WO2023119850A1 - 水性樹脂組成物、塗膜の製造方法、水性樹脂組成物セット - Google Patents

水性樹脂組成物、塗膜の製造方法、水性樹脂組成物セット Download PDF

Info

Publication number
WO2023119850A1
WO2023119850A1 PCT/JP2022/039715 JP2022039715W WO2023119850A1 WO 2023119850 A1 WO2023119850 A1 WO 2023119850A1 JP 2022039715 W JP2022039715 W JP 2022039715W WO 2023119850 A1 WO2023119850 A1 WO 2023119850A1
Authority
WO
WIPO (PCT)
Prior art keywords
aqueous resin
resin composition
mass
group
copolymer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/039715
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
卓也 葛谷
直樹 村田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Resonac Corp
Original Assignee
Resonac Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Resonac Corp filed Critical Resonac Corp
Priority to JP2023569113A priority Critical patent/JPWO2023119850A1/ja
Publication of WO2023119850A1 publication Critical patent/WO2023119850A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D7/00—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials
    • B05D7/24—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials for applying particular liquids or other fluent materials
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/18—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing
    • C08G59/40—Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups ; e.g. general methods of curing characterised by the curing agents used
    • C08G59/50—Amines
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K5/00—Use of organic ingredients
    • C08K5/54—Silicon-containing compounds
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L33/00—Compositions of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides or nitriles thereof; Compositions of derivatives of such polymers
    • C08L33/04—Homopolymers or copolymers of esters
    • C08L33/06—Homopolymers or copolymers of esters of esters containing only carbon, hydrogen and oxygen, which oxygen atoms are present only as part of the carboxyl radical
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L63/00—Compositions of epoxy resins; Compositions of derivatives of epoxy resins
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D133/00—Coating compositions based on homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Coating compositions based on derivatives of such polymers
    • C09D133/04—Homopolymers or copolymers of esters
    • C09D133/06—Homopolymers or copolymers of esters of esters containing only carbon, hydrogen and oxygen, the oxygen atom being present only as part of the carboxyl radical
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D163/00—Coating compositions based on epoxy resins; Coating compositions based on derivatives of epoxy resins
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D5/00—Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
    • C09D5/02—Emulsion paints including aerosols
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D5/00—Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
    • C09D5/08—Anti-corrosive paints
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F283/00—Macromolecular compounds obtained by polymerising monomers on to polymers provided for in subclass C08G
    • C08F283/10—Macromolecular compounds obtained by polymerising monomers on to polymers provided for in subclass C08G on to polymers containing more than one epoxy radical per molecule

