WO2023276649A1 - 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法 - Google Patents

電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法 Download PDF

Info

Publication number
WO2023276649A1
WO2023276649A1 PCT/JP2022/023760 JP2022023760W WO2023276649A1 WO 2023276649 A1 WO2023276649 A1 WO 2023276649A1 JP 2022023760 W JP2022023760 W JP 2022023760W WO 2023276649 A1 WO2023276649 A1 WO 2023276649A1
Authority
WO
WIPO (PCT)
Prior art keywords
phase
carbon black
less
charging roll
elastic layer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/023760
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
仁宏 齋藤
新平 宮川
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Riko Co Ltd
Original Assignee
Sumitomo Riko Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Riko Co Ltd filed Critical Sumitomo Riko Co Ltd
Priority to CN202280028015.1A priority Critical patent/CN117120939B/zh
Publication of WO2023276649A1 publication Critical patent/WO2023276649A1/ja
Priority to US18/500,102 priority patent/US12686761B2/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L9/00—Compositions of homopolymers or copolymers of conjugated diene hydrocarbons
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/02—Elements
    • C08K3/04—Carbon
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L71/00—Compositions of polyethers obtained by reactions forming an ether link in the main chain; Compositions of derivatives of such polymers
    • C08L71/02—Polyalkylene oxides
    • C08L71/03—Polyepihalohydrins
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L9/00—Compositions of homopolymers or copolymers of conjugated diene hydrocarbons
    • C08L9/02—Copolymers with acrylonitrile
    • F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
    • F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
    • F16C—SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS
    • F16C13/00—Rolls, drums, discs, or the like; Bearings or mountings therefor
    • G—PHYSICS
    • G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
    • G03G—ELECTROGRAPHY; ELECTROPHOTOGRAPHY; MAGNETOGRAPHY
    • G03G15/00—Apparatus for electrographic processes using a charge pattern
    • G03G15/02—Apparatus for electrographic processes using a charge pattern for laying down a uniform charge, e.g. for sensitising; Corona discharge devices
    • G—PHYSICS
    • G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
    • G03G—ELECTROGRAPHY; ELECTROPHOTOGRAPHY; MAGNETOGRAPHY
    • G03G15/00—Apparatus for electrographic processes using a charge pattern
    • G03G15/02—Apparatus for electrographic processes using a charge pattern for laying down a uniform charge, e.g. for sensitising; Corona discharge devices
    • G03G15/0208—Apparatus for electrographic processes using a charge pattern for laying down a uniform charge, e.g. for sensitising; Corona discharge devices by contact, friction or induction, e.g. liquid charging apparatus
    • G03G15/0216—Apparatus for electrographic processes using a charge pattern for laying down a uniform charge, e.g. for sensitising; Corona discharge devices by contact, friction or induction, e.g. liquid charging apparatus by bringing a charging member into contact with the member to be charged, e.g. roller, brush chargers
    • G03G15/0233—Structure, details of the charging member, e.g. chemical composition, surface properties
    • G—PHYSICS
    • G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
    • G03G—ELECTROGRAPHY; ELECTROPHOTOGRAPHY; MAGNETOGRAPHY
    • G03G15/00—Apparatus for electrographic processes using a charge pattern
    • G03G15/06—Apparatus for electrographic processes using a charge pattern for developing
    • G03G15/08—Apparatus for electrographic processes using a charge pattern for developing using a solid developer, e.g. powder developer
    • G03G15/0806—Apparatus for electrographic processes using a charge pattern for developing using a solid developer, e.g. powder developer on a donor element, e.g. belt, roller
    • G03G15/0818—Apparatus for electrographic processes using a charge pattern for developing using a solid developer, e.g. powder developer on a donor element, e.g. belt, roller characterised by the structure of the donor member, e.g. surface properties

