WO2023188504A1 - 鋼板および部材、ならびに、それらの製造方法 - Google Patents

鋼板および部材、ならびに、それらの製造方法 Download PDF

Info

Publication number
WO2023188504A1
WO2023188504A1 PCT/JP2022/040833 JP2022040833W WO2023188504A1 WO 2023188504 A1 WO2023188504 A1 WO 2023188504A1 JP 2022040833 W JP2022040833 W JP 2022040833W WO 2023188504 A1 WO2023188504 A1 WO 2023188504A1
Authority
WO
WIPO (PCT)
Prior art keywords
less
steel plate
section
temperature
tempering
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/040833
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
真平 吉岡
英之 木村
佑馬 本田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JFE Steel Corp
Original Assignee
JFE Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JFE Steel Corp filed Critical JFE Steel Corp
Priority to US18/844,574 priority Critical patent/US20250179602A1/en
Priority to JP2023508472A priority patent/JP7311070B1/ja
Priority to CN202280092849.9A priority patent/CN118786234A/zh
Priority to EP22935635.7A priority patent/EP4477773A4/en
Priority to KR1020247030706A priority patent/KR20240148909A/ko
Publication of WO2023188504A1 publication Critical patent/WO2023188504A1/ja
Priority to MX2024011891A priority patent/MX2024011891A/es
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D1/00—General methods or devices for heat treatment, e.g. annealing, hardening, quenching or tempering
    • C21D1/18—Hardening; Quenching with or without subsequent tempering
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D1/00—General methods or devices for heat treatment, e.g. annealing, hardening, quenching or tempering
    • C21D1/84—Controlled slow cooling
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D6/00—Heat treatment of ferrous alloys
    • C21D6/001—Heat treatment of ferrous alloys containing Ni
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D6/00—Heat treatment of ferrous alloys
    • C21D6/002—Heat treatment of ferrous alloys containing Cr
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D6/00—Heat treatment of ferrous alloys
    • C21D6/005—Heat treatment of ferrous alloys containing Mn
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D6/00—Heat treatment of ferrous alloys
    • C21D6/007—Heat treatment of ferrous alloys containing Co
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D6/00—Heat treatment of ferrous alloys
    • C21D6/008—Heat treatment of ferrous alloys containing Si
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0221—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the working steps
    • C21D8/0226—Hot rolling
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0221—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the working steps
    • C21D8/0236—Cold rolling
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0247—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment
    • C21D8/0263—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment following hot rolling
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0247—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment
    • C21D8/0273—Final recrystallisation annealing
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
    • C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
    • C21D8/0278—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips involving a particular surface treatment 
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D9/00—Heat treatment, e.g. annealing, hardening, quenching or tempering, adapted for particular articles; Furnaces therefor
    • C21D9/46—Heat treatment, e.g. annealing, hardening, quenching or tempering, adapted for particular articles; Furnaces therefor for sheet metals
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/001—Ferrous alloys, e.g. steel alloys containing N
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/002—Ferrous alloys, e.g. steel alloys containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/008—Ferrous alloys, e.g. steel alloys containing tin
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/02—Ferrous alloys, e.g. steel alloys containing silicon
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/04—Ferrous alloys, e.g. steel alloys containing manganese
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/06—Ferrous alloys, e.g. steel alloys containing aluminium
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/08—Ferrous alloys, e.g. steel alloys containing nickel
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/10—Ferrous alloys, e.g. steel alloys containing cobalt
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/10—Ferrous alloys, e.g. steel alloys containing cobalt
    • C22C38/105—Ferrous alloys, e.g. steel alloys containing cobalt containing Co and Ni
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/12—Ferrous alloys, e.g. steel alloys containing tungsten, tantalum, molybdenum, vanadium, or niobium
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/14—Ferrous alloys, e.g. steel alloys containing titanium or zirconium
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/16—Ferrous alloys, e.g. steel alloys containing copper
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
    • C22C38/22—Ferrous alloys, e.g. steel alloys containing chromium with molybdenum or tungsten
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
    • C22C38/28—Ferrous alloys, e.g. steel alloys containing chromium with titanium or zirconium
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
    • C22C38/32—Ferrous alloys, e.g. steel alloys containing chromium with boron
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
    • C22C38/38—Ferrous alloys, e.g. steel alloys containing chromium with more than 1.5% by weight of manganese
    • C—CHEMISTRY; METALLURGY
    • C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
    • C22C—ALLOYS
    • C22C38/00—Ferrous alloys, e.g. steel alloys
    • C22C38/60—Ferrous alloys, e.g. steel alloys containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B15/00—Layered products comprising a layer of metal
    • B32B15/01—Layered products comprising a layer of metal all layers being exclusively metallic
    • B32B15/013—Layered products comprising a layer of metal all layers being exclusively metallic one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2311/00—Metals, their alloys or their compounds
    • B32B2311/20—Zinc
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D2211/00—Microstructure comprising significant phases
    • C21D2211/002—Bainite
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D2211/00—Microstructure comprising significant phases
    • C21D2211/004—Dispersions; Precipitations
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D2211/00—Microstructure comprising significant phases
    • C21D2211/005—Ferrite
    • C—CHEMISTRY; METALLURGY
    • C21—METALLURGY OF IRON
    • C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
    • C21D2211/00—Microstructure comprising significant phases
    • C21D2211/008—Martensite