Definitions

  • the present invention relates to an aqueous resin composition, a method for producing a coating film, and an aqueous resin composition set.
  • This application claims priority based on Japanese Patent Application No. 2021-206028 filed in Japan on December 20, 2021, the content of which is incorporated herein.
  • metal products In general, the surface of metal products is surface-treated.
  • metal products used outdoors and metal products expected to be exposed to moisture are often surface-coated in order to prevent the generation of rust.
  • Patent Document 1 describes a coating composition for thick coating containing an emulsion composition in which polymer particles are dispersed in an aqueous medium and an aggregate.
  • the polymer particles described in Patent Document 1 are composed of a structural unit obtained by polymerizing an alkyl (meth)acrylate monomer having an alkyl group having 4 to 14 carbon atoms, and an ethylenically unsaturated carboxylic acid monomer. and a structural unit obtained by polymerizing other monomers, in the presence of a compound having at least two epoxy groups in one molecule and a basic catalyst, by emulsion polymerization. is.
  • Patent Document 2 describes a composition comprising an aqueous dispersion of thermoplastic polymer particles imbibed with a thermosetting compound having oxirane groups.
  • US Pat. No. 6,200,001 describes that the polymer particles have a sufficient concentration of anti-aggregating functional groups to stabilize the latex against aggregation.
  • Patent Document 3 describes forming an acrylate resin (acrylic/epoxy latex) that absorbs an epoxy compound by mixing an epoxy emulsion with an emulsion of an acrylate resin.
  • coating films formed on the surfaces of metal products made of cured products of conventional water-based resin compositions are required to exhibit antirust properties for a longer period of time.
  • coating films formed on the surfaces of metal products used outdoors, such as steel towers, bridges, ships, and harbor facilities are required to exhibit their anticorrosive properties for a longer period of time.
  • the present invention has been made in view of the above circumstances, and provides an aqueous resin composition, an aqueous resin composition set, and a dispersion liquid used for preparing an aqueous resin composition capable of forming a coating film exhibiting anticorrosive properties for a long period of time.
  • intended to provide Another object of the present invention is to provide a coating film comprising a cured product of the aqueous resin composition of the present invention and exhibiting anticorrosive properties for a long period of time, a method for producing the coating film, and a method for protecting metals.
  • a first aspect of the present invention provides the following aqueous resin composition.
  • an aqueous resin emulsion ( ⁇ ); a curing agent ( ⁇ ); a curing accelerator ( ⁇ ); and a silane coupling agent ( ⁇ ) comprises a copolymer (X), a polyepoxy compound (Y) having no ethylenically unsaturated bonds and having two or more epoxy groups in one molecule, and an aqueous medium (Z ), including
  • the copolymer (X) contains a structural unit derived from (meth)acrylic acid ester (A) and a structural unit derived from ethylenically unsaturated carboxylic acid (B),
  • the (meth)acrylic acid ester (A)-derived structural unit includes a (meth)acrylic acid ester (A1)-derived structural unit in which the number of carbon atoms in the alcohol-derived portion is 2 or less, and the copolymer ( The content of the polyepoxy compound
  • the content of structural units derived from the ethylenically unsaturated carboxylic acid (B) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 0.1% by mass or more and 10% by mass or less.
  • the curing agent ( ⁇ ) contains a polyamine (F) having active hydrogen reactive with epoxy groups
  • the curing accelerator ( ⁇ ) contains a tertiary amine that does not have an active hydrogen reactive with an epoxy group
  • the content of the silane coupling agent ( ⁇ ) is 0.03 parts by mass with respect to a total of 100 parts by mass of the copolymer (X) and the polyepoxy compound (Y) in the aqueous resin emulsion ( ⁇ ). part or more and 25 parts by mass or less.
  • the aqueous resin composition of the first aspect of the present invention preferably has the following features [2] to [15]. Combinations of two or more of the following features are also preferred.
  • [2] The aqueous resin composition according to [1], wherein the (meth)acrylic acid ester (A) is a (meth)acrylic acid alkyl ester.
  • the ethylenically unsaturated carboxylic acid (B) is at least selected from the group consisting of ⁇ , ⁇ -unsaturated monocarboxylic acids, ⁇ , ⁇ -unsaturated dicarboxylic acids, and vinyl compounds containing a carboxy group.
  • the water-based resin composition according to [1] or [2] which contains one type.
  • the polyepoxy compound (Y) consists of a bisphenol-type epoxy compound, a hydrogenated bisphenol-type epoxy compound, a diglycidyl ether, a triglycidyl ether, a tetraglycidyl ether, a diglycidyl ester, a triglycidyl ester, and a tetraglycidyl ester.
  • the aqueous resin composition according to any one of [1] to [3], comprising at least one selected from the group.
  • the copolymer (X) comprises a structural unit derived from the (meth)acrylic acid ester (A) and a structural unit derived from the ethylenically unsaturated carboxylic acid (B), [1] to [4 ] The water-based resin composition according to any one of the above.
  • the copolymer (X) includes a structural unit derived from an ethylenically unsaturated aromatic compound (C) having a benzene ring and an ethylenically unsaturated bond, any one of [1] to [4] The aqueous resin composition described.
  • the content of the polyamine (F) contained in the curing agent ( ⁇ ) is the active hydrogen contained in the polyamine (F) per equivalent of the epoxy group contained in the aqueous resin emulsion ( ⁇ ). is 0.10 equivalents or more and 1.50 equivalents or less, the aqueous resin composition according to any one of [1] to [6].
  • the content of the curing accelerator ( ⁇ ) is 0.0070 mol or more and 1.5 mol or less with respect to 1 equivalent of the epoxy group contained in the aqueous resin emulsion ( ⁇ ), [1] to [7] ]
  • the water-based resin composition according to any one of the above.
  • the content of the silane coupling agent ( ⁇ ) is 2 parts per 100 parts by mass of the copolymer (X) and the polyepoxy compound (Y) in the aqueous resin emulsion ( ⁇ ). .0 parts by mass or less, the aqueous resin composition according to any one of [1] to [8].
  • the curing accelerator ( ⁇ ) contains at least one selected from the group consisting of tertiary aliphatic amines, tertiary alicyclic amines, and tertiary heteroaromatic amines [1] The aqueous resin composition according to any one of to [9].
  • the silane coupling agent ( ⁇ ) is at least selected from the group consisting of an alkoxysilyl group (G) in which 1 to 3 alkoxy groups are bonded to a silicon atom, and an epoxy group, an amino group, and a mercapto group.
  • R 1 to R 3 are each independently an alkoxy group having 1 to 20 carbon atoms or an alkyl group having 1 to 20 carbon atoms, and at least one of R 1 to R 3 has a carbon number an alkoxy group of 1 to 20; n is an integer of 0 to 20; R 4 is any selected from the group consisting of a glycidoxy group, an amino group that is unsubstituted or has only one substituent, and a mercapto group is the basis of
  • a second aspect of the present invention provides the following coating film.
  • a coating film comprising a cured product of the aqueous resin composition according to any one of [1] to [15].
  • a third aspect of the present invention provides the following method for producing a coating film. [17] By mixing the aqueous resin emulsion ( ⁇ ), the curing agent ( ⁇ ), the curing accelerator ( ⁇ ), and the silane coupling agent ( ⁇ ), [1] to [15] ] ] A mixing step of preparing the aqueous resin composition according to any one of and a coating step of applying the aqueous resin composition to a surface to be coated.
  • a fourth aspect of the present invention provides the following aqueous resin composition set.
  • An aqueous resin composition set in which the components of the aqueous resin composition according to any one of [1] to [15] are stored separately in a first liquid and a second liquid, The first liquid contains the aqueous resin emulsion ( ⁇ ) and the silane coupling agent ( ⁇ ), An aqueous resin composition set, wherein the second liquid contains the curing agent ( ⁇ ) and the curing accelerator ( ⁇ ).
  • a fifth aspect of the present invention provides the following aqueous resin composition set.
  • An aqueous resin composition set in which the components of the aqueous resin composition according to any one of [1] to [15] are stored separately as a first liquid and a second liquid,
  • the first liquid contains the aqueous resin emulsion ( ⁇ )
  • a sixth aspect of the present invention provides the following dispersion.
  • [20] A dispersion that is used for preparing the aqueous resin composition according to any one of [1] to [15] and contains the aqueous resin emulsion ( ⁇ ).
  • a seventh aspect of the present invention provides the following metal protection method. [21] A method of protecting a metal with a coating film provided on the surface, wherein the coating film is a cured product of the water-based resin composition according to any one of [1] to [15]. .
  • the water-based resin composition and water-based resin composition set which can form the coating film which exhibits rust prevention for a long period of time can be provided. Further, according to the present invention, it is possible to provide a dispersion used for preparing the aqueous resin composition of the present invention. Further, according to the present invention, it is possible to provide a coating film comprising a cured product of the water-based resin composition of the present invention and exhibiting antirust properties for a long period of time, and a metal protection method for protecting metal with this coating film. Further, according to the present invention, it is possible to provide a method for producing a coating film comprising a cured product of the aqueous resin composition of the present invention.
  • aqueous resin composition Preferred examples of the aqueous resin composition, the coating film, the method for producing the coating film, the aqueous resin composition set, the dispersion, and the method for protecting metal of the present invention are described below in detail.
  • this invention is not limited only to embodiment shown below.
  • the number, type, position, amount, ratio, material, configuration, etc. can be added, omitted, replaced, changed, etc. without departing from the gist of the present invention.
  • (Meth)acrylate means acrylate or methacrylate.
  • (meth)acryl means acryl or methacryl.
  • “Ethylenically unsaturated bond” means a double bond between carbon atoms, excluding carbon atoms forming an aromatic ring.
  • Weight average molecular weight is a standard polystyrene conversion value measured by gel permeation chromatography (GPC).
  • the structural unit derived from the compound having an ethylenically unsaturated bond includes the chemical structure of the portion other than the ethylenically unsaturated bond in the compound, and the It means a unit having the same chemical structure as the portion other than the portion corresponding to the ethylenically unsaturated bond of the structural unit in the polymer.
  • the ethylenically unsaturated bonds of the compounds may be converted to single bonds in forming the polymer.
  • the structural unit derived from methyl methacrylate is represented by -CH 2 -C(CH 3 )(COOCH 3 )-.
  • a structural unit (b) derived from an ethylenically unsaturated carboxylic acid (B) described later for structural units having an ionic functional group such as a carboxy group, whether or not part of the functional group is ion-exchanged, the structural unit derived from the same ionic compound may be
  • a structural unit represented by —CH 2 —C(CH 3 )(COONa)— is also considered a structural unit derived from methacrylic acid.
  • one or more ethylenically unsaturated bonds may remain inside the structural unit as the structural unit of the polymer of the compound.
  • a plurality of independent ethylenically unsaturated bonds means a plurality of ethylenically unsaturated bonds that do not form a conjugated diene with each other.
  • the structural unit derived from divinylbenzene has a structure that does not have an ethylenically unsaturated bond (the portions corresponding to the two ethylenically unsaturated bonds of divinylbenzene are both polymer chains It may be a form incorporated in), or a structure having one ethylenically unsaturated bond (a form in which only the portion corresponding to one ethylenically unsaturated bond is incorporated into the polymer chain).
  • portions other than the chain structure (-C-C-) corresponding to the ethylenically unsaturated bond in the polymer for example, a functional group such as a carboxy group, correspond to the chemical structure of the monomer through a chemical reaction.
  • the chemical structure after polymerization is used as a reference for structural units derived from a compound having an ethylenically unsaturated bond in the polymer.
  • the “Curing” means that the molecules contained in the raw material bond with each other through a chemical reaction to form a polymer with a network structure.
  • the “coating film” is composed of a cured product formed by curing the resin component contained in the aqueous resin composition of the present embodiment, and a method such as applying the aqueous resin composition to the surface to be coated and drying the medium. It is integrated with the surface to be coated obtained by.
  • the "film” is a film-like cured product formed by curing the resin component contained in the aqueous resin composition of the present embodiment, after curing the resin component on the substrate, from the substrate It can be obtained by peeling.
  • the aqueous resin composition of this embodiment contains an aqueous resin emulsion ( ⁇ ), a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ).
  • the aqueous resin composition of the present embodiment is obtained by mixing an aqueous resin emulsion ( ⁇ ), a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ). manufactured.
  • the aqueous resin emulsion ( ⁇ ) comprises a copolymer (X), a polyepoxy compound (Y) having no ethylenically unsaturated bonds and having two or more epoxy groups in one molecule, and an aqueous medium (Z).
