W JP2024008283 W JP 2024008283W WO 2024195518 A1 WO2024195518 A1 WO 2024195518A1
Authority
WO
WIPO (PCT)
Prior art keywords
radio wave
pellet
particles
composition
wave absorber
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2024/008283
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
浩一 橋本
孝一 畠山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fujifilm Corp
Original Assignee
Fujifilm Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fujifilm Corp filed Critical Fujifilm Corp
Priority to JP2025508292A priority Critical patent/JPWO2024195518A1/ja
Priority to EP24774661.3A priority patent/EP4686333A4/en
Publication of WO2024195518A1 publication Critical patent/WO2024195518A1/ja
Priority to US19/335,155 priority patent/US20260018323A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01F—MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
    • H01F1/00—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties
    • H01F1/01—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials
    • H01F1/03—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity
    • H01F1/12—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials
    • H01F1/34—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials non-metallic substances, e.g. ferrites
    • H01F1/36—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials non-metallic substances, e.g. ferrites in the form of particles
    • H01F1/37—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials non-metallic substances, e.g. ferrites in the form of particles in a bonding agent
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
    • B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
    • B29C45/00—Injection moulding, i.e. forcing the required volume of moulding material through a nozzle into a closed mould; Apparatus therefor
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01F—MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
    • H01F1/00—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties
    • H01F1/01—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials
    • H01F1/03—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity
    • H01F1/12—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials
    • H01F1/34—Magnets or magnetic bodies characterised by the magnetic materials therefor; Selection of materials for their magnetic properties of inorganic materials characterised by their coercivity of soft-magnetic materials non-metallic substances, e.g. ferrites
    • H01F1/342—Oxides
    • H01F1/344—Ferrites, e.g. having a cubic spinel structure (X2+O)(Y23+O3), e.g. magnetite Fe3O4
    • H01F1/348—Hexaferrites with decreased hardness or anisotropy, i.e. with increased permeability in the microwave (GHz) range, e.g. having a hexagonal crystallographic structure
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01Q—ANTENNAS, i.e. RADIO AERIALS
    • H01Q17/00—Devices for absorbing waves radiated from an antenna; Combinations of such devices with active antenna elements or systems
    • H01Q17/004—Devices for absorbing waves radiated from an antenna; Combinations of such devices with active antenna elements or systems using non-directional dissipative particles, e.g. ferrite powders
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01Q—ANTENNAS, i.e. RADIO AERIALS
    • H01Q17/00—Devices for absorbing waves radiated from an antenna; Combinations of such devices with active antenna elements or systems

