WO2023189424A1 - 化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法 - Google Patents

化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法 Download PDF

Info

Publication number
WO2023189424A1
WO2023189424A1 PCT/JP2023/009322 JP2023009322W WO2023189424A1 WO 2023189424 A1 WO2023189424 A1 WO 2023189424A1 JP 2023009322 W JP2023009322 W JP 2023009322W WO 2023189424 A1 WO2023189424 A1 WO 2023189424A1
Authority
WO
WIPO (PCT)
Prior art keywords
compound
formula
integer
resin composition
solvent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/009322
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
隆行 遠島
昌典 橋本
政隆 中西
篤彦 長谷川
嵩 今井
弥生 多田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Kayaku Co Ltd
Original Assignee
Nippon Kayaku Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Kayaku Co Ltd filed Critical Nippon Kayaku Co Ltd
Priority to CN202380031324.9A priority Critical patent/CN119032113B/zh
Priority to KR1020247032231A priority patent/KR102766816B1/ko
Priority to JP2023534115A priority patent/JP7353538B1/ja
Publication of WO2023189424A1 publication Critical patent/WO2023189424A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G61/00—Macromolecular compounds obtained by reactions forming a carbon-to-carbon link in the main chain of the macromolecule
    • C08G61/02—Macromolecular compounds containing only carbon atoms in the main chain of the macromolecule, e.g. polyxylylenes
    • C—CHEMISTRY; METALLURGY
    • C07—ORGANIC CHEMISTRY
    • C07C—ACYCLIC OR CARBOCYCLIC COMPOUNDS
    • C07C1/00—Preparation of hydrocarbons from one or more compounds, none of them being a hydrocarbon
    • C07C1/26—Preparation of hydrocarbons from one or more compounds, none of them being a hydrocarbon starting from organic compounds containing only halogen atoms as hetero-atoms
    • C07C1/30—Preparation of hydrocarbons from one or more compounds, none of them being a hydrocarbon starting from organic compounds containing only halogen atoms as hetero-atoms by splitting-off the elements of hydrogen halide from a single molecule
    • C—CHEMISTRY; METALLURGY
    • C07—ORGANIC CHEMISTRY
    • C07C—ACYCLIC OR CARBOCYCLIC COMPOUNDS
    • C07C15/00—Cyclic hydrocarbons containing only six-membered aromatic rings as cyclic parts
    • C07C15/40—Cyclic hydrocarbons containing only six-membered aromatic rings as cyclic parts substituted by unsaturated carbon radicals
    • C07C15/50—Cyclic hydrocarbons containing only six-membered aromatic rings as cyclic parts substituted by unsaturated carbon radicals polycyclic non-condensed
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F12/00—Homopolymers and copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by an aromatic carbocyclic ring
    • C08F12/02—Monomers containing only one unsaturated aliphatic radical
    • C08F12/04—Monomers containing only one unsaturated aliphatic radical containing one ring
    • C08F12/06—Hydrocarbons
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G2261/00—Macromolecular compounds obtained by reactions forming a carbon-to-carbon link in the main chain of the macromolecule
    • C08G2261/10—Definition of the polymer structure
    • C08G2261/14—Side-groups
    • C08G2261/146—Side-chains containing halogens
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G2261/00—Macromolecular compounds obtained by reactions forming a carbon-to-carbon link in the main chain of the macromolecule
    • C08G2261/30—Monomer units or repeat units incorporating structural elements in the main chain
    • C08G2261/34—Monomer units or repeat units incorporating structural elements in the main chain incorporating partially-aromatic structural elements in the main chain
    • C08G2261/342—Monomer units or repeat units incorporating structural elements in the main chain incorporating partially-aromatic structural elements in the main chain containing only carbon atoms
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G2261/00—Macromolecular compounds obtained by reactions forming a carbon-to-carbon link in the main chain of the macromolecule
    • C08G2261/70—Post-treatment