  • the aqueous resin emulsion ( ⁇ ) is an emulsion obtained by emulsion polymerization of monomers, which are structural units of the copolymer (X), in the aqueous medium (Z) in the presence of the polyepoxy compound (Y).
  • the water-based resin emulsion ( ⁇ ) is mixed with a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ), which will be described later, and cured to produce a cured product that exhibits rust prevention for a long period of time.
  • a curing agent ⁇
  • ⁇ curing accelerator
  • ⁇ silane coupling agent
  • the copolymer (X) has a structural unit (a) derived from the (meth)acrylic acid ester (A) and a structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B).
  • the structural unit (a) derived from the (meth)acrylic acid ester (A) includes a structural unit (a1) derived from the (meth)acrylic acid ester (A1) having 2 or less carbon atoms in the alcohol-derived portion.
  • the copolymer (X) may consist of only the structural unit (a) and the structural unit (b) (referred to as copolymer (X1)).
  • the copolymer (X) comprises a structural unit (a), a structural unit (b), and a structural unit (c) derived from an ethylenically unsaturated aromatic compound (C) having a benzene ring and an ethylenically unsaturated bond. ) and (referred to as a copolymer (X2)).
  • the copolymer (X2) may consist of structural units (a) to (c) only.
  • the copolymer (X) may have a structural unit (d) other than the structural units (a) to (c) (which is assumed to be a structural unit derived from another monomer (D)).
  • the amount of the copolymer (X) contained in the aqueous resin emulsion ( ⁇ ) can be arbitrarily selected. It is more preferably 25% by mass or more, and more preferably 25% by mass or more.
  • the amount of the copolymer (X) contained in the aqueous resin emulsion ( ⁇ ) can be arbitrarily selected, but it is preferably 60% by mass or less, preferably 50% by mass, based on the total amount of the aqueous resin emulsion ( ⁇ ). It is more preferably 40% by mass or less, more preferably 40% by mass or less. However, it is not limited only to these examples.
  • the content of the copolymer (X) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) described later is 60% by mass or more, preferably 70% by mass or more, and 80% by mass or more. % or more is more preferable.
  • the content of the copolymer (X) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) described later is 99% by mass or less, preferably 95% by mass or less. It is more preferably 90% by mass or less, more preferably 90% by mass or less.
  • the (meth)acrylic acid ester (A) preferably contains a (meth)acrylic acid alkyl ester, and more preferably consists of a (meth)acrylic acid alkyl ester.
  • a (meth)acrylic acid alkyl ester having a linear, branched or cyclic alkyl group having 1 to 18 carbon atoms is more preferable.
  • Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, and the like. These may be used alone or in combination of two or more.
  • Examples of the (meth)acrylic acid ester (A) may also include examples of the (meth)acrylic acid ester (A1) in which the alcohol-derived portion has 2 or less carbon atoms, which will be described later.
  • a (meth)acrylic acid ester having a carboxy group is not included in the (meth)acrylic acid ester (A), but is included in the ethylenically unsaturated carboxylic acid (B) described below.
  • the (meth)acrylic acid ester (A) may include a (meth)acrylic acid ester having an epoxy group. This is because the rust prevention property of the coating film made of the cured product of the aqueous resin composition of the present embodiment is improved.
  • Examples of (meth)acrylic acid esters having an epoxy group include glycidyl (meth)acrylate, ⁇ -methylglycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and 3,4-epoxycyclohexyl. Examples include methyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, and 3,4-epoxycyclohexylpropyl (meth)acrylate. These may be used alone or in combination of two or more. Among these epoxy group-containing (meth)acrylic acid esters, glycidyl (meth)acrylate is preferably included.
  • the (meth)acrylic acid ester (A) may be a (meth)acrylic acid ester that is neither an alkyl (meth)acrylic acid ester nor a (meth)acrylic acid ester having an epoxy group.
  • examples of such (meth)acrylic acid esters include (meth)acrylic acid esters having a hydroxy group.
  • Examples of (meth)acrylic acid esters having a hydroxy group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth) acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, polyethylene glycol Mono(meth)acrylic acid esters, mono(meth)acrylic acid esters of polyalkylene glycol such as mono(meth)acrylic acid esters of polypropylene glycol, and the like. These hydroxy group-containing (meth)acrylic acid esters may be used alone, or two or more of them may be used in combination.
  • the structural unit (a) derived from (meth)acrylic acid ester (A) may contain a structural unit derived from only one of these compounds, or may contain a structural unit derived from two or more of these compounds. may contain.
  • the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) is 20% by mass or more with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y). This is because the dispersibility of the monomer of the copolymer (X) and the polyepoxy compound (Y) can be improved in the method for producing the aqueous resin emulsion ( ⁇ ) described later. From this point of view, the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 35% by mass or more. is preferred, and 45% by mass or more is more preferred.
  • the content of the structural unit derived from the compound contained in the copolymer may mean a value calculated based on the mass of the compound used as the raw material of the copolymer.
  • the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is the total It may mean the mass ratio (% by mass) of the (meth)acrylic acid ester (A) used in the production of the copolymer (X) with respect to the amount.
  • the copolymer (X) is composed of the structural unit (a) and the structural unit (b), i.e., when the copolymer (X1) is a copolymer (X1), a monomer to form the copolymer (X1) and a polyepoxy compound From the viewpoint of improving dispersibility with (Y), the following proportions are preferred. That is, the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) with respect to the total amount of the copolymer (X1) and the polyepoxy compound (Y) is 35% by mass or more. More preferably, it is particularly preferably 45% by mass or more. It may be 50% by mass or more or 60% by mass or more as necessary.
  • the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) is 98% by mass or less with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y). This is because if the amount exceeds 98% by mass, the dispersibility of the aqueous resin emulsion ( ⁇ ) tends to decrease. From this point of view, the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 92% by mass or less. is preferred, and 87% by mass or less is more preferred. It may be 85% by mass or less, or 80% by mass or less, as necessary.
  • the copolymer (X) has the structural unit (a), the structural unit (b), and the structural unit (c), that is, when the copolymer (X) is the copolymer (X2), the aqueous Since the dispersibility of the resin emulsion ( ⁇ ) tends to decrease, the following proportions are preferred.
  • the content of the structural unit (a) derived from the (meth)acrylic acid ester (A) in the copolymer (X2) is more preferably 75% by mass or less, particularly preferably 60% by mass or less.
  • the (meth)acrylic acid ester (A)-derived structural unit includes a (meth)acrylic acid ester (A1)-derived structural unit in which the number of carbon atoms in the alcohol-derived portion is 2 or less.
  • the number of carbon atoms in the moieties other than the acryloyloxy group may be, for example, 1 or 2.
  • (Meth)acrylic acid ester (A1) includes methyl (meth)acrylate, ethyl (meth)acrylate, and the like.
  • the (meth)acrylic acid ester (A1) is preferably an alkyl (meth)acrylic acid ester in which the alcohol-derived moiety has 2 or less carbon atoms, more preferably methyl methacrylate.
  • the content of the structural unit (a1) derived from the (meth)acrylic acid ester (A1) is 15% by mass or more with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y).
  • the content of the structural unit (a1) derived from the (meth)acrylic acid ester (A1) is less than 15% by mass, the aqueous resin emulsion ( ⁇ ), the curing agent ( ⁇ ) containing a polyamine, and the curing accelerator ( This is because gelation proceeds rapidly by mixing with ⁇ ).
  • the content of the structural unit (a1) derived from the (meth)acrylic acid ester (A1) relative to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 15% by mass or more, and 20% by mass. It is preferably 30% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. This is because the water resistance and rust resistance of the coating film made of the cured product of the aqueous resin composition of the present embodiment are further improved.
  • the content of the structural unit (a1) may be 45% by mass or more or 50% by mass or more.
  • the upper limit of the content of the structural unit (a1) derived from the (meth)acrylic acid ester (A1) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is the (meth)acrylic acid ester (A ) is the same as the upper limit of the content described in (a). That is, the upper limit is 98% by mass or less, preferably 92% by mass or less, and more preferably 87% by mass or less.
  • the ratio of the structural unit (a1) to the structural unit (a) is is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, and particularly preferably 60% by mass or less. This is to improve the affinity between the copolymer (X) and the polyepoxy compound (Y).
  • Ethylenically unsaturated carboxylic acid (B) is a compound having an ethylenically unsaturated bond and a carboxy group.
  • Ethylenically unsaturated carboxylic acid (B) includes ⁇ , ⁇ -unsaturated monocarboxylic acid, ⁇ , ⁇ -unsaturated dicarboxylic acid, monoalkyl ester of ⁇ , ⁇ -unsaturated dicarboxylic acid, and vinyl containing a carboxy group.
  • It preferably contains at least one of the group consisting of compounds selected from the group consisting of ⁇ , ⁇ -unsaturated monocarboxylic acids, ⁇ , ⁇ -unsaturated dicarboxylic acids, and vinyl compounds containing a carboxy group. At least one type is preferably included.
  • Examples of ⁇ , ⁇ -unsaturated mono- or dicarboxylic acids include acrylic acid, methacrylic acid, crotonic acid, citraconic acid, itaconic acid, maleic acid, and fumaric acid.
  • Examples of vinyl compounds containing a carboxy group include monohydroxyethyl phthalate (meth)acrylate and monohydroxypropyl oxalate (meth)acrylate.
  • the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) may be a structural unit derived from only one of these compounds, or may contain structural units derived from two or more of these compounds. good too.
  • the ethylenically unsaturated carboxylic acid (B) includes a compound having a (meth)acryloyl group and a carboxy group, or consists only of a compound having a (meth)acryloyl group and a carboxy group. is preferred. It is also preferable that the ethylenically unsaturated carboxylic acid (B) contains (meth)acrylic acid or consists only of (meth)acrylic acid.
  • Structural unit (b) preferably consists of only structural units derived from a compound having a (meth)acryloyl group and a carboxy group, and further preferably contains structural units derived from (meth)acrylic acid.
  • the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) is 0.1% by mass or more with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y). This is for improving the dispersibility of the aqueous resin emulsion ( ⁇ ).
  • the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 0.3% by mass or more. It is preferably 0.5% by mass or more, and more preferably 0.5% by mass or more.
  • the content of the structural unit (b) may be 0.8% by mass or more, or 1.0% by mass or more.
  • the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) is 10% by mass or less with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y). This is for suppressing gelation of the copolymer (X) in a high-temperature environment and improving the high-temperature stability of the aqueous resin emulsion ( ⁇ ).
  • the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 7% by mass or less. is preferable, and it is more preferably 5% by mass or less.
  • the content of the structural unit (b) may be 4% by mass or less, or 3% by mass or less.
  • the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) with respect to the total amount of the copolymer (X) is preferably 0.2% by mass or more, and 0.5% by mass. It is more preferably 0.8% by mass or more, and more preferably 0.8% by mass or more.
  • the content of the structural unit (b) derived from the ethylenically unsaturated carboxylic acid (B) with respect to the total amount of the copolymer (X) is preferably 12% by mass or less, more preferably 8% by mass or less. It is preferably 5% by mass or less, more preferably 3% by mass or less.
  • the ethylenically unsaturated aromatic compound (C) is neither a (meth)acrylic acid ester (A) nor an ethylenically unsaturated carboxylic acid (B), and has a benzene ring and an ethylenically unsaturated bond. is a compound.
  • the maleimide compound described later is not included in the ethylenically unsaturated aromatic compound (C).
  • the ethylenically unsaturated aromatic compound (C) is preferably an aromatic vinyl compound.
  • aromatic vinyl compound as the ethylenically unsaturated aromatic compound (C) examples include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, ⁇ -methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, tert-butoxystyrene, vinyltoluene, divinyltoluene, vinylnaphthalene, monochlorostyrene, dichlorostyrene, monobromostyrene, dibromostyrene, tribromostyrene, fluorostyrene, styrene sulfone acids and salts thereof, ⁇ -methylstyrenesulfonic acid and salts thereof, p-hydroxystyrene, m-hydroxystyrene, o-hydroxystyrene, p-isoprop
  • the structural unit (c) derived from the ethylenically unsaturated aromatic compound (C) may be derived from only one of these compounds, or may contain structural units derived from two or more of these compounds.
  • the structural unit (c) is more preferably composed of a structural unit derived from a hydrocarbon, and particularly preferably a structural unit derived from styrene.