Definitions

  • the present invention relates to a charging roll for electrophotographic equipment, which is preferably used in electrophotographic equipment such as copiers, printers and facsimiles employing an electrophotographic system, and a method for manufacturing the charging roll for electrophotographic equipment.
  • the problem to be solved by the present invention is to provide a charging roll for an electrophotographic machine and a method for producing the charging roll for an electrophotographic machine, in which the charge attenuation from the roll surface due to local uneven resistance is suppressed and good images can be obtained. to provide.
  • a charging roll for electrophotographic equipment comprises a shaft, an elastic layer formed on the outer peripheral surface of the shaft, and a surface layer formed on the outer peripheral surface of the elastic layer,
  • the elastic layer includes a high-resistance first phase having a surface resistance of 1.6 ⁇ 10 14 ⁇ cm or more and 8.8 ⁇ 10 15 ⁇ cm or less, and a surface resistance of 1.3 ⁇ 10 2 .
  • a second phase having a low resistance of ⁇ cm or more and 4.9 ⁇ 10 3 ⁇ cm or less, and the second phase has a DBP absorption of 115 cm 3 /100 g or more and 160 cm 3 /100 g or less.
  • Two types of carbon black, carbon black A and carbon black B having a DBP absorption of 70 cm 3 /100 g or more and 110 cm 3 /100 g or less, are contained.
  • the first phase may constitute a sea phase
  • the second phase may constitute an island phase.
  • the specific surface area of the carbon black A is preferably 25 m 2 /g or more and 75 m 2 /g or less
  • the specific surface area of the carbon black B is preferably 140 m 2 /g or more and 180 m 2 /g or less.
  • the average particle size of the carbon black A is preferably 35 nm or more and 75 nm or less
  • the average particle size of the carbon black B is preferably 20 nm or more and 30 nm or less.
  • the first phase may contain a non-polar polymer and the second phase may contain a polar polymer.
  • the non-polar polymer may be isoprene rubber or natural rubber, and the polar polymer may be nitrile rubber or hydrin rubber.
  • the first phase is preferably interposed between the second phase and the surface layer.
  • a method for manufacturing a charging roll for an electrophotographic machine according to the present invention is the above-described method for manufacturing a charging roll for an electrophotographic machine, wherein the carbon black A and the After kneading two kinds of carbon blacks, carbon black B, the polymer component constituting the first phase is kneaded.
  • a shaft, an elastic layer formed on the outer peripheral surface of the shaft, and a surface layer formed on the outer peripheral surface of the elastic layer are provided.
  • the elastic layer includes a high-resistance first phase having a surface resistance value of 1.6 ⁇ 10 14 ⁇ cm or more and 8.8 ⁇ 10 15 ⁇ cm or less, and a surface resistance value of 1.3 ⁇ and a second phase having a low resistance of 10 2 ⁇ cm or more and 4.9 ⁇ 10 3 ⁇ cm or less, and the second phase has a DBP absorption of 115 cm 3 /100 g or more and 160 cm 3 /100 g or less. and carbon black B with a DBP absorption of 70 cm 3 /100 g or more and 110 cm 3 /100 g or less. is suppressed, and a good image can be obtained.
  • the first phase constitutes a sea phase and the second phase constitutes an island phase. Resistance unevenness is absorbed more. This further suppresses charge decay from the roll surface.
  • the carbon black A When the specific surface area of the carbon black A is 25 m 2 /g or more and 75 m 2 /g or less, the carbon black A has a high resistance and tends to maintain the capacitance within a suitable range.
  • the specific surface area of the carbon black B is 140 m 2 /g or more and 180 m 2 /g or less, the carbon black B has a low resistance and is easy to maintain the resistance within a suitable range.
  • the specific surface area of the carbon black A can easily be adjusted to a suitable range, and the carbon black A can be easily made to have a high resistance.
  • the average particle size of the carbon black B is 20 nm or more and 30 nm or less, the specific surface area of the carbon black B can easily be adjusted to a suitable range, and the resistance of the carbon black B can be easily reduced.
  • the content of the carbon black A is 5 parts by mass or more and 75 parts by mass or less with respect to 100 parts by mass of the polymer component contained in the elastic layer, it is easy to maintain the capacitance within a suitable range.
  • the content of the carbon black B is 1.5 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the polymer component contained in the elastic layer, the resistance can be easily maintained within a suitable range.
  • the phase separation between the first phase and the second phase becomes good, and local resistance unevenness Attenuation of charge from the roll surface due to is easily suppressed.
  • the non-polar polymer is isoprene rubber or natural rubber, and the polar polymer is nitrile rubber or hydrin rubber, the phase separation between the first phase and the second phase is good, and the roll surface due to local uneven resistance Attenuation of electric charge from is easily suppressed.
  • the effect of blocking electric charges by the first phase is improved, and local unevenness in resistance is more absorbed. This further suppresses charge decay from the roll surface.
  • a charging roll for an electrophotographic machine According to the method of manufacturing a charging roll for an electrophotographic machine according to the present invention, it is possible to provide a charging roll for an electrophotographic machine that can suppress charge attenuation from the roll surface due to local unevenness in resistance and obtain good images. can.
  • FIG. 1 is a schematic external view (a) of a charging roll for electrophotographic equipment according to one embodiment of the present invention, and a cross-sectional view (b) taken along line AA thereof.
  • FIG. 3 is a schematic diagram showing a phase structure in an arbitrary range of 5 ⁇ m ⁇ 5 ⁇ m in the vicinity of the surface layer of the elastic layer.