Definitions

  • the present invention relates to a compound, a curable resin composition, a cured product thereof, and a method for producing the compound, and relates to a semiconductor encapsulant, a printed wiring board, an electric/electronic component such as a build-up laminate, and a carbon fiber reinforced plastic. , lightweight, high-strength materials such as glass fiber reinforced plastics, and suitably used for 3D printing applications.
  • CPUs central processing units
  • PKG semiconductor packages
  • PCB printed circuit board
  • Patent Document 1 describes a thermosetting resin composition containing (A) an imide compound having a maleimide group and (B) a phenol aralkyl resin having an aliphatic unsaturated bond in one molecule as essential components.
  • Patent Document 2 describes an allyl ether-modified biphenylaralkyl novolak resin.
  • Patent Document 3 describes a compound having a styrene structure.
  • the present invention was made in view of these circumstances, and aims to provide a compound having excellent solvent stability and low dielectric properties, a curable resin composition, a cured product thereof, and a method for producing the compound. shall be.
  • the present invention relates to the following [1] to [13].
  • [1] A compound represented by the following formula (1), in which the compound in which n in formula (1) is 1 accounts for less than 50% in terms of GPC area percentage in the total amount of the compounds.
  • R's each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • p and r are integers of 0 to 4, and q is an integer of 0 to 3.
  • n is an integer, where n is the number of repetitions, and the average value n ave satisfies 1 ⁇ n ave ⁇ 20.
  • the total HP-LC peak area ( ⁇ ) of the compounds represented by the following formulas (2) to (4) is calculated as the HP-LC peak area ( ⁇ ) of the compound where n in the formula (1) is 1.
  • each of the plurality of R's independently represents a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • the plurality of s's are each independently an integer of 0 to 4. .
  • each of the plurality of R's independently represents a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • the plurality of A's each independently represents the following formula (3-a ) to (3-c). The plural s's are each independently an integer of 0 to 4, and t is an integer of 0 to 3.
  • R's each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • a plurality of B's each independently represent the following formula (4-d ) or (4-e).
  • D is the following formula (4-f). Multiple s are each independently an integer of 0 to 4, and t is an integer of 0 to 3. Formula (4 ), one of the five m's is 1, and the other four are 0.)
  • R's exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms.
  • p and r are integers of 0 to 4, and q is an integer of 0 to 4. is an integer of 3, n is the number of repetitions, and the average value n ave of n satisfies 1 ⁇ n ave ⁇ 20.
  • X represents a halogen atom.
  • the curable resin composition according to item [6] which contains any one or more of a polyphenylene ether compound, polybutadiene and a modified product thereof, and polystyrene and a modified product thereof.
  • the following formula obtained by dehydrohalogenating the compound represented by the following formula (5) in the presence of a basic catalyst in a solvent 4 to 7 times the weight of the compound represented by the following formula (5) A method for producing a compound represented by (1).
  • each of the plurality of R's exists independently and represents a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms.
  • p and r are integers of 0 to 4, and q is an integer of 0 to 4.
  • n is an integer of 3, n is the number of repetitions, and the average value n ave satisfies 1 ⁇ n ave ⁇ 20.
  • R's exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms.
  • p and r are integers of 0 to 4, and q is an integer of 0 to 4. is an integer of 3, n is the number of repetitions, and the average value n ave of n satisfies 1 ⁇ n ave ⁇ 20.
  • X represents a halogen atom.
  • the compound of the present invention has excellent solvent solubility, and its cured product has excellent low dielectric properties. Therefore, it is a useful material for sealing electrical and electronic parts, circuit boards, carbon fiber composite materials, etc.
  • a GPC chart of Synthesis Example 1 is shown.
  • a GPC chart of Example 1 is shown.
  • a 1 H-NMR chart of Example 1 is shown.
  • An LC-MS chart of Example 1 is shown.
  • the HP-LC chart of Example 1 is shown.
  • a GPC chart of Example 2 is shown.
  • the HP-LC chart of Example 2 is shown.
  • a GPC chart of Example 3 is shown.
  • the HP-LC chart of Example 3 is shown.
  • a GPC chart of Example 4 is shown.
  • the HP-LC chart of Example 4 is shown.
  • a GPC chart of Comparative Synthesis Example 1 is shown.
  • a GPC chart of Comparative Synthesis Example 2 is shown.
  • the HP-LC chart of Comparative Synthesis Example 2 is shown.
  • the compound of the present embodiment is represented by the following formula (1), and in the total amount of the compound, the formula (1) in the chromatogram obtained by gel permeation chromatography (hereinafter also referred to as GPC) is The ratio (area percentage) of the area (time integral value of signal value) of the compound where n in formula (1) is 1 to the total area (time integral value of signal value) of the compound having the represented structure is Less than 50%. If the area percentage of the compound having a structure where n in formula (1) is 1 is 50% or more, crystals may precipitate when a resin solution containing the compound represented by formula (1) is stored. (i.e., the solubility in the solvent decreases).
  • R's each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • p and r are integers of 0 to 4, and q is an integer of 0 to 3. It is an integer.
  • n is the number of repetitions, and the average value n ave satisfies 1 ⁇ n ave ⁇ 20.
  • n ave is usually 1 ⁇ n ⁇ 20, preferably 1.1 ⁇ n ave ⁇ 20, more preferably 1.1 ⁇ n ave ⁇ 10, and 1.1 ⁇ n ave ⁇ 5. It is particularly preferable that there be.
  • the value of n ave can be calculated from the value of the number average molecular weight (Mn) determined by GPC measurement of the compound of formula (1).
  • Mn number average molecular weight
  • the number average molecular weight is preferably 200 or more and less than 5,000, more preferably 300 or more and less than 3,000, and particularly preferably 400 or more and less than 2,000. When the number average molecular weight is less than 5,000, purification by washing with water becomes easy, and when it is 200 or more, the target compound does not volatilize in the solvent distillation step.
  • R is a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group, preferably a hydrocarbon group having 1 to 10 carbon atoms, and more preferably a hydrocarbon group having 1 to 5 carbon atoms. It is a hydrocarbon group, particularly preferably a hydrocarbon group having 1 to 3 carbon atoms. If R has a small number of carbon atoms, molecular vibration will be difficult to occur when exposed to high frequency, so when R is a hydrocarbon group having 1 to 3 carbon atoms among the above descriptions, the electrical properties are particularly excellent.
  • GPC Online degassing unit (DGU-20A3R), binary liquid feeding unit (LC-20AD), autosampler (SIL-20AHT), differential refractive index detector (RID-20A), column oven (CTO-20A), system Controller (CBM-20A) (both manufactured by Shimadzu Corporation)
  • DGU-20A3R Online degassing unit
  • LC-20AD binary liquid feeding unit
  • SIL-20AHT autosampler
  • RID-20A differential refractive index detector
  • CTO-20A column oven
  • CBM-20A system Controller
  • the compound represented by the above formula (1) may contain compounds represented by the following formulas (2) to (4) as by-products, and can be analyzed by high performance liquid chromatography (HP-LC).
  • HP-LC high performance liquid chromatography
  • the sum total ( ⁇ ) of the peak areas of the compounds represented by the following formulas (2) to (4) in the obtained chromatogram is calculated as the HP-LC peak area (
  • the value ( ⁇ / ⁇ ) divided by ⁇ ) is preferably 0.10 or less, more preferably 0.07 or less.
  • the "peak area” is the area surrounded by the peak and a straight line connecting both sides of the peak. In reality, it is determined by an approximate value using the half-width method or by the number of integrated counts of the output at the peak time (JIS K0214:2013).
  • the lower limit value of ( ⁇ / ⁇ ) may be 0, but is more preferably 0.01. This is because when it is 0.01 or more, adhesiveness, solvent solubility, and compatibility with a compound having a polar group are improved.
  • R's exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms.
  • s is an integer of 0 to 4.
  • each of the plurality of R's independently represents a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • the plurality of A's each independently represents the following formula (3-a ) to (3-c). s is an integer from 0 to 4, and t is an integer from 0 to 3.
  • R's each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group.
  • a plurality of B's each independently represent the following formula (4-d ) or (4-e).
  • D is the following formula (4-f). Multiple s are each independently an integer of 0 to 4, and t is an integer of 0 to 3. Formula (4 ), one of the five m's is 1, and the other four are 0.)
  • by-products such as compounds represented by formulas (2) to (4) above can be removed by purification, but in the case of compounds represented by formula (1) above, distillation, recrystallization, etc. It is difficult to remove the compounds represented by formulas (2) to (4) using purification methods such as washing with water.
  • the compound represented by the formula (1) since the compound represented by the formula (1) has a styrene structure as a functional group, it has high reactivity, and unintended polymerization occurs in purification methods that require overheating such as distillation. .
  • the compound represented by the formula (1) is a liquid compound after the solvent is distilled off, it is difficult to obtain a crystal structure, and therefore it is difficult to recrystallize it with a good yield.
  • LC-MS liquid chromatography mass spectrometry
  • HP-LC high performance liquid chromatography
  • Equipment Binary liquid feeding unit (LC-20AB), online degassing unit (DGU-20A3R), autosampler (SIL-20A), column oven (CTO-20A), system controller (CBM-20A), photodiode array detection Equipment (SPD-M20A) (both manufactured by Shimadzu Corporation)
  • LC-20AB Binary liquid feeding unit
  • DGU-20A3R online degassing unit
  • SIL-20A autosampler
  • CTO-20A column oven
  • CBM-20A system controller
  • SPD-M20A photodiode array detection Equipment
  • Flow rate 0.5ml/min.
  • the hydroxyl equivalent of the compound represented by formula (1) is 100000 g/eq. It is preferable that it is below.
  • the hydroxyl equivalent is 100000g/eq. This is because if it is below, the adhesion, solvent solubility, and compatibility with a compound having a polar group will be improved without impairing electrical properties or low heat properties.
  • the compound represented by the above formula (1) is derived from the compound represented by the following formula (5).
  • R's exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms.
  • p and r are integers of 0 to 4
  • q is an integer of 0 to 4.
  • n is the number of repetitions, and the average value n ave of n satisfies 1 ⁇ n ave ⁇ 20.
  • X represents a halogen atom.
  • R in the above formula (5) and the preferred range of the average value n ave of p, r, q, and n are the same as in the above formula (1).
  • the halogen atom in R and X are preferably a bromine atom or a chlorine atom, and a bromine atom is particularly preferred.
  • the compound represented by the formula (1) can be obtained, for example, by dehydrohalogenation of the compound represented by the formula (5) in a solvent in the presence of a basic catalyst.
  • the amount of solvent used is preferably 4 to 7 times the weight of the compound represented by formula (5).
  • the solvent used is preferably an aprotic polar solvent, such as dimethylsulfone, dimethylsulfoxide, dimethylformamide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, N-methylpyrrolidone, etc. may be used together. It is also preferable to use a water-insoluble solvent in combination with the aprotic polar solvent to form a mixed solvent.
  • the aprotic polar solvent is preferably dimethyl sulfoxide, dimethylformamide, 1,3-dimethyl-2-imidazolidinone, or N-methylpyrrolidone.