  • the copolymer (X) contains the structural unit (c) derived from the ethylenically unsaturated aromatic compound (C), i.e. when the copolymer (X) is the copolymer (X2)
  • the copolymer The content of structural unit (c) with respect to the total amount of (X2) and polyepoxy compound (Y) is preferably 5% by mass or more. This is for improving the water resistance of the coating film made of the cured product of the aqueous resin composition of the present embodiment. From this point of view, the content of the structural unit (c) with respect to the total amount of the copolymer (X2) and the polyepoxy compound (Y) is more preferably 10% by mass or more, and more preferably 15% by mass or more. is even more preferred. The content of the structural unit (c) may be 18% by mass or more.
  • the content of the structural unit (c) with respect to the total amount of the copolymer (X2) and the polyepoxy compound (Y) is 50% by mass or less.
  • the content of the structural unit (c) with respect to the total amount of the copolymer (X2) and the polyepoxy compound (Y) is more preferably 40% by mass or less, more preferably 35% by mass or less. is more preferred.
  • the content of structural unit (c) may be 33% by mass or less, 30% by mass or less, 28% by mass or less, or 23% by mass or less.
  • the content of the structural unit (c) with respect to the total amount of the copolymer (X2) is preferably 5% by mass or more, more preferably 15% by mass or more, and further preferably 25% by mass or more. preferable.
  • the content of the structural unit (c) with respect to the total amount of the copolymer (X2) is preferably 55% by mass or less, more preferably 45% by mass or less, and further preferably 35% by mass or less. preferable.
  • the other monomer (D) is none of the (meth)acrylic acid ester (A), the ethylenically unsaturated carboxylic acid (B), and the ethylenically unsaturated aromatic compound (C), and It is a compound having an ethylenically unsaturated bond that can be copolymerized with the compound used for synthesizing the copolymer (X).
  • Other monomers (D) include, for example, conjugated diene compounds, maleimide compounds, vinyl ether compounds, allyl ether compounds, dialkyl esters of unsaturated dicarboxylic acids, and vinyl compounds having a cyano group.
  • conjugated diene compound examples include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3 butadiene, and chloroprene (2-chloro-1,3-butadiene). etc. These conjugated diene compounds may be used alone or in combination of two or more.
  • maleimide compound examples include maleimide, N-methylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-dodecylmaleimide, N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4- methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-(2,6-diethylphenyl)maleimide, N-(2-methoxyphenyl)maleimide, N-benzylmaleimide, N-(4-hydroxy phenyl)maleimide, N-naphthylmaleimide, N-cyclohexylmaleimide and the like. These maleimide compounds may be used alone or in combination of two or more.
  • vinyl ether compound examples include alkyl vinyl ethers such as methyl vinyl ether and ethyl vinyl ether, and hydroxyl group-containing alkyl vinyl ethers in which some hydrogen atoms are substituted with hydroxyl groups.
  • allyl ether compounds include allyl alkyl ethers such as allyl methyl ether and allyl ethyl ether, hydroxyl group-containing allyl alkyl ethers in which some hydrogen atoms are substituted with hydroxyl groups, and allyl glycidyl ethers.
  • dialkyl esters of unsaturated dicarboxylic acids examples include dialkyl esters of unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid. These dialkyl esters of unsaturated dicarboxylic acids may be used alone or in combination of two or more.
  • Examples of vinyl compounds having a cyano group include acrylonitrile, methacrylonitrile, ⁇ -ethylacrylonitrile, ⁇ -isopropylacrylonitrile, ⁇ -chloroacrylonitrile, and ⁇ -fluoroacrylonitrile.
  • One of these cyano group-containing vinyl monomers may be used alone, or two or more thereof may be used in combination.
  • Polyepoxy compound (Y) is a compound having no ethylenically unsaturated bond and having two or more epoxy groups in one molecule.
  • the polyepoxy compound (Y) is selected from the group consisting of bisphenol-type epoxy compounds, hydrogenated bisphenol-type epoxy compounds, diglycidyl ethers, triglycidyl ethers, tetraglycidyl ethers, diglycidyl esters, triglycidyl esters, and tetraglycidyl esters. It is preferable to include at least one of
  • Examples of compounds having two or more epoxy groups in one molecule include diglycidyl ether of bisphenol A, diglycidyl ether of hydrogenated bisphenol A, diglycidyl ether of bisphenol F, diglycidyl ether of hydrogenated bisphenol F, and glycerin.
  • the polyepoxy compound (Y) is more preferably a bisphenol type epoxy compound or a hydrogenated bisphenol type epoxy compound, more preferably a bisphenol A type epoxy compound or a hydrogenated bisphenol A type epoxy compound. Epoxy compounds are more preferred. This is because the water resistance and rust resistance of the coating film made of the cured product of the aqueous resin composition of the present embodiment are further improved.
  • the weight average molecular weight of the polyepoxy compound (Y) is not particularly limited, it is preferably 1000 or less, more preferably 800 or less, and still more preferably 500 or less. This is because the compatibility of the polyepoxy compound (Y) with the copolymer (X) is improved, and the aqueous resin emulsion ( ⁇ ) is excellent in dispersibility and storage stability.
  • the lower limit of the weight-average molecular weight of the polyepoxy compound (Y) can be arbitrarily selected, and may be, for example, 200 or 300, but is not limited to these.
  • the epoxy equivalent of the polyepoxy compound (Y) (mass of the polyepoxy compound (Y) per 1 mol of epoxy group) is preferably 500 g/mol or less, more preferably 350 g/mol or less, and 250 g/mol. It is more preferably 200 g/mol or less, particularly preferably 200 g/mol or less. This is because the strength of the film made of the cured product of the aqueous resin composition of the present embodiment is increased.
  • the lower limit of the epoxy equivalent can be arbitrarily selected, and may be, for example, 70 g/mol or more, or 120 g/mol or more, but is not limited to these examples.
  • the content of the polyepoxy compound (Y) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 1% by mass or more. This is because a coating film having excellent rust resistance can be obtained by curing the aqueous resin composition. From this point of view, the content of the polyepoxy compound (Y) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is preferably 5% by mass or more, and 8% by mass or more. is more preferable, and 10% by mass or more is even more preferable. If necessary, it may be 12% by mass or more, or 20% by mass or more.
  • the content of the polyepoxy compound (Y) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is 40% by mass or less. This is because a highly dispersible aqueous resin emulsion ( ⁇ ) can be obtained. From this point of view, the content of the polyepoxy compound (Y) with respect to the total amount of the copolymer (X) and the polyepoxy compound (Y) is preferably 35% by mass or less, more preferably 30% by mass or less. is more preferred.
  • the amount of the polyepoxy compound (Y) contained in the aqueous resin emulsion ( ⁇ ) is preferably 1% by mass or more, more preferably 3% by mass or more, relative to the total amount of the aqueous resin emulsion ( ⁇ ). It is preferably 4% by mass or more, and more preferably 4% by mass or more.
  • the amount of the polyepoxy compound (Y) contained in the aqueous resin emulsion ( ⁇ ) is preferably 30% by mass or less, more preferably 20% by mass or less, relative to the total amount of the aqueous resin emulsion ( ⁇ ). It is preferably 15% by mass or less, and more preferably 15% by mass or less.
  • the hydrophilic (water-soluble) solvent to be added to water can be arbitrarily selected, and examples thereof include methanol, ethanol, N-methylpyrrolidone, and the like.
  • the amount of the aqueous medium (Z) in the aqueous resin emulsion ( ⁇ ) can be selected as necessary, but it is preferably an amount such that the concentration of non-volatile matter in the aqueous resin emulsion ( ⁇ ) is 20% by mass or more. , more preferably 30% by mass or more, more preferably 40% by mass or more.
  • the amount of the aqueous medium (Z) in the aqueous resin emulsion ( ⁇ ) can be selected as required, but is preferably 80% by mass or less, more preferably 70% by mass or less.
  • the concentration of nonvolatile matter in the aqueous resin emulsion ( ⁇ ) may be 50 to 70% by mass, or may be 55 to 65% by mass.
  • the aqueous resin emulsion ( ⁇ ) comprises (meth)acrylic acid ester (A), ethylenically unsaturated carboxylic acid (B), and optional components in the presence of polyepoxy compound (Y).
  • a monomer containing an ethylenically unsaturated aromatic compound (C) and / or another monomer (D) (that is, a monomer for constituting the copolymer (X)) is added in an aqueous medium (Z) can be produced by an emulsion polymerization method.
  • the content of each raw material in the total raw materials used for the production of the aqueous resin emulsion ( ⁇ ) is the same as the content of the structural unit derived from the raw material or the compound corresponding to the raw material in the aqueous resin emulsion ( ⁇ ). .
  • a method of collectively charging each component including a monomer, a method of polymerizing while continuously supplying each component, and the like can be used. Stirring is preferred during the polymerization reaction.
  • Emulsion polymerization is carried out at an arbitrarily selected temperature, for example, preferably at a temperature of 30 to 90°C, more preferably at a temperature of 40 to 80°C, and even more preferably at a temperature of 40 to 70°C. . This is to prevent the carboxy group contained in the monomer from reacting with the epoxy group contained in the polyepoxy compound (Y).
  • An emulsifier may be used for emulsion polymerization.
  • the emulsifier to be used can be arbitrarily selected, for example, nonionic surfactants such as polyoxyalkylene alkyl ethers, polyoxyalkylene alkylphenol ethers, polyoxyalkylene fatty acid esters, polyoxyalkylene sorbitan fatty acid esters, alkyl sulfate salts, alkyl benzene
  • Anionic surfactants such as sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, polyoxyalkylene alkyl sulfates, and polyoxyalkylene alkyl phosphates are included.
  • alkylbenzenesulfonates are preferably used, and sodium dodecylbenzenesulfonate is more preferably used.
  • a polymerization initiator In emulsion polymerization, it is preferable to use a polymerization initiator.
  • the polymerization initiator it is preferable to use, for example, a peroxide.
  • peroxides used as polymerization initiators include persulfates such as potassium persulfate and ammonium persulfate, and hydrogen peroxide.
  • a redox initiator can also be used in combination with a peroxide and a reducing agent.
  • reducing agents include sodium hydrogen sulfite, sodium sulfoxylate formaldehyde, ascorbic acid, sulfites, tartaric acid and salts thereof.
  • Alcohols and mercaptans may also be used as chain transfer agents, if necessary.
  • an aqueous resin emulsion ( ⁇ ) in which the polyepoxy compound (Y) is uniformly dispersed in the particles of the copolymer (X) produced is obtained.
  • uniformly dispersed does not necessarily mean that the copolymer (X) and the polyepoxy compound (Y) are compatible with each other. and the surface side, the domains of the polyepoxy compound (Y) should be present evenly.
  • the pH of the aqueous resin emulsion ( ⁇ ) is preferably 2-10, more preferably 5-9. When the pH is within this range, the mechanical stability and chemical stability of the aqueous resin emulsion ( ⁇ ) can be improved.
  • the pH is a value measured at a liquid temperature of 25° C. using a pH meter with a hydrogen ion concentration indicator using a glass electrode as a standard electrode.
  • the pH can be adjusted by adding a basic substance to the aqueous resin emulsion ( ⁇ ) during or after emulsion polymerization. Examples of basic substances used for pH adjustment include ammonia, triethylamine, ethanolamine, caustic soda, and the like. These may be used individually by 1 type, and may be used in combination of 2 or more type.
  • Non-volatile content concentration of aqueous resin emulsion ( ⁇ ) The nonvolatile content of the aqueous resin emulsion ( ⁇ ) is preferably 10 to 65% by mass, more preferably 15 to 60% by mass, and more preferably 20 to 55% by mass.
  • the nonvolatile content concentration may be 30 to 50% by mass, or 35 to 45% by mass.
  • the concentration of non-volatile matter in the aqueous resin emulsion ( ⁇ ) is determined by mixing the aqueous resin emulsion ( ⁇ ), the curing agent ( ⁇ ), the curing accelerator ( ⁇ ), the silane coupling agent ( ⁇ ), etc., which will be described later.
  • the concentration of non-volatile matter in the aqueous resin emulsion ( ⁇ ) can be appropriately adjusted by adjusting the amount of the aqueous medium (Z) added.
  • the non-volatile content concentration of the aqueous resin emulsion ( ⁇ ) can be determined by the method shown below. 1 g of the water-based resin emulsion ( ⁇ ) is weighed into an aluminum dish having a diameter of 5 cm, and dried at 105° C. for 1 hour at atmospheric pressure in a drier while air is circulated. The mass of the residue obtained is then determined. Then, the ratio (% by mass) of the measured mass of the residue to the mass of the aqueous resin emulsion ( ⁇ ) before drying is determined as the non-volatile content of the aqueous resin emulsion ( ⁇ ).
  • the viscosity of the aqueous resin emulsion ( ⁇ ) is measured at 23°C.
  • the viscosity of the aqueous resin emulsion ( ⁇ ) is measured using a Brookfield viscometer at a rotational speed of 60 rpm with a rotor selected according to the viscosity of the aqueous resin emulsion. For example, when the viscosity of the aqueous resin emulsion ( ⁇ ) is several mPa ⁇ s to several hundred mPa ⁇ s, rotor No. Measured using 1.
  • the viscosity may be, for example, 0.1 to 300 mPa ⁇ s, 1 to 100 mPa ⁇ s, 3 to 50 mPa ⁇ s, or 5 to 25 mPa ⁇ s. .
  • the glass transition point Tg of the copolymer (X) is calculated based on the glass transition point of the homopolymer of each monomer used to synthesize the copolymer (X).