  • FIG. 1 is a schematic external view (a) of a charging roll for electrophotographic equipment according to one embodiment of the present invention and a cross-sectional view (b) taken along the line AA.
  • FIG. 2 is a schematic diagram showing a phase structure in an arbitrary range of 5 ⁇ m ⁇ 5 ⁇ m near the surface layer of the elastic layer.
  • the charging roll 10 includes a shaft 12 , an elastic layer 14 formed on the outer peripheral surface of the shaft 12 , and a surface layer 16 formed on the outer peripheral surface of the elastic layer 14 .
  • the elastic layer 14 is a layer (base layer) that serves as the base of the charging roll 10 .
  • the surface layer 16 is a layer that appears on the surface of the charging roll 10 .
  • the shaft 12 is not particularly limited as long as it has conductivity. Specifically, solid bodies made of metals such as iron, stainless steel and aluminum, core metals made of hollow bodies, and the like can be exemplified. An adhesive, a primer, or the like may be applied to the surface of the shaft 12, if necessary. That is, the elastic layer 14 may be adhered to the shaft 12 via an adhesive layer (primer layer). Adhesives, primers and the like may be made conductive as necessary.
  • the elastic layer 14 includes a high resistance first phase 14a having a surface resistance of 1.6 ⁇ 10 14 ⁇ cm or more and 8.8 ⁇ 10 15 ⁇ cm or less and a surface resistance of 1.3 ⁇ 10 ⁇ cm or more. and a second phase 14b having a low resistance of 2 ⁇ cm or more and 4.9 ⁇ 10 3 ⁇ cm or less. As shown in FIG. 2, the first phase 14a and the second phase 14b exist separately from each other.
  • the first phase 14a contains one or more polymers. From the viewpoint of high resistance, the polymer of the first phase 14a is preferably a non-polar polymer. Polymers of the first phase 14a include isoprene rubber (IR), hydrogenated isoprene rubber, natural rubber (NR), butadiene rubber (BR), styrene-butadiene rubber (SBR), butyl rubber (IIR), ethylene-propylene rubber ( EPM), ethylene-propylene-diene terpolymer rubber (EPDM), silicone rubber (Q) and the like. These may be used alone as the polymer of the first phase 14a, or may be used in combination of two or more.
  • IR isoprene rubber
  • NR natural rubber
  • BR butadiene rubber
  • SBR styrene-butadiene rubber
  • IIR butyl rubber
  • EPM ethylene-propylene rubber
  • EPDM ethylene-propylene-diene terpolymer rubber
  • Q silicone rubber
  • the first phase 14a preferably does not contain a conductive agent such as carbon black, or if it does contain a small amount.
  • the first phase 14a contains at least a smaller amount of conductive agent than the second phase 14b.
  • the second phase 14b contains two types of carbon black.
  • the carbon black of the second phase 14b includes carbon black A having a DBP absorption of 115 cm 3 /100 g or more and 160 cm 3 /100 g or less and carbon black B having a DBP absorption of 70 cm 3 /100 g or more and 110 cm 3 /100 g or less.
  • Carbon black A which has a high DBP absorption amount, serves as a dielectric to store electric charges.
  • Carbon black B which has a low DBP absorption amount, allows the charge to flow quickly.
  • the DBP absorption amount of carbon black is calculated from the amount of DBP (dibutyl phthalate) absorbed by 100 g of carbon black in accordance with JIS K6221.
  • the DBP absorption amount of carbon black A is more preferably 120 cm 3 /100 g or more from the viewpoint of improving the capacitance. In addition, from the viewpoint of improving discharge performance, it is more preferably 150 cm 3 /100 g or less, and still more preferably 140 cm 3 /100 g or less.
  • the DBP absorption amount of carbon black B is more preferably 80 cm 3 /100 g or more from the viewpoint of improving the capacitance. In addition, from the viewpoint of improving discharge performance, it is more preferably 100 cm 3 /100 g or less, and still more preferably 90 cm 3 /100 g or less.
  • Carbon black A which has a high DBP absorption amount, preferably has a relatively high resistance from the viewpoint of being excellent in the function of storing charges as a dielectric. From this point of view, the carbon black A preferably has a relatively small specific surface area and a large particle size. Specifically, carbon black A preferably has a specific surface area of 25 m 2 /g or more and 75 m 2 /g or less. Moreover, it is preferable that the average particle diameter is 35 nm or more and 75 nm or less.
  • the specific surface area of carbon black A is more preferably 30 m 2 /g or more and 70 m 2 /g or less, and still more preferably 30 m 2 /g or more and 60 m 2 /g or less.
  • the average particle diameter of carbon black A is more preferably 40 nm or more and 70 nm or less, still more preferably 40 nm or more and 60 nm or less.
  • the average particle size of carbon black A is 35 nm or more and 75 nm or less, the specific surface area of carbon black A is easily adjusted to a suitable range, and the resistance of carbon black A is easily increased.
  • Carbon black B which has a low DBP absorption amount, preferably has a relatively low resistance from the viewpoint of being excellent in the ability to quickly conduct electric charges. From this point of view, the carbon black B preferably has a relatively large specific surface area and a small particle size. Specifically, carbon black B preferably has a specific surface area of 140 m 2 /g or more and 180 m 2 /g or less. Moreover, it is preferable that the average particle diameter is 20 nm or more and 30 nm or less. The specific surface area of carbon black B is more preferably 150 m 2 /g or more and 180 m 2 /g or less, and still more preferably 150 m 2 /g or more and 170 m 2 /g or less.
  • the average particle size of carbon black B is more preferably 20 nm or more and 25 nm or less.
  • the average particle size of the carbon black B is 20 nm or more and 30 nm or less, the specific surface area of the carbon black B is easily adjusted to a suitable range, and the resistance of the carbon black B is easily reduced.
  • the specific surface area of carbon black is a value measured by the BET method.
  • the average particle diameter of carbon black is represented by the arithmetic mean diameter obtained by observing the carbon black with an electron microscope.