Definitions

  • the present invention relates to steel plates and members, and methods of manufacturing them.
  • Patent Document 1 describes "In mass%, C: more than 0.140%, less than 0.400%, Si: more than 0.35%, less than 1.50%, Mn: more than 1.50%, less than 4.00%, P: 0 .100% or less, S: 0.010% or less, Al: 0.100% or less, N: 0.0100% or less, Ti: 0% or more, less than 0.050%, Nb: 0% or more, 0.050 %, V: 0% or more, 0.50% or less, Cr: 0% or more, 1.00% or less, Mo: 0% or more, 0.50% or less, B: 0% or more, 0.0100% or less , Ca: 0% or more, 0.0100% or less, Mg: 0% or more, 0.0100% or less, REM: 0% or more, 0.0500% or less, Bi: 0% or more, 0.050% or less.
  • the structure at a position 1/4 of the plate thickness from the surface has a volume fraction of tempered martensite of 70.0% or more, retained austenite of more than 3.0% and less than 10.0%, and a total of 25.0%.
  • the structure at a position 25 ⁇ m from the surface contains, in terms of volume fraction, a total of 70% or more of ferrite and bainite, and a total of 30% or less of martensite and tempered martensite, At a position 25 ⁇ m from the surface, the average grain size of the martensite and the tempered martensite is 5.0 ⁇ m or less, The tensile strength is 1310 MPa or more, the uniform elongation is 5.0% or more, and R/t, which is the ratio of the limit bending radius R to the plate thickness t at 90° V bending, is 5.0 or less. High strength cold rolled steel plate. ” is disclosed.
  • the chemical composition is C: 0.08 to 0.20% (meaning mass %; the same applies below for chemical composition), Si: 0.20-3.0%, Mn: 1.0 to 3.5%, Al: 3% or less (not including 0%), P: 0.15% or less (not including 0%), S: 0.02% or less (not including 0%), and N: 0.01% or less (not including 0%) and the remainder consists of iron and unavoidable impurities,
  • delayed fracture may occur due to an increase in residual stress within the component and deterioration of delayed fracture resistance due to the material itself. becomes apparent.
  • delayed failure is a phenomenon that leads to failure in the following manner. That is, when the component is placed in a hydrogen intrusion environment with high stress applied to the component, hydrogen infiltrates into the component. This causes a decrease in interatomic bonding force and local deformation, resulting in microcracks, which propagate and lead to destruction.
  • the area ratio of carbides in martensite is kept below a certain level, so the amount of solid solution C in the prior ⁇ grains is large, and the strength within the prior ⁇ grains is high.
  • delayed fracture usually occurs starting from the prior ⁇ grain boundary. Therefore, when the strength within the prior ⁇ grains is high, the strength at the prior ⁇ grain boundaries becomes relatively low, promoting delayed fracture due to grain boundary fracture.
  • the present invention was developed to meet the above requirements, and provides a steel plate that simultaneously achieves a strength of TS: 1310 MPa or more and excellent delayed fracture resistance, together with an advantageous manufacturing method thereof.
  • the purpose is to Another object of the present invention is to provide a member made of the above-mentioned steel plate, and a method for manufacturing the same.
  • the intragranular strength of martensite and bainite is proportional to the amount of solute C, and the amount of solute C correlates with the amount of carbide precipitation. Therefore, in order to obtain a strength of TS: 1310 MPa or more while suppressing delayed fracture at grain boundaries, it is important to control the amount and size of carbide precipitation.
  • Fine carbides inhibit the diffusion of hydrogen, which causes delayed fracture, and have the effect of improving delayed fracture resistance. However, if all the carbides are to be finely precipitated, the amount of carbides precipitated will be insufficient, and the effect of suppressing delayed fracture at grain boundaries will not be obtained.
  • the manufacturing conditions in particular, the tempering process should be divided into two sections, and the tempering parameters calculated from the residence time and intermediate temperature should be individually and appropriately controlled in each section. is important.
  • the present invention was completed based on the above findings and further studies.
  • the gist of the present invention is as follows. 1. In mass%, C: 0.12% or more and 0.40% or less, Si: 1.50% or less, Mn: 0.20% or more and 3.50% or less, P: 0.050% or less, S: 0.0100% or less, sol.
  • the total area ratio of martensite and bainite is 95% or more and 100% or less, The area ratio of carbides present in the grains of the martensite and the bainite is 5% or more and 25% or less, The average equivalent circular diameter of the carbide is 10 nm or more and 80 nm or less, and The particle size distribution of the carbide satisfies the following formula (1), A steel plate having a tensile strength of 1310 MPa or more.
  • xi Number density of carbides whose circle equivalent diameter is (5.0 ⁇ i) nm or more and less than (5.0 ⁇ (i+1)) nm [number/ ⁇ m 2 ]
  • i Integer from 1 to n n: 31
  • the steel sheet according to 1, wherein the component composition further contains at least one of the following groups A and B in mass %.
  • groups A and B Cu: 1.00% or less, Ni: 1.00% or less, Mo: 0.50% or less, Cr: 1.00% or less, Zr: 0.100% or less, Ca: 0.0100% or less, Ti: 0.100% or less, Nb: 0.100% or less, B: 0.0100% or less, V: 0.200% or less, W: 0.200% or less, Sb: 0.100% or less, One or more types selected from Sn: 0.100% or less and Mg: 0.0100% or less
  • group B One or two selected from Se, As, Pb, Bi, Zn, Cs, Rb, Co, La, Tl, Nd, Y, In, Be, Hf, Tc, Ta, O, La, Ce, and Pr. More than: 0.02% or less in total
  • a first cooling step in which the steel plate is cooled at an average cooling rate of 10° C./second or less in a temperature range from the annealing temperature to the second cooling start temperature;
  • the steel plate is cooled to a cooling stop temperature of 50°C or less, with the second cooling start temperature: 680°C or more, and the average cooling rate in the temperature range from the second cooling start temperature to 50°C: 30°C/second or more.
  • the first section and the second section of the tempering process are divided into two equal parts of the time period in the temperature range of 100 ° C or higher in the tempering process, and the first half is the first section of the tempering process and the second half is the second section of the tempering process. This is what I did.
  • a method for manufacturing a member comprising the step of subjecting the steel plate according to any one of 1 to 3 above to at least one of forming and bonding to produce a member.
  • a steel plate can be obtained that simultaneously achieves a strength of TS: 1310 MPa or more and excellent delayed fracture resistance.
  • the steel sheet of the present invention can be applied to various parts requiring high strength by cold pressing, which is more advantageous in terms of cost and productivity. It can contribute to improvement and weight reduction.
  • the steel sheet of the present invention is suitable as a steel sheet for cold pressing that is applied to automobiles, home appliances, etc. through cold pressing.