Definitions

  • the present invention relates to a pellet mixture, a radio wave absorber, a radio wave absorbing article, and a method for manufacturing a radio wave absorber.
  • the radio wave absorber can be incorporated into various articles as a molded product made by molding a composition containing a radio wave absorbing material (see, for example, Patent Document 1).
  • an in-vehicle radar transmits radio waves and receives the radio waves reflected by the object (pedestrian, vehicle, etc.), thereby being able to recognize the presence of the object and the distance from the object.
  • an automobile's automatic driving control system can automatically brake the vehicle to a halt as necessary to prevent a collision with the object, or automatically control the speed to maintain a distance from the object.
  • radio wave absorbers that exhibit stable radio wave absorption properties (i.e., radio wave absorbers with little variation in radio wave absorption properties) could be mass-produced when mass-producing molded articles made from compositions containing radio wave absorbing materials, this would lead to further improvements in the usefulness of radio wave absorbers.
  • One aspect of the present invention aims to enable the mass production of radio wave absorbers that exhibit stable radio wave absorption properties.
  • Pellet 0 which is a pellet of a composition containing at least a resin
  • Pellet 1 is a pellet of a composition comprising one or more types of particles selected from the group consisting of magnetic particles and dielectric particles, and a resin, the volume content of the particles being higher than the volume content of the particles in the composition of Pellet 0;
  • the pellet mixture according to [1], wherein the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.50 or more and 0.80 or less.
  • the particles are magnetic particles, The pellet mixture according to [1] or [2], wherein the magnetic particles are hexagonal ferrite particles.
  • the substitutional hexagonal ferrite is a magnetoplumbite-type hexagonal ferrite having a composition represented by the following formula 1; In formula 1, A represents one or more atoms selected from the group consisting of Sr, Ba, Ca, and Pb, and x satisfies 0.50 ⁇ x ⁇ 8.00.
  • A represents one or more atoms selected from the group consisting of Sr, Ba, Ca, and Pb, and x satisfies 0.50 ⁇ x ⁇ 8.00.
  • the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.50 or more and 0.80 or less
  • the magnetic particles are particles of hexagonal ferrite
  • the hexagonal ferrite is a substitutional hexagonal ferrite
  • A represents one or more atoms selected from the group consisting of Sr, Ba, Ca, and Pb, the atoms represented by A include Sr, and x satisfies 0.50 ⁇ x ⁇ 8.00.
  • a radio wave absorber which is a molded product obtained by molding the pellet mixture according to any one of [1] to [7].
  • a radio wave absorbing article comprising the radio wave absorber according to [8].
  • a method for producing a radio wave absorber comprising molding the pellet mixture according to any one of [1] to [7] into a molded article.
  • the method for producing a radio wave absorber according to [10], wherein the molding is injection molding.
  • a pellet mixture that can contribute to enabling mass production of radio wave absorbers that exhibit stable radio wave absorption properties.
  • a radio wave absorber that is a molded product formed from the pellet mixture, a radio wave absorbing article that includes this radio wave absorber, and a method for manufacturing a radio wave absorber that includes molding the pellet mixture into a molded product.
  • FIG. 2 is an explanatory diagram of a method for measuring a friction coefficient.
  • FIG. 1 is a schematic configuration diagram of an injection molding machine.
  • FIG. 2 is a schematic diagram of a pellet supply section of an injection molding machine used to produce injection-molded articles in the examples and comparative examples.
  • radio waves refers to electromagnetic waves with a frequency of 3 terahertz (THz) or less.
  • a “radio wave absorber” has radio wave absorption properties for radio waves of one or more frequencies.
  • Pellet mixture which is a pellet of a composition containing at least a resin
  • Pellet 1 which is a pellet of a composition containing one or more particles selected from the group consisting of magnetic particles and dielectric particles, and a resin, and in which the volume content of the particles is higher than the volume content of the particles in the composition of Pellet 0.
  • the friction coefficient of the composition of Pellet 0 with metal is ⁇ 0
  • the friction coefficient of the composition of Pellet 1 with metal is ⁇ 1
  • the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.80 or less.
  • pellets refer to granular matter of a resin-containing composition.
  • the shape of the granular matter is not particularly limited, and can be any shape, such as spherical, approximately spherical, cylindrical, approximately cylindrical, rectangular, approximately rectangular, or flake-like.
  • Each of "pellet 0" and “pellet 1” is an aggregate of granular matter of a resin-containing composition.
  • the “aggregate” is not limited to a form in which the granular matter constituting the aggregate is in direct contact with each other in the pellet mixture.
  • composition of pellet 0 and the composition of pellet 1 will be collectively referred to simply as the composition.
  • the "pellet 0" contained in the pellet mixture is a pellet of a composition containing at least a resin
  • the "pellet 1" is a pellet of a composition containing one or more particles selected from the group consisting of magnetic particles and dielectric particles, and a resin, and the volume content of the particles is higher than the volume content of the particles in the composition of the pellet 0.
  • the higher the volume content of the particles the higher the specific gravity of the pellets.
  • the inventor believes that the large difference in timing at which the two types of pellets with different specific gravities are supplied to the molding section of the molding machine in this way can cause variations in the radio wave absorption properties of multiple radio wave absorbers mass-produced by molding.
  • the present inventor considered that the higher the friction coefficient against metal, the greater the resistance the pellets receive in the molding machine, and therefore the slower the supply speed of the pellets to the molding section. In other words, the lower the friction coefficient against metal, the smaller the resistance the pellets receive in the molding machine, and therefore the faster the supply speed of the pellets to the molding section.
  • a pellet mixture containing pellets 0 and 1 in a combination in which the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.80 or less, where the friction coefficient of the composition of pellet 0 is ⁇ 0 and the friction coefficient of the composition of pellet 1 is ⁇ 1, can exhibit stable radio wave absorption properties. This is presumably because a pellet mixture containing pellets 0 and 1 in a combination in which the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.80 or less can suppress a large difference between the timing of pellets 0 and 1 being supplied to the molding section in the molding machine.
  • the present invention is not limited to the presumption described in this specification.
  • the pellet mixture is described in more detail below.
  • the friction coefficients ⁇ 0 and ⁇ 1 are values determined by the following method.
  • Pellet 0 and pellet 1 are taken out from the pellet mixture. Each pellet can be taken out from the pellet mixture by a known separation method such as a method utilizing the difference in specific gravity. Alternatively, pellets for friction coefficient measurement may be taken from the same lot as the lot of each pellet used to prepare the pellet mixture.
  • a flat plate having a size of 80 mm x 60 mm and a thickness of 1 mm is prepared as a sample for measuring the friction coefficient. Five samples for measuring the friction coefficient are prepared for each of pellet 0 and pellet 1. The method for preparing the flat plate is not particularly limited.
  • the flat plate can be prepared by a molding method usually used for preparing flat plates, such as injection molding, extrusion molding, and compression molding.
  • a molding method usually used for preparing flat plates such as injection molding, extrusion molding, and compression molding.
  • the surface in contact with the counter material and the surface in contact with the sliding piece are visually confirmed to be free of significant burrs and significant warping.
  • the arithmetic mean roughness Ra of the surface in contact with the counter material in the friction coefficient measurement is 3.0 ⁇ m or less.
  • the method described in the Examples section below can be used as a method for measuring Ra.
  • FIG. 1 is an explanatory diagram of a method for measuring the coefficient of friction. The coefficient of friction is measured in a measurement environment with an ambient temperature of 23° C. and a relative humidity of 50%.
  • a SUS (Steel Use Stainless) plate is used as the counter material.
  • a sample and a sliding piece are placed on the counter material as shown in FIG. 1.
  • the sliding piece may have a bottom surface that contacts the sample surface with a size of 63 mm ⁇ 63 mm and a total mass of 200 g (1.96 N).
  • the bottom surface of the sliding piece that contacts the sample surface is covered with an elastic material.
  • the total mass of the sliding piece is a mass including the mass of the material that covers the bottom surface. Examples of elastic materials include felt, foam rubber, etc., and in the measurement of the coefficient of friction described in the Examples section below, a sliding piece with a bottom surface covered with foam rubber was used.
  • the load cell capacity is 50N (Newton), the test speed is 100mm/min (min), and the static friction coefficient is used as the friction coefficient.
  • the arithmetic average of the friction coefficient values of the five samples for each of pellet 0 and pellet 1 is set as the friction coefficient ⁇ 0, ⁇ 1 of the composition of each pellet against the metal.
  • SUS plate is used as the counter material is that SUS is a representative example of the metal that constitutes the inside of the molding machine, and the molding machine used when molding a molded product using the above pellet mixture is not limited to one with an inside made of SUS.