  • the second phase 14b contains one or more polymers. From the viewpoint of low resistance, the polymer of the second phase 14b is preferably a polar polymer. Examples of the polymer of the second phase 14b include nitrile rubber (NBR), hydrin rubber, urethane rubber (U), acrylic rubber (a copolymer of acrylic acid ester and 2-chloroethyl vinyl ether, ACM), chloroprene rubber (CR), and the like. is mentioned.
  • hydrin rubber examples include epichlorohydrin homopolymer (CO), epichlorohydrin-ethylene oxide binary copolymer (ECO), epichlorohydrin-allyl glycidyl ether binary copolymer (GCO), epichlorohydrin-ethylene oxide-allyl glycidyl ether ternary A copolymer (GECO) and the like are included. These may be used alone as the polymer of the second phase 14b, or may be used in combination of two or more. Among these, nitrile rubber (NBR) and hydrin rubber are preferable from the viewpoint of lower resistance.
  • CO epichlorohydrin homopolymer
  • ECO epichlorohydrin-ethylene oxide binary copolymer
  • GCO epichlorohydrin-allyl glycidyl ether binary copolymer
  • GECO epichlorohydrin-ethylene oxide-allyl glycidyl ether ternary A copolymer
  • NBR nitrile rubber
  • the phase separation between the first phase 14a and the second phase 14b is good, and the local resistance Attenuation of charge from the roll surface due to unevenness is easily suppressed.
  • the polymer of the first phase 14a preferably has a higher resistance than the polymer of the second phase 14b.
  • Preferred combinations of the polymer of the first phase 14a and the polymer of the second phase 14b are a combination of isoprene rubber (IR) and nitrile rubber (NBR), and a combination of natural rubber (NR) and nitrile rubber (NBR).
  • the surface resistance value of the first phase 14a can be adjusted within a desired range depending on the type of polymer and vulcanization conditions.
  • the surface resistance value of the second phase 14b can be adjusted within a desired range depending on the type of polymer, vulcanization conditions, amount of carbon black A and carbon black B added, and the like.
  • A/B is more preferably 3.0 or more and 7.0 or less, and further preferably A/B is 4.0 or more and 7.0 or less.
  • the content of carbon black A is preferably 5 parts by mass or more with respect to 100 parts by mass of the polymer component contained in the elastic layer 14, from the viewpoint of easily securing the capacitance. More preferably 10 parts by mass or more, still more preferably 20 parts by mass or more. Moreover, the content of carbon black A is preferably 75 parts by mass or less with respect to 100 parts by mass of the polymer component contained in the elastic layer 14 from the viewpoint of easily suppressing insufficient discharge. It is more preferably 70 parts by mass or less, still more preferably 60 parts by mass or less. When the content of carbon black A is 5 parts by mass or more and 75 parts by mass or less with respect to 100 parts by mass of the polymer component contained in the elastic layer 14, it is easy to maintain the capacitance within a suitable range.
  • the content of carbon black B is preferably 1.5 parts by mass or more with respect to 100 parts by mass of the polymer component contained in the elastic layer 14, from the viewpoint of easily ensuring low resistance. It is more preferably 3.0 parts by mass or more, still more preferably 5.0 parts by mass or more. Moreover, the content of carbon black B is preferably 20 parts by mass or less with respect to 100 parts by mass of the polymer component contained in the elastic layer 14 from the viewpoint of easily suppressing excessive discharge. More preferably, it is 15 parts by mass or less. When the content of carbon black B is 1.5 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the polymer component contained in the elastic layer 14, the resistance can be easily maintained within a suitable range.
  • the first phase 14a preferably constitutes a sea phase
  • the second phase 14b preferably constitutes an island phase.
  • the first phase 14a improves the effect of blocking electric charges, absorbs local unevenness in resistance, and further suppresses electric charge attenuation from the roll surface.
  • the existence ratio of the first phase 14a and the second phase 14b can be adjusted, the content ratio of the carbon black A and the carbon black B can be adjusted, and the first phase 14a and the second phase 14a can be adjusted. It can be formed by adjusting the kneading method of 14b.
  • the sea phase can be called a matrix phase, a continuous phase, or the like.
  • the island phase can be called a domain phase, a dispersed phase, or the like.
  • the second phase 14b is represented as island-like phases scattered in the sea of the first phase 14a.
  • the second phase 14b is a phase that does not appear at the interface with the surface layer 16. becomes.
  • the second phase 14b is preferably a phase that is not in contact with the surface layer 16.
  • the first phase 14a is interposed between the second phase 14b and the surface layer 16, as shown in FIG.
  • the effect of blocking electric charges by the first phase 14a is improved, and local unevenness in resistance is more absorbed. This further suppresses charge decay from the roll surface.
  • the thickness t of the first phase 14a interposed between the second phase 14b and the surface layer 16 is preferably 10 nm or more from the viewpoint of the excellent effect of blocking electric charges by the first phase 14a. It is more preferably 50 nm or more, still more preferably 100 nm or more. Moreover, the thickness t of the first phase 14a interposed between the second phase 14b and the surface layer 16 is preferably 2.0 ⁇ m or less from the viewpoint of ease of discharge. It is more preferably 1.5 ⁇ m or less, still more preferably 1.0 ⁇ m or less. The thickness t of the first phase 14a interposed between the second phase 14b and the surface layer 16 can be obtained by observing with an electron microscope.
  • the first phase 14a preferably has a resistance higher than that of the surface layer 16 from the viewpoint of exhibiting the effect of blocking electric charges by the first phase 14a.
  • the first phase 14a preferably has a higher resistance than the second phase 14b and a higher resistance than the surface layer 16 .