  • the water-insoluble solvent benzene, toluene, xylene, mesitylene, hexane, cyclohexane, and methylcyclohexane are preferred. Among these, the most preferred combination is dimethyl sulfoxide and toluene.
  • the aprotic polar solvent is preferably used in an amount of 1 to 10 times the weight of the water-insoluble solvent, more preferably 1 to 8 times, particularly preferably 2 to 6 times. If it is less than 1 time, the reaction will be difficult to proceed and there is a risk that raw materials may remain. If it exceeds 10 times, the reaction promoting effect is high, but the amount of the compounds represented by formulas (2) to (4) tends to increase.
  • the reaction proceeds in a state where the layers are separated into two layers, an aprotic polar solvent layer and an aqueous-insoluble solvent layer, so the above range is preferable from the viewpoint of controlling the reactivity at the interface.
  • the total amount of the solvent used is preferably 1 to 9 times the weight of the compound represented by formula (5), more preferably 2 to 8 times, particularly preferably 3 to 7 times the weight. be. If it is less than 1 times by weight, stirring may become difficult due to salt precipitation, and if it is more than 9 times by weight, there is a risk that the kettle efficiency (the amount of resin that can be synthesized in one batch) will be significantly reduced.
  • the reaction temperature is preferably 0 to 80°C, more preferably 10 to 60°C, even more preferably 26 to 70°C. If the temperature is lower than 0°C, the reaction may not proceed sufficiently, and if the temperature is higher than 80°C, the polymerization reaction of the styrene structure may occur simultaneously, so that gelation may proceed.
  • the catalyst is not particularly limited, but includes basic catalysts such as sodium hydroxide, potassium hydroxide, and potassium carbonate. Since it is difficult to allow the dehydrohalogenation reaction to proceed completely, the aprotic polar solvent may be used in large excess relative to the substrate, or the dehydrohalogenation reaction may be carried out twice or three times or more. This may be repeated multiple times. For example, in the presence of a base catalyst in an organic solvent, the compound represented by formula (2) is subjected to a dehydrohalogenation reaction, and the resulting solution is washed with water, then returned to the reaction vessel, and a base catalyst is added thereto. You may react. By doing so, the degree of progress of the dehydrohalogenation reaction can be increased.
  • basic catalysts such as sodium hydroxide, potassium hydroxide, and potassium carbonate.
  • the mass concentration of residual halogen in the target substance is preferably 1 to 10,000 ppm, more preferably 1 to 1,000 ppm, and still more preferably 1 to 750 ppm. If the mass concentration of residual halogen contained in the compound represented by formula (1) is high, molecular vibration may occur when exposed to high frequency waves, which may have a negative effect on electrical properties, particularly dielectric loss tangent. In addition, if the mass concentration of residual halogen is high, there is a risk of increasing the risk of problems such as metal corrosion and ion migration in environmental tests such as HAST tests (High Accelerated Stress Tests). It is preferable.
  • the method for producing the compound represented by formula (5) is not particularly limited, but for example, a compound having a (2-bromoethyl)benzene structure and a bishalogenated methylaryl compound (or a bishydroxymethylaryl compound, etc.) are mixed with hydrochloric acid or The reaction may be carried out under an acid catalyst such as sulfonic acid or activated clay, or a compound having a (2-bromoethyl)benzene structure and a bishydroxymethylaryl compound may be reacted under an acid catalyst such as hydrochloric acid, sulfonic acid or activated clay. good.
  • the extraction step may be performed after neutralization with an alkali metal such as sodium hydroxide or potassium hydroxide.
  • an aromatic hydrocarbon solvent such as toluene or xylene may be used alone, or a non-aromatic hydrocarbon solvent such as cyclohexane or toluene may be used in combination.
  • the organic layer is washed with water until the waste water becomes neutral, and the solvent and excess (2-bromoethyl)benzene-containing compound are distilled off using an evaporator or the like to remove at least two or more compounds in the target molecule. , a compound having a 2-bromoethylethylbenzene structure can be obtained.
  • the charging ratio of the compound having a (2-bromoethyl)benzene structure is preferably 1.0 to 4.0 times per mole of the bishalogenated methylaryl compound (or bishydroxymethylaryl compound, etc.). , more preferably from 1.0 to 3.0, even more preferably from 1.0 to 2.0.
  • the charging ratio is 4.0 times or less, significant precipitation of crystals can be avoided when the resin solution containing the compound represented by formula (1) is refrigerated or frozen. Further, if the charging ratio is 1.0 times or more, significant formation of high molecular weight substances can be avoided and purification by washing with water becomes possible.
  • the content of the compound where n in the formula (5) is 1 is determined using slice data of a chromatogram using an RI (differential refractive index) detector of GPC analysis. of the slice data corresponding to the compound where n in formula (5) is 1 with respect to the total area (time integral value of signal value) of the slice data corresponding to the compound represented by formula (5). It can be determined from the area ratio (area percentage).
  • the content (area percentage) of the compound where n in the formula (5) is 1 is preferably 25 to 75%, more preferably 30 to 60%, even more preferably 35 to 50%. be.
  • Examples of compounds having a (2-bromoethyl)benzene structure include (2-bromoethyl)benzene, 1-(2-bromoethyl)-2-methylbenzene, 1-(2-bromoethyl)-3-methylbenzene, 1- (2-bromoethyl)-4-methylbenzene, 1-(2-bromoethyl)-2,3-dimethylbenzene, 1-(2-bromoethyl)-2,4-dimethylbenzene, 1-(2-bromoethyl)-2 , 5-dimethylbenzene, 1-(2-bromoethyl)-2,6-dimethylbenzene and the like, but are not limited to these.
  • the number of carbon atoms may be used alone or in combination of two or more.
  • the number of carbon atoms is large, solvent solubility improves, but heat resistance decreases, so it is preferable that the number of carbon atoms is unsubstituted or substituted with an alkyl group having 1 to 3 carbon atoms. It is more preferably substituted with a group, and most preferably unsubstituted or substituted with a methyl group.
  • Examples of the bishalogenated methylaryl compound include schreib-xylylene difluoride, m-xylylene difluoride, p-xylylene difluoride, Occasionally-xylylene dichloride, m-xylylene dichloride, p-xylylene dichloride, Examples include, but are not limited to, o-xylylene dibromide, m-xylylene dibromide, p-xylylene dibromide, Occasionally-xylylene diiodide, m-xylylene diiodide, p-xylylene diiodide, etc. isn't it. These may be used alone or in combination of two or more. From the viewpoint of reactivity of raw materials during synthesis, chloride compounds, bromide compounds, and iodide compounds are preferred, and chloride compounds and bromide compounds are more preferred.
  • Examples of the bishydroxymethylaryl compound include, but are not limited to, schreib-benzenedimethanol, m-benzenedimethanol, p-benzenedimethanol, and the like. These may be used alone or in combination of two or more.
  • the amount used is preferably 0.05 to 0.8 parts by mass, more preferably 0.1 to 0.6 parts by mass, per 1 part by mass of the compound having a (2-bromoethyl)benzene structure. be.
  • the amount of the catalyst used is 0.05 to 0.8 mol, preferably 0.1 to 0.7 mol, per 1 mol of the compound having a (2-bromoethyl)benzene structure. If the amount of catalyst used is too large, the viscosity of the reaction solution may be too high and stirring may become difficult, while if it is too small, the progress of the reaction may be slowed down.
  • the reaction may be carried out using an organic solvent such as hexane, cyclohexane, octane, toluene, xylene, etc., selected as necessary, or may be carried out without a solvent.
  • the catalyst for example, after adding an acidic catalyst to a mixed solution of a compound having a (2-bromoethyl)benzene structure, a halogenated methylaryl compound, and a solvent, if the catalyst contains water, water is removed from the system by azeotropy. Thereafter, the reaction is carried out at 40 to 180°C, preferably 50 to 170°C, for 0.5 to 40 hours.
  • the acidic catalyst may be neutralized with an aqueous alkali solution, but it is also possible to proceed to the water washing step without neutralization. In the water washing process, a water-insoluble organic solvent is added to the oil layer and water washing is repeated until the wastewater becomes neutral.
  • the softening point of the compound represented by formula (5) is preferably 80°C or lower, more preferably 70°C or lower.
  • the viscosity when the compound represented by the formula (5) is induced into the compound represented by the formula (1) becomes low. This makes it easy to ensure fluidity, does not impair the impregnation of fibrous materials such as glass cloth and carbon fibers, and makes it possible to semi-cure the curable resin composition, such as by making it into a prepreg (B staging) becomes easier. If the viscosity is lowered by increasing the amount of diluting solvent, the curable resin composition may not adhere sufficiently to the fibrous material during the impregnation step.
  • the compound of this embodiment and the curable resin composition may contain a polymerization inhibitor.
  • a polymerization inhibitor By containing a polymerization inhibitor, storage stability is improved and the reaction initiation temperature can be controlled. By controlling the reaction initiation temperature, fluidity can be easily ensured, impregnating properties into glass cloth etc. are not impaired, and B-stage formation such as prepreg formation is facilitated. If the polymerization reaction progresses too much during prepreg formation, problems such as difficulty in lamination during the lamination process are likely to occur.
  • the polymerization inhibitor may be added when synthesizing the compound represented by formula (1), or may be added after synthesis.
  • the amount of the polymerization inhibitor used is 0.008 to 1 part by weight, preferably 0.01 to 0.5 part by weight, based on 100 parts by weight of the compound represented by formula (1).
  • polymerization inhibitors examples include phenol-based, sulfur-based, phosphorus-based, hindered amine-based, nitroso-based, nitroxyl radical-based, and the like. Furthermore, one kind of polymerization inhibitor may be used or a plurality of them may be used in combination. Among these, in this embodiment, phenol type, hindered amine type, nitroso type, and nitroxyl radical type are preferable.
  • phenolic polymerization inhibitor examples include 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-p-ethylphenol, and stearyl- ⁇ -( 3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,4-bis-(n-octylthio) Monophenols such as -6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, 2,4-bis[(octylthio)methyl]-o-cresol, 2 , 2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-
  • sulfur-based polymerization inhibitor examples include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, and the like. However, it is not limited to these.
  • Examples of the phosphorus polymerization inhibitor include triphenyl phosphite, diphenylisodecyl phosphite, phenyl diisodecyl phosphite, tris(nonylphenyl) phosphite, diisodecylpentaerythritol phosphite, tris(2,4-di-t -butylphenyl) phosphite, cyclic neopentanetetryrubis(octadecyl)phosphite, cyclic neopentanetetryruby(2,4-di-t-butylphenyl)phosphite, cyclic neopentanetetryruby(2, 4-di-t-butyl-4-methylphenyl) phosphite, bis[2-t-butyl-6-methyl-4- ⁇ 2-(octadecyloxy
  • hindered amine polymerization inhibitor examples include ADEKA STAB LA-40MP, ADEKA STAB LA-40Si, ADEKA STAB LA-402AF, ADEKA STAB LA-87, ADEKA STAB LA-82, ADEKA STAB LA-81, ADEKA STAB LA- 77Y, ADK STAB LA-77G, ADK STAB LA-72, ADK STAB LA-68, ADK STAB LA-63P, ADK STAB LA-57, ADK STAB LA-52, Chimassorb2020FDL, Chimassorb944FDL, Chimassorb944LD, Ti manufactured by BASF Japan Co., Ltd.
  • nuvin622SF TinuvinPA144, Tinuvin765, Tinuvin770DF , TinuvinXT55FB, Tinuvin111FDL, Tinuvin783FDL, Tinuvin791FB, etc., but are not limited to these.
  • nitroso-based polymerization inhibitor examples include, but are not limited to, p-nitrosophenol, N-nitrosodiphenylamine, ammonium salt of N-nitrosophenylhydroxyamine (cuperone), and the like. Among these, preferred is the ammonium salt of N-nitrosophenylhydroxyamine (cuperone).