  • the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.80 or less, preferably 0.78 or less, and more preferably 0.76 or less, 0.75 or less, 0.74 or less, 0.72 or less, 0.70 or less, 0.68 or less, 0.66 or less, and 0.64 or less, in that order, from the viewpoint of enabling mass production of radio wave absorbers that exhibit stable radio wave absorption properties.
  • the friction coefficient ratio ( ⁇ 0/ ⁇ 1) can be, for example, 0.50 or more, 0.52 or more, or 0.54 or more.
  • the friction coefficient ⁇ 0 can be 0.30 or more and 0.50 or less
  • the friction coefficient ⁇ 1 can be 0.40 or more and 0.70 or less.
  • the friction coefficient ⁇ 0 and the friction coefficient ⁇ 1 are not limited to the above ranges as long as the friction coefficient ratio ( ⁇ 0/ ⁇ 1) is 0.80 or less.
  • the friction coefficient of each pellet can be adjusted, for example, by the type of resin contained in the pellet, the mixing ratio of the multiple resins if multiple resins are contained, the addition of a slip agent, etc.
  • Pellet 0 is a pellet of a composition containing at least a resin, and in one embodiment does not contain one or more types of particles selected from the group consisting of magnetic particles and dielectric particles, and in another embodiment contains one or more types of particles selected from the group consisting of magnetic particles and dielectric particles.
  • pellet 1 is a pellet of a composition containing one or more types of particles selected from the group consisting of magnetic particles and dielectric particles, and a resin, and the volume content of the particles in the composition of pellet 1 is higher than the volume content of the particles in the composition of pellet 0.
  • the particles are one or more types of particles selected from the group consisting of magnetic particles and dielectric particles.
  • Each of the composition of pellet 0 and the composition of pellet 1 may contain different types of particles in any ratio as particles selected from the group consisting of magnetic particles and dielectric particles. This also applies to the radio wave absorber described below.
  • “magnetic” means ferromagnetic property
  • “dielectric” means a material having a volume resistivity ( ⁇ v ) at 20° C., which is an inherent value of the material, of 1 ⁇ 10 5 ⁇ m or more.
  • dielectric particles As the dielectric particles that can be contained in the composition, various dielectric particles can be used.
  • the dielectric particles can be carbon-based particles.
  • “based” is used to mean “including.”
  • the carbon-based particles particles of various carbon-based materials such as carbon black and graphite can be used.
  • Magnetic Particles examples of magnetic particles that can be contained in the composition include particles of various magnetic materials such as ferrite, iron oxide, cobalt, and chromium oxide. From the viewpoint of radio wave absorption, hexagonal ferrite particles are preferable as the magnetic particles.
  • the type of magnetic material constituting the magnetic particles can be confirmed by performing analysis by X-ray diffraction. For example, a powder of magnetic particles can be taken out from a composition containing magnetic particles or a radio wave absorber containing magnetic particles by a known method, and the taken powder can be analyzed by X-ray diffraction. Alternatively, a part of the powder of magnetic particles used in the preparation of the composition can be collected, and the collected powder can be analyzed by X-ray diffraction.
  • a part or the whole of the radio wave absorber is finely chopped, immersed in a solvent (e.g., hexafluoroisopropanol) for 1 to 2 days, and then dried.
  • the radio wave absorber after drying is further finely ground, and analyzed by X-ray diffraction.
  • Hexagonal ferrite particles refers to magnetic particles in which the crystal structure of hexagonal ferrite is detected as the main phase by analysis performed by X-ray diffraction.
  • the main phase refers to the structure to which the most intense diffraction peak belongs in the X-ray diffraction spectrum obtained by X-ray diffraction. For example, when the most intense diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction is attributed to the crystal structure of hexagonal ferrite, it is determined that the crystal structure of hexagonal ferrite is detected as the main phase.
  • the crystal structure of hexagonal ferrite contains at least iron atoms, divalent metal atoms, and oxygen atoms as constituent atoms.
  • the atoms that constitute the crystal structure of hexagonal ferrite are only iron atoms, divalent metal atoms, and oxygen atoms.
  • substitutional hexagonal ferrite contains one or more other atoms as well as iron atoms, divalent metal atoms, and oxygen atoms as atoms constituting the crystal structure of hexagonal ferrite.
  • the one or more other atoms are usually atoms that replace part of iron in the crystal structure of hexagonal ferrite.
  • the divalent metal atoms are metal atoms that can become divalent cations as ions, and examples of such metal atoms include alkaline earth metal atoms such as strontium atoms, barium atoms, and calcium atoms, and lead atoms.
  • the particles of hexagonal strontium ferrite refer to particles in which the main divalent metal atom contained in the particles is a strontium atom
  • the particles of hexagonal barium ferrite refer to particles in which the main divalent metal atom contained in the particles is a barium atom. The same applies to particles of other types of hexagonal ferrite.
  • the main divalent metal atoms refer to the divalent metal atoms that occupy the largest number of the divalent metal atoms contained in the particles on an atomic % basis. However, the above divalent metal atoms do not include rare earth atoms.
  • the "rare earth atom" in the present invention and this specification is selected from the group consisting of scandium atom (Sc), yttrium atom (Y), and lanthanoid atom.
  • the lanthanoid atom is selected from the group consisting of lanthanum atom (La), cerium atom (Ce), praseodymium atom (Pr), neodymium atom (Nd), promethium atom (Pm), samarium atom (Sm), europium atom (Eu), gadolinium atom (Gd), terbium atom (Tb), dysprosium atom (Dy), holmium atom (Ho), erbium atom (Er), thulium atom (Tm), ytterbium atom (Yb), and lutetium atom (Lu).
  • La lanthanum atom
  • Ce cerium atom
  • Pr praseodymium atom
  • Nd neodymium atom
  • promethium atom Pm
  • Sm samarium atom
  • Eu europium atom
  • Gd gadolinium atom
  • Tb terbium
  • the hexagonal ferrite constituting the particles can be one or more selected from the group consisting of hexagonal strontium ferrite, hexagonal barium ferrite, hexagonal calcium ferrite, and hexagonal lead ferrite. From the viewpoint of radio wave absorption in the high frequency band, one or more selected from the group consisting of hexagonal strontium ferrite, hexagonal barium ferrite, and hexagonal calcium ferrite are preferred, hexagonal strontium ferrite and/or hexagonal barium ferrite are more preferred, and hexagonal strontium ferrite is even more preferred.
  • the hexagonal ferrite particles can be magnetoplumbite type (commonly referred to as "M type") hexagonal ferrite particles.
  • M type magnetoplumbite type
  • magnetoplumbite type hexagonal ferrite is an unsubstituted type that does not contain atoms that substitute for iron, it has a composition represented by the composition formula: AFe12O19 .
  • A can represent one or more atoms selected from the group consisting of Sr, Ba, Ca, and Pb , and also includes a form in which two or more of these are contained in any ratio.
  • a preferred hexagonal ferrite from the viewpoint of radio wave absorption is substitutional hexagonal ferrite.
  • substitutional hexagonal ferrite is magnetoplumbite-type hexagonal ferrite in which some of the iron atoms of magnetoplumbite-type hexagonal ferrite are replaced with aluminum atoms.
  • hexagonal ferrite having a composition represented by the following formula 1.
  • A represents one or more types of atoms selected from the group consisting of Sr, Ba, Ca, and Pb (hereinafter also referred to as "A atom"), and may contain only one type or two or more types in any ratio, and preferably contains only one type from the viewpoint of improving the uniformity of the composition among particles contained in the radio wave absorber.
  • a in formula 1 is preferably one or more atoms selected from the group consisting of Sr, Ba, and Ca, more preferably one or more atoms selected from the group consisting of Sr and Ba, further preferably includes Sr, and even more preferably is Sr.
  • x can satisfy 1.50 ⁇ x ⁇ 8.00.
  • x is preferably 1.50 or more, more preferably greater than 1.50, even more preferably 2.00 or more, and even more preferably greater than 2.00.
  • x is 8.00 or less, preferably less than 8.00, more preferably 6.00 or less, and even more preferably less than 6.00.
  • magnetoplumbite type substitutional hexagonal ferrite represented by formula 1, where x satisfies 1.50 ⁇ x ⁇ 8.00 include SrFe (9.58) Al (2.42) O 19 , SrFe (9.37) Al (2.63) O 19 , SrFe (9.27) Al (2.73) O 19 , SrFe (9.85) Al (2.15) O 19 , SrFe (10.00) Al (2.00) O 19 , SrFe (9.74) Al (2.26) O 19 , SrFe (10.44) Al (1.56) O 19 , and SrFe (9.79) Al (2.21) O 19 , SrFe (9.33) Al (2.67) O 19 , SrFe ( 7.88) Al ( 4.12) O 19 , SrFe (7.04) Al (4.96) O 19 , SrFe (7.37 ) Al (4.63 ) O 19 , SrFe (6 .25) Al (5.75) O 19 , SrFe (7.
  • composition of the magnetic particles can be confirmed, for example, by performing high-frequency inductively coupled plasma optical emission spectroscopy on a solution in which the magnetic particles are dissolved.
  • confirmation method include the method described in the Examples section below.
  • the composition of the magnetic particles contained in the radio wave absorber can be confirmed by, for example, cutting the radio wave absorber to expose a cross section, and then performing, for example, energy dispersive X-ray analysis on the exposed cross section.
  • x can satisfy 0.50 ⁇ x ⁇ 1.50.
  • x can be 0.50 or more, and is preferably greater than 0.80.
  • x is preferably less than 1.50, and more preferably 1.20 or less.
  • the substitutional hexagonal ferrite may have a single crystal phase or may include multiple crystal phases, preferably a single crystal phase, and more preferably a magnetoplumbite-type substitutional hexagonal ferrite having a single crystal phase.
  • crystal phase is single phase