  • the second phase 14b preferably has a resistance lower than that of the surface layer 16 or the same resistance as that of the surface layer 16 from the viewpoint of ease of discharge. The resistance in this case is the surface resistance.
  • the first phase 14a and the second phase 14b are preferably finely dispersed.
  • the area ratio is more preferably 0.5 or more and 10 or less, further preferably 1.0 or more and 5.0 or less.
  • the dispersion structure of the elastic layer 14 can be adjusted by adjusting the existence ratio of the first phase 14a and the second phase 14b, by adjusting the content ratio of the carbon black A and the carbon black B, or by adjusting the content ratio of the first phase 14a and the second phase It can be formed by adjusting the kneading method of 14b.
  • the dispersion structure of the elastic layer 14 can be obtained by observing with an electron microscope.
  • Additives include lubricants, vulcanization accelerators, antioxidants, light stabilizers, viscosity modifiers, processing aids, flame retardants, plasticizers, foaming agents, fillers, dispersants, antifoaming agents, pigments, release agents, Molding agents and the like can be mentioned.
  • the thickness of the elastic layer 14 is not particularly limited, and may be appropriately set within the range of 0.1 to 10 mm depending on the application.
  • the main material forming the surface layer 16 is not particularly limited, and may include polyamide (nylon), acrylic, urethane, silicone, and fluorine polymers. These polymers may be modified. Examples of modifying groups include N-methoxymethyl groups, silicone groups, and fluorine groups.
  • the surface layer 16 may contain roughness forming particles.
  • the roughness-forming particles are particles for imparting roughness to the surface of the surface layer 16 . In other words, they are particles for providing unevenness to the surface of the surface layer 16 .
  • the surface unevenness of the surface layer 16 increases the discharge space between the photoreceptor and the charging roll 10, promoting discharge. As a result, it is possible to improve charging performance and suppress image defects such as horizontal streaks and unevenness.
  • Resin particles and the like are used as the roughness forming particles.
  • the material of the roughness forming particles is not particularly limited.
  • the roughness forming particles are preferably composed of a polymer having a carbonyl group. This is because a polymer having a carbonyl group is a material with a relatively high dielectric constant, and the charging roll 10 can easily secure excellent charging properties.
  • Examples of polymers having carbonyl groups include urethane resins, polyamide resins, acrylic resins, acrylic silicone resins, silicone-grafted acrylic polymers, acrylic-grafted silicone polymers, and urethane rubbers.
  • the size of the roughness-forming particles is not particularly limited, but from the viewpoint of facilitating ensuring uniform chargeability, the average particle size is preferably 3.0 ⁇ m or more and 50 ⁇ m or less. More preferably, those having an average particle size of 5.0 ⁇ m or more and 30 ⁇ m or less are preferable.
  • the average particle diameter of the roughness-forming particles is expressed by an average of arbitrary 20 points obtained by observing the surface of the surface layer 16 with a laser microscope and taking the diameter of the roughness-forming particles that can be seen at the time of surface observation as the particle diameter.
  • the content of the roughness-forming particles in the surface layer 16 is not particularly limited, but from the viewpoint of easily ensuring uniform chargeability, it is 3 parts by mass or more with respect to 100 parts by mass of the binder polymer of the surface layer 16. It is preferably 50 parts by mass or less. More preferably, it is 5 parts by mass or more and 30 parts by mass or less.
  • conductive agents can be appropriately added.
  • various additives may be appropriately added as necessary.
  • the volume resistivity of the surface layer 16 is preferably set in a semi-conductive region from the viewpoint of chargeability. Specifically, for example, it may be set within the range of 1.0 ⁇ 10 7 to 1.0 ⁇ 10 10 ⁇ cm. Volume resistivity can be measured according to JIS K6911.
  • the thickness of the surface layer 16 is not particularly limited, and may be set within the range of 0.1 to 3.0 ⁇ m. The thickness of the surface layer 16 can be measured by observing the cross section using a laser microscope (such as "VK-9510" manufactured by Keyence). For example, the distance from the surface of the elastic layer 14 to the surface of the surface layer 16 is measured at five arbitrary positions, and the average distance can be obtained.
  • the charging roll 10 can be produced by forming the elastic layer 14 on the outer peripheral surface of the shaft and forming the surface layer 16 on the outer peripheral surface of the elastic layer 14 .
  • the elastic layer 14 can be formed, for example, as follows. First, the shaft is coaxially placed in the hollow part of the roll molding die, and an uncrosslinked composition for forming an elastic layer is injected, heated and cured (crosslinked), and then removed from the mold, or An elastic layer 14 is formed on the outer periphery of the shaft by extrusion molding an uncrosslinked elastic layer-forming composition on the surface of the shaft.
  • the elastic layer-forming composition is obtained by kneading two types of carbon blacks, carbon black A and carbon black B, with a polymer component that constitutes the second phase 14b, and then kneading the polymer component that constitutes the first phase 14a. It can be formed by kneading.
  • a surface layer forming composition is used to form the surface layer 16 .
  • the surface layer-forming composition contains the main material, a conductive agent, and other additives if necessary.
  • the surface layer forming composition can be used in organic solvents such as methyl ethyl ketone, toluene, acetone, ethyl acetate, butyl acetate, methyl isobutyl ketone (MIBK), THF and DMF, and water solutions such as methanol and ethanol.