  • the glass transition point Tg of the copolymer (X) is preferably -30°C (243K) or higher. This is because the strength of the film made of the cured product of the aqueous resin composition of the present embodiment is improved. From this point of view, the glass transition point Tg of the copolymer (X) is preferably ⁇ 10° C. (263 K) or higher, more preferably 0° C. (273 K) or higher. The glass transition point Tg of the copolymer (X) may be 5°C or higher. The glass transition point Tg of the copolymer (X) is preferably 100°C (373K) or lower, more preferably 80°C (353K) or lower.
  • the glass transition point Tg of copolymer (X) is more preferably 60° C. (333 K) or lower, particularly preferably 50° C. (323 K) or lower. This is because in the case of such a range, the flexibility of the coating film made of the cured product of the aqueous resin composition of the present embodiment can be improved.
  • the glass transition point Tg of the copolymer (X) may be 40°C or lower, 30°C or lower, or 20°C or lower.
  • Epoxy group content in aqueous resin emulsion ( ⁇ ) The content of epoxy groups in the aqueous resin emulsion ( ⁇ ) is the ratio of the number of moles of epoxy groups contained in 1 g of the aqueous resin emulsion ( ⁇ ).
  • the method for determining the amount N 1 [mol/g] of the epoxy groups contained per 1 g of the aqueous resin emulsion ( ⁇ ) is as described in Examples described later.
  • Epoxy group content in total amount of copolymer (X) and polyepoxy compound (Y) contains an epoxy group.
  • the content of epoxy groups in the total amount of copolymer (X) and polyepoxy compound (Y) is preferably 0.50 ⁇ 10 ⁇ 4 mol/g or more, more preferably 1.0 ⁇ 10 ⁇ 4 It is more preferably at least 4.0 ⁇ 10 ⁇ 4 mol/g, even more preferably at least 6.0 ⁇ 10 ⁇ 4 mol/g. This is because the water resistance, rust resistance, and adhesion to the substrate of the coating film made of the cured product of the water-based resin composition of the present embodiment can be enhanced.
  • the content of epoxy groups in the total amount of copolymer (X) and polyepoxy compound (Y) is preferably 50 ⁇ 10 ⁇ 4 mol/g or less, and 30 ⁇ 10 ⁇ 4 mol/g or less. is more preferably 20 ⁇ 10 ⁇ 4 mol/g or less.
  • the content of epoxy groups in the total amount of copolymer (X) and polyepoxy compound (Y) may be 15 ⁇ 10 ⁇ 4 mol/g or less.
  • the epoxy group content in the nonvolatile matter of the aqueous resin emulsion ( ⁇ ) is preferably 0.50 ⁇ 10 ⁇ 4 mol/g or more, and is preferably 3.0 ⁇ 10 ⁇ 4 mol/g or more. More preferably, it is 5.0 ⁇ 10 ⁇ 4 mol/g or more. This is because the water resistance, rust resistance, and adhesion to the substrate of the coating film made of the cured product of the water-based resin composition of the present embodiment can be enhanced.
  • the epoxy group content in the nonvolatile matter of the aqueous resin emulsion ( ⁇ ) may be 6.0 ⁇ 10 ⁇ 4 mol/g or more.
  • the epoxy group content in the nonvolatile matter of the aqueous resin emulsion ( ⁇ ) is preferably 50 ⁇ 10 ⁇ 4 mol/g or less, more preferably 30 ⁇ 10 ⁇ 4 mol/g or less, and 20 It is more preferably not more than ⁇ 10 -4 mol/g.
  • the epoxy group content in the nonvolatile matter of the aqueous resin emulsion ( ⁇ ) may be 15 ⁇ 10 ⁇ 4 mol/g or less.
  • Carboxy group content in aqueous resin emulsion ( ⁇ ) The content of carboxy groups in the aqueous resin emulsion ( ⁇ ) is the ratio of the number of moles of carboxy groups contained in 1 g of the aqueous resin emulsion ( ⁇ ).
  • the method for determining the number of moles of carboxyl groups contained per 1 g of the aqueous resin emulsion ( ⁇ ) is as described in the examples below.
  • the copolymer (X) contained in the aqueous resin emulsion ( ⁇ ) contains a carboxy group.
  • the content of carboxy groups in the total amount of copolymer (X) and polyepoxy compound (Y) is preferably 0.10 ⁇ 10 ⁇ 4 mol/g or more, more preferably 0.50 ⁇ 10 ⁇ 4 mol /g or more, more preferably 1.0 ⁇ 10 ⁇ 4 mol/g or more. This is because aggregation of the copolymer (X) can be suppressed during storage of the aqueous resin emulsion ( ⁇ ) during and after polymerization.
  • the content of carboxy groups in the total amount of copolymer (X) and polyepoxy compound (Y) is preferably 10 ⁇ 10 ⁇ 4 mol/g or less, more preferably 5.0 ⁇ 10 ⁇ 4 mol/g. g or less is more preferable. It may be 3.0 ⁇ 10 ⁇ 4 mol/g or less, 2.5 ⁇ 10 ⁇ 4 mol/g or less, or 2.0 ⁇ 10 ⁇ 4 mol/g or less.
  • Carboxy group content in non-volatile matter of aqueous resin emulsion ( ⁇ ) is preferably 0.10 ⁇ 10 ⁇ 4 mol/g or more, more preferably 0.50 ⁇ 10 ⁇ 4 mol/g or more. More preferably, it is 1.0 ⁇ 10 ⁇ 4 mol/g or more. This is because aggregation of the copolymer (X) can be suppressed during storage of the aqueous resin emulsion ( ⁇ ) during and after polymerization.
  • the content of carboxy groups in the nonvolatile matter of the aqueous resin emulsion ( ⁇ ) is preferably 10 ⁇ 10 ⁇ 4 mol/g or less, more preferably 5.0 ⁇ 10 ⁇ 4 mol/g or less. . It may be 3.0 ⁇ 10 ⁇ 4 mol/g or less, 2.5 ⁇ 10 ⁇ 4 mol/g or less, or 2.0 ⁇ 10 ⁇ 4 mol/g or less.
  • the carboxy group includes not only —COOH but also a structure in which a cation other than a hydrogen ion and —COO 2 — are bonded.
  • the content of carboxy groups in the non-volatile matter of the water-based resin emulsion ( ⁇ ) is, as shown by the following formula, the content of carboxy groups in the raw materials, the functional groups that react with the carboxy groups in the raw materials, polymerization It is obtained from the value obtained by subtracting the amount of decrease before and after.
  • the raw materials refer to the components used for the synthesis of the aqueous resin emulsion ( ⁇ ).
  • the functional group that reacts with the carboxy group is an epoxy group in this embodiment, and the hydroxy group is not considered as a functional group that reacts with the carboxy group.
  • N 3 [mol/g] is the total amount of carboxyl groups in the raw materials (including initiators, solvents, other additives, etc.), and the total amount of epoxy groups in the raw materials (including initiators, solvents, other additives, etc.). is N 2 [mol/g], and the amount of epoxy groups contained per 1 g of the aqueous resin emulsion ( ⁇ ) is N 1 [mol/g].
  • the non-volatile content concentration of the aqueous resin emulsion ( ⁇ ) is defined as C S [% by mass].
  • R CX is represented by the formula (30). How to obtain N1 and N2 will be described later in Examples. N2 can be obtained by calculation.
  • R CX [mol/g] ⁇ N 3 ⁇ (N 2 ⁇ N 1 ) ⁇ /(C S /100) (30)
  • the curing agent ( ⁇ ) contains a polyamine (F) having active hydrogens with reactivity towards epoxy groups.
  • polyamine (F) is a compound having two or more amino groups in one molecule.
  • the amino group of the polyamine (F) having active hydrogen is an unsubstituted amino group (—NH 2 (no substituent), or an amino group having only one substituent (—NHR (R is a substituent)).
  • the number of types of polyamine (F) having active hydrogen for epoxy groups contained in the curing agent ( ⁇ ) may be one, or two or more.
  • Polyamines (F) include, for example, aliphatic polyamines, alicyclic polyamines, and aromatic polyamines.
  • aliphatic polyamines examples include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, modified products thereof, and the like.
  • aromatic polyamines examples include m-xylylenediamine, diaminodiphenylmethane, m-phenylenediamine, diaminodiphenylsulfone, and modified products thereof.
  • a commercially available product may be used as the curing agent ( ⁇ ).
  • examples of commercially available curing agents include ADEKA HARDNER EH-8051 (polyamine) (manufactured by ADEKA Corporation); Fujicure FXI-919, Tomide TXH-674-B and TXS-53-C (manufactured by T&K TOKA Corporation); Gaskamine 328 (Mitsubishi Gas Chemical Co., Ltd.); Jeffamine D-230 and Jeffamine ED-600 (Huntsman Japan Co., Ltd.).
  • the content of the polyamine (F) contained in the curing agent ( ⁇ ) is such that the active hydrogen contained in the polyamine (F) is 0.10 equivalent or more per equivalent of the epoxy group contained in the aqueous resin emulsion ( ⁇ ). It is preferably 0.20 equivalents or more, more preferably 0.50 equivalents or more, and particularly preferably 0.60 equivalents or more.
  • the active hydrogen contained in the polyamine (F) is 0.10 equivalent or more
  • the crosslink density of the aqueous resin composition after curing is increased, and the coating film further suppresses the permeation of water and ions.
  • the coating film has good adhesion to metal materials. From these facts, the coating film made of the cured product of the water-based resin composition in which the active hydrogen contained in the polyamine (F) is 0.10 equivalent or more exhibits antirust properties for a long period of time.
  • the content of the polyamine (F) contained in the curing agent ( ⁇ ) is such that the active hydrogen contained in the polyamine (F) is 1.5 equivalents or less per equivalent of the epoxy group contained in the aqueous resin emulsion ( ⁇ ). preferably 1.3 equivalents or less, even more preferably 1.2 equivalents or less. This is because excessive curing shrinkage of the epoxy resin is suppressed, and the adhesion of the coating film to the substrate is improved.
  • the curing accelerator ( ⁇ ) has the function of accelerating the curing of the water-based resin composition and forming a film with high film yield strength.
  • Curing accelerators ( ⁇ ) include tertiary amines that do not have active hydrogens that are reactive towards epoxy groups.
  • the tertiary amine in the present embodiment is represented by NR 11 R 22 R 33 (wherein R 11 R 22 R 33 is a substituent, each of which may be different, or two or more of which are the same). R 11 R 22 R 33 may combine with each other to form a ring.).
  • the curing accelerator ( ⁇ ) preferably contains at least one selected from the group consisting of tertiary aliphatic amines, tertiary alicyclic amines and tertiary heteroaromatic amines. This is because the nucleophilicity of the curing accelerator ( ⁇ ) is increased and the curing reaction proceeds efficiently.
  • tertiary aliphatic amines examples include triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, tri-sec-butylamine, and tri-n-hexylamine.
  • Tertiary alicyclic amines include, for example, 1,4-diazabicyclo[2.2.2]octane (DABCO), 1,5-diazabicyclo[4.3.0]non-5-ene, 1,8 -diazabicyclo[5.4.0]undec-7-ene and the like.
  • DABCO 1,4-diazabicyclo[2.2.2]octane
  • 1,5-diazabicyclo[4.3.0]non-5-ene 1,8 -diazabicyclo[5.4.0]undec-7-ene and the like.
  • a compound having an imidazole skeleton it is preferable to use a compound having an imidazole skeleton, and specific examples include imidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, and the like.
  • the curing accelerator ( ⁇ ) may be a tertiary aromatic amine having a phenyl group not directly bonded to the nitrogen atom of the tertiary amine (NR 11 R 22 R 33 ).
  • tertiary aromatic amines include dimethylbenzylamine, diethylbenzylamine, tribenzylamine, 2,4,6-trisdimethylaminomethylphenol, 2-phenylimidazole, and the like.
  • curing accelerators ( ⁇ ) it is particularly preferable to use the following compounds (i) and/or (ii).
  • Tertiary alicyclic amines include, for example, 1,4-diazabicyclo[2.2.2]octane (DABCO).
  • Tertiary heteroaromatic amines include, for example, imidazole.
  • the curing accelerator ( ⁇ ) may be used singly or in combination of two or more.
  • the content of the curing accelerator ( ⁇ ) is preferably 0.0070 mol or more, more preferably 0.010 mol or more, with respect to 1 equivalent of epoxy groups contained in the aqueous resin emulsion ( ⁇ ). It is more preferably 0.05 mol or more, and particularly preferably 0.10 mol or more. This is because the coating film made of the cured product of the water-based resin composition of the present embodiment has a high crosslink density and high adhesion to the substrate, and exhibits antirust properties over a long period of time.
  • the content of the curing accelerator ( ⁇ ) is preferably 1.5 mol or less, more preferably 0.70 mol or less, more preferably 0.70 mol or less, relative to 1 equivalent of epoxy groups contained in the aqueous resin emulsion ( ⁇ ). It is more preferably 0.44 mol or less, particularly preferably 0.38 mol or less. This is because the cured product of the aqueous resin composition of the present embodiment forms a coating film having good adhesion to metal materials. Further, when the content of the curing accelerator ( ⁇ ) is 1.5 mol or less, gelling of the water-based resin composition in a short time can be suppressed, and a cured product with good rust resistance can be obtained.
  • the silane coupling agent ( ⁇ ) is a silicon atom to which an alkoxy group is bonded in one molecule, a vinyl group, a (meth)acryloyl group, an epoxy group, an amino group, a mercapto group, an isocyanato group, or the like. and a functional group having reactivity with an organic substance.
  • the silane coupling agent ( ⁇ ) is an alkoxysilyl group (G) in which 1 to 3 alkoxy groups are bonded to a silicon atom, and at least one functional group selected from the group consisting of an epoxy group, an amino group, and a mercapto group.
  • the silane coupling agent ( ⁇ ) is a compound having at least one alkoxysilyl group (G) in one molecule, and may have multiple alkoxysilyl groups (G) in one molecule.
  • the silane coupling agent ( ⁇ ) is preferably a compound having only one alkoxysilyl group (G) in one molecule.
  • a compound that corresponds to the silane coupling agent ( ⁇ ) and corresponds to the curing agent ( ⁇ ) and/or the curing accelerator ( ⁇ ) is the silane coupling agent ( ⁇ ). .
  • the silane coupling agent ( ⁇ ) is preferably a compound represented by the following general formula (1).
  • R 1 to R 3 are each independently an alkoxy group having 1 to 20 carbon atoms or an alkyl group having 1 to 20 carbon atoms, and at least one of R 1 to R 3 has a carbon number an alkoxy group of 1 to 20; n is an integer of 0 to 20; R 4 is any selected from the group consisting of a glycidoxy group, an amino group that is unsubstituted or has only one substituent, and a mercapto group is the basis of
  • R 1 to R 3 are each independently an alkoxy group having 1 to 20 carbon atoms or an alkyl group having 1 to 20 carbon atoms.
  • the alkoxy group having 1 to 20 carbon atoms includes methoxy, ethoxy, propoxy, butoxy, pentoxy, octoxy and the like.
  • Examples of alkyl groups having 1 to 20 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, butyl group, pentyl group, hexyl group, octyl group, 2-ethylhexyl group, decyl group, dodecyl group and tetradecyl group. , hexadecyl group, octadecyl group and the like.
  • R 1 to R 3 are an alkoxy group having 1 to 20 carbon atoms
  • the number of carbon atoms in the alkoxy group is preferably 1 to 8, more preferably 1 to 3, particularly 1 or 2. is preferably