  • the analysis by the X-ray diffraction method can be performed by the method described in the Examples section below.
  • two or more types of diffraction patterns showing any crystal structure are observed in the analysis by the X-ray diffraction method.
  • the database of the International Centre for Diffraction Data (ICDD: International Centre for Diffraction Data (registered trademark)
  • ICDD International Centre for Diffraction Data
  • magnetoplumbite-type hexagonal ferrite containing Sr "00-033-1340" of the International Centre for Diffraction Data (ICDD) can be referred to.
  • substitution atoms such as aluminum atoms
  • Method for producing hexagonal ferrite particles There are various methods for producing hexagonal ferrite particles, and when the composition contains hexagonal ferrite particles, the method for producing the hexagonal ferrite particles is not particularly limited. Below, a solid-phase method will be described as an example of a method for producing hexagonal ferrite particles.
  • the solid-phase method is a method for producing hexagonal ferrite particles by mixing a plurality of solid raw materials and firing the mixture obtained.
  • the solid raw materials used in the solid phase method include compounds of iron atoms and compounds of A atoms, and when producing a powder of substitutional hexagonal ferrite, compounds of substitutional atoms can be further included. These compounds can be oxides, carbonates, etc.
  • the A atoms and substitutional atoms are as described above.
  • the mixing ratio of the multiple solid raw materials may be determined according to the desired hexagonal ferrite composition.
  • a raw material mixture can be obtained by simultaneously mixing the multiple solid raw materials or sequentially mixing them in any order.
  • the mixing of the solid raw materials is not limited to being performed under dry conditions. It is also possible to add a solvent such as water under wet conditions and mix in a slurry state.
  • the mixing of the solid raw materials can be performed using a commercially available mixer or a mixer with a known configuration.
  • An example of a mixer is a paint shaker.
  • An example of a means for strengthening the mixing conditions is the use of a dispersion medium such as dispersion beads.
  • the above mixing can be performed, for example, under air atmosphere at room temperature.
  • the obtained raw material mixture can be fired.
  • the crystallization of the raw material mixture can be promoted, and thereby a hexagonal ferrite crystal structure can be formed.
  • the firing temperature can be in the range of 1000°C to 1500°C.
  • the firing temperature can be, for example, the atmospheric temperature in the device in which the firing is performed (for example, the temperature inside the heating furnace).
  • the firing time can be in the range of 1 hour to 6 hours.
  • firing can be performed under conditions that allow the formation of a hexagonal ferrite crystal structure. Firing can be performed, for example, in an air atmosphere.
  • a flux can be added to the powder of the raw material mixture before firing.
  • various fluxes can be used, for example, SrCl 2 , SrCl 2.6H 2 O, CaCl 2.2H 2 O, MgCl 2 , KCl, NaCl, BaCl 2.2H 2 O, Na 2 B 4 O 7 , etc.
  • the amount of the flux added is preferably, for example, 0.1 to 10 parts by mass, more preferably 0.1 to 8.0 parts by mass, relative to 100 parts by mass of the powder of the raw material mixture.
  • the raw material mixture before sintering can be subjected to a dry or wet grinding process, and/or the sintered product after sintering can be subjected to a dry or wet grinding process.
  • the size of the particles constituting the hexagonal ferrite powder can be adjusted. Grinding can be carried out by known grinding means such as a mortar and pestle, or a grinder (cutter mill, ball mill, bead mill, roller mill, jet mill, hammer mill, attritor, etc.). The stronger the grinding conditions, the greater the value of the slope of the peak frequency versus temperature described above tends to be.
  • the fired product obtained after firing can be subjected to a process such as crushing if necessary, and then annealed.
  • a process such as crushing if necessary
  • annealing By performing annealing, the slope value of the peak frequency with respect to the temperature described above tends to become smaller.
  • the annealing can be performed, for example, for about 1 to 10 hours in a heating furnace with an internal temperature of 500 to 1100°C.
  • one or more known steps such as washing and drying can be optionally performed.
  • volume content The composition and the radio wave absorber obtained by molding the pellet mixture contain the particles and resin.
  • the volume content of the particles in the composition and the radio wave absorber is not particularly limited.
  • the volume content means a content based on volume with the total volume of the composition (excluding the solvent when the composition contains a solvent; the same applies below) or the total volume of the radio wave absorber being 100 volume %.
  • the volume content of the particles in the radio wave absorber can be 35 volume % or less, for example, in the range of 15 to 35 volume %.
  • the volume content of the particles in the radio wave absorber can be 35 volume % or more. In this case, the volume content can be, for example, in the range of 35 to 60 volume %, or in the range of 35 to 50 volume %.
  • Pellet 1 is a pellet of a composition that includes one or more types of particles selected from the group consisting of magnetic particles and dielectric particles, and a resin, and the volume content of the particles is higher than the volume content of the particles in the composition of Pellet 0.
  • the volume content of the particles in the composition of Pellet 1 can be 35 volume% or less, for example, in the range of 15 to 35 volume%.
  • the volume content of the particles in the composition of Pellet 1 can be 35 volume% or more. In this case, the volume content can be, for example, in the range of 35 to 60 volume%, or in the range of 35 to 50 volume%.
  • Pellet 0 is a pellet of a composition containing at least a resin, and in one embodiment does not contain one or more types of particles selected from the group consisting of magnetic particles and dielectric particles, and in another embodiment contains one or more types of particles selected from the group consisting of magnetic particles and dielectric particles.
  • the volume content of the particles in the composition of Pellet 0 is 0 volume% or more, and can be 0 volume% or more than 0 volume%.
  • the volume content of the particles in the composition of Pellet 0 can be, for example, less than 35 volume%, 30 volume% or less, 25 volume% or less, 20 volume% or less, 15 volume% or less, 10 volume% or less, 5 volume% or less, or 1 volume% or less.
  • the volume content of the particles can be determined from the composition of the composition for a composition.
  • the particles are collected from the radio wave absorber by a known method, and the volume content of the particles can be determined by "(volume of collected particles/total volume of radio wave absorber) x 100".
  • the total volume of the radio wave absorber and the volume of the particles can be determined by a known method.
  • the composition of the composition used to prepare the radio wave absorber is known
  • the volume content of the particles in the radio wave absorber can also be determined from this known composition.
  • the volume content of the particles in the radio wave absorber can also be determined by the following method using a cross-sectional SEM image obtained by a scanning electron microscope (SEM).
  • a measurement sample having a square plane with sides of 5 mm is cut out from a randomly determined position of the radio wave absorber to be measured.
  • a cross-sectional observation sample is prepared from the cut out sample.
  • the cross-sectional observation sample is prepared by FIB (Focused Ion Beam) processing.
  • the prepared cross-sectional observation sample is observed by SEM, and a cross-sectional image (cross-sectional SEM image) is taken.
  • a field emission scanning electron microscope (FE-SEM) is used as the SEM.
  • the cross-sectional observation sample is set on the stage so that the FIB-processed cross section faces upward, and a cross-sectional SEM image with a field of view of 30 ⁇ m ⁇ 40 ⁇ m is obtained under conditions of an acceleration voltage of 15 kV and an observation magnification of 3000 times.
  • the obtained cross-sectional SEM image is binarized, and the ratio (area basis) occupied by the above particles is calculated.
  • the above operation is performed for five measurement samples cut out from different positions of the radio wave absorber to be measured, and the volume content of the above particles can be obtained as the arithmetic average of the five values obtained.
  • the portion of the above particles in the cross-sectional SEM image can also be specified by performing elemental analysis of the cross-sectional observation sample.
  • the loadings of other components described in this specification can be determined in the same manner as above.
  • the specific gravities of pellet 1 and pellet 0 are not particularly limited.
  • the specific gravity of the pellet 1 can be, for example, 1.5 or more and 3.0 or less.
  • the specific gravity of the pellet 0 can be, for example, not less than 0.5 and less than 1.5.
  • the difference between the specific gravity of pellet 1 and the specific gravity of pellet 0 can be, for example, 0.5 or more and 2.0 or less, or 0.5 or more and 1.5 or less.
  • the "specific gravity" is measured by the underwater displacement method described in JIS K 7112-1:2023.
  • the term “resin” is synonymous with the term “polymer,” and the term “polymer” includes homopolymers and copolymers.
  • the resin can function as a binder in the composition and the radio wave absorber.
  • Resins include thermoplastic resins and thermosetting resins.
  • the thermoplastic resin include acrylic resin, polyacetal, polyamide, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanedimethanol terephthalate copolymer, polylactic acid, polycarbonate, polystyrene, polyphenylene sulfide, polyvinyl chloride, ABS (acrylonitrile butadiene styrene) resin obtained by copolymerization of acrylonitrile, butadiene, and styrene, and AS (acrylonitrile styrene) resin obtained by copolymerization of acrylonitrile and styrene.