  • C 0.12% or more and 0.40% or less C increases the strength of martensite and bainite, and is included from the viewpoint of ensuring a strength of TS: 1310 MPa or more.
  • the C content is set to 0.12% or more.
  • the C content is preferably 0.18% or more.
  • the C content is more preferably 0.24% or more.
  • the C content is set to 0.40% or less.
  • the C content is preferably 0.36% or less, more preferably 0.32% or less.
  • Si 1.50% or less Si can be added as a strengthening element through solid solution strengthening.
  • the lower limit of the Si content is not particularly limited, and may be 0%. However, from the viewpoint of obtaining the above effects, the Si content is preferably 0.02% or more. The Si content is more preferably 0.10% or more. On the other hand, when the Si content exceeds 1.50%, the effect is saturated. Furthermore, the amount of Si segregation increases, which deteriorates delayed fracture resistance. Therefore, the Si content is set to 1.50% or less.
  • the Si content is preferably 1.20% or less, more preferably 1.00% or less, even more preferably 0.80% or less.
  • Mn 0.20% or more and 3.50% or less
  • Mn is an element that improves the hardenability of steel, and is included to ensure martensite.
  • the Mn content is set to 0.20% or more from the viewpoint of ensuring martensite in an industrially stable manner.
  • the Mn content is preferably 0.80% or more.
  • the Mn content is set to 3.50% or less.
  • the Mn content is preferably 3.00% or less, more preferably 2.50% or less, even more preferably 2.00% or less.
  • P 0.050% or less
  • P is an element that strengthens steel, but when its content is large, spot weldability deteriorates. Therefore, the P content is set to 0.050% or less. From the above viewpoint, the P content is preferably 0.020% or less. Note that the lower limit of the P content is not particularly limited. However, reducing the P content to less than 0.002% requires a great deal of cost. Therefore, from the viewpoint of cost, the P content is preferably 0.002% or more.
  • the S content is set to 0.0100% or less. From the above viewpoint, the S content is preferably 0.0050% or less, more preferably 0.0020% or less. Note that the lower limit of the S content is not particularly limited. However, reducing the S content to less than 0.0002% requires a great deal of cost. Therefore, from the viewpoint of cost, the S content is preferably 0.0002% or more.
  • sol. Al 1.00% or less Al can be included in order to perform sufficient deoxidation and reduce inclusions in the steel.
  • the lower limit of the Al content is not particularly limited and may be 0%. However, from the viewpoint of stably deoxidizing, sol.
  • the Al content is preferably 0.005% or more, more preferably 0.01% or more.
  • the Al content is preferably 0.80% or less, more preferably 0.50% or less.
  • N 0.010% or less N forms coarse nitrides and deteriorates delayed fracture resistance. Therefore, N should be 0.010% or less.
  • the N content is preferably 0.0080% or less.
  • the lower limit of the N content is not particularly limited and may be 0%. However, from the viewpoint of industrial implementation, the N content is preferably 0.0005% or more.
  • the basic components of the steel sheet according to one embodiment of the present invention have been described above.
  • the steel sheet according to one embodiment of the present invention contains the above basic components, and the remainder other than the above basic components is Fe (iron) and inevitable impurities. It has a component composition including.
  • the steel plate according to one embodiment of the present invention has a composition containing the above-mentioned basic components, with the remainder consisting of Fe and unavoidable impurities.
  • the steel plate according to one embodiment of the present invention may contain one or more selected from the following optional additive components.
  • Cu 1.00% or less
  • Ni 1.00% or less
  • Mo 0.50% or less
  • Cr 1.00% or less
  • Zr 0.100% or less
  • Ca 0.0100% or less
  • Ti 0.100% or less
  • Nb 0.100% or less
  • B 0.0100% or less
  • V 0.200% or less
  • W 0.200% or less
  • Sb 0.100% or less
  • Sn 0.100% or less
  • Mg 0.0100% or less
  • Cu 1.00% or less
  • Cu is an element that improves corrosion resistance.
  • Cu also has the effect of coating the surface of the steel plate with corrosion products, suppressing hydrogen penetration into the steel plate, and improving delayed fracture resistance.
  • the Cu content is preferably more than 0%, more preferably 0.01% or more.
  • the Cu content is more preferably 0.05% or more.
  • too much Cu content causes surface defects. Therefore, when Cu is contained, the content is preferably 1.00% or less.
  • Ni 1.00% or less
  • Ni is also an element that improves corrosion resistance.
  • the Ni content is preferably more than 0%, more preferably 0.01% or more.
  • the content is preferably 1.00% or less.
  • Mo 0.50% or less Mo can be contained for the purpose of improving the hardenability of steel and stably ensuring a predetermined strength. From the viewpoint of obtaining the above effects, the Mo content is preferably more than 0%, more preferably 0.001% or more, and still more preferably 0.005% or more. However, when the Mo content exceeds 0.50%, chemical conversion treatment properties deteriorate. Therefore, when Mo is contained, the content is preferably 0.50% or less.
  • Cr 1.00% or less Cr can be contained for the purpose of improving the hardenability of steel. From the viewpoint of obtaining the above effects, the Cr content is preferably more than 0%, more preferably 0.001% or more. However, when the Cr content exceeds 1.00%, chemical conversion treatment properties deteriorate. Therefore, when Cr is contained, the content is preferably 1.00% or less. Note that from the viewpoint of preventing deterioration of chemical conversion treatment properties, the Cr content is more preferably 0.20% or less.
  • Zr 0.100% or less Zr contributes to high strength through the refinement of the prior ⁇ grain size and the resulting refinement of the internal structure of martensite. From this viewpoint, the Zr content is preferably more than 0%, more preferably 0.001% or more. However, when Zr is contained excessively, coarse Zr-based precipitates increase, leading to deterioration of delayed fracture resistance. Therefore, when Zr is contained, the content is preferably 0.100% or less.
  • Ca 0.0100% or less
  • Ca has the effect of fixing S as CaS and improving delayed fracture resistance.
  • the Ca content is preferably more than 0%, more preferably 0.0001% or more.
  • the content is preferably 0.0100% or less.
  • the Ca content is more preferably 0.0050% or less.
  • Ti 0.100% or less Ti forms TiN prior to forming BN. Thereby, solid solution B is ensured, and the effect of stabilizing hardenability is obtained. From the viewpoint of obtaining such effects, the Ti content is preferably more than 0%, more preferably 0.002% or more. On the other hand, when Ti is contained excessively, a large amount of coarse inclusions such as TiN and TiC are generated, which deteriorates delayed fracture resistance. Therefore, the Ti content is set to 0.100% or less. The Ti content is preferably 0.060% or less, more preferably 0.055% or less.