  • the alkoxy group in the alkoxysilyl group (G) of the silane coupling agent ( ⁇ ) undergoes a hydrolysis reaction with the aqueous medium (Z). to have a low molecular weight. If the alcohol produced by the hydrolysis reaction remains in the coating film, it may cause the coating film to swell, thereby reducing the rust-preventive properties of the coating film.
  • the alcohol produced by the hydrolysis reaction has a low molecular weight, it is easily volatilized by applying the water-based resin composition and drying it. Therefore, the alcohol produced by the hydrolysis reaction does not remain in the coating film, and the water-based resin composition provides a coating film with excellent rust resistance.
  • R 1 to R 3 are an alkyl group having 1 to 20 carbon atoms
  • the number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 1 to 3, because of easy availability. More preferably, 1 or 2 is particularly preferred.
  • R 1 to R 3 is an alkoxy group having 1 to 20 carbon atoms, and two or three of R 1 to R 3 are alkoxy groups having 1 to 3 carbon atoms. It is preferably an alkoxy group of 20 (in other words, dialkoxysilane or trialkoxysilane), and more preferably all of R 1 to R 3 are alkoxy groups having 1 to 20 carbon atoms.
  • the two or three alkoxy groups may all be the same or different. are all the same because it is easier to
  • n represents an integer of 0 to 20 and is easily available, so it is preferably an integer of 1 to 10, more preferably an integer of 1 to 5, 2 to 4 is more preferably an integer of
  • R 4 is any selected from the group consisting of a glycidoxy group represented by the following formula (2), an unsubstituted or substituted amino group, and a mercapto group (—SH).
  • a group preferably a glycidoxy group, or an amino group that is unsubstituted or has only one substituent, and from the viewpoint of achieving both long-term rust prevention and blending stability of the aqueous resin composition, it is a glycidoxy group. is more preferred.
  • R 4 is an amino group, it is preferably an unsubstituted amino group (--NH 2 ).
  • R 4 is an amino group having only one substituent, the substituent includes an alkyl group having 1 to 3 carbon atoms.
  • silane coupling agent ( ⁇ ) is an epoxysilane having an epoxy group, specifically, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyl Methyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexy)ethyltrimethoxysilane and the like can be used.
  • silane coupling agent ( ⁇ ) is an aminosilane having an amino group, specifically, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3- Aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, and the like can be used.
  • silane coupling agent ( ⁇ ) is a mercaptosilane having a mercapto group
  • 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, etc. can be used.
  • the content of the silane coupling agent ( ⁇ ) is 0.03 parts by mass or more with respect to a total of 100 parts by mass of the copolymer (X) and the polyepoxy compound (Y) in the aqueous resin emulsion ( ⁇ ). , preferably 0.12 parts by mass or more, more preferably 0.25 parts by mass or more. This is because the cured water-based resin composition has improved rust resistance and adhesion to metal materials.
  • the content of the silane coupling agent ( ⁇ ) is 25 parts by mass or less with respect to a total of 100 parts by mass of the copolymer (X) and the polyepoxy compound (Y) in the aqueous resin emulsion ( ⁇ ).
  • .5 parts by mass or less more preferably 6.5 parts by mass or less, even more preferably 2.5 parts by mass or less, particularly preferably 2.0 parts by mass or less, Most preferably, it is 1.8 parts by mass or less. This is because deterioration of long-term rust resistance can be suppressed. Further, when the content of the silane coupling agent ( ⁇ ) is 2.0 parts by mass or less, the blending stability of the aqueous resin composition is improved.
  • the aqueous resin composition of this embodiment contains an aqueous resin emulsion ( ⁇ ), a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ). Therefore, the coating film made of the cured product of the water-based resin composition of the present embodiment exhibits antirust properties for a long period of time. Due to the synergistic effect of the following (1) and (2), the adhesion between the coating film and the surface to be coated made of a metal material or the like is improved, and the diffusion of moisture in the surface direction of the coating film is suppressed.
  • the alkoxysilyl group (G) of the silane coupling agent ( ⁇ ) contained in the aqueous resin composition reacts with the aqueous medium (Z) and hydrolyzes to form a silanol group.
  • the hydroxyl groups possessed by the generated silanol groups bond with each other through a dehydration condensation reaction, and partially bond with the surface to be coated, which is made of a metal material or the like, by interaction.
  • the hydroxyl group of the silanol group derived from the silane coupling agent ( ⁇ ) is the epoxy compound (Y) and the curing agent in the water-based resin emulsion ( ⁇ ). It also chemically bonds with the polyamine (F) in ( ⁇ ).
  • the silanol group does not chemically bond with the structural unit derived from the (meth)acrylic acid ester (A) contained in the copolymer (X) in the aqueous resin emulsion ( ⁇ ). Therefore, the epoxy compound (Y) and the polyamine (F) in the water-based resin composition are oriented in the vicinity of the surface to be coated due to the silanol groups bonded through interaction with the surface to be coated.
  • the concentration distribution of the epoxy compound (Y) and the polyamine (F) in the aqueous resin composition becomes uneven, and the ratio of the epoxy compound (Y) and the polyamine (F) interacting with the surface to be coated increases. , the epoxy compound (Y) and the polyamine (F) interact with the surface to be coated.
  • the aqueous resin composition according to this embodiment may contain a pigment.
  • pigments include titanium oxide, talc, barium sulfate, carbon black, red iron oxide, calcium carbonate, silicon oxide, talc, mica, kaolin, clay, ferrite, and silica sand.
  • a pigment only one type of compound may be included, or two or more types of compounds may be included.
  • the pigment content in the aqueous resin composition is preferably 0.1 to 50% by mass, more preferably 1 to 40% by mass. This is because the concealability of the coating film is improved.
  • the aqueous resin composition includes fillers, organic or inorganic hollow balloons, dispersing agents (e.g., amino alcohols, polycarboxylates, etc.), surfactants, coupling agents (excluding silane coupling agents ( ⁇ )), desorption Foaming agents, preservatives (such as biocides, fungicides, fungicides, algaecides, and combinations thereof), flow agents, leveling agents, neutralizing agents (such as hydroxides, amines, ammonia , carbonates, etc.).
  • the aqueous resin composition according to the present embodiment may or may not contain an organic solvent such as a hydrophilic solvent. Although organic solvents other than hydrophilic solvents may be included, it is preferable not to include them.
  • the aqueous resin composition of the present embodiment comprises an aqueous resin emulsion ( ⁇ ), a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), a silane coupling agent ( ⁇ ), and other components that are optionally contained. It can be manufactured by a method of mixing ingredients. As a method for mixing each component contained in the aqueous resin composition of the present embodiment, a known method can be used.
  • the aqueous resin composition of this embodiment contains an aqueous resin emulsion ( ⁇ ), a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ). Therefore, it is possible to form a coating film that exhibits antirust properties for a long period of time.
  • the coating film of the present embodiment is composed of a cured product of the aqueous resin composition of the present embodiment.
  • the coating film of the present embodiment may be one layer of a coating film having a multilayer structure. That is, the coating film of the present embodiment is, if necessary, the undercoat layer provided as a lower layer of the coating film made of the cured product of the aqueous resin composition of the present invention, and / or the topcoat layer provided as an upper layer. It may be provided by being laminated with a coating film.
  • the coating film of the present embodiment is one layer of a coating film having a multilayer structure, it is preferably the layer of the coating film having a multilayer structure that is in contact with the surface to be coated.
  • a method for producing a coating film composed of a cured product of the aqueous resin composition of the present embodiment will be described in detail.
  • a water-based resin emulsion ( ⁇ ), a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ) are contained as necessary. Mix with other ingredients to be used.
  • the aqueous resin composition of the present embodiment is prepared (mixing step).
  • the aqueous resin composition obtained in the mixing step is applied to the surface to be coated (application step).
  • the aqueous resin emulsion ( ⁇ ), the curing agent ( ⁇ ), the curing accelerator ( ⁇ ), the silane coupling agent ( ⁇ ), and optionally other components are mixed by a known method. Mix and stir. As a result, an aqueous resin composition in which each component is dispersed is obtained. Stirring in the mixing process can be performed, for example, by Robomics (manufactured by Primix Co., Ltd.).
  • the stirring time in the mixing step is preferably 5 minutes or longer.
  • the stirring time is preferably within 1 hour.
  • the aqueous resin composition is applied to the surface of the article to be coated.
  • materials forming the surface to be coated include metallic materials such as iron.
  • the surface to be coated may be previously subjected to a surface treatment such as a primer or an undercoat.
  • a known method can be used as a method of applying the aqueous resin composition.
  • the coating method include, but are not limited to, a method using a brush, a roller, or the like.
  • the coating process is preferably completed within 1 hour after the mixing process is completed, and the coating process is completed within 30 minutes. It is more preferable to complete within
  • the method for producing a coating film of the present embodiment it is preferable to perform a curing step of curing the coating film obtained by coating the surface to be coated after the coating step.
  • the surface of the object coated with the aqueous resin composition is dried and cured to cure the resin component contained in the aqueous resin composition.
  • Curing time varies depending on the temperature of the curing atmosphere. For example, at room temperature (20° C.), the time is preferably 5 hours or more, at 40° C. it is preferably 1 hour or more, and at 60° C. it is preferably 5 minutes or more.
  • the coating film of the present embodiment is composed of a cured product of the aqueous resin composition of the present embodiment. For this reason, the coating film of the present embodiment exhibits antirust properties for a long period of time. Further, in the method for producing a coating film of the present embodiment, the aqueous resin emulsion ( ⁇ ), the curing agent ( ⁇ ), the curing accelerator ( ⁇ ), and the silane coupling agent ( ⁇ ) are mixed to form an aqueous A resin composition is prepared and applied to the surface to be coated. Therefore, the coating film of this embodiment can be formed from the cured product of the aqueous resin composition of this embodiment.
  • the coating film of the present embodiment exhibits antirust properties for a long period of time, it is particularly suitable as a coating film formed on the surfaces of metal products used outdoors such as steel towers, bridges, ships, and harbor facilities. More specifically, metal products used outdoors are expected to be used in severe corrosive environments. In general, a coating film having a multilayer structure is formed on the surface of metal products used outdoors. A coating film with a multi-layer structure exhibits excellent rust resistance, but it is difficult to repaint frequently because it takes time and effort to repaint.
  • the coating film of this embodiment When the coating film of this embodiment is formed on the surface of a metal product used outdoors, the anti-rust property of the coating film is exhibited for a long time, so even if it is used in a severe corrosive environment, the frequency of repainting is reduced. can be lowered.
  • the metal protection method of the present embodiment is a method of protecting the metal with a coating film provided on the surface, and a cured product of the water-based resin composition of the present embodiment is used as the coating film.
  • the coating film made of the cured product of the water-based resin composition of the present embodiment exhibits antirust properties for a long period of time. Therefore, it is suitable as a method for protecting metals, more specifically as a method for protecting metal surfaces.
  • the aqueous resin composition of the present embodiment may be stored as an aqueous resin composition set in which constituent components of the aqueous resin composition are divided into a plurality of solutions.
  • the constituent components of the aqueous resin composition of the present embodiment may be divided into two liquids, the first liquid and the second liquid, and stored.
  • first set first form
  • second set second form
  • the first liquid contains an aqueous resin emulsion ( ⁇ ) and a silane coupling agent ( ⁇ ), and the second liquid contains a curing agent ( ⁇ ) and a curing accelerator ( ⁇ ). .
  • the first set is excellent in storage stability because the aqueous resin emulsion ( ⁇ ) and the curing agent ( ⁇ ) do not react and harden during storage.
  • the silane coupling agent ( ⁇ ) it is preferable to use an epoxysilane having an epoxy group, preferably not including an aminosilane having an amino group and/or a mercaptosilane having a mercapto group. This is because the aqueous resin emulsion ( ⁇ ) and the silane coupling agent ( ⁇ ) do not react and harden during storage, and the storage stability of the first liquid in the first set is improved.
  • the first liquid contains an aqueous resin emulsion ( ⁇ ), and the second liquid contains a curing agent ( ⁇ ), a curing accelerator ( ⁇ ), and a silane coupling agent ( ⁇ ).