  • nitroxyl radical polymerization inhibitor examples include di-tert-butyl nitroxide, 2,2,6,6-tetramethylpiperidine-1-oxyl, 4-hydroxy-2,2,6,6- Tetramethylpiperidine-1-oxyl, 4-oxo-2,2,6,6-tetramethylpiperidine-1-oxyl, 4-amino-2,2,6,6-tetramethylpiperidine-1-oxyl, 4- Methoxy-2,2,6,6-tetramethylpiperidine-1-oxyl, 4-acetoxy-2,2,6,6-tetramethylpiperidine-1-oxyl, 4-benzoyloxy-2,2,6,6 Examples include, but are not limited to, -tetramethylpiperidine-1-oxyl and the like.
  • the curable resin composition of this embodiment may contain a polyphenylene ether compound.
  • the polyphenylene ether compound is preferably a polyphenylene ether compound having an ethylenically unsaturated bond, and more preferably a polyphenylene ether compound having an acrylic group, methacrylic group, or styrene structure.
  • Commercially available products include SA-9000 (manufactured by SABIC, a polyphenylene ether compound having a methacrylic group) and OPE-2St 1200 (manufactured by Mitsubishi Gas Chemical Co., Ltd., a polyphenylene ether compound having a styrene structure).
  • the number average molecular weight (Mn) of the polyphenylene ether compound is preferably from 500 to 5,000, more preferably from 2,000 to 5,000, and even more preferably from 2,000 to 4,000. If the molecular weight is less than 500, the cured product tends to have insufficient heat resistance. Furthermore, if the molecular weight is greater than 5,000, the melt viscosity becomes high and sufficient fluidity cannot be obtained, which tends to result in poor molding. In addition, the reactivity decreases, and the curing reaction takes a long time, and unreacted substances increase without being incorporated into the curing system, lowering the glass transition temperature of the cured product and reducing the heat resistance of the cured product.
  • the number average molecular weight of the polyphenylene ether compound is 500 to 5000, excellent heat resistance, moldability, etc. can be exhibited while maintaining excellent dielectric properties. Note that the number average molecular weight here can be specifically measured using gel permeation chromatography or the like.
  • the polyphenylene ether compound may be one obtained by a polymerization reaction, or one obtained by subjecting a high molecular weight polyphenylene ether compound having a number average molecular weight of about 10,000 to 30,000 to a redistribution reaction.
  • radical polymerizability may be imparted to these raw materials by reacting them with a compound having an ethylenically unsaturated bond, such as methacryl chloride, acrylic chloride, or chloromethylstyrene.
  • the polyphenylene ether compound obtained by the redistribution reaction is obtained, for example, by heating a high molecular weight polyphenylene ether compound in a solvent such as toluene in the presence of a phenol compound and a radical initiator to cause a redistribution reaction.
  • the polyphenylene ether compound obtained by this redistribution reaction has hydroxyl groups derived from phenolic compounds that contribute to curing at both ends of the molecular chain, and therefore can maintain even higher heat resistance. This is preferable because functional groups can be introduced at both ends of the molecular chain even after modification with a compound having a sexually unsaturated bond. Further, polyphenylene ether compounds obtained by polymerization reactions are preferred because they exhibit excellent fluidity.
  • the molecular weight of the polyphenylene ether compound can be adjusted by adjusting the polymerization conditions, etc. Further, in the case of a polyphenylene ether compound obtained by a redistribution reaction, the molecular weight of the obtained polyphenylene ether compound can be adjusted by adjusting the conditions of the redistribution reaction. More specifically, it may be possible to adjust the amount of the phenolic compound used in the redistribution reaction. That is, the larger the amount of the phenolic compound blended, the lower the molecular weight of the resulting polyphenylene ether compound.
  • poly(2,6-dimethyl-1,4-phenylene ether) or the like can be used as the high molecular weight polyphenylene ether compound that undergoes the redistribution reaction.
  • the phenolic compound used in the redistribution reaction is not particularly limited, but for example, a polyfunctional phenol having two or more phenolic hydroxyl groups in the molecule, such as bisphenol A, phenol novolak, cresol novolak, etc. type compounds are preferably used. These may be used alone or in combination of two or more.
  • the content of the polyphenylene ether compound is not particularly limited, but it is preferably 5 to 1000 parts by mass, more preferably 10 to 750 parts by mass, based on 100 parts by mass of the compound represented by formula (1). preferable.
  • a cured product not only has excellent heat resistance but also fully exhibits the excellent dielectric properties of the polyphenylene ether compound.
  • the curable resin composition of this embodiment may contain polybutadiene and a modified product thereof.
  • Polybutadiene and its modified products are polybutadiene or compounds having a structure derived from polybutadiene in the molecule. In the structure derived from polybutadiene, some or all of the unsaturated bonds may be converted into single bonds by hydrogenation.
  • Examples of polybutadiene and modified products thereof include, but are not limited to, polybutadiene, hydroxyl group-terminated polybutadiene, terminal (meth)acrylated polybutadiene, carboxylic acid-terminated polybutadiene, amine-terminated polybutadiene, styrene-butadiene rubber, etc. .
  • polybutadiene or styrene-butadiene rubber is preferred from the viewpoint of dielectric properties.
  • SBR styrene-butadiene rubber
  • examples of styrene-butadiene rubber (SBR) include RICON-100, RICON-181, RICON-184 (all manufactured by Clay Valley), and 1,2-SBS (manufactured by Nippon Soda)
  • examples of polybutadiene include: Examples include B-1000, B-2000, and B-3000 (all manufactured by Nippon Soda Co., Ltd.).
  • the weight average molecular weight of polybutadiene and styrene-butadiene rubber is preferably 500 to 10,000, more preferably 750 to 7,500, and even more preferably 1,000 to 5,000.
  • the amount of volatilization is large, making it difficult to adjust the solid content during preparation of prepreg, and above the upper limit of the above range, compatibility with other curable resins deteriorates.
  • compounds containing heteroatoms such as oxygen and nitrogen, such as bismaleimide and polymaleimide due to their polarity, compounds consisting mainly of hydrocarbons or compounds consisting only of hydrocarbons have low polarity. It is difficult to ensure compatibility with other compounds.
  • the compound represented by formula (1) itself does not have a skeleton design that actively introduces heteroatoms such as oxygen or nitrogen, so it is a material with low polarity and low dielectric properties, It also has excellent compatibility with compounds composed only of hydrocarbons.
  • the content of polybutadiene and its modified product is not particularly limited, but it is preferably 5 to 1000 parts by mass, and 10 to 750 parts by mass, based on 100 parts by mass of the compound represented by formula (1). is more preferable. It is preferable that the polybutadiene and its modified products are within the above range, since not only are they excellent in heat resistance, but also cured products can be obtained that fully exhibit the excellent dielectric properties of the polybutadiene and its modified products.
  • the curable resin composition of this embodiment may contain polystyrene and a modified product thereof.
  • Polystyrene and modified products thereof are polystyrene or compounds having a structure derived from polystyrene in the molecule.
  • Examples of polystyrene and its modified products include polystyrene, styrene/2-isopropenyl-2-oxazoline copolymer (Epocross RPS-1005, RP-61, both manufactured by Nippon Shokubai Co., Ltd.), and SEP (styrene-ethylene/propylene copolymer).
  • SEPTON 1020 manufactured by Kuraray Co., Ltd.
  • SEPS styrene-ethylene propylene-styrene copolymer: SEPTON 2002, SEPTON 2004F, SEPTON 2005, SEPTON 2006, SEPTON 2063, SEPTON 2104 manufactured by Kuraray Co., Ltd.
  • SEEPS Styrene - Ethylene/ethylene propylene-styrene block copolymer: SEPTON 4003, SEPTON 4044, SEPTON 4055, SEPTON 4077, SEPTON 4099 (all manufactured by Kuraray), SEBS (styrene-ethylene/butylene-styrene block copolymer: SEPTON 8004) , SEPTON 8006, SEPTON 8007L (all manufactured by Kuraray), SEEPS-OH (a compound having a hydroxyl group at the end of a styrene-ethylene/ethylene propylene-styrene block copolymer: SEPTON HG
  • Polystyrene and its modified products have higher heat resistance and are less susceptible to oxidative deterioration, so polystyrenes that do not have unsaturated bonds are preferred.
  • the weight average molecular weight of polystyrene and its modified products is not particularly limited as long as it is 10,000 or more, but if it is too large, in addition to polyphenylene ether compounds, low molecular weight components with weight average molecular weights of about 50 to 1,000 and weight average molecular weights of 1,000 to 1,000 are used.
  • the molecular weight is preferably about 10,000 to 300,000, since the compatibility with oligomer components of about 5,000 will deteriorate and it will be difficult to ensure mixing and solvent stability.
  • the content of polystyrene and its modified product is not particularly limited, but it is preferably 5 to 1000 parts by mass, and 10 to 750 parts by mass, based on 100 parts by mass of the compound represented by formula (1). is more preferable.
  • a cured product not only has excellent heat resistance but also fully exhibits the excellent dielectric properties of polystyrene and its modified products.
  • the curable resin composition of this embodiment may contain an inorganic filler.
  • inorganic fillers include fused silica, crystalline silica, porous silica, alumina, zircon, calcium silicate, calcium carbonate, quartz powder, silicon carbide, silicon nitride, boron nitride, zirconia, aluminum nitride, graphite, forsterite, Examples include, but are not limited to, powders such as steatite, spinel, mullite, titania, talc, clay, iron oxide asbestos, glass powder, and inorganic fillers made of these in spherical or crushed shapes. It's not a thing. Further, these may be used alone or in combination.
  • the amount of inorganic filler used when obtaining a curable resin composition for semiconductor encapsulation is preferably 80 to 92 parts by mass, more preferably 83 to 90 parts by mass, based on 100 parts by mass of the curable resin composition. be.
  • the amount of the above-mentioned inorganic filler used is 100 parts by mass of the curable resin composition.
  • the amount is preferably 5 to 80 parts by weight, more preferably 10 to 60 parts by weight.
  • the curability of the curable resin composition of this embodiment can also be improved by adding a curing accelerator.
  • curing accelerators include anionic curing accelerators that promote the curing reaction by generating anions by irradiation or heating with ultraviolet rays or visible light, or anionic curing accelerators that promote the curing reaction by generating cations by irradiating or heating ultraviolet rays or visible light. Cationic curing accelerators are preferred.
  • anionic curing accelerators examples include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, and benzyldimethyl.
  • imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole
  • trialkylamines such as triethylamine and tributylamine
  • 4-dimethylaminopyridine 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, etc.
  • 4-dimethylaminopyridine, 1,8-diazabicyclo(5, 4,0)-undecene is preferred.
  • phosphines such as triphenylphosphine
  • quaternary ammonium salts such as tetrabutylammonium salt, triisopropylmethylammonium salt, trimethyldecanylammonium salt, cetyltrimethylammonium salt, and hexadecyltrimethylammonium hydroxide.
  • cationic curing accelerators include quaternary phosphonium salts such as triphenylbenzylphosphonium salt, triphenylethylphosphonium salt, and tetrabutylphosphonium salt (the counter ion of the quaternary salt is halogen, organic Acid ions, hydroxide ions, etc.
  • tin octylate zinc carboxylate (zinc 2-ethylhexanoate, zinc stearate, behenic acid)
  • examples include, but are not limited to, transition metal compounds (transition metal salts) such as zinc, zinc myristate) and zinc phosphate esters (octyl zinc phosphate, zinc stearyl phosphate). Further, these may be used alone or in combination.