  • Nb 0.100% or less Nb contributes to high strength through refining the prior ⁇ grain size and thereby refining the internal structure of martensite.
  • the Nb content is preferably more than 0%, more preferably 0.002% or more.
  • the content is preferably 0.100% or less.
  • B 0.0100% or less
  • B is an element that improves the hardenability of steel, and has the advantage of increasing the amount of martensite produced even with a small Mn content.
  • the B content is preferably greater than 0%, more preferably 0.0002% or more, and even more preferably 0.0005% or more.
  • the B content is set to 0.0100% or less.
  • V 0.200% or less
  • V can be contained for the purpose of improving the hardenability of steel and increasing the strength by refining martensite. From the viewpoint of obtaining such effects, the V content is preferably more than 0%, more preferably 0.001% or more. However, when the V content exceeds 0.200%, castability deteriorates. Therefore, when V is contained, the content is preferably 0.200% or less.
  • W 0.200% or less W contributes to high strength through the formation of fine W-based carbides and carbonitrides. From this point of view, the W content is preferably more than 0%, more preferably 0.001% or more. However, when W is contained excessively, coarse precipitates that remain undissolved during slab heating in the hot rolling process increase, leading to deterioration of delayed fracture resistance. Therefore, when W is contained, the content is preferably 0.200% or less.
  • Sb 0.100% or less Sb suppresses oxidation and nitridation in the surface layer of the steel sheet, thereby suppressing reduction of C and B. By suppressing the reduction of C and B, ferrite formation in the surface layer of the steel sheet is suppressed, contributing to higher strength.
  • the Sb content is preferably more than 0%, more preferably 0.001% or more.
  • the content is preferably 0.100% or less.
  • Sn 0.100% or less Sn suppresses oxidation and nitridation in the surface layer of the steel sheet, thereby suppressing reduction of C and B. By suppressing the reduction of C and B, ferrite formation in the surface layer of the steel sheet is suppressed, contributing to increased strength and further improved delayed fracture resistance.
  • the Sn content is preferably more than 0%, more preferably 0.001% or more.
  • the Sn content exceeds 0.100%, castability deteriorates.
  • Sn segregates at prior ⁇ grain boundaries, leading to deterioration of delayed fracture resistance. Therefore, when Sn is contained, the content is preferably 0.100% or less.
  • Mg 0.0100% or less Mg fixes O as MgO and improves delayed fracture resistance. From this point of view, the Mg content is preferably greater than 0%, more preferably 0.0001% or more. However, excessive Mg content causes deterioration of surface quality and delayed fracture resistance. Therefore, when Mg is contained, the content is preferably 0.0100% or less.
  • the structure of the steel plate according to one embodiment of the present invention is The total area ratio of martensite and bainite is 95% or more and 100% or less, The area ratio of carbides present in the grains of the martensite and the bainite is 5% or more and 25% or less, The average equivalent circular diameter of the carbide is 10 nm or more and 80 nm or less, and The structure satisfies the above formula (1) regarding the particle size distribution of the carbide. The reasons for each limitation will be explained below. Note that the area ratio is the area ratio for the entire tissue.
  • Total area ratio of martensite and bainite 95% or more and 100% or less
  • the total area ratio of martensite and bainite is 95% or more.
  • the total area ratio of martensite and bainite is less than 95%, residual structures such as ferrite, retained austenite, and pearlite increase, making it difficult to obtain a predetermined strength.
  • the tempering temperature is lowered, the toughness decreases and the delayed fracture resistance deteriorates.
  • the method of increasing the amount of C may deteriorate weldability. Therefore, the total area ratio of martensite and bainite is 95% or more. Note that the upper limit of the total area ratio of martensite and bainite is not particularly limited, and may be 100%.
  • Area ratio of remainder 5% or less Structures constituting the remainder other than martensite and bainite may reduce strength or promote delayed fracture. Therefore, the area ratio of the remaining portion is set to 5% or less.
  • the lower limit of the area ratio of the remainder is not particularly limited, and the area ratio of the remainder may be 0%. Note that structures constituting the remainder other than martensite and bainite include ferrite, retained austenite, and pearlite.
  • the total area ratio of martensite and bainite is measured as follows. That is, after polishing the L cross section (vertical cross section parallel to the rolling direction) of the steel plate, it was corroded with nital, and the L cross section of the steel plate was observed with SEM at 1/4 the thickness of the steel plate in 4 fields at 2000x magnification. do. Next, the photographed tissue photograph is image analyzed. Both martensite and bainite are gray contrasting regions. Martensite and bainite may contain inclusions such as carbides, nitrides, sulfides, and oxides, but the area occupied by these inclusions shall be included in the area of martensite and bainite. do.
  • the area exhibiting the gray contrast described above may contain retained austenite
  • the area ratio of retained austenite is subtracted from the area ratio of the area exhibiting the gray contrast using the method described below. , calculate the total area ratio of martensite and bainite.
  • martensite and bainite are mainly composed of so-called tempered martensite and tempered bainite that have been tempered during the manufacturing process.
  • the tempered martensite and tempered bainite also include martensite and bainite that have undergone self-tempering during continuous cooling.
  • some of the martensite may contain less than 5% area ratio of so-called fresh martensite, which has not undergone tempering (also in the invention examples of the examples described later), The area ratio of fresh martensite was 5% or less in all cases).
  • Tempered martensite usually contains white contrasting carbides inside. On the other hand, in fresh martensite, no carbide is observed inside.
  • ferrite is a region that exhibits a black contrast.
  • Pearlite is a layered structure of ferrite and plate-shaped white contrasting cementite.
  • martensite and bainite can basically be distinguished from the contrast difference in the above-mentioned SEM microstructure photographs. However, if it is difficult to distinguish between the two, it is possible to do so by observing the position and variant of the carbide contained inside using an SEM at a magnification of 10,000 times. That is, in bainite, carbides are generated at the interface of the lath-like structure or within the lath. Moreover, since the crystal orientation relationship between bainitic ferrite and cementite is one type, the generated carbide extends in one direction. On the other hand, in tempered martensite, which mainly constitutes martensite, carbides are generated within the lath.