  • the thermosetting resin include phenol resin, epoxy resin, melamine resin, urea resin, unsaturated polyester, diallyl phthalate resin, urethane resin, and silicone resin.
  • resin also includes rubber and elastomer.
  • examples of rubber from the viewpoint of being able to produce a radio wave absorber that has good mixability with magnetic particles and is superior in durability, weather resistance, and impact resistance, examples of rubber that can be used include butadiene rubber, isoprene rubber, chloroprene rubber, halogenated butyl rubber, fluororubber, urethane rubber, acrylic rubber (abbreviated as ACM) obtained by copolymerizing acrylic esters (e.g., ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate) with other monomers, ethylene-propylene rubber obtained by coordination polymerization of ethylene and propylene using a Ziegler catalyst, butyl rubber (abbreviated as IIR) obtained by copolymerization of isobutylene and isoprene, styrene butadiene rubber (abbreviated as SBR) obtained by copolymerization of butadiene and styrene, acryl
  • the composition may contain various additives such as vulcanizing agents, vulcanization assistants, softeners, and plasticizers in addition to rubber.
  • vulcanizing agents include sulfur, organic sulfur compounds, and metal oxides.
  • thermoplastic elastomers examples include thermoplastic elastomers (TPE).
  • thermoplastic elastomers examples include olefin-based thermoplastic elastomers (TPO), styrene-based thermoplastic elastomers (TPS), amide-based thermoplastic elastomers (TPA), and polyester-based thermoplastic elastomers (TPC).
  • the wave absorber obtained by molding the above composition and the above pellet mixture may contain only one type of resin, or may contain two or more types of resin.
  • the volume content of the resin in the composition of the pellet 0 is not particularly limited, and can be, for example, 65 vol. % or more and 100 vol. % or less.
  • the volume content of the resin in the composition of pellet 1 and the radio wave absorber is not particularly limited, and can be, for example, 65 volume % or more, 65 volume % or more and 92 volume % or less, or 65 volume % or more and 85 volume % or less.
  • the volume content refers to the total volume content of the two or more types of resin. This also applies to the volume contents of other components.
  • the radio wave absorber obtained by molding the above composition and the above pellet mixture may or may not contain one or more additives at any ratio.
  • additives include antioxidants, light stabilizers, dispersants, dispersion aids, antifungal agents, antistatic agents, plasticizers, impact strength improvers, crystal nucleating agents, lubricants, surfactants, pigments, dyes, fillers, release agents (fatty acids, fatty acid metal salts, oxyfatty acids, fatty acid esters, partially saponified aliphatic esters, paraffins, low molecular weight polyolefins, fatty acid amides, alkylene bis fatty acid amides, aliphatic ketones, fatty acid lower alcohol esters, fatty acid polyhydric alcohol esters, fatty acid polyglycol esters, modified silicones, etc.), processing aids, antifogging agents, drip prevention agents, antibacterial agents, etc.
  • the additives may be ones in which one component plays two or more functions.
  • Various additives can be
  • the preferred additives can include antioxidants.
  • the antioxidant is not particularly limited, and any known antioxidant can be used. Examples of antioxidants are described in, for example, "Comprehensive Technology of Polymer Stabilization - Mechanism and Application Development -" edited by Yasukazu Ohkatsu, published by CMC Co., Ltd. The description is incorporated herein by reference. Examples of the types of antioxidants include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. As the antioxidant, it is preferable to use a phenol-based antioxidant and/or an amine-based antioxidant in combination with a phosphorus-based antioxidant and/or a sulfur-based antioxidant.
  • Phenol-based antioxidants include ADEKA's ADK STAB AO-20, ADK STAB AO-30, ADK STAB AO-40, ADK STAB AO-50, ADK STAB AO-60, ADK STAB AO-80, and ADK STAB AO-330, and BASF Japan's IRGANOX 1010, IRGANOX 1035, IRGANOX 1076, IRGANOX 1098, IRGANOX 1135, IRGANOX 1330, IRGANOX 1726, IRGANOX 245, IRGANOX 259, IRGANOX 3114, and IRGANOX 565. Please note that both "ADK STAB" and "IRGANOX" are registered trademarks.
  • amine-based antioxidant examples include Sanol LS-770, Sanol LS-765, and Sanol LS-2626 from Sankyo Lifetech Co., Ltd., Adeka STAB LA-77, Adeka STAB LA-57, Adeka STAB LA-52, Adeka STAB LA-62, Adeka STAB LA-63, Adeka STAB LA-67, Adeka STAB LA-68, and Adeka STAB LA-72 from ADEKA Corporation, and TINUVIN 123, TINUVIN 144, TINUVIN 622, TINUVIN 765, and TINUVIN 944 from BASF Japan Ltd. Both "ADK STAB" and "TINUVIN” are registered trademarks.
  • an amine compound capable of quenching radicals can also be used.
  • examples of such amine compounds include polyethylene glycol bis-TEMPO (Sigma-Aldrich), sebacate bis-TEMPO, etc.
  • TEMPO is an abbreviation for tetramethylpiperidine-1-oxyl.
  • phosphorus-based antioxidants examples include Adeka STAB PEP-8, Adeka STAB PEP-36, Adeka STAB HP-10, and Adeka STAB 2112 from ADEKA Corporation, and IRGAFOS 168 from BASF Japan. Note that both "Adeka STAB” and “IRGAFOS” are registered trademarks.
  • Sulfur-based antioxidants include Adeka STAB AO-412S and Adeka STAB AO-503S from ADEKA. Note that the above “Adeka STAB” is a registered trademark.
  • the phenol-based antioxidant is preferably one or more selected from the group consisting of ADK STAB AO-20, ADK STAB AO-60, ADK STAB AO-80, and IRGANOX 1010
  • the amine-based antioxidant is preferably ADK STAB LA-52
  • the phosphorus-based antioxidant is preferably ADK STAB PEP-36
  • the sulfur-based antioxidant is preferably ADK STAB AO-412S.
  • the wave absorber obtained by molding the composition and the pellet mixture contains an antioxidant, it may contain only one type of antioxidant or may contain two or more types of antioxidant.
  • the content of the antioxidant in the composition or radio wave absorber is not particularly limited, and from the viewpoint of both preventing decomposition of the resin and preventing the antioxidant from bleeding, for example, it is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of resin.
  • preferred additives can include light stabilizers.
  • light stabilizers include HALS (i.e., hindered amine light stabilizers), ultraviolet light absorbers, singlet oxygen quenchers, and the like.
  • HALS i.e., hindered amine light stabilizers
  • ultraviolet light absorbers i.e., ultraviolet light absorbers
  • singlet oxygen quenchers i.e., singlet oxygen quenchers
  • the HALS may be a high molecular weight HALS, a low molecular weight HALS, or a combination of high molecular weight and low molecular weight HALS.
  • the radio wave absorber obtained by molding the above composition and the above pellet mixture contains a light stabilizer, it may contain only one type of light stabilizer or may contain two or more types of light stabilizers.
  • High molecular weight HALS refers to a hindered amine light stabilizer having a weight average molecular weight of more than 1,000.
  • high molecular weight HALS include oligomer type HALS such as poly[6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino] and polycondensation product of dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine.
  • commercially available high molecular weight HALS include CHIMASSORB 944LD and TINUVIN 622LD manufactured by BASF Japan Ltd. Both "CHIMASSORB” and "TINUVIN” are registered trademarks.
  • the weight average molecular weight (Mw) in the present invention and this specification is a value measured by gel permeation chromatography (GPC).
  • GPC gel permeation chromatography
  • HLC registered trademark
  • 8220GPC manufactured by Tosoh Corporation
  • TSKgel registered trademark
  • Super HZM-M 4.6 mm ID x 15 cm, manufactured by Tosoh Corporation
  • Super HZ4000 4.6 mm ID x 15 cm, manufactured by Tosoh Corporation
  • Super HZ3000 4.6 mm ID x 15 cm, manufactured by Tosoh Corporation
  • Super HZ2000 4.6 mm ID x 15 cm, manufactured by Tosoh Corporation
  • THF tetrahydrofuran
  • the measurement conditions can be a sample concentration of 0.2 mass%, a flow rate of 0.35 mL/min, a sample injection amount of 10 ⁇ L, and a measurement temperature of 40° C., and a refractive index (RI) detector can be used as the detector.
  • the calibration curve can be prepared using standard samples "TSK standard, polystyrene", “F-40”, “F-20”, “F-4”, “F-1”, “A-5000”, “A-2500”, and "A-1000” manufactured by Tosoh Corporation.
  • the content of the high molecular weight HALS in the composition and the wave absorber is not particularly limited, and is preferably, for example, 0.2 mass % to 10 mass % relative to the total mass of the composition or the wave absorber. It is preferable from the viewpoint of improving weather resistance that the content of high molecular weight HALS in the radio wave absorber is 0.2 mass % or more relative to the total mass of the radio wave absorber.
  • the content of high molecular weight HALS in the radio wave absorber is 10 mass % or less relative to the total mass of the radio wave absorber, there is a tendency that the decrease in mechanical strength and the occurrence of blooming can be suppressed.
  • low molecular weight HALS refers to a hindered amine light stabilizer having a molecular weight of 1000 or less (preferably 900 or less, more preferably 600 to 900).
  • Low molecular weight HALS include tris(2,2,6,6-tetramethyl-4-piperidyl)benzene-1,3,5-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)-2-acetoxypropane-1,2,3-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)-2-hydroxypropane-1,2,3-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)triazine-2,4,6-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidyl)bran tetrakis(2,2,6,6-tetramethyl-4-piperidyl)propane-1,1,2,3-tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)1,2,3,4-butane tetracarboxylate, tetra
  • HALS products examples include ADK STAB LA-57 and ADK STAB LA-52 from ADEKA Corporation, and TINUVIN 144 from BASF Japan Ltd. Both "ADK STAB” and “TINUVIN” are registered trademarks.
  • the content of the low molecular weight HALS in the composition and the wave absorber is not particularly limited, and is preferably, for example, 0.2 mass % to 10 mass % relative to the total mass of the composition or the wave absorber. It is preferable from the viewpoint of improving weather resistance that the content of low molecular weight HALS in the radio wave absorber is 0.2 mass % or more relative to the total mass of the radio wave absorber.