  • the amount of the curing accelerator used is 0.01 to 5.0 parts by mass, if necessary, based on 100 parts by mass of the total nonvolatile components excluding inorganic fillers in the curable resin composition.
  • Polymerization initiator The curability of the curable resin composition of this embodiment can also be improved by adding a polymerization initiator.
  • Polymerization initiators are compounds that can polymerize olefin functional groups such as ethylenically unsaturated bonds, and include olefin metathesis polymerization initiators, anionic polymerization initiators, cationic polymerization initiators, and radical polymerization initiators. Can be mentioned. Among these, it is preferable to use a radical polymerization initiator that has curability and appropriate stability.
  • a radical polymerization initiator is a compound that generates radicals upon irradiation with ultraviolet rays or visible light or heating, and initiates a chain polymerization reaction.
  • radical polymerization initiators include organic peroxides, azo compounds, and benzopinacols.
  • organic peroxides examples include ketone peroxides such as methyl ethyl ketone peroxide and acetylacetone peroxide, diacyl peroxides such as benzoyl peroxide, dicumyl peroxide, and 1,3-bis-(t-butyl peroxide).
  • ketone peroxides such as methyl ethyl ketone peroxide and acetylacetone peroxide
  • diacyl peroxides such as benzoyl peroxide, dicumyl peroxide, and 1,3-bis-(t-butyl peroxide).
  • (oxyisopropyl)-dialkyl peroxides such as benzene, peroxyketals such as t-butylperoxybenzoate, 1,1-di-t-butylperoxycyclohexane, ⁇ -cumylperoxyneodecanoate, t- Butylperoxyneodecanoate, t-butylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-amylperoxy-2-ethylhexanoate, t -Butylperoxy-2-ethylhexanoate, t-amylperoxy-3,5,5-trimethylhexanoate, t-butylperoxy-3,5,5-trimethylhexanoate, t-amylperoxy-3,5,5-trimethylhexanoate Alkyl peresters such as oxybenzoate, di-2-ethy
  • azo compounds include azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile), and the like. However, it is not limited to these. Further, these may be used alone or in combination.
  • the amount of the polymerization initiator added is preferably 0.01 to 5 parts by mass, and 0.01 to 5 parts by mass, when the total nonvolatile content excluding inorganic fillers in the curable resin composition is 100 parts by mass. 3 parts by mass is particularly preferred. If the amount of the polymerization initiator used is less than 0.01 parts by mass, the molecular weight may not be sufficiently extended during the polymerization reaction, and if it is more than 5 parts by mass, dielectric properties such as dielectric constant and dielectric loss tangent may be impaired.
  • the curable resin composition of this embodiment may contain a flame retardant.
  • flame retardants include halogen-based flame retardants, inorganic flame retardants (antimony compounds, metal hydroxides, nitrogen compounds, boron compounds, etc.), phosphorus-based flame retardants, etc., but halogen-free flame retardance has been achieved. From this viewpoint, phosphorus-based flame retardants are preferred.
  • the above-mentioned phosphorus-based flame retardant may be a reactive type flame retardant or an additive type flame retardant.
  • trimethyl phosphate triethyl phosphate, tricresyl phosphate, tricylenyl phosphate, cresyl diphenyl phosphate, cresyl-di-2,6-xylenyl phosphate, 1,3-phenylenebis(dixylenyl phosphate).
  • phosphoric acid esters such as 1,4-phenylenebis(dixylenyl phosphate), 4,4'-biphenyl(dixylenyl phosphate), 9,10-dihydro-9-oxa-10-phosphaphenanthrene-
  • epoxy resins are reacted with the active hydrogen of the phosphanes.
  • the resulting phosphorus-containing epoxy compounds include, but are not limited to, red phosphorus and the like. Further, these may be used alone or in combination.
  • phosphoric acid esters, phosphanes, or phosphorus-containing epoxy compounds are preferred, and 1,3-phenylene bis(dixylenyl phosphate), 1,4-phenylene bis(dixylenyl phosphate), 4,4 '-Biphenyl (dixylenyl phosphate) or phosphorus-containing epoxy compounds are particularly preferred.
  • the content of the flame retardant is preferably in the range of 0.1 to 0.6 parts by mass, when the total nonvolatile content excluding inorganic fillers in the curable resin composition is 100 parts by mass. If it is less than 0.1 parts by mass, the flame retardance may be insufficient, and if it is more than 0.6 parts by mass, it may adversely affect the hygroscopicity and dielectric properties of the cured product.
  • a light stabilizer may be used in the curable resin composition of this embodiment.
  • hindered amine light stabilizers particularly HALS, etc. are suitable.
  • HALS include dibutylamine/1,3,5-triazine/N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-( 2,2,6,6-tetramethyl-4-piperidyl)butylamine reaction product, dimethyl-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine succinate reaction product , poly[ ⁇ 6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl ⁇ (2,2,6,6-tetramethyl-4- piperidyl)imino ⁇ hexamethylene ⁇ (2,2,6,6-tetramethyl-4-piperidyl)imino ⁇ ], bis(1,2,
  • the content of the light stabilizer is preferably in the range of 0.001 to 10 parts by mass, when the total nonvolatile content excluding inorganic fillers in the curable resin composition is 100 parts by mass. If it is less than 0.001 parts by mass, it may be insufficient to exhibit a photostabilizing effect, and if it is more than 10 parts by mass, it may adversely affect the hygroscopicity and dielectric properties of the cured product.
  • the curable resin composition of this embodiment may use a binder resin.
  • the binder resin include butyral resin, acetal resin, acrylic resin, epoxy-nylon resin, NBR-phenol resin, epoxy-NBR resin, silicone resin, etc., but are not limited to these. It's not something you can do. Further, these may be used alone or in combination.
  • the blending amount of the binder resin is preferably within a range that does not impair the flame retardancy and heat resistance of the cured product, and the total nonvolatile content excluding inorganic fillers in the curable resin composition is 100 parts by mass. If so, the amount is preferably 0.05 to 50 parts by weight, more preferably 0.05 to 20 parts by weight.
  • the curable resin composition of this embodiment may use additives.
  • additives include modified acrylonitrile copolymers, polyethylene, fluororesins, silicone gels, silicone oils, surface treatment agents for fillers such as silane coupling agents, mold release agents, carbon black, phthalocyanine blue, Examples include colorants such as phthalocyanine green.
  • the blending amount of the additive is preferably 1,000 parts by mass or less, more preferably 700 parts by mass or less, based on 100 parts by mass of the curable resin composition.
  • the curable resin composition of this embodiment further includes an epoxy resin, an active ester compound, a phenol resin, an amine resin, a maleimide compound, a compound having an ethylenically unsaturated bond, an isocyanate resin, a polyamide resin, a polyimide resin, and a cyanate ester resin. etc., and these may be used alone or in combination.
  • these compounds it is preferable to contain a compound having an ethylenically unsaturated bond and a cyanate ester resin in view of the balance of heat resistance, adhesion, and dielectric properties.
  • the amount of the compound to be used is preferably 10 times or less, more preferably 5 times or less, particularly preferably 3 times or less by mass, relative to the compound represented by formula (1). mass range. Further, a preferable lower limit is 0.1 times by mass or more, more preferably 0.25 times by mass or more, still more preferably 0.5 times by mass or more. By being within the above range, the effects of each compound added can be added while taking advantage of the effects of the heat resistance and dielectric properties of the compound represented by the formula (1). Regarding these components, those illustrated below can be used.
  • epoxy resin Preferred examples of the epoxy resin are shown below, but the invention is not limited thereto.
  • the epoxy resin may be liquid or solid, and may be used alone or in combination.
  • liquid epoxy resins examples include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AF epoxy resin, naphthalene epoxy resin, glycidyl ester epoxy resin, glycidylamine epoxy resin, phenol novolac epoxy resin, and ester.
  • examples include alicyclic epoxy resins having a skeleton, cyclohexane-type epoxy resins, cyclohexanedimethanol-type epoxy resins, glycidylamine-type epoxy resins, and epoxy resins having a butadiene structure.
  • solid epoxy resin examples include bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, Biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, tetraphenylethane type epoxy resin are preferred, naphthol type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin and biphenyl-type epoxy resins.
  • HP4032H manufactured by DIC, naphthalene type epoxy resin
  • HP-4700 manufactured by DIC
  • HP-4710 all of the above are naphthalene type tetrafunctional epoxy resins, manufactured by DIC
  • N-690 manufactured by DIC
  • the active ester compound refers to a compound that contains at least one ester bond in its structure and has an aliphatic chain, an aliphatic ring, or an aromatic ring bonded to both sides of the ester bond.
  • Examples of active ester compounds include compounds having two or more ester groups with high reaction activity in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds. It can be obtained by a condensation reaction of at least one of a carboxylic acid compound, an acid chloride, or a thiocarboxylic acid compound and at least one of a hydroxy compound or a thiol compound.
  • a carboxylic acid compound or an acid chloride and a hydroxy compound it is preferable to use a carboxylic acid compound or an acid chloride and a hydroxy compound.
  • a phenol compound or a naphthol compound is preferable.
  • the active ester compounds may be used alone or in combination of two or more.
  • carboxylic acid compounds examples include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, and the like.
  • Examples of the acid chloride include acetyl chloride, acrylic chloride, methacrylic chloride, malonyl chloride, succinic dichloride, diglycolyl chloride, glutaric dichloride, suberic dichloride, sebacic dichloride, adipic dichloride, and dodecanedioyl.
  • dichloride azeroyl chloride, 2,5-furandicarbonyl dichloride, phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, trimesic acid chloride, bis(4-chlorocarbonylphenyl) ether, 4,4'-diphenyl dichloride Examples include carbonyl chloride and 4,4'-azodibenzoyl dichloride.
  • phenol compound and naphthol compound examples include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalin, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, ⁇ -naphthol, ⁇ -naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, Examples include phloroglucin, benzenetriol, dicyclopentadiene type diphenol compounds, phenol novolac, and phenol resins described below.
  • dicyclopentadiene type diphenol compound refers to a diphenol compound obtained by condensing two molecules of phenol with one molecule of dicyclopent
  • the active ester compound examples include an active ester compound containing a dicyclopentadiene type diphenol structure, an active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, and an active ester compound containing a benzoylated product of phenol novolac.
  • Examples include ester compounds, the compound described in Example 2 of International Publication No. 2020/095829, and the compound disclosed in International Publication No. 2020/059625.
  • active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene type diphenol structure are more preferable.
  • the dicyclopentadiene type diphenol structure represents a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.
  • active ester compounds include, for example, "EXB9451”, “EXB9460”, “EXB9460S”, “HPC-8000-65T”, and “HPC-8000H-” as active ester compounds containing a dicyclopentadiene type diphenol structure.
  • the ratio ( ⁇ / ⁇ ) of active ester equivalent ( ⁇ ) to epoxy equivalent ( ⁇ ) is preferably 0.5 to 1.5, more preferably 0. 8 to 1.2, more preferably 0.90 to 1.10. If it is out of the above range, there is a risk that excess epoxy groups or active ester groups may remain in the system. :85%, etc.), the characteristics may deteriorate in long-term reliability tests.
  • a phenolic resin is a compound having two or more phenolic hydroxyl groups in its molecule.