  • organic solvents such as methyl ethyl ketone, toluene, acetone, ethyl acetate, butyl acetate, methyl isobutyl ketone (MIBK), THF and DMF, and water solutions such as methanol and ethanol.
  • MIBK methyl isobutyl ketone
  • THF methyl isobutyl ketone
  • DMF methyl isobutyl ketone
  • water solutions such as methanol and ethanol.
  • a solvent such as a polar solvent may be included as appropriate.
  • the surface layer 16 can be formed by a method such as coating a composition for forming a surface layer on the outer peripheral surface of the elastic layer 14 .
  • Various coating methods such as a roll coating method, a dipping method, and a spray coating method can be applied as the coating method. If necessary, the coated surface layer 16 may be subjected to ultraviolet irradiation or heat treatment.
  • carbon black B having a small DBP absorption amount is present in the second phase 14b having a low resistance, so that electric charge flows quickly and a low resistance is ensured. be able to.
  • the carbon black A having a large DBP absorption amount present in the low-resistance second phase 14b together with the carbon black B exerts a function of accumulating charges as a dielectric, and is separated from the low-resistance second phase 14b.
  • the existing high-resistance first phase 14a serves as a dielectric phase to block and equalize electric charges, thereby absorbing local unevenness in resistance. As a result, electric charge attenuation from the roll surface due to local unevenness in resistance is suppressed, and good images can be obtained.
  • Example 1 ⁇ Preparation of Composition for Forming Elastic Layer> 50 parts by mass of carbon black A-1 and 10 parts by mass of carbon black B-1 were blended with 40 parts by mass of NBR, and these were stirred and mixed with a stirrer to prepare a composition for forming the second phase. Next, 60 parts by mass of isoprene rubber, 5 parts by mass of a peroxide cross-linking agent, 3 parts by mass of a vulcanization aid, and 3 parts by mass of a catalyst are blended with the composition for forming the second phase, and these are stirred and mixed with a stirrer. Thus, a composition for forming an elastic layer was prepared.
  • a metal core (diameter 8 mm) is set in a molding die (pipe shape), an elastic layer forming composition is injected, heated at 180°C for 30 minutes, cooled, removed from the mold, and placed on the outer periphery of the metal core. , an elastic layer having a thickness of 1.9 mm was molded.
  • a surface layer forming composition was prepared by blending roughness forming particles and a binder polymer, adding 200 parts by mass of methyl ethyl ketone (MEK), and mixing and stirring at a predetermined stirring speed.
  • Example 2 A charging roll was produced in the same manner as in Example 1, except that the blending amounts of carbon black A and carbon black B were changed in the preparation of the composition for forming an elastic layer.
  • Example 3 A charging roll was produced in the same manner as in Example 1, except that the compounding ratio of IR and NBR was changed and the type of carbon black A was changed in the preparation of the composition for forming an elastic layer.
  • Examples 4-5 A charging roll was produced in the same manner as in Example 1, except that the type of carbon black A was changed in the preparation of the composition for forming an elastic layer.
  • Example 6 A charging roll was produced in the same manner as in Example 1, except that the type of carbon black B and the blending amounts of carbon black A and carbon black B were changed in the preparation of the composition for forming an elastic layer.
  • Example 7 A charging roll was produced in the same manner as in Example 1, except that the compounding ratio of IR and NBR and the compounding amount of carbon black B were changed in the preparation of the composition for forming an elastic layer.
  • Example 8-11 A charging roll was produced in the same manner as in Example 1, except that the blending amounts of carbon black A and carbon black B were changed in the preparation of the composition for forming an elastic layer.
  • Example 12-13 A charging roll was produced in the same manner as in Example 1, except that the compounding ratio of IR and NBR was changed in the preparation of the composition for forming an elastic layer.
  • Comparative Examples 6-7 A charging roll was produced in the same manner as in Example 1, except that the IR and NBR vulcanization conditions were changed in the preparation of the elastic layer-forming composition. Compared to Example 1, Comparative Example 6 increased the vulcanization temperature and shortened the vulcanization time. Moreover, compared with Example 1, Comparative Example 7 lowered the vulcanization temperature and lengthened the vulcanization time.
  • the following materials were prepared as materials for the elastic layer-forming composition.
  • base polymer ⁇ Isoprene rubber (IR): “Nipol IR2200” manufactured by Nippon Zeon ⁇ Nitrile rubber (NBR): Nippon Zeon "Nipol 1041" (Carbon black A) ⁇ A-1 (DBP absorption 124 ml/100 g, BET specific surface area 43 m 2 /g, average particle size 41 nm): “Asahi #60H (N-568)” manufactured by Asahi Carbon ⁇ A-2 (DBP absorption 160 ml/100 g, BET specific surface area 75 m 2 /g, average particle size 35 nm): “Denka Black” manufactured by Denka ⁇ A-3 (DBP absorption 115 ml/100 g, BET specific surface area 42 m 2 /g, average particle size 44 nm): Tokai Carbon “Seist SO” ⁇ A-4 (DBP absorption 155
  • the surface resistance values of the first and second phases of the produced charging roll were measured. Also, the area ratio between the first phase and the second phase was measured. Furthermore, the following image evaluation was performed.
  • the cross-section of the prepared charging roll was scanned by 1 ⁇ m using a scanning probe microscope “AFM5100N” manufactured by Hitachi High-Tech Science Co., Ltd. using a cantilever “SI-DF3” in DFM mode, and the surface resistance ( ⁇ cm) was derived.
  • the produced conductive roll is incorporated into Konica Minolta's multifunction machine "bizhub C658" as a conductive roll, and after printing 550,000 sheets in ruled line mode with a print density of 1% in an environment of 10 ° C x 10% RH, the print density is 25%. printed a halftone image of A case where no uneven image was observed was rated as good, and a case where an uneven image was observed was rated as bad.