  • the generated carbide extends in multiple directions. Therefore, it is possible to distinguish between tempered martensite and bainite by observing the position and variant of carbides contained inside using SEM at a magnification of 10,000 times.
  • the total area of the four fields of view of the region exhibiting the gray contrast is calculated, and a value is obtained by dividing the total area by the total area of the four fields of view and multiplying by 100. Then, the area ratio of retained austenite measured by the method described later is subtracted from the obtained value, and the value is taken as the total area ratio of martensite and bainite. However, among the regions exhibiting a gray contrast, island-like regions having an area of less than 1 ⁇ m 2 are excluded to calculate the total area ratio of martensite and bainite.
  • the area ratio of retained austenite is measured as follows. That is, a steel plate is chemically polished with oxalic acid to a depth of 200 ⁇ m from its surface. Then, using the chemically polished surface as an observation surface, observation is performed using an X-ray diffraction method. MoK ⁇ rays were used for the incident X-rays, and the diffraction intensity of the (200), (211) and (220) planes of BCC iron was compared with the (200), (220) and (311) planes of FCC iron (austenite). Find the ratio of the diffraction intensities. Next, the volume fraction of retained austenite is calculated from the ratio of the diffraction intensities of each surface. Then, assuming that the retained austenite is three-dimensionally homogeneous, the volume fraction of the retained austenite is defined as the area fraction of the retained austenite.
  • Carbides present within the grains of martensite and bainite are hydrogen oxides that cause delayed fracture. inhibits diffusion.
  • carbides reduce the intragranular strength, thereby reducing the difference between the intragranular strength and the grain boundary strength, and relatively strengthen the grain boundaries. Through these, delayed fracture resistance is improved.
  • the area ratio of carbides is less than 5%, the above-mentioned effect of improving delayed fracture resistance cannot be sufficiently obtained.
  • the area ratio of carbides is set to 5% or more and 25% or less.
  • the area ratio of carbide is preferably 10% or more.
  • the area ratio of carbides is preferably 20% or less.
  • Average circular equivalent diameter of carbide 10 nm or more and 80 nm or less
  • the average equivalent circular diameter of carbide is set to 10 nm or more and 80 nm or less.
  • the average equivalent circular diameter of the carbide is preferably 60 nm or less, more preferably 40 nm or less.
  • Particle size distribution of carbide satisfies the following formula (1).
  • the grain size of carbides becomes coarser as the tempering temperature increases. Further, when tempering is performed at a constant temperature, the grain size distribution of carbides becomes a distribution close to a normal distribution.
  • the following formula (1) represents a state in which the particle size distribution of carbides is not a normal distribution, but is mainly composed of relatively fine carbides, and also contains a certain amount of coarse carbides.
  • the inventors have conducted various studies and found that excellent delayed fracture resistance can be obtained by satisfying the following formula (1). Although the mechanism for this is not clear, the inventors believe that the hydrogen trapping effect of relatively fine carbides and the reduction of the amount of dissolved C due to the formation of coarse carbides work synergistically. There is.
  • the left-hand side value of the following formula (1) is preferably 1.35 or more, more preferably 1.50 or more. Further, the upper limit of the left-hand side value of the following equation (1) is not particularly limited, but for example, it is preferable that the left-hand side value of the following equation (1) is 2.20 or less.
  • xi Number density of carbides whose circle equivalent diameter is (5.0 ⁇ i) nm or more and less than (5.0 ⁇ (i+1)) nm [number/ ⁇ m 2 ]
  • i Integer from 1 to n n: 31
  • X Average value of xi ((arithmetic) average value from x1 to x31)
  • s standard deviation of xi (standard deviation from x1 to x31) It is.
  • the measurement of the area ratio and average equivalent circle diameter of carbides and the calculation of the left-hand side value of the above equation (1) are performed as follows. That is, after polishing the L cross section (vertical cross section parallel to the rolling direction) of the steel plate, it is corroded with nital. Next, the L cross section of the steel plate is observed by SEM at a position of 1/4 of the thickness of the steel plate, and an in-lens SE image is obtained.
  • in-lens SE images are affected by the work function of the material surface and changes in surface potential due to local electrification, and provide images that are sensitive to differences in materials, so the boundary between the base iron and carbide is clearly visible. You can check it.
  • the acceleration voltage 1 kV
  • the working distance 4 mm
  • the magnification 15,000 times.
  • the obtained in-lens SE image is analyzed by ImageJ and binarized into carbide and base metal.
  • the total area ratio of carbides is calculated using the particle analysis function, and this value is taken as the area ratio of carbides.
  • the equivalent circle diameter of each carbide is calculated, and the average value thereof is taken as the average equivalent circle diameter of the carbide.
  • count the number of carbides whose circle-equivalent diameter is (5.0 x i) nm or more and less than (5.0 x (i + 1)) nm, and calculate xi (yen).
  • the number density of carbides having an equivalent diameter of (5.0 ⁇ i) nm or more and less than (5.0 ⁇ (i+1)) nm) is determined.
  • the left-hand side value of the above equation (1) is calculated from the obtained xi.
  • carbides with an equivalent circle diameter of less than 5 nm are excluded.
  • the martensite region contains prior ⁇ grain boundaries, packet boundaries, and block boundaries, and carbides may precipitate in the form of a film on these grain boundaries and boundaries. It is not included in the carbides present in the grains.
  • the steel plate according to an embodiment of the present invention is characterized by excellent delayed fracture resistance even when the TS is 1310 MPa or more. Therefore, TS is set to 1310 MPa or more.
  • TS is preferably 1470 MPa or more, more preferably 1700 MPa or more.
  • the upper limit of the TS is not particularly limited, but, for example, it may be suitable that the TS is 2500 MPa or less. Note that TS is measured by a tensile test based on JIS Z 2241. The details are as described in the examples described later.
  • the steel plate according to an embodiment of the present invention may have a plating layer on its surface (one or both surfaces).
  • the type of the plating layer is not particularly limited, and examples include a galvanized layer and a plating layer of a metal other than zinc. Further, the plating layer may contain components other than the main component such as zinc. Examples of the galvanized layer include a hot-dip galvanized layer, an alloyed hot-dip galvanized layer, and an electrogalvanized layer.