  • phenolic resins include reactants of phenols and aldehydes, reactants of phenols and diene compounds, reactants of phenols and ketones, reactants of phenols and substituted biphenyls, and phenols. Examples include, but are not limited to, reaction products of and substituted phenyls, and reaction products of bisphenols and aldehydes. Further, these may be used alone or in combination. Specific examples of each of the above-mentioned raw materials are illustrated below, but are not limited thereto.
  • Phenol alkyl-substituted phenol, aromatic substituted phenol, hydroquinone, resorcinol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.
  • ⁇ Aldehydes > Formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, furfural, etc.
  • ⁇ Diene compound Dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.
  • ⁇ Ketones Acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, fluorenone, etc.
  • ⁇ Substituted biphenyls > 4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl, 4,4'-bis(hydroxymethyl)-1,1' -Biphenyl etc.
  • ⁇ Substituted phenyls > 1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.
  • An amine resin is a compound having two or more amino groups in its molecule.
  • amine resins include diaminodiphenylmethane, diaminodiphenylsulfone, isophorone diamine, naphthalene diamine, aniline novolac (a reaction product of aniline and formalin), N-methylaniline novolac (a reaction product of N-methylaniline and formalin), orthoethyl.
  • Aniline novolac reaction product of orthoethylaniline and formalin
  • reaction product of 2-methylaniline and formalin reaction product of 2,6-diisopropylaniline and formalin
  • reaction product of 2,6-diethylaniline and formalin reaction product of 2,6-diethylaniline and formalin
  • 2-ethyl - Reaction product of 6-ethylaniline and formalin reaction product of 2,6-dimethylaniline and formalin
  • aniline resin obtained by reaction of aniline and xylylene chloride, substituted with aniline described in Japanese Patent No.
  • a maleimide compound is a compound having one or more maleimide groups in its molecule.
  • the curable resin composition of this embodiment may contain a maleimide compound.
  • maleimide compounds include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene), Zyrock-type maleimide compound (Anilix Maleimide, manufactured by Mits
  • the amount of the maleimide compound added is preferably 10 times or less, more preferably 5 times or less, particularly preferably 3 times or less by mass relative to the compound represented by formula (1) above. Further, a preferable lower limit is 0.01 times by mass or more, more preferably 0.1 times by mass or more. Within the above range, the heat resistance, dielectric properties, and low water absorption effects of the compound represented by formula (1) can be utilized.
  • a compound containing an ethylenically unsaturated bond is a compound having one or more ethylenically unsaturated bonds in its molecule that can be polymerized by heat or light, regardless of whether a polymerization initiator is used or not.
  • Examples of compounds containing ethylenically unsaturated bonds include the above-mentioned phenolic resins and halogenated compounds containing ethylenically unsaturated bonds (chloromethylstyrene, allyl chloride, methallyl chloride, acrylic acid chloride, methacrylic acid chloride, etc.) reactants, phenols containing ethylenically unsaturated bonds (2-allylphenol, 2-propenylphenol, 4-allylphenol, 4-propenylphenol, eugenol, isoeugenol, etc.) and halogen compounds (1,4-bis( (chloromethyl)benzene, 4,4'-bis(chloromethyl)biphenyl, 4,4'-difluorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-dibromobenzophenone, cyanuric chloride, etc.), epoxy Examples include, but are not limited to, reaction products of resins or
  • An isocyanate resin is a compound having two or more isocyanate groups in its molecule.
  • Examples of the isocyanate resin include p-phenylene diisocyanate, m-phenylene diisocyanate, p-xylene diisocyanate, m-xylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate.
  • aromatic diisocyanates such as naphthalene diisocyanate, aliphatic or alicyclic diisocyanates such as isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hydrogenated xylene diisocyanate, norbornene diisocyanate, lysine diisocyanate, isocyanate monomers
  • polyisocyanates such as isocyanate bodies obtained by trimerizing one or more types of burettes or the above diisocyanate compounds, and polyisocyanates obtained by a urethanization reaction between the above isocyanate compounds and a polyol compound. It's not a thing. Further, these may be used alone or in combination.
  • polyamide resin examples include a reaction product of dicarboxylic acid with one or more of diamine, diisocyanate, and oxazoline, a reaction product of diamine and acid chloride, and a ring-opening polymer of a lactam compound. Further, these may be used alone or in combination. Specific examples of each of the above-mentioned raw materials are illustrated below, but are not limited thereto.
  • ⁇ Dicarboxylic acid> Oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, terephthalic acid, isophthalic acid, 5-hydroxyisophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, cyclohexanedicarboxylic acid, biphenyldicarboxylic acid, naphthalenedicarboxylic acid, benzophenonedicarboxylic acid, furandicarboxylic acid, 4 , 4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfide, etc.
  • ⁇ Acid chloride Acetyl chloride, acrylic acid chloride, methacrylic acid chloride, malonyl chloride, succinic acid dichloride, diglycolyl chloride, glutaric acid dichloride, suberic acid dichloride, sebacyl dichloride, adipic acid dichloride, dodecanedioyl dichloride, azeloyl chloride, 2, 5-furandicarbonyl dichloride, phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, trimesic acid chloride, bis(4-chlorocarbonylphenyl)ether, 4,4'-diphenyldicarbonyl chloride, 4,4'-azo Dibenzoyl dichloride etc.
  • ⁇ Lactam > ⁇ -caprolactam, ⁇ -undecanelactam, ⁇ -laurolactam, etc.
  • polyimide resin examples include, but are not limited to, reaction products of the diamines described above and tetracarboxylic dianhydrides exemplified below. Further, these may be used alone or in combination.
  • Cyanate ester resin is a cyanate ester compound obtained by reacting a phenolic resin with cyanogen halide, and specific examples include dicyanatobenzene, tricyanatobenzene, dicyanatonaphthalene, dicyanatobiphenyl, 2, 2'-bis(4-cyanatophenyl)propane, bis(4-cyanatophenyl)methane, bis(3,5-dimethyl-4-cyanatophenyl)methane, 2,2'-bis(3,5- Dimethyl-4-cyanatophenyl)propane, 2,2'-bis(4-cyanatophenyl)ethane, 2,2'-bis(4-cyanatophenyl)hexafluoropropane, bis(4-cyanatophenyl) Examples include, but are not limited to, sulfone, bis(4-cyanatophenyl)thioether, phenol novolac cyanate, and those obtained
  • cyanate ester compounds whose synthesis method is described in Japanese Patent Application Laid-open No. 2005-264154 are particularly preferred as cyanate ester compounds because they have low moisture absorption, excellent flame retardancy, and excellent dielectric properties.
  • the cyanate ester resin can optionally trimerize cyanate groups to form a sym-triazine ring. Catalysts such as lead acetylacetonate and dibutyltin maleate can also be included.
  • the catalyst is preferably used in an amount of 0.0001 to 0.10 parts by weight, preferably 0.00015 to 0.0015 parts by weight, per 100 parts by weight of the cyanate ester resin.
  • the curable resin composition of this embodiment is obtained by preparing the above-mentioned components in a predetermined ratio, is precured at 130 to 180°C for 30 to 500 seconds, and is further cured at 150 to 200°C for 200 to 200 seconds. By post-curing for ⁇ 15 hours, a sufficient curing reaction proceeds, and the cured product of this embodiment is obtained.
  • the components of the curable resin composition can be uniformly dispersed or dissolved in a solvent or the like, and the composition can be cured after removing the solvent.
  • the method for preparing the curable resin composition of this embodiment is not particularly limited, but the components may be simply mixed uniformly or may be prepolymerized. For example, by heating a mixture of the compound represented by formula (1) and other compounds in the presence or absence of a curing accelerator or polymerization initiator, and in the presence or absence of a solvent. Convert into prepolymer. Similarly, compounds such as amine compounds, compounds having ethylenically unsaturated bonds, maleimide compounds, cyanate ester compounds, polybutadiene and modified products thereof, polystyrene and modified products thereof, inorganic fillers, and other additives are added to preform. It may also be made into a polymer.
  • an extruder, kneader, roll, etc. are used in the absence of a solvent, and a reaction vessel equipped with a stirring device, etc., is used in the presence of a solvent.
  • the method for uniformly mixing is to knead the resin composition using a device such as a kneader, roll, or planetary mixer at a temperature within the range of 50 to 100° C. to obtain a uniform resin composition.
  • a device such as a kneader, roll, or planetary mixer
  • a curable resin composition molded product by melting it and molding it into a sheet with a thickness of 0.05 mm to 10 mm.
  • the obtained molded product becomes a non-sticky molded product at 0 to 20°C, and its fluidity and hardenability hardly decrease even if it is stored at -25 to 0°C for one week or more.
  • the obtained molded product can be molded into a cured product using a transfer molding machine or a compression molding machine.
  • the curable resin composition of this embodiment can also be made into a varnish-like composition (hereinafter simply referred to as varnish) by adding an organic solvent.
  • the curable resin composition of this embodiment is dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethyl formamide, dimethyl acetamide, N-methyl pyrrolidone, etc. as necessary to form a varnish, which can be applied to glass fibers or carbon.
  • a cured product of the curable resin composition of this embodiment is obtained by hot press molding a prepreg obtained by impregnating a base material such as fiber, polyester fiber, polyamide fiber, alumina fiber, or paper and drying by heating.
  • the solvent used in this case is used in an amount that accounts for 10 to 70% by weight, preferably 15 to 70% by weight in the mixture of the curable resin composition of the present embodiment and the solvent. Further, if the composition is a liquid composition, a cured resin containing carbon fibers can be obtained as it is, for example, by the RTM method.
  • the curable composition of this embodiment can also be used as a modifier for film-type compositions. Specifically, it can be used to improve flexibility in the B-stage.
  • a film-type resin composition is obtained by applying the curable resin composition of the present embodiment as the curable resin composition varnish onto a release film, removing the solvent under heating, and then B-staging it. By doing this, a sheet-like adhesive is obtained.
  • This sheet adhesive can be used as an interlayer insulating layer in multilayer substrates and the like.
  • a prepreg can also be obtained by heating and melting the curable resin composition of this embodiment, reducing the viscosity, and impregnating it into reinforcing fibers such as glass fibers, carbon fibers, polyester fibers, polyamide fibers, and alumina fibers.
  • reinforcing fibers such as glass fibers, carbon fibers, polyester fibers, polyamide fibers, and alumina fibers.
  • Specific examples include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, as well as inorganic fibers other than glass and polyester fibers.
  • Examples include, but are not limited to, paraphenylene terephthalamide (Kevlar (registered trademark), manufactured by DuPont), fully aromatic polyamide, polyester, polyparaphenylenebenzoxazole, polyimide, and organic fibers such as carbon fiber.
  • the shape of the base material is not particularly limited, and examples thereof include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like.
  • plain weaving, Nanako weaving, twill weaving, etc. are known as weaving methods of the woven fabric, and the weaving method can be appropriately selected from these known methods depending on the intended use and performance.
  • woven fabrics subjected to opening treatment or glass woven fabrics whose surface is treated with a silane coupling agent or the like are preferably used.
  • the thickness of the base material is not particularly limited, but is preferably about 0.01 to 0.4 mm. Further, a prepreg can also be obtained by impregnating reinforcing fibers with the varnish and drying the impregnated fibers by heating.