  • the produced conductive roll is incorporated into Konica Minolta's multifunction machine "bizhub C658" as a conductive roll, and after printing 550,000 sheets in ruled line mode with a print density of 1% in an environment of 10 ° C x 10% RH, the print density is 25%. printed a halftone image of A case where no horizontal streak image was observed was evaluated as "good", and a case where a horizontal streak image was observed was evaluated as "bad".
  • the produced conductive roll is incorporated into Konica Minolta's multifunction machine "bizhub C658" as a conductive roll, and after printing 550,000 sheets in ruled line mode with a print density of 1% in an environment of 10 ° C x 10% RH, the print density is 25%.
  • printed a halftone image of A case where no black spots were observed in the image was evaluated as "Good”, and a case where black spots were observed in the image was evaluated as "Bad”.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR. Carbon black A with a weight of 100 g or less is not included, and only carbon black B with a DBP absorption of 70 cm 3 /100 g or more and 110 cm 3 /100 g or less is included. For this reason, the electrostatic capacity is insufficient, charging is insufficient, and horizontal streaks occur in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR, but carbon black A is not contained in the second phase. It contains B and carbon black with a DBP absorption greater than 160 cm 3 /100 g. For this reason, the electrostatic capacity is too large, resulting in insufficient discharge and insufficient charging, which causes horizontal streaks in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR, but carbon black B is not contained in the second phase. Contains only A. For this reason, the dielectric property is given too much priority, resulting in insufficient discharge and insufficient charging, which causes horizontal streaks in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR, but carbon black B is not contained in the second phase. A and carbon black with a DBP absorption of less than 70 cm 3 /100 g are included. As a result, the electrostatic capacity is insufficient, charging is insufficient, and horizontal streaks occur in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR, but carbon black B is not contained in the second phase.
  • a and carbon black with a DBP absorption greater than 160 cm 3 /100 g are included.
  • Carbon black with a DBP absorption of more than 160 cm 3 /100 g has a high specific surface area of 800 m 2 /g, so that excessive electric charge flows and excessive discharge (abnormal discharge) occurs, resulting in black spots in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR. Due to insufficient discharge and insufficient charging, horizontal streaks occur in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR. Excessive discharge (abnormal discharge) occurs, and black spots are generated in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR. Excessive discharge (abnormal discharge) occurs, and black spots are generated in image evaluation.
  • the elastic layer is composed of two phases, a first phase containing IR and a second phase containing NBR. Insufficient, horizontal streaks occur in image evaluation.
  • the elastic layer is not composed of two phases, the first phase containing IR and the second phase containing NBR, but is composed of only one phase containing IR, and two phases in the phase containing IR. of carbon blacks A and B are included.
  • the elastic layer was not composed of two phases, the first phase containing IR and the second phase containing NBR, but was composed of only one phase containing NBR, and two phases in the phase containing NBR. It contains two types of carbon blacks A and B. Therefore, in Comparative Examples 10 and 11, there is no phase that becomes a dielectric phase, the electrostatic capacity is insufficient, charging is insufficient, and horizontal streaks occur in image evaluation.
  • the elastic layer includes a high-resistance first phase having a surface resistance of 1.6 ⁇ 10 14 ⁇ cm or more and 8.8 ⁇ 10 15 ⁇ cm or less, and a surface resistance of is 1.3 ⁇ 10 2 ⁇ cm or more and 4.9 ⁇ 10 3 ⁇ cm or less, and the second phase has a DBP absorption of 115 cm 3 /100 g or more and 160 cm 3/100 g or less, and carbon black B having a DBP absorption of 70 cm 3 /100 g or more and 110 cm 3 /100 g or less. For this reason, electric charge attenuation from the roll surface due to local unevenness in resistance is suppressed, and good images can be obtained.
  • Comparative Example 1 even if the elastic layer contains the first phase with high resistance, if it contains only carbon black B with a small DBP absorption amount, the electrostatic capacity is insufficient, resulting in insufficient charging. Inadequate. Further, as shown in Comparative Example 3, even if the elastic layer contains the second phase of low resistance, if only the carbon black A having a large DBP absorption amount is contained, the dielectric property is given too much priority, resulting in insufficient discharge. , charging is insufficient. Further, as shown in Comparative Examples 10 and 11, even if the elastic layer contains two types of carbon blacks A and B, if only one phase containing the two types of carbon blacks A and B is present, static Insufficient charging due to lack of electric capacity.
  • the elastic layer includes a high-resistance first phase and a low-resistance second phase, and carbon black A with a large DBP absorption and carbon black B with a small DBP absorption are combined in the second phase.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Physics & Mathematics (AREA)
  • Engineering & Computer Science (AREA)
  • Health & Medical Sciences (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Physics & Mathematics (AREA)
  • General Engineering & Computer Science (AREA)
  • Plasma & Fusion (AREA)
  • Mechanical Engineering (AREA)
  • Electrostatic Charge, Transfer And Separation In Electrography (AREA)
  • Rolls And Other Rotary Bodies (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
PCT/JP2022/023760 2021-06-29 2022-06-14 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法 Ceased WO2023276649A1 (ja)