  • the second set is excellent in storage stability because the water-based resin emulsion ( ⁇ ) does not react with the curing agent ( ⁇ ) and/or the silane coupling agent ( ⁇ ) during storage to cure.
  • the coating film of this embodiment may be produced using the aqueous resin composition set of this embodiment. That is, the aqueous resin composition of the present embodiment is prepared by mixing the first liquid and the second liquid in the aqueous resin composition set of the present embodiment (mixing step). Thereafter, the water-based resin composition is applied to the surface to be coated in the same manner as in the method for producing a coating film described above (coating step).
  • the aqueous resin composition set of the present embodiment it is possible to form a coating film exhibiting antirust properties for a long period of time, as in the case of using the aqueous resin composition of the present embodiment.
  • the dispersion liquid of the present embodiment is used for preparing the aqueous resin composition of the present embodiment described above.
  • the dispersion liquid of the present embodiment contains the aqueous resin emulsion ( ⁇ ) contained in the aqueous resin composition of the present embodiment described above. That is, the dispersion liquid of the present embodiment is a part of raw materials of the aqueous resin composition of the present embodiment and the aqueous resin composition set of the present embodiment, and the aqueous resin composition and the aqueous resin composition set of the present embodiment. can be used as an aqueous resin emulsion ( ⁇ ) when producing
  • the aqueous resin composition of the present invention is useful in various fields.
  • the water-based resin composition of the present invention is particularly suitable for use as an anticorrosive paint to be applied to the surfaces of metal products used outdoors such as steel towers, bridges, ships, port facilities and the like.
  • An article on which a coating film comprising a cured product of the aqueous resin composition of the present invention is formed, that is, an object to be coated with the aqueous resin composition of the present invention can be selected arbitrarily.
  • Specific examples of applicable objects include steel towers, bridges, ships, metal products used outdoors such as port facilities, various household goods, home appliances such as refrigerators, and installations in amusement parks and parks. playground equipment, sporting goods, buildings (interior, exterior, etc.), various industrial goods and their parts including transportation machinery and machine tools, automobile bodies and chassis, railway vehicle bodies and underfloor equipment, marine containers, aircraft, etc. mentioned.
  • aqueous resin emulsion ( ⁇ )> (Aqueous resin emulsion ( ⁇ -1))
  • a separable flask equipped with a condenser, a thermometer, a stirrer and a dropping funnel was charged with 158 parts by mass of ion-exchanged water and heated to 60°C. Nitrogen gas was blown into the contents of the separable flask to deoxygenate the contents.
  • An emulsion comprising the amounts (parts by mass) shown in Table 1 of methyl methacrylate, 2-ethylhexyl acrylate, methacrylic acid, hydrogenated bisphenol A type epoxy, sodium dodecylbenzenesulfonate as an emulsifier, and 356 parts by mass of deionized water. was added dropwise over 3 hours.
  • 1.2 parts by mass of potassium persulfate as an oxidizing agent dissolved in 41 parts by mass of ion-exchanged water and 0.4 parts by mass of sodium bisulfite as a reducing agent were dissolved in 21 parts by mass of ion-exchanged water. was added dropwise at 60° C.
  • Table 1 shows the amount (parts by mass) of each material used in the synthesis of the aqueous resin emulsion ( ⁇ -1).
  • the numerical value of "ion-exchanged water” shown in Table 1 indicates the content of ion-exchanged water contained in the synthesized aqueous resin emulsion ( ⁇ -1).
  • the values in parentheses for the contents of the copolymer (X) and the polyepoxy compound (Y) are the total amount (100%) of the copolymer (X) and the polyepoxy compound (Y). Shows the ratio (mass%) of each material to
  • Aqueous resin emulsion ( ⁇ -2) to ( ⁇ -4) ( ⁇ '-5)) Aqueous resin emulsions ( ⁇ -2) to ( ⁇ -4) were prepared in the same manner as the aqueous resin emulsion ( ⁇ -1) except that each material shown in Table 1 was used in the amount (parts by mass) shown in Table 1. ) ( ⁇ ′-5) was synthesized.
  • the numerical value of "ion-exchanged water" shown in Table 1 is the same as the synthesized aqueous resin emulsion ( ⁇ -1).
  • the content of ion-exchanged water contained in the synthesized aqueous resin emulsions ( ⁇ -2) to ( ⁇ -4) and ( ⁇ '-5) is shown.
  • aqueous resin emulsion ( ⁇ ) > The following items were evaluated for the aqueous resin emulsions ( ⁇ -1) to ( ⁇ -4) and ( ⁇ '-5). Table 2 shows the results.
  • the water-based resin emulsion ( ⁇ '-5) having an excessive content of the polyepoxy compound (Y) was not evaluated because it aggregated during synthesis.
  • the aqueous resin emulsions ( ⁇ -1) to ( ⁇ -4) ( ⁇ '-5) are collectively referred to, they may be referred to as the aqueous resin emulsion ( ⁇ ).
  • the residual ratio of epoxy groups in the water-based resin emulsion ( ⁇ ) is the amount N 1 [mol/g] of the epoxy groups contained in the water-based resin emulsion ( ⁇ ) after synthesis. It is the ratio to the total amount N 2 [mol/g] of epoxy groups contained in components (including raw materials, initiators, solvents, other additives, etc.).
  • the amount N 1 [mol/g] of epoxy groups in the aqueous resin emulsion ( ⁇ ) after synthesis was measured by the following method. An excess amount of hydrogen chloride was added to the total amount of epoxy groups contained in the components (raw materials) used in the synthesis of the aqueous resin emulsion ( ⁇ ) to react with the epoxy groups. Next, the amount of remaining hydrogen chloride was confirmed by titrating unreacted hydrogen chloride with potassium hydroxide. At this time, potassium hydroxide is consumed by reaction with acidic components such as carboxylic acid contained in the aqueous resin emulsion ( ⁇ ). Therefore, the amount of acidic components was titrated in advance by blank measurement without using hydrogen chloride, and the result of this measurement was corrected. Specific measurement procedures are as follows (i) to (ii).
  • the amount of the potassium hydroxide/ethanol solution used for titration is defined as V KOH1 [mL].
  • the solution was titrated with a 0.1 M potassium hydroxide/ethanol solution while stirring. After the potassium hydroxide/ethanol solution was added dropwise, the point at which the purple color persisted for 30 seconds was taken as the equivalence point.
  • the amount of potassium hydroxide/ethanol solution used for titration is defined as V KOH2 [mL].
  • N 1 (0.2 ⁇ V HCl /1000 ⁇ 0.1 ⁇ V KOH2 /1000)/W 2 +(0.1 ⁇ V KOH1 /1000)/W 1 (40)
  • the components used for the synthesis of the aqueous resin emulsion ( ⁇ ) mean all the components listed in Table 1 as raw materials for the aqueous resin emulsion ( ⁇ ).
  • N 2 ⁇ (m i /EP i )/ ⁇ m i (50)
  • 1/EP i 0 for compounds that do not contain an epoxy group, such as methyl methacrylate and ion-exchanged water. From the amount of epoxy groups determined in this way, the residual rate of epoxy groups in the aqueous resin emulsion ( ⁇ ) is expressed as 100 ⁇ N 1 /N 2 [mol %].
  • Epoxy Group Content in Non-Volatile Content, Epoxy Group Content in Components (X) + (Y)> From the non-volatile content concentration CS [mass%] and the epoxy group content N 1 in the aqueous resin emulsion ( ⁇ ) obtained by the above method, the epoxy group content R in the non-volatile content of the aqueous resin emulsion ( ⁇ ) EP [mol/g] was determined based on equation (20) explained above. R EP [mol/g] N 1 /(C S /100) (20)
  • the epoxy group content N 1 in the aqueous resin emulsion ( ⁇ ) determined by the above method, the total amount N 2 of epoxy groups in the raw material, and the components (raw materials) used in the synthesis of the aqueous resin emulsion ( ⁇ ) The total amount of carboxy groups N 3 , the total mass ⁇ [g] of all components (raw materials) used in the synthesis of the aqueous resin emulsion ( ⁇ ), the mass X [g] of the raw materials used in the copolymer (X), Using the mass Y [g] of the raw material used for the polyepoxy compound (Y), the carboxy group content R CX [mol/g] in the component (X) + (Y) is calculated based on the following formula. bottom.
  • R CX in (X)+(Y) ⁇ N 3 ⁇ (N 2 ⁇ N 1 ) ⁇ / ⁇ (X+Y)/ ⁇
  • the high-temperature stability of the aqueous resin emulsion ( ⁇ ) was evaluated as follows. First, the water-based resin emulsion ( ⁇ ) was put into a 70 ml glass bottle, which was then sealed and allowed to stand at 60° C. for 7 days. After that, the state of the aqueous resin emulsion ( ⁇ ) in the glass bottle was visually observed and evaluated according to the following criteria. ⁇ (Possible): Aggregation, thickening, precipitation, separation, and gelation were not observed. ⁇ (improper): At least one of aggregation, thickening, precipitation, separation, and gelation was observed.
  • Examples 1 to 17 and Comparative Examples 1 to 4 (Preparation of aqueous resin composition)> 100 parts by mass of the aqueous resin emulsion ( ⁇ ) shown in Tables 3 to 5 (nonvolatile content of 40% by mass), 60 parts by mass of ion-exchanged water, and the curing agent ( ⁇ ) shown in Tables 3 to 5 A curing accelerator ( ⁇ ) and a silane coupling agent ( ⁇ ) were added in the amounts (parts by mass) shown in Tables 3 to 5 and stirred for 10 minutes, Examples 1 to 17 and Comparative Examples 1 to 4. was prepared.
  • the "active hydrogen equivalent to epoxy group" in each curing agent ( ⁇ ) is the active hydrogen contained in the curing agent ( ⁇ ) with respect to 1 equivalent of the epoxy group contained in the aqueous resin emulsion ( ⁇ ). It is a numerical value indicating the equivalent of active hydrogen contained in the polyamine (F) having The "number of moles per epoxy group” in the curing accelerator ( ⁇ ) is a numerical value indicating the number of moles of the curing accelerator ( ⁇ ) per equivalent of epoxy groups contained in the aqueous resin emulsion ( ⁇ ).
  • EH-8051 (trade name; ADEKA HARDNER EH-8051, manufactured by ADEKA Corporation) was used.
  • the equivalent weight of active hydrogen reactive to epoxy groups contained in ADEKA HARDNER EH-8051 is 180 g/mol.
  • the content of the silane coupling agent ( ⁇ ) shown in Tables 3 to 5 is based on a total of 100 parts by mass of the copolymer (X) of the aqueous resin emulsion ( ⁇ ) and the polyepoxy compound (Y). amount (parts by mass).
  • the water-based resin composition was applied to a cold-rolled steel plate (thickness: 800 ⁇ m) (hereinafter referred to as “substrate”) with a brush so as to have a basis weight of 50 g/m 2 . After drying the coated base material in a constant temperature bath at 60° C. for 10 minutes, it was cured at 23° C. for 1 day to form a coating film on the surface of the base material. As a result, a rectangular test piece having a coating film on the surface and measuring 70 mm long and 150 mm wide was formed. The test area was a rectangular area of 45 mm long and 125 mm wide in the coating film of the test piece.
  • the thickness of the coating film on the specimen was about 100 ⁇ m.
  • An incision consisting of two intersecting straight lines (ie, X-shaped) was cut into the coating to form the diagonal of the rectangle forming the test area. Using a cutter knife, the incision was formed so as to extend from the coating film to the substrate.
  • a neutral salt spray test (Section 4.2.1) was performed on the test piece with the notches in accordance with JIS Z-2371 (2000).
  • the area occupied by the blister of the coating film in the test area [area %] and the size of the blister [mm ] was measured to evaluate the rust prevention property. That is, the appearance of the test piece was visually observed and evaluated by finger touch, and the presence or absence of an area in which the surface of the coating film was swollen due to storage was examined. As a result, the planar shape of each bulging region was substantially circular. For this reason, the planar shape of each bulging region was assumed to be a perfect circle, and the maximum straight distance connecting the contour lines of the bulging region was measured with a ruler, and the result was taken as the diameter.
  • the total area of the swollen area in the test area is calculated, and the ratio of the swollen area [%] to the area of the test area (% of the test area The area occupied by swelling of the coating film) was determined.
  • the maximum diameter in each test piece was defined as the size of the swelling.
  • test piece was formed in the same manner as for rust prevention.
  • the test area was a rectangular area of 45 mm long and 125 mm wide in the coating film of the test piece.
  • the thickness of the coating film on the specimen was about 100 ⁇ m.
  • the test pieces thus prepared were stored in a constant temperature bath at a temperature of 40° C. and a relative humidity (RH) of 98% for 3 days. After that, according to JIS K-5400 (1990) "Section 8.5.2 Cross-cut tape method", cut a cross-cut at intervals of 1 mm with a cutter so as to penetrate the coating film formed in the test area of the test piece.
  • the state in which the fluidity is lost is a state in which the aqueous resin composition is partially or wholly gelled (solidified) by visual observation. Alternatively, it means that although gelation is not observed, spray coating cannot be performed due to the increase in viscosity.
  • the state in which spray painting is not possible means that a gravity spray gun (manufactured by Anest Iwata Co., Ltd., trade name: WIDER1-10E1G, nozzle diameter: 1.0 mm diameter) is connected to a compressor, and the spraying air pressure is 0.3 MPa, and the amount of air used is 75 L/ It means that the water-based resin composition is not atomized when air-sprayed on the condition of min.
  • an aqueous resin composition and an aqueous resin composition set capable of forming a coating film exhibiting antirust properties for a long period of time.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Wood Science & Technology (AREA)
  • Medicinal Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Materials Engineering (AREA)
  • Polymers & Plastics (AREA)
  • Dispersion Chemistry (AREA)
  • Epoxy Resins (AREA)
  • Paints Or Removers (AREA)
PCT/JP2022/039715 2021-12-20 2022-10-25 水性樹脂組成物、塗膜の製造方法、水性樹脂組成物セット Ceased WO2023119850A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2023569113A JPWO2023119850A1 (cg-RX-API-DMAC7.html) 2021-12-20 2022-10-25