  • the thickness of the steel plate according to an embodiment of the present invention is not particularly limited, but is preferably 0.5 mm or more and 3.0 mm or less.
  • the steel plate according to one embodiment of the present invention may be a hot-rolled steel plate or a cold-rolled steel plate.
  • a member according to an embodiment of the present invention is a member made of (made of) the above-mentioned steel plate.
  • a steel plate material is subjected to at least one of forming and bonding, preferably cold pressing, to form a member.
  • the above-mentioned steel plate simultaneously realizes a strength of TS: 1310 MPa or more and excellent delayed fracture resistance.
  • the above steel sheet can be applied in cold press to various parts that require high strength, which is more advantageous in terms of cost and productivity, and improves the strength of parts. and can contribute to weight reduction. Therefore, the member according to one embodiment of the present invention is particularly suitable for application to members used in automobiles, home appliances, and the like.
  • a method for manufacturing a steel plate according to an embodiment of the present invention includes: A rolling process of rolling a steel slab having the above-mentioned composition to produce a steel plate; an annealing step of annealing the steel plate at an annealing temperature of 3 points or more of A and an annealing time of 30 seconds or more; Next, a first cooling step in which the steel plate is cooled at an average cooling rate of 10° C./second or less in a temperature range from the annealing temperature to the second cooling start temperature; The steel plate is cooled to a cooling stop temperature of 50°C or less, with the second cooling start temperature: 680°C or more, and the average cooling rate in the temperature range from the second cooling start temperature to 50°C: 30°C/second or more.
  • each temperature mentioned above means the surface temperature of a steel slab and a steel plate unless otherwise specified.
  • a steel slab is rolled, for example, hot rolled, or hot rolled and cold rolled to form a steel plate.
  • the preparation method (manufacturing conditions), hot rolling conditions, and cold rolling conditions of the steel slab are not particularly limited, and may be carried out according to conventional methods.
  • the hot rolled steel sheet after hot rolling may be optionally pickled.
  • the pickling conditions are not particularly limited either, and conventional methods may be followed.
  • the cold rolled steel sheet after cold rolling may optionally be pickled.
  • the pickling conditions are not particularly limited either, and conventional methods may be followed.
  • the steel plate (hot-rolled steel plate or cold-rolled steel plate) obtained as described above is annealed at an annealing temperature of 3 points or more of A and an annealing time of 30 seconds or more.
  • Annealing temperature 3 points or more of A
  • the annealing temperature is set to A3 point or higher.
  • the annealing temperature is preferably 1000°C or less.
  • the annealing temperature is the highest temperature reached in the annealing process, and the temperature during holding during annealing may be constant or may vary as long as it is A3 points or higher.
  • the A3 points are determined by the following formula.
  • Annealing time 30 seconds or more If the annealing time is less than 30 seconds, sufficient austenite will not be generated during annealing. As a result, a predetermined total area ratio of martensite and bainite cannot be obtained in the final product, and as a result, a TS of 1310 MPa or more cannot be obtained. Therefore, the annealing time is set to 30 seconds or more. Although the upper limit of the annealing time is not particularly limited, if the annealing time exceeds a certain value, the austenite grain size may become coarse and the toughness may deteriorate. Therefore, the annealing time is preferably 900 seconds or less. Note that the annealing time is the holding time (residence time) in the temperature range of A3 points or higher.
  • Average cooling rate in the temperature range from annealing temperature to second cooling start temperature 10°C/second or less
  • Average cooling rate in the temperature range from annealing temperature to second cooling start temperature (hereinafter also referred to as first cooling rate) is 10 If it exceeds .degree. C./second, temperature variations will occur in the steel sheet before the start of secondary cooling, and the shape of the sheet after the second cooling step may not be flat. If the plate shape is not flat, problems arise such as, for example, it becomes difficult to ensure dimensional accuracy when molding into automobile parts. Therefore, the first cooling rate is set to 10° C./second or less.
  • the first cooling rate is preferably 8° C./second or less. Note that the lower limit of the first cooling rate is not particularly limited, but the first cooling rate is preferably 1° C./second or more.
  • Second cooling start temperature 680°C or higher If the second cooling start temperature is less than 680°C, excessive residual ⁇ and pearlite may be generated, and there is a risk that the desired total area ratio of martensite and bainite may not be obtained in the final product. be. Additionally, martensite and bainite may be tempered during cooling, and carbides may become excessively coarse. Therefore, the second cooling start temperature is set to 680° C. or higher. Although the upper limit of the second cooling start temperature is not particularly limited, for example, the second cooling start temperature is preferably 850° C. or lower. Further, the second cooling start temperature is preferably ⁇ 50° C. or lower than the annealing temperature.
  • Average cooling rate in the temperature range from second cooling start temperature to 50°C: 30°C/sec or more Average cooling rate in the temperature range from second cooling start temperature to 50°C (hereinafter also referred to as second cooling rate) is 30°C If it is less than 0.degree. C./sec, residual .gamma. and pearlite will be excessively produced, and there is a possibility that a predetermined total area ratio of martensite and bainite cannot be obtained in the final product. Additionally, martensite and bainite may be tempered during cooling, and carbides may become excessively coarse. Therefore, the second cooling rate is set to 30° C./second or more. The second cooling rate is preferably 50°C/second or more, more preferably 100°C/second or more. Note that the upper limit of the second cooling rate is not particularly limited, but the second cooling rate is preferably 2000° C./second or less.
  • Cooling stop temperature 50°C or less From the viewpoint of suppressing coarsening of carbides, the cooling stop temperature is set to 50°C or less. Note that the lower limit of the cooling stop temperature is not particularly limited, but the cooling stop temperature is preferably 5° C. or higher.
  • ⁇ 1 is set to 5000 or less.
  • ⁇ 1 is more preferably 4700 or less.
  • the lower limit of ⁇ 1 is not particularly limited, for example, ⁇ 1 is preferably 3500 or more.
  • ⁇ 2 becomes too small, it becomes difficult to obtain fine carbides that contribute to hydrogen trapping, and it becomes difficult to obtain a particle size distribution of carbides that satisfies the above formula (1). Therefore, ⁇ 2 is set to 3100 or more.