Priority Applications (2)

Application Number Priority Date Filing Date Title
CN202280028015.1A CN117120939B (zh) 2021-06-29 2022-06-14 电子照相设备用带电辊以及电子照相设备用带电辊的制造方法
US18/500,102 US12686761B2 (en) 2021-06-29 2023-11-01 Charging roll for electrophotographic device and method for manufacturing charging roll for electrophotographic device

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021107167A JP7291747B2 (ja) 2021-06-29 2021-06-29 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法
JP2021-107167 2021-06-29

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US18/500,102 Continuation US12686761B2 (en) 2021-06-29 2023-11-01 Charging roll for electrophotographic device and method for manufacturing charging roll for electrophotographic device

Publications (1)

Publication Number Publication Date
WO2023276649A1 true WO2023276649A1 (ja) 2023-01-05

Family

ID=84692279

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/023760 Ceased WO2023276649A1 (ja) 2021-06-29 2022-06-14 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法

Country Status (4)

Country Link
US (1) US12686761B2 (enExample)
JP (1) JP7291747B2 (enExample)
CN (1) CN117120939B (enExample)
WO (1) WO2023276649A1 (enExample)

Families Citing this family (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2024101379A (ja) * 2023-01-17 2024-07-29 株式会社ユニバーサルエンターテインメント 遊技機
JP7863065B2 (ja) * 2023-03-29 2026-05-20 住友理工株式会社 電子写真機器用帯電ロール
JP7788483B2 (ja) * 2024-03-26 2025-12-18 住友理工株式会社 電子写真機器用帯電ロール

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2020166259A (ja) * 2019-03-29 2020-10-08 キヤノン株式会社 導電性部材、電子写真用プロセスカートリッジ、及び電子写真画像形成装置
JP2020166208A (ja) * 2019-03-29 2020-10-08 キヤノン株式会社 導電性部材及びその製造方法、プロセスカートリッジ並びに電子写真画像形成装置

Family Cites Families (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP3594053B2 (ja) * 1996-04-10 2004-11-24 株式会社ブリヂストン 導電性部材及び電子写真装置
JP3248455B2 (ja) * 1997-07-03 2002-01-21 富士ゼロックス株式会社 画像形成装置と同装置に用いられる中間転写ベルトの製造方法
JP2011138004A (ja) * 2009-12-28 2011-07-14 Canon Chemicals Inc 電子写真装置用導電性ローラー及びこれを用いた帯電ローラー
JP6784079B2 (ja) * 2016-07-07 2020-11-11 富士ゼロックス株式会社 帯電部材、帯電装置、プロセスカートリッジ及び画像形成装置
WO2019203238A1 (ja) * 2018-04-18 2019-10-24 キヤノン株式会社 導電性部材及びその製造方法、プロセスカートリッジ並びに電子写真画像形成装置
CN113039489A (zh) * 2019-07-30 2021-06-25 住友理工株式会社 电子照相设备用导电性辊

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2020166259A (ja) * 2019-03-29 2020-10-08 キヤノン株式会社 導電性部材、電子写真用プロセスカートリッジ、及び電子写真画像形成装置
JP2020166208A (ja) * 2019-03-29 2020-10-08 キヤノン株式会社 導電性部材及びその製造方法、プロセスカートリッジ並びに電子写真画像形成装置

Also Published As

Publication number Publication date
US12686761B2 (en) 2026-07-21
CN117120939B (zh) 2025-08-19
US20240059875A1 (en) 2024-02-22
CN117120939A (zh) 2023-11-24
JP7291747B2 (ja) 2023-06-15
JP2023005335A (ja) 2023-01-18

Similar Documents

Publication Publication Date Title
JP7291747B2 (ja) 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法
JP5612805B2 (ja) 帯電ロール
CN109952540B (zh) 电子照相设备用带电辊
JP6714529B2 (ja) 電子写真機器用帯電部材および電子写真機器用帯電部材の製造方法
JP6576709B2 (ja) 電子写真機器用導電性部材
JP2013071965A (ja) ゴム組成物および帯電ロール
JP5186128B2 (ja) 導電性ロール
US20200012210A1 (en) Development roll for electrophotography device
JP2021096377A (ja) 電子写真機器用導電性ロール
WO2022176820A1 (ja) 電子写真機器用帯電ロール
JP7623135B2 (ja) 電子写真機器用帯電ロール
JP2017116685A (ja) 電子写真機器用導電性部材
JP7717885B1 (ja) 電子写真機器用帯電ロール
JP6722613B2 (ja) 電子写真機器用帯電ロール
JP7710979B2 (ja) 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法
CN112771277B (zh) 电子照相设备用带电辊
JP7258708B2 (ja) 電子写真機器用帯電ロール
JP7863065B2 (ja) 電子写真機器用帯電ロール
JP2023067019A (ja) 電子写真機器用帯電ロールおよび電子写真機器用帯電ロールの製造方法
JP2022173957A (ja) 転写ローラ
JP2020086198A (ja) 電子写真機器用導電性部材

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22830367

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 22830367

Country of ref document: EP

Kind code of ref document: A1

WWG Wipo information: grant in national office

Ref document number: 202280028015.1

Country of ref document: CN