  • the content of low molecular weight HALS in the radio wave absorber is 10 mass % or less based on the total mass of the radio wave absorber, there is a tendency that the decrease in mechanical strength and the occurrence of blooming can be suppressed.
  • Ultraviolet absorbers include 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-methyl-phenyl)benzotriazole, 2-(2'-hydroxy-5'-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-amylphenyl)benzotriazole, 2-[2'-hydroxy-3 '-(3'',4'',5'',6''-tetrahydro-phthalimidomethyl)-5'-methylphenyl]benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-[2-hydroxy-3,5-bis( ⁇ , ⁇ -di
  • Examples of commercially available ultraviolet absorbents include TINUVIN 320, TINUVIN 328, TINUVIN 234, TINUVIN 1577, TINUVIN 622, and IRGANOX series from BASF Japan, ADK STAB LA31 from ADEKA, and SEESORB 102, SEESORB 103, and SEESORB 501 from Shipro Chemical Co., Ltd.
  • TINUVIN IRGANOX
  • ADK STAB SEESORB 103
  • SEESORB 501 from Shipro Chemical Co., Ltd.
  • the above-mentioned "TINUVIN”, “IRGANOX”, “ADK STAB”, and “SEESORB” are all registered trademarks.
  • the content of the ultraviolet absorbing agent in the composition and the wave absorber is not particularly limited and is, for example, preferably 0.2 mass % to 10 mass % relative to the total mass of the composition or the wave absorber. It is preferable from the viewpoint of improving weather resistance that the content of the ultraviolet absorbing agent in the radio wave absorber is 0.2 mass % or more relative to the total mass of the radio wave absorber.
  • the content of the ultraviolet absorbing agent in the radio wave absorber is 10 mass % or less with respect to the total mass of the radio wave absorber, there is a tendency that the decrease in mechanical strength and the occurrence of blooming can be suppressed.
  • the content of the singlet oxygen quencher in the composition and the radio wave absorber is not particularly limited and is, for example, preferably 0.2 mass % to 10 mass % with respect to the total mass of the composition or the radio wave absorber. It is preferable from the viewpoint of improving weather resistance that the content of the singlet oxygen quencher in the radio wave absorber is 0.2 mass % or more relative to the total mass of the radio wave absorber.
  • the content of the singlet oxygen quencher in the radio wave absorber is 10 mass % or less with respect to the total mass of the radio wave absorber, there is a tendency that a decrease in mechanical strength and the occurrence of blooming can be suppressed.
  • the composition may or may not contain a solvent.
  • the solvent is not particularly limited, and examples thereof include water, an organic solvent, and a mixed solvent of water and an organic solvent.
  • the organic solvent include alcohols such as methanol, ethanol, n-propanol, i-propanol, and methoxypropanol, ketones such as acetone, methyl ethyl ketone, and cyclohexanone, tetrahydrofuran, acetonitrile, ethyl acetate, and toluene.
  • the solvent is preferably a ketone, and more preferably cyclohexanone.
  • the content of the solvent in the composition is not particularly limited and may be appropriately determined.
  • the method for producing pellets (pellet 0 and pellet 1) from the above composition is not particularly limited.
  • the composition containing the above various components can be kneaded while being heated to form a kneaded mixture, and then the kneaded mixture can be cut to obtain pellets.
  • a commercially available pelletizer or a pelletizer of a known configuration can be used to cut the kneaded mixture.
  • commercially available resin pellets can be used as pellet 0, which is a pellet of a composition that contains at least a resin.
  • the mixing ratio of pellet 0 and pellet 1 in the pellet mixture is not particularly limited.
  • pellet 0 and pellet 1 can be mixed to prepare a pellet mixture so that the volume content of the particles in the radio wave absorber to be molded is a desired value.
  • the total amount of pellet 0 and pellet 1 in the pellet mixture is 100 parts by volume, and the content of pellet 1 can be, for example, 10 parts by volume or more and 90 parts by volume or less.
  • the above pellet mixture can be prepared by mixing pellet 0 and pellet 1.
  • the above pellet mixture may be distributed on the market in the form of a pellet mixture in which pellet 0 and pellet 1 are mixed, or pellet 0 and pellet 1 may be packaged separately and distributed on the market, and then mixed when used to mold a molded product to become a pellet mixture.
  • pellet 0 and pellet 1 can be mixed by a known method such as the so-called dry blend method.
  • Radio wave absorber and method of manufacturing the radio wave absorber One aspect of the present invention relates to a radio wave absorber which is a molded article obtained by molding the above-mentioned pellet mixture.
  • Another aspect of the present invention relates to a method for producing a radio wave absorber, which includes molding the above-mentioned pellet mixture into a molded product.
  • the molding method for molding a molded article from pellets is well known.
  • the above pellet mixture can be molded into a molded article by a known molding method such as injection molding or extrusion molding.
  • FIG. 2 is a schematic diagram of an injection molding machine.
  • the injection molding machine 1 shown in Figure 2 is equipped with a heating cylinder 3 having a nozzle 2 at its tip, and an injection screw 4 is disposed within the heating cylinder 3.
  • a heater 5 is attached to the outer periphery of the heating cylinder 3, and a hopper 6 that supplies pellets 7 to the injection screw 4 is attached to the opposite end of the nozzle 2.
  • the tip of the nozzle 2 is connected to the gate 13 of the fixed mold 11 and the movable mold 12 that form a cavity 10 inside.
  • pellets 0 and 1 can be supplied to the injection screw 4 without significantly shifting the timing at which pellets 0 and 1 fall from hopper 6 to the injection screw 4.
  • the pellets 7 fed from hopper 6 are subjected to plasticization operations, including transfer, compression, kneading, melting, and metering of the resin, by the rotating injection screw 4 and heater 5.
  • the molten material around the injection screw 4 is then moved toward the nozzle 2 while the moving speed is controlled by the servo motor cylinder set 9, and the molten material discharged from the nozzle 2 at a constant speed fills the cavity 10, where it is cooled while being held at the set holding pressure for a specified time, forming a molded product.
  • the shape of the radio wave absorber which is a molded product obtained by molding the pellet mixture, is not particularly limited, and can be any shape, such as a plate or a line. "Plate” includes sheet and film shapes. A plate-shaped radio wave absorber can also be called a radio wave absorbing plate, a radio wave absorbing sheet, a radio wave absorbing film, etc.
  • the radio wave absorber may be a radio wave absorber of a single composition (e.g., a single-layer radio wave absorbing plate), or a combination of two or more parts with different compositions (e.g., a laminate).
  • the radio wave absorber may have a planar shape, a three-dimensional shape, or a combination of a part having a planar shape and a part having a three-dimensional shape.
  • planar shapes include a sheet shape, a film shape, etc.
  • three-dimensional shapes include a tube shape (cylindrical shape, square tube shape, etc.), a horn shape, a box shape (e.g., at least one of the faces is open), etc.
  • the thickness of the radio wave absorber is preferably 20 mm or less, more preferably 10 mm or less, and even more preferably 5 mm or less. From the viewpoint of mechanical properties, the thickness is preferably 1 mm or more, and more preferably 2 mm or more.
  • the thickness of the radio wave absorber refers to the total thickness of the radio wave absorbers that make up the laminate.
  • the thickness of the radio wave absorber is a value measured using a digital length measuring device, and specifically, it is the arithmetic average of measurements taken at nine randomly selected points.
  • the radio wave absorber can be incorporated into various articles to which it is desired to impart radio wave absorbing properties.
  • a plate-shaped radio wave absorber can be incorporated into an article in any shape, either as is or by curving any part.
  • the pellet mixture can also be molded into a desired shape by injection molding or the like and incorporated into an article.
  • automotive radar which has been attracting attention in recent years, is a radar that uses radio waves in the millimeter wave frequency band.
  • Millimeter waves are electromagnetic waves with frequencies between 30.0 GHz and 300.0 GHz.
  • the radio wave absorber described above is suitable as a radio wave absorber to be incorporated into the front side (the side where radio waves enter from outside) of a radio wave transmitting/receiving unit in an automotive radar, for example, to reduce the side lobes of the millimeter wave radar for use in vehicles.
  • the radio wave absorber can also be incorporated into radio wave absorbing articles used in wireless technology fields such as motion sensors.
  • the radio wave absorber is suitable as a radio wave absorber for improving recognition accuracy by removing unnecessary radio waves in wireless devices such as mobile phone internal sensors and biometric sensors.
  • Such a radio wave absorber can be preferably used, for example, in a 55.0 to 66.0 GHz band radio wave absorbing article.
  • a radio wave absorbing article is an article that has radio wave absorption properties for radio waves of one or more frequencies, and the radio wave absorption properties can be achieved by incorporating a radio wave absorber as at least a part of this article.
  • a 55.0 to 66.0 GHz band radio wave absorbing article is an article that has radio wave absorption properties for radio waves of one or more frequencies in the 55.0 to 66.0 GHz frequency band.
  • Examples of such articles include the various wireless devices described above.
  • the bandwidth may be broadband.
  • a 60 GHz band radar may be used with a bandwidth of 7.0 GHz in the range of 57.0 to 64.0 GHz.
  • a radio wave absorber capable of supporting broadband operation may be produced by mixing multiple types of particles selected from the group consisting of magnetic particles and dielectric particles, and/or a radio wave absorber capable of supporting broadband operation may be produced by mixing multiple types of radio wave absorbers.