  • a laminate can also be manufactured using the above prepreg.
  • the laminate is not particularly limited as long as it includes one or more prepregs, and may include any other layers.
  • the method for manufacturing the laminate is not particularly limited, and any generally known method can be appropriately applied. For example, when molding a metal foil-clad laminate, a multi-stage press machine, a multi-stage vacuum press machine, a continuous molding machine, an autoclave molding machine, etc. can be used. Obtainable. At this time, the heating temperature is not particularly limited, but is preferably 65 to 300°C, more preferably 120 to 270°C.
  • the pressure to be applied is not particularly limited, but if the pressure is too high, it will be difficult to adjust the solids content of the resin in the laminate, and the quality will not be stable. If the pressure is too low, air bubbles and adhesion between the laminates may occur. 2.0 to 5.0 MPa is preferable, and 2.5 to 4.0 MPa is more preferable.
  • the laminate of this embodiment can be suitably used as a metal foil-clad laminate, which will be described later, by including a layer made of metal foil. After cutting the above prepreg into a desired shape and laminating it with copper foil etc. if necessary, the curable resin composition is heated and cured while applying pressure to the laminate using a press molding method, an autoclave molding method, a sheet winding molding method, etc. Electrical and electronic laminates (printed wiring boards) and carbon fiber reinforced materials can be obtained.
  • the curable resin composition of this embodiment can also be made into a resin sheet.
  • the curable resin composition is coated on a support film (support), and then dried, and the resin composition is coated on the support film.
  • Examples include a method of forming a layer.
  • the film softens under the laminating temperature conditions (70°C to 140°C) in the vacuum lamination method, and is present on the circuit board at the same time as the circuit board is laminated.
  • the resin exhibits fluidity (resin flow) that allows the resin to be filled in via holes or through holes, and it is preferable to mix the above-mentioned components so as to exhibit such characteristics.
  • the resulting resin sheets and circuit boards do not exhibit locally different characteristic values due to phase separation, and can maintain a constant level of performance at any location. In order to achieve this, uniformity in appearance is required.
  • the diameter of the through hole of the circuit board is 0.1 to 0.5 mm, and the depth is 0.1 to 1.2 mm, and it is preferable that resin filling is possible within this range. Note that when laminating both sides of the circuit board, it is desirable that about 1/2 of the through holes be filled.
  • the resin sheet after preparing a varnished resin composition by blending an organic solvent, applying the varnished resin composition to the surface of the support film (Y), Further, a method of forming the resin composition layer (X) by drying the organic solvent by heating or blowing hot air may be mentioned.
  • organic solvent used here examples include ketones such as acetone, methyl ethyl ketone, and cyclohexanone, acetic acid esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, cellosolve, butyl carbitol, and the like. It is preferable to use carbitols, aromatic hydrocarbons such as toluene and xylene, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc., and it is also preferable to use them in a proportion such that the nonvolatile content is 30 to 60% by mass. preferable.
  • ketones such as acetone, methyl ethyl ketone, and cyclohexanone
  • acetic acid esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene
  • the thickness of the resin composition layer (X) to be formed needs to be greater than or equal to the thickness of the conductor layer. Since the conductor layer of the circuit board has a thickness in the range of 5 to 70 ⁇ m, the resin composition layer (X) preferably has a thickness of 10 to 100 ⁇ m.
  • the said resin composition layer (X) in this embodiment may be protected with the protective film mentioned later. By protecting with a protective film, it is possible to prevent dust and the like from adhering to the surface of the resin composition layer and from scratching it.
  • the supporting film and protective film may be made of polyolefin such as polyethylene, polypropylene, or polyvinyl chloride, polyester such as polyethylene terephthalate (PET) or polyethylene naphthalate, polycarbonate, polyimide, or release paper or metal foil such as copper foil or aluminum foil. etc. can be mentioned.
  • PET polyethylene terephthalate
  • the support film and the protective film may be subjected to a release treatment in addition to mud treatment and corona treatment.
  • the thickness of the support film is not particularly limited, but is 10 to 150 ⁇ m, preferably 25 to 50 ⁇ m. Further, the thickness of the protective film is preferably 1 to 40 ⁇ m.
  • the support film (Y) is peeled off after being laminated onto the circuit board or after forming an insulating layer by heating and curing. If the support film (Y) is peeled off after the resin composition layer constituting the resin sheet is cured by heating, it is possible to prevent dust and the like from adhering during the curing process. If the support film is to be peeled off after curing, a release treatment is applied to the support film in advance.
  • a multilayer printed circuit board can be manufactured from the resin sheet obtained as described above.
  • the resin composition layer (X) is protected with a protective film, after peeling off the protective film, apply the resin composition layer (X) to one or both sides of the circuit board so as to be in direct contact with the circuit board.
  • the lamination method may be a batch method or a continuous method using rolls.
  • the resin sheet and the circuit board may be heated (preheated) before lamination.
  • the pressure bonding temperature (laminate temperature) is 70 to 140°C, and the pressure bonding pressure is 1 to 11 kgf/cm 2 (9.8 ⁇ 10 4 to 107.9 ⁇ 10 4 N/m 2 ). It is preferable that the lamination is carried out under a reduced air pressure of 20 mmHg (26.7 hPa) or less.
  • a semiconductor device can be manufactured using the curable resin composition of this embodiment.
  • semiconductor devices include DIP (dual in-line package), QFP (quad flat package), BGA (ball grid array), CSP (chip size package), SOP (small outline package), TSOP (thin small outline package), and TQFP. (Think Quad Flat Package), etc.
  • the curable resin composition of this embodiment and its cured product can be used in a wide range of fields. Specifically, it can be used for various purposes such as molding materials, adhesives, composite materials, and paints. Since the cured product of the curable resin composition described in this embodiment exhibits excellent heat resistance and dielectric properties, it can be used as an encapsulant for semiconductor devices, an encapsulant for liquid crystal display devices, an encapsulant for organic EL devices, and a laminate. Suitable for use in electrical and electronic components such as (printed wiring boards, BGA boards, build-up boards, etc.), lightweight and high-strength structural composite materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, 3D printing, etc. .
  • GPC Online degassing unit (DGU-20A3R), binary liquid feeding unit (LC-20AD), autosampler (SIL-20AHT), differential refractive index detector (RID-20A), column oven (CTO-20A), system Controller (CBM-20A) (both manufactured by Shimadzu Corporation)
  • DGU-20A3R Online degassing unit
  • LC-20AD binary liquid feeding unit
  • SIL-20AHT autosampler
  • RID-20A differential refractive index detector
  • CTO-20A column oven
  • CBM-20A system Controller
  • HP-LC Binary liquid transfer unit (LC-20AB), online degassing unit (DGU-20A3), autosampler (SIL-20A), column oven (CTO-20A), system controller (CBM-20A), photodiode Array detector (SPD-M20A) (both manufactured by Shimadzu Corporation)
  • LC-20AB Binary liquid transfer unit
  • DGU-20A3 online degassing unit
  • SIL-20A autosampler
  • CTO-20A column oven
  • CBM-20A system controller
  • SPD-M20A photodiode Array detector
  • Example 1 300 parts of BEB-1 obtained in Synthesis Example 1, 245 parts of toluene, 735 parts of dimethyl sulfoxide, and 4-hydroxy-2,2,6,6-tetramethylpiperidine were placed in a flask equipped with a thermometer, a cooling tube, and a stirrer. 0.15 parts of -1-oxyl free radicals and 146.4 parts of a 50 wt% aqueous sodium hydroxide solution were added, and the reaction was continued at 40°C for 6 hours. After washing the organic layer by adding 100 parts of water, the organic layer was returned to the reaction vessel.
  • Example 2 300 parts of BEB-1 obtained in Synthesis Example 1, 245 parts of toluene, 735 parts of dimethyl sulfoxide, and 4-hydroxy-2,2,6,6-tetramethylpiperidine were placed in a flask equipped with a thermometer, a cooling tube, and a stirrer. 0.15 parts of -1-oxyl free radicals and 107.4 parts of a 50 wt% aqueous sodium hydroxide solution were added, and the reaction was continued at 40°C for 6 hours. After washing the organic layer by adding 100 parts of water, the organic layer was returned to the reaction vessel.
  • the area ratio (area percentage) of the compound having the structure where n is 1 in formula (7) to the total area of the compound having the structure represented by formula (7) is 41%.
  • the average molecular weight of the resin component was Mn: 799, Mw: 1297).
  • the HP-LC chart is shown in FIG.
  • Example 3 300 parts of BEB-1 obtained in Synthesis Example 1, 375 parts of toluene, 1125 parts of dimethyl sulfoxide, and 4-hydroxy-2,2,6,6-tetramethylpiperidine were placed in a flask equipped with a thermometer, a cooling tube, and a stirrer. 0.15 parts of -1-oxyl free radicals and 146.4 parts of a 50 wt% aqueous sodium hydroxide solution were added, and the reaction was continued at 40°C for 6 hours. After washing the organic layer by adding 100 parts of water, the organic layer was returned to the reaction vessel.
  • the area ratio (area percentage) of the compound having a structure where n in formula (7) is 1 to the total area of the compound having the structure represented by formula (7) is 35%.
  • the average molecular weight of the resin component was Mn: 834, Mw: 1170).
  • the HP-LC chart is shown in FIG.
  • Example 4 300 parts of BEB-1 obtained in Synthesis Example 1, 245 parts of toluene, 735 parts of dimethyl sulfoxide, and 4-hydroxy-2,2,6,6-tetramethylpiperidine were placed in a flask equipped with a thermometer, a cooling tube, and a stirrer. 0.15 parts of -1-oxyl free radicals and 146.4 parts of a 50 wt% aqueous sodium hydroxide solution were added, and the reaction was continued at 25°C for 6 hours. After washing the organic layer by adding 100 parts of water, the organic layer was returned to the reaction vessel.
  • the area ratio (area percentage) of the compound having the structure where n is 1 in formula (7) to the total area of the compound having the structure represented by formula (7) is 41%.
  • the average molecular weight of the resin component was Mn: 802, Mw: 1291).
  • the HP-LC chart is shown in FIG.
  • the average value n ave of repeating units n calculated from the area percentage of the GPC chart was 2.2. Furthermore, the ratio of the area of the compound having the structure where n is 1 in formula (7) to the total area of the compound having the structure represented by formula (7) in the product (GPC area percentage) is 65 % (the average molecular weight of the resin component was Mn: 624, Mw: 778).
  • the HP-LC chart is shown in FIG.
  • the sum ⁇ of the peak areas of the compounds represented by formulas (2) to (4) in the chromatogram obtained by HPLC is calculated as "the content of the compounds V to Y in each compound.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Low-Molecular-Weight Compounds And Preparation Thereof (AREA)
  • Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
  • Heterocyclic Carbon Compounds Containing A Hetero Ring Having Oxygen Or Sulfur (AREA)
PCT/JP2023/009322 2022-03-29 2023-03-10 化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法 Ceased WO2023189424A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
CN202380031324.9A CN119032113B (zh) 2022-03-29 2023-03-10 化合物、硬化性树脂组合物及其硬化物和化合物的制造方法
KR1020247032231A KR102766816B1 (ko) 2022-03-29 2023-03-10 화합물, 혼합물, 경화성 수지 조성물 및 그의 경화물
JP2023534115A JP7353538B1 (ja) 2022-03-29 2023-03-10 化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022-054487 2022-03-29
JP2022054487 2022-03-29