  • ⁇ 1 tempering parameter of the first section of the tempering process
  • ⁇ 2 tempering parameter of the second section of the tempering process
  • ⁇ 1 T1 ⁇ (logt1+20)...(5)
  • ⁇ 2 T2 ⁇ (logt2+20)...(6)
  • t1 residence time in the first section of the tempering process [s]
  • t2 residence time [s] of the second section of the tempering process
  • T2 intermediate temperature in the second section of the tempering process [°C]
  • the first section and the second section of the tempering process are divided into two equal parts of the time period in the temperature range of 100 ° C or higher in the tempering process, and the first half is the first section of the tempering process and the second half is the second section of the tempering process. This is what I did.
  • T1 and T2 measure the temperature at the middle point of the first section and the second section, and let the measured values be T1 and T2, respectively.
  • t1 and t2 are not particularly limited, and are preferably set to, for example, 200 to 700 seconds each. Further, T1 and T2 are also not particularly limited, and for example, it is preferable that T1 be 150 to 220°C and T2 be 150 to 200°C.
  • the obtained steel plate may optionally be subjected to skin pass rolling (temper rolling) or leveler processing from the viewpoint of stabilizing the shape accuracy of press forming, such as adjusting the surface roughness and flattening the plate shape.
  • skin pass rolling and leveler processing are not particularly limited, and conventional methods may be followed.
  • the obtained steel plate may be subjected to plating treatment.
  • plating treatment By performing plating treatment, a steel plate having a plating layer on the surface can be obtained.
  • the plating method is not particularly limited, and examples thereof include hot-dip plating and electroplating.
  • a plating process may be performed in which alloying is performed after hot-dip plating.
  • the type of plating is not particularly limited, and examples thereof include zinc plating and plating of a metal other than zinc.
  • the conditions for the plating treatment are not particularly limited, and any conventional method may be followed.
  • the plating bath may contain components other than the main component such as zinc.
  • each step after the above-mentioned annealing step may be performed by continuous annealing or batch annealing, but from the viewpoint of productivity, it is preferable to perform continuous annealing.
  • Conditions other than the above are not particularly limited and may be according to conventional methods.
  • a method for manufacturing a member according to an embodiment of the present invention preferably includes a step of subjecting the above steel plate (for example, a steel plate manufactured by the above steel plate manufacturing method) to at least one of a forming process and a joining process to form a member.
  • the method includes a step of applying cold pressing to form a member.
  • the molding method is not particularly limited, and for example, a general processing method such as press working can be used.
  • the joining method is not particularly limited, and for example, common welding such as spot welding, laser welding, arc welding, rivet joining, caulking joining, etc. can be used.
  • the molding conditions and bonding conditions are not particularly limited, and conventional methods may be followed.
  • Cold pressing conditions are not particularly limited either, and conventional methods may be followed.
  • a part of the cold rolled steel sheet (cold rolled steel sheet No. 17) was subjected to plating treatment (electrogalvanizing treatment) to provide a plating layer on the surface of the cold rolled steel sheet.
  • the plate thickness of the steel plate serving as the final product was 1.4 mm.
  • No. The annealing time of No. 27 is as follows. This is the holding time at an annealing temperature of 27. Conditions other than those specified were in accordance with conventional law.
  • the tensile test was conducted in accordance with JIS Z 2241. That is, a JIS No. 5 test piece was taken from the steel plate so that the longitudinal direction was perpendicular to the rolling direction of the steel plate. Using the sampled test piece, a tensile test was conducted at a crosshead speed of 10 mm/min, and the TS was measured. The results are also listed in Table 3. The evaluation criteria are as follows. ⁇ TS Pass: 1310MPa or more Fail: Less than 1310MPa
  • the delayed fracture test was conducted using a low strain rate tensile test in the following manner. That is, a test piece was prepared by grinding both sides of a steel plate to a thickness of 1.2 mm, buffing the surface, and processing the steel plate into a shape with a parallel part length of 15 mm and a parallel part width of 6 mm. Next, the test piece was preliminarily charged with hydrogen (if the thickness of the steel plate is less than 1.2 mm, at least one side is ground to a depth of 0.1 mm or more, and the surface is buffed to prepare the test piece). ).
  • Preliminary hydrogen charging was performed in a treatment solution in which 3 g/L of ammonium thiocyanate was added to a 3 mass % NaCl aqueous solution at a liquid temperature of 20 to 30°C, current density: 0.05 mA/cm 2 , and holding time: 48 hours. I went there. After the completion of preliminary charging, the treatment liquid was replaced, hydrogen charging was performed under the same conditions as the preliminary hydrogen charging, and a tensile test was conducted using the above test piece at a strain rate of 0.005 mm/min to determine the maximum stress value ( ⁇ H) was calculated.
  • a test piece was prepared from each steel plate in the same manner as above, and a tensile test was conducted in an atmospheric environment under the same conditions as above, except for preliminary hydrogen charging and no hydrogen charging, and the maximum stress value ( ⁇ N) was determined. .
  • the stress ratio ⁇ H/ ⁇ N was determined, and the stress ratio ⁇ H/ ⁇ N was used as an index of delayed fracture resistance.
  • the plate shape is required to be good. Therefore, we cut a steel plate to a width of 1000 mm and a length of 500 mm, and placed the cut steel plate horizontally on a surface plate, and measured the height (distance from the surface of the surface plate) at the highest point on the surface plate. It was measured. Then, the value obtained by subtracting the thickness of the steel plate from the measured value was defined as the maximum warp height, and was used as an index of the plate shape.
  • a steel plate can be obtained that simultaneously achieves a strength of TS: 1310 MPa or more and excellent delayed fracture resistance.
  • the steel sheet of the present invention can be applied to various parts requiring high strength by cold pressing, which is more advantageous in terms of cost and productivity. It can contribute to improvement and weight reduction.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Mechanical Engineering (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Physics & Mathematics (AREA)
  • Thermal Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Heat Treatment Of Sheet Steel (AREA)
PCT/JP2022/040833 2022-03-30 2022-10-31 鋼板および部材、ならびに、それらの製造方法 Ceased WO2023188504A1 (ja)