  • Radio wave absorbing articles One aspect of the present invention relates to a radio wave absorbing article including the radio wave absorber.
  • a specific example of the radio wave absorbing article is an in-vehicle radar. Specific examples include wireless devices such as internal sensors of mobile phones and biometric sensors.
  • the radio wave absorbing article can be a radio wave absorbing article for the 55.0 GHz to 66.0 GHz band.
  • the radio wave absorbing article may include the radio wave absorber according to one aspect of the present invention, and other configurations are not particularly limited, and known techniques related to radio wave absorbing articles can be applied.
  • the obtained raw material mixture was milled three times for 30 seconds using a mill (Osaka Chemical Absolute 3) with the variable speed dial set to "maximum" to obtain a powder.
  • Strontium chloride ( SrCl2 ) was dissolved in 100 mL of water to prepare a 10% by mass aqueous solution of strontium chloride, which was added to the obtained powder and ultrasonically dispersed for 10 minutes, then dried in a heating furnace at an internal temperature of 95°C for 12 hours, and further milled with the mill to obtain a pulverized product.
  • the resulting pulverized material was then fired in a heating furnace at an internal temperature of 1250°C for 4 hours, and the fired material was then ground three times for 30 seconds in the mill with the variable dial set to "5".
  • the material was then washed by ultrasonic treatment until the electrical conductivity was 30 ⁇ S (microsiemens) or less, and then dried in a heating furnace at an internal temperature of 95°C for 12 hours to obtain magnetic particles.
  • the magnetic particles thus obtained were then subjected to an annealing treatment in a heating furnace at an internal temperature of 1000° C. for 2 hours. Thus, magnetic particles 1 were obtained.
  • the crystal structure of the magnetic material constituting the magnetic particle 1 was confirmed by X-ray diffraction analysis.
  • the measurement device used was a powder X-ray diffraction device, X'Pert Pro, manufactured by PANalytical Corporation.
  • the measurement conditions are as follows: - Measurement conditions - X-ray source: CuK ⁇ ray [wavelength: 1.54 ⁇ (0.154 nm), output: 40 mA, 45 kV] Scan range: 20° ⁇ 2 ⁇ 70° Scan interval: 0.05° Scan speed: 0.33°/min
  • magnetic particle 1 has a magnetoplumbite crystal structure and is a powder of single-phase magnetoplumbite hexagonal ferrite that does not contain any crystal structure other than magnetoplumbite.
  • composition of the magnetic material constituting the magnetic particles 1 was confirmed by high-frequency inductively coupled plasma optical emission spectrometry. Specifically, the confirmation was performed by the following method. A container (beaker) containing 12 mg of magnetic particles and 10 mL of hydrochloric acid aqueous solution with a concentration of 4 mol/L was held on a hot plate set at 120°C for 3 hours to obtain a solution. After adding 30 mL of pure water to the obtained solution, it was filtered using a membrane filter with a filter pore size of 0.1 ⁇ m. Elemental analysis of the filtrate thus obtained was performed using a high-frequency inductively coupled plasma optical emission spectrometer [Shimadzu Corporation ICPS-8100].
  • the content of each atom relative to 100 atomic % of iron atoms was calculated. Then, based on the obtained content, the composition of the magnetic material was confirmed. As a result, it was confirmed that the composition of the magnetic particle 1 was a composition in which A in formula 1 was Sr and x was 1.65.
  • resin pellet A Polypropylene resin (Novatec PP MA3H manufactured by Japan Polypropylene Corporation) was kneaded using a twin-screw kneader and then cut using a pelletizer to obtain resin pellets A. Resin pellets A are resin pellets that do not contain magnetic particles.
  • a pellet mixture was prepared by dry blending resin pellet A into magnetic particle-containing resin pellet 1 (volume content of magnetic particle 1: 30 volume%) so that the volume content of magnetic particle 1 in the pellet mixture was 15 volume%. Specifically, the above two types of pellets were weighed, placed in a vinyl bag, and mixed by shaking for about 5 minutes. The amount of each mixture (batch) was 2 to 3 kg. In the prepared pellet mixture, the total content of resin pellet A and magnetic particle-containing resin pellet 1 was 100 volume parts, and the content of magnetic particle-containing resin pellet 1 was 70 volume parts.
  • FIG. 3 shows a schematic diagram of the pellet supply section of the injection molding machine used to produce the injection molded product.
  • the pellet supply unit shown in Fig. 3 is composed of a stainless steel hopper (diameter 160 mm, taper angle 35°, capacity approximately 2.5 kg), a glass tube (diameter 50 mm) and an iron tube (diameter 60 mm), and has a total length of approximately 600 mm and a total capacity of approximately 3.3 kg.
  • Magnetic particle-containing resin pellets 2 were prepared by the method described for preparing the magnetic particle-containing resin pellets 1, except that the polypropylene resin was changed to 99% by mass of polypropylene resin and 1% by mass of olefin-based thermoplastic elastomer (hereinafter referred to as "TPO resin") (LVG9541S manufactured by Riken Technos Corporation) relative to 100% by mass of the total resin. Except for the above points, the preparation of a pellet mixture and the production of an injection-molded article were carried out in the same manner as described for Comparative Example 1.
  • TPO resin olefin-based thermoplastic elastomer
  • Magnetic particle-containing resin pellets 3 were prepared by the same method as described for preparing magnetic particle-containing resin pellets 1, except that the polypropylene resin was changed to 98% by mass of polypropylene resin and 2% by mass of TPO resin (LVG9541S manufactured by Riken Technos Corporation) relative to 100% by mass of the total resin. Except for the above points, the preparation of a pellet mixture and the production of an injection-molded article were carried out in the same manner as described for Comparative Example 1.
  • Magnetic particle-containing resin pellets 4 were prepared by the same method as described for preparing magnetic particle-containing resin pellets 1, except that the polypropylene resin was changed to 97% by mass of polypropylene resin and 3% by mass of TPO resin (LVG9541S manufactured by Riken Technos Corporation) relative to 100% by mass of the total resin. Except for the above points, the preparation of a pellet mixture and the production of an injection-molded article were carried out in the same manner as described for Comparative Example 1.
  • Magnetic particle-containing resin pellets 5 were prepared by the method described for preparing magnetic particle-containing resin pellets 1, except that in preparing the magnetic particle-containing resin pellets, the polypropylene resin was changed to 95% by mass of polypropylene resin and 5% by mass of TPO resin (LVG9541S manufactured by Riken Technos Corporation) relative to 100% by mass of the total resin. Except for the above points, the preparation of a pellet mixture and the production of an injection-molded article were carried out in the same manner as described for Comparative Example 1.
  • Magnetic particle-containing resin pellets 6 were prepared by the method described for preparing magnetic particle-containing resin pellets 1, except that in preparing the magnetic particle-containing resin pellets, the polypropylene resin was changed to 90% by mass of polypropylene resin and 10% by mass of TPO resin (LVG9541S manufactured by Riken Technos Corporation) relative to 100% by mass of the total resin. Except for the above points, the preparation of a pellet mixture and the production of an injection-molded article were carried out in the same manner as described for Comparative Example 1.
  • the arithmetic average of the Ra values obtained by five measurements at each measurement position (hence three measurement values per measurement position, and a total of nine measurement values for the three measurement positions) excluding the minimum and maximum values is adopted as the arithmetic average roughness Ra of the surface to be measured.
  • the specific gravity of each of the resin pellets A and the magnetic particle-containing resin pellets 1 to 6 was determined by the underwater displacement method described in JIS K 7112-1: 2023.
  • the specific gravity of the resin pellets A was 0.9, and the specific gravity of each of the magnetic particle-containing resin pellets 1 to 6 was 2.1.
  • the transmittance (unit: %) of each of the above flat plates was measured by the following method.
  • a vector network analyzer product name: N5225B
  • a horn antenna product name: RH12S23
  • the S-parameters were measured by the free space method with an incident angle of 0°, a sweep frequency of 60 GHz to 90 GHz, and one of the flat surfaces of each of the above-mentioned plates facing the incident side, and the S-parameter S21 at a frequency of 76.5 GHz was taken as the transmittance.
  • the maximum value, minimum value, arithmetic mean and standard deviation ⁇ of S21 (transmittance) determined for each of the 20 flat plates are shown in Table 1.
  • One aspect of the present invention is useful in the technical field of performing various types of automatic driving control, such as automatic driving control of automobiles, and in the wireless technical field of motion sensors, etc.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Dispersion Chemistry (AREA)
  • Power Engineering (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Manufacturing & Machinery (AREA)
  • Mechanical Engineering (AREA)
  • Shielding Devices Or Components To Electric Or Magnetic Fields (AREA)
PCT/JP2024/008283 2023-03-23 2024-03-05 ペレット混合物、電波吸収体、電波吸収物品および電波吸収体の製造方法 Ceased WO2024195518A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
JP2025508292A JPWO2024195518A1 (cg-RX-API-DMAC7.html) 2023-03-23 2024-03-05
EP24774661.3A EP4686333A4 (en) 2023-03-23 2024-03-05 MIXTURE OF PASTILLES, RADIO WAVE ABSORBER, RADIO WAVE ABSORBENT ARTICLE AND METHOD FOR MANUFACTURED RADIO WAVE ABSORBERS
US19/335,155 US20260018323A1 (en) 2023-03-23 2025-09-22 Pellet mixture, radio wave absorber, radio wave absorbing article, and method for producing radio wave absorber