Publications (1)

Publication Number Publication Date
WO2023189424A1 true WO2023189424A1 (ja) 2023-10-05

Family

ID=88200829

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/009322 Ceased WO2023189424A1 (ja) 2022-03-29 2023-03-10 化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法

Country Status (5)

Country Link
JP (1) JP7353538B1 (cg-RX-API-DMAC7.html)
KR (1) KR102766816B1 (cg-RX-API-DMAC7.html)
CN (1) CN119032113B (cg-RX-API-DMAC7.html)
TW (1) TW202406970A (cg-RX-API-DMAC7.html)
WO (1) WO2023189424A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2025159098A1 (ja) * 2024-01-26 2025-07-31 日本化薬株式会社 化合物、硬化性樹脂組成物およびその硬化物

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2021100658A1 (ja) * 2019-11-19 2021-05-27 日本化薬株式会社 化合物、混合物、硬化性樹脂組成物およびその硬化物、並びに化合物の製造方法
WO2022244728A1 (ja) * 2021-05-17 2022-11-24 パナソニックIpマネジメント株式会社 樹脂組成物、並びに、それを用いたプリプレグ、樹脂付きフィルム、樹脂付き金属箔、金属張積層板及び配線基板

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2570923B2 (ja) 1991-06-07 1997-01-16 信越化学工業株式会社 熱硬化性樹脂組成物
GB2511574B (en) 2013-03-08 2017-10-04 Magnomatics Ltd Permanent magnet assembly for mounting to a rotor
JP2020105352A (ja) * 2018-12-27 2020-07-09 日鉄ケミカル&マテリアル株式会社 硬化性樹脂組成物、プリプレグ、金属張積層板、及びプリント配線板

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2021100658A1 (ja) * 2019-11-19 2021-05-27 日本化薬株式会社 化合物、混合物、硬化性樹脂組成物およびその硬化物、並びに化合物の製造方法
WO2022244728A1 (ja) * 2021-05-17 2022-11-24 パナソニックIpマネジメント株式会社 樹脂組成物、並びに、それを用いたプリプレグ、樹脂付きフィルム、樹脂付き金属箔、金属張積層板及び配線基板

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2025159098A1 (ja) * 2024-01-26 2025-07-31 日本化薬株式会社 化合物、硬化性樹脂組成物およびその硬化物

Also Published As

Publication number Publication date
KR102766816B1 (ko) 2025-02-11
CN119032113B (zh) 2025-12-16
JPWO2023189424A1 (cg-RX-API-DMAC7.html) 2023-10-05
CN119032113A (zh) 2024-11-26
JP7353538B1 (ja) 2023-09-29
KR20240151239A (ko) 2024-10-17
TW202406970A (zh) 2024-02-16

Similar Documents

Publication Publication Date Title
JP7530537B1 (ja) 化合物および化合物の製造方法、硬化性樹脂組成物およびその硬化物
JP7551036B1 (ja) 化合物、硬化性樹脂組成物およびその硬化物
JP7340904B1 (ja) 硬化性樹脂組成物、樹脂シート、およびその硬化物
JP7353538B1 (ja) 化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法
JP2025006205A (ja) 化合物、混合物、硬化性樹脂組成物およびこれらの硬化物
JP7565403B1 (ja) 硬化性樹脂組成物およびその硬化物
JP7418644B2 (ja) マレイミド化合物、硬化性樹脂組成物及びその硬化物、並びにアミン化合物
JP7602311B1 (ja) 化合物、その製造方法、硬化性樹脂組成物およびその硬化物
JP7716605B1 (ja) 化合物、硬化性樹脂組成物およびその硬化物ならびに化合物の製造方法
JP7590495B1 (ja) 硬化性樹脂組成物およびその硬化物
JP7570449B2 (ja) 硬化性樹脂組成物およびその硬化物
JP7814626B2 (ja) 化合物、硬化性樹脂組成物およびその硬化物
JP7759530B1 (ja) 化合物、硬化性樹脂組成物およびその硬化物
JP7744267B2 (ja) 硬化性樹脂組成物、樹脂シート、およびその硬化物
JP7572496B1 (ja) 硬化性樹脂組成物およびその硬化物
JP2024161933A (ja) 硬化性樹脂組成物およびその硬化物
JP2024161934A (ja) 硬化性樹脂組成物およびその硬化物
WO2024154628A1 (ja) 混合物、硬化性樹脂組成物およびその硬化物
KR20260069594A (ko) 화합물, 그의 제조 방법, 경화성 수지 조성물 및 그의 경화물
JP2024139797A (ja) 化合物、硬化性樹脂組成物およびその硬化物
WO2026018825A1 (ja) 混合物、硬化性樹脂組成物およびその硬化物
JP2023130778A (ja) 硬化性樹脂組成物、およびその硬化物
WO2026100585A1 (ja) 硬化性樹脂組成物、プリプレグおよびそれらの硬化物
JP2024139796A (ja) 硬化性樹脂組成物、プリプレグおよびそれらの硬化物

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 2023534115

Country of ref document: JP

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23779448

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 20247032231

Country of ref document: KR

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 1020247032231

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 202380031324.9

Country of ref document: CN

Ref document number: 2401006463

Country of ref document: TH

NENP Non-entry into the national phase

Ref country code: DE

WWE Wipo information: entry into national phase

Ref document number: 11202406759P

Country of ref document: SG

122 Ep: pct application non-entry in european phase

Ref document number: 23779448

Country of ref document: EP

Kind code of ref document: A1

WWG Wipo information: grant in national office

Ref document number: 11202406759P

Country of ref document: SG

WWP Wipo information: published in national office

Ref document number: 11202406759P

Country of ref document: SG