Priority Applications (6)

Application Number Priority Date Filing Date Title
US18/844,574 US20250179602A1 (en) 2022-03-30 2022-10-31 Steel sheet, member, and methods of producing same
JP2023508472A JP7311070B1 (ja) 2022-03-30 2022-10-31 鋼板および部材、ならびに、それらの製造方法
CN202280092849.9A CN118786234A (zh) 2022-03-30 2022-10-31 钢板和部件以及它们的制造方法
EP22935635.7A EP4477773A4 (en) 2022-03-30 2022-10-31 STEEL SHEET, ELEMENT, METHOD FOR PRODUCING THE STEEL SHEET AND METHOD FOR PRODUCING SAID ELEMENT
KR1020247030706A KR20240148909A (ko) 2022-03-30 2022-10-31 강판 및 부재, 그리고, 그들의 제조 방법
MX2024011891A MX2024011891A (es) 2022-03-30 2024-09-26 Lamina de acero, miembro y metodos para producir los mismos

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022057719 2022-03-30
JP2022-057719 2022-03-30

Publications (1)

Publication Number Publication Date
WO2023188504A1 true WO2023188504A1 (ja) 2023-10-05

Family

ID=88200636

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/040833 Ceased WO2023188504A1 (ja) 2022-03-30 2022-10-31 鋼板および部材、ならびに、それらの製造方法

Country Status (7)

Country Link
US (1) US20250179602A1 (cg-RX-API-DMAC7.html)
EP (1) EP4477773A4 (cg-RX-API-DMAC7.html)
JP (1) JP7311070B1 (cg-RX-API-DMAC7.html)
KR (1) KR20240148909A (cg-RX-API-DMAC7.html)
CN (1) CN118786234A (cg-RX-API-DMAC7.html)
MX (1) MX2024011891A (cg-RX-API-DMAC7.html)
WO (1) WO2023188504A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN118957429A (zh) * 2024-09-27 2024-11-15 邯郸市濮政工矿配件制造有限公司 一种高强度桥梁螺栓及其制备方法

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2022185804A1 (ja) * 2021-03-02 2022-09-09 Jfeスチール株式会社 鋼板、部材およびそれらの製造方法

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2016152163A1 (ja) * 2015-03-25 2016-09-29 Jfeスチール株式会社 冷延鋼板およびその製造方法
WO2018123356A1 (ja) * 2016-12-28 2018-07-05 株式会社神戸製鋼所 高強度鋼板および高強度電気亜鉛めっき鋼板
WO2020090303A1 (ja) * 2018-10-31 2020-05-07 Jfeスチール株式会社 高強度鋼板およびその製造方法
WO2020229898A1 (en) * 2019-05-15 2020-11-19 Arcelormittal A cold rolled martensitic steel and a method of martensitic steel thereof
WO2021153392A1 (ja) * 2020-01-31 2021-08-05 Jfeスチール株式会社 鋼板、部材及びそれらの製造方法

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS596154U (ja) 1982-07-06 1984-01-14 植村 厚一 防護通路
TW201938816A (zh) 2018-03-19 2019-10-01 日商新日鐵住金股份有限公司 高強度冷軋鋼板及其製造方法
CN114981462B (zh) * 2020-01-31 2023-11-14 杰富意钢铁株式会社 钢板、部件及其制造方法

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2016152163A1 (ja) * 2015-03-25 2016-09-29 Jfeスチール株式会社 冷延鋼板およびその製造方法
WO2018123356A1 (ja) * 2016-12-28 2018-07-05 株式会社神戸製鋼所 高強度鋼板および高強度電気亜鉛めっき鋼板
WO2020090303A1 (ja) * 2018-10-31 2020-05-07 Jfeスチール株式会社 高強度鋼板およびその製造方法
WO2020229898A1 (en) * 2019-05-15 2020-11-19 Arcelormittal A cold rolled martensitic steel and a method of martensitic steel thereof
WO2021153392A1 (ja) * 2020-01-31 2021-08-05 Jfeスチール株式会社 鋼板、部材及びそれらの製造方法

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4477773A4 *

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN118957429A (zh) * 2024-09-27 2024-11-15 邯郸市濮政工矿配件制造有限公司 一种高强度桥梁螺栓及其制备方法

Also Published As

Publication number Publication date
EP4477773A4 (en) 2025-05-21
KR20240148909A (ko) 2024-10-11
JP7311070B1 (ja) 2023-07-19
US20250179602A1 (en) 2025-06-05
JPWO2023188504A1 (cg-RX-API-DMAC7.html) 2023-10-05
EP4477773A1 (en) 2024-12-18
MX2024011891A (es) 2024-11-08
CN118786234A (zh) 2024-10-15

Similar Documents

Publication Publication Date Title
CN116897215B (zh) 钢板、构件和它们的制造方法
EP3971308B1 (en) High strength member, method for manufacturing high strength member, and method for manufacturing steel sheet for high strength member
US12077831B2 (en) Steel sheet, member, and methods for producing them
JP5983895B2 (ja) 高強度鋼板およびその製造方法、ならびに高強度亜鉛めっき鋼板の製造方法
KR102865563B1 (ko) 강판, 부재 및 그것들의 제조 방법
EP3875616B1 (en) Steel sheet, member, and methods for producing them
CN115003841A (zh) 钢板、部件及它们的制造方法
JP7311070B1 (ja) 鋼板および部材、ならびに、それらの製造方法
JP7287592B1 (ja) 鋼板および部材、ならびに、それらの製造方法
KR102739362B1 (ko) 고강도 강판 및 충격 흡수 부재 그리고 고강도 강판의 제조 방법
JP7311067B1 (ja) 鋼板および部材、ならびに、それらの製造方法
WO2024185764A1 (ja) 高強度鋼板およびその製造方法
KR102865564B1 (ko) 강판, 부재 및 그것들의 제조 방법
CN116897217A (zh) 钢板、构件和它们的制造方法
KR102738553B1 (ko) 고강도 강판 및 충격 흡수 부재 그리고 고강도 강판의 제조 방법
JP7817663B1 (ja) 鋼板及び外板部材
JP7666748B2 (ja) 高強度鋼板およびその製造方法
JP7779298B2 (ja) 高強度鋼板、鋼帯、高強度鋼板の製造方法、鋼帯の製造方法および部材
CN117321236A (zh) 高强度钢板及其制造方法和部件
CN117651786A (zh) 钢板、构件和它们的制造方法

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 2023508472

Country of ref document: JP

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22935635

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 202417053899

Country of ref document: IN

WWE Wipo information: entry into national phase

Ref document number: 202280092849.9

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 18844574

Country of ref document: US

WWE Wipo information: entry into national phase

Ref document number: 2022935635

Country of ref document: EP

ENP Entry into the national phase

Ref document number: 20247030706

Country of ref document: KR

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 1020247030706

Country of ref document: KR

ENP Entry into the national phase

Ref document number: 2022935635

Country of ref document: EP

Effective date: 20240911

WWE Wipo information: entry into national phase

Ref document number: 2401006211

Country of ref document: TH

WWE Wipo information: entry into national phase

Ref document number: MX/A/2024/011891

Country of ref document: MX

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 18844574