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021-206028 2021-12-20
JP2021206028 2021-12-20

Publications (1)

Publication Number Publication Date
WO2023119850A1 true WO2023119850A1 (ja) 2023-06-29

Family

ID=86902029

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/039715 Ceased WO2023119850A1 (ja) 2021-12-20 2022-10-25 水性樹脂組成物、塗膜の製造方法、水性樹脂組成物セット

Country Status (2)

Country Link
JP (1) JPWO2023119850A1 (cg-RX-API-DMAC7.html)
WO (1) WO2023119850A1 (cg-RX-API-DMAC7.html)

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2025192096A1 (ja) * 2024-03-15 2025-09-18 コニカミノルタ株式会社 二液型インクセット、硬化物の形成方法、及び製品
JP7864237B1 (ja) * 2025-09-30 2026-05-22 大日本塗料株式会社 塗料組成物及び複層膜形成方法

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH03182519A (ja) * 1989-12-13 1991-08-08 Kansai Paint Co Ltd 樹脂組成物およびそれを用いてなる缶内面用水性塗料
JPH1025308A (ja) * 1996-07-11 1998-01-27 Kansai Paint Co Ltd 重合体エマルション組成物
JP2002194035A (ja) * 2000-12-26 2002-07-10 Nippon Nsc Ltd エポキシ樹脂水分散体の製造方法及びそれを用いて製造されるエポキシ樹脂水分散体
CN1814663A (zh) * 2005-02-05 2006-08-09 广州慧谷化学有限公司 一种热固性丙烯酸乳液及其制备方法以及含有该乳液的涂料
CN108912281A (zh) * 2018-07-20 2018-11-30 滁州学院 水性环氧树脂、水性op保护剂及其制备方法
CN112724789A (zh) * 2021-01-14 2021-04-30 邓昭霞 一种室外用抗紫外线耐磨环氧地坪涂料及其制备方法

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH03182519A (ja) * 1989-12-13 1991-08-08 Kansai Paint Co Ltd 樹脂組成物およびそれを用いてなる缶内面用水性塗料
JPH1025308A (ja) * 1996-07-11 1998-01-27 Kansai Paint Co Ltd 重合体エマルション組成物
JP2002194035A (ja) * 2000-12-26 2002-07-10 Nippon Nsc Ltd エポキシ樹脂水分散体の製造方法及びそれを用いて製造されるエポキシ樹脂水分散体
CN1814663A (zh) * 2005-02-05 2006-08-09 广州慧谷化学有限公司 一种热固性丙烯酸乳液及其制备方法以及含有该乳液的涂料
CN108912281A (zh) * 2018-07-20 2018-11-30 滁州学院 水性环氧树脂、水性op保护剂及其制备方法
CN112724789A (zh) * 2021-01-14 2021-04-30 邓昭霞 一种室外用抗紫外线耐磨环氧地坪涂料及其制备方法

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2025192096A1 (ja) * 2024-03-15 2025-09-18 コニカミノルタ株式会社 二液型インクセット、硬化物の形成方法、及び製品
JP7864237B1 (ja) * 2025-09-30 2026-05-22 大日本塗料株式会社 塗料組成物及び複層膜形成方法

Also Published As

Publication number Publication date
JPWO2023119850A1 (cg-RX-API-DMAC7.html) 2023-06-29

Similar Documents

Publication Publication Date Title
JP6937942B2 (ja) 水性樹脂エマルジョン及びその製造方法、並びに水性樹脂組成物
EP2495281B2 (en) Epoxy resin imbibed polymer particles
JP7380709B2 (ja) 水性樹脂組成物、皮膜および皮膜の形成方法
EP2966135B1 (en) Anticorrosive coating composition, anticorrosive coating film, and method for preventing corrosion of base material
EP2966134B1 (en) Anti-corrosion paint composition, anti-corrosion coating, and method for preventing corrosion of base material
CN104271691B (zh) 用于具有改善的再涂性的船舶维护与维修涂料的环氧树脂组合物
US20120301621A1 (en) Epoxy Resin Imbibed Polymer Particles
CN104411765B (zh) 用于具有改善的再涂性的船舶维护与维修涂料的环氧树脂组合物
WO2022255272A1 (ja) 水性樹脂組成物、塗膜、塗膜の製造方法、水性樹脂組成物セット
JP2021042363A (ja) 水性被覆材
WO2022145227A1 (ja) 水性樹脂組成物、皮膜、塗膜の製造方法、水性樹脂組成物セット、および金属の保護方法
WO2024143375A1 (ja) 水性エマルジョン、水性エマルジョンの製造方法、水性樹脂組成物、水性樹脂組成物セット、及び塗膜の製造方法
JP2024092400A (ja) 水性エマルジョン、水性樹脂組成物、及び塗膜の製造方法
WO2022145228A1 (ja) 水性樹脂組成物、皮膜、塗膜の製造方法、水性樹脂組成物セット、および金属の保護方法
JP2021055062A (ja) 水性被覆材
CN120424307A (zh) 水性环氧反应性固化剂以及由其形成的双组分水性环氧涂料组合物和制品

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22910571

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2023569113

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 22910571

Country of ref document: EP

Kind code of ref document: A1