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2023-046125 2023-03-23
JP2023046125 2023-03-23

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US19/335,155 Continuation US20260018323A1 (en) 2023-03-23 2025-09-22 Pellet mixture, radio wave absorber, radio wave absorbing article, and method for producing radio wave absorber

Publications (1)

Publication Number Publication Date
WO2024195518A1 true WO2024195518A1 (ja) 2024-09-26

Family

ID=92841968

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2024/008283 Ceased WO2024195518A1 (ja) 2023-03-23 2024-03-05 ペレット混合物、電波吸収体、電波吸収物品および電波吸収体の製造方法

Country Status (4)

Country Link
US (1) US20260018323A1 (cg-RX-API-DMAC7.html)
EP (1) EP4686333A4 (cg-RX-API-DMAC7.html)
JP (1) JPWO2024195518A1 (cg-RX-API-DMAC7.html)
WO (1) WO2024195518A1 (cg-RX-API-DMAC7.html)

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH0568325B2 (cg-RX-API-DMAC7.html) * 1984-10-23 1993-09-28 Toshiba Chem Prod
JP2008282862A (ja) * 2007-05-08 2008-11-20 Kokoku Intech Co Ltd 電波吸収体用組成物、電波吸収体及び電波吸収体の製造方法
JP4674380B2 (ja) * 2006-03-16 2011-04-20 Dowaエレクトロニクス株式会社 電波吸収体用磁性粉体および製造法並びに電波吸収体
WO2020044649A1 (ja) 2018-08-28 2020-03-05 富士フイルム株式会社 マグネトプランバイト型六方晶フェライトの粉体の製造方法及び電波吸収体の製造方法
CN210759047U (zh) * 2019-10-11 2020-06-16 苏州市金龙植绒滴塑工艺厂 一种高效熔融的注塑机螺杆

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP3887031B2 (ja) * 1995-07-13 2007-02-28 株式会社プライムポリマー 熱可塑性樹脂成形材料
JP7175805B2 (ja) * 2019-03-14 2022-11-21 マクセル株式会社 電磁ホーンアンテナ、および、指向性制御システム

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH0568325B2 (cg-RX-API-DMAC7.html) * 1984-10-23 1993-09-28 Toshiba Chem Prod
JP4674380B2 (ja) * 2006-03-16 2011-04-20 Dowaエレクトロニクス株式会社 電波吸収体用磁性粉体および製造法並びに電波吸収体
JP2008282862A (ja) * 2007-05-08 2008-11-20 Kokoku Intech Co Ltd 電波吸収体用組成物、電波吸収体及び電波吸収体の製造方法
WO2020044649A1 (ja) 2018-08-28 2020-03-05 富士フイルム株式会社 マグネトプランバイト型六方晶フェライトの粉体の製造方法及び電波吸収体の製造方法
CN210759047U (zh) * 2019-10-11 2020-06-16 苏州市金龙植绒滴塑工艺厂 一种高效熔融的注塑机螺杆

Non-Patent Citations (2)

* Cited by examiner, † Cited by third party
Title
See also references of EP4686333A1
YASUKAZU OKATSU: "Comprehensive Technology for Polymer Stabilization - Mechanism and Application Development", CMC PUBLISHING CO., LTD.

Also Published As

Publication number Publication date
EP4686333A1 (en) 2026-01-28
JPWO2024195518A1 (cg-RX-API-DMAC7.html) 2024-09-26
US20260018323A1 (en) 2026-01-15
EP4686333A4 (en) 2026-06-24

Similar Documents

Publication Publication Date Title
JP7762252B2 (ja) 電波吸収体および電波吸収性組成物
KR102538732B1 (ko) 마그네토플럼바이트형 육방정 페라이트 분체, 전파 흡수체, 및 마그네토플럼바이트형 육방정 페라이트 분체의 공명 주파수를 제어하는 방법
KR102602993B1 (ko) 전파 흡수체
JP7702432B2 (ja) 電波吸収体用磁性粉体およびその製造方法、電波吸収体、電波吸収物品ならびに電波吸収性組成物
KR102542810B1 (ko) 전파 흡수체
US20240380122A1 (en) Radio wave absorber and radio wave absorbing article
CN113812043A (zh) 电波吸收体
US20260018323A1 (en) Pellet mixture, radio wave absorber, radio wave absorbing article, and method for producing radio wave absorber
EP4561286A1 (en) Method for manufacturing radio wave absorber, radio wave absorber, and radio-wave-absorbing article
WO2025089326A1 (ja) 電波吸収体を備えた物品および電波吸収体
WO2026042695A1 (ja) 電波吸収体および電波吸収体を含む物品
WO2025225474A1 (ja) 電波吸収体および電波吸収体を含む物品
JP2024000812A (ja) 電磁波吸収材
CN116830219A (zh) 电波吸收体用磁性粉体及其制造方法、电波吸收体、电波吸收物品以及电波吸收性组合物

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 24774661

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2025508292

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025508292

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 2024774661

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2024774661

Country of ref document: EP

Effective date: 20251023

ENP Entry into the national phase

Ref document number: 2024774661

Country of ref document: EP

Effective date: 20251023

ENP Entry into the national phase

Ref document number: 2024774661

Country of ref document: EP

Effective date: 20251023

ENP Entry into the national phase

Ref document number: 2024774661

Country of ref document: EP

Effective date: 20251023

ENP Entry into the national phase

Ref document number: 2024774661

Country of ref document: EP

Effective date: 20251023

ENP Entry into the national phase

Ref document number: 2024774661

Country of ref document: EP

Effective date: 20251023