WO2022158222A1 - プリプレグ、成形体および一体化成形体 - Google Patents
プリプレグ、成形体および一体化成形体 Download PDFInfo
- Publication number
- WO2022158222A1 WO2022158222A1 PCT/JP2021/047257 JP2021047257W WO2022158222A1 WO 2022158222 A1 WO2022158222 A1 WO 2022158222A1 JP 2021047257 W JP2021047257 W JP 2021047257W WO 2022158222 A1 WO2022158222 A1 WO 2022158222A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- prepreg
- resin
- thermoplastic resin
- thermosetting resin
- mold
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29B—PREPARATION OR PRETREATMENT OF THE MATERIAL TO BE SHAPED; MAKING GRANULES OR PREFORMS; RECOVERY OF PLASTICS OR OTHER CONSTITUENTS OF WASTE MATERIAL CONTAINING PLASTICS
- B29B11/00—Making preforms
- B29B11/14—Making preforms characterised by structure or composition
- B29B11/16—Making preforms characterised by structure or composition comprising fillers or reinforcement
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/06—Layered products comprising a layer of synthetic resin as the main or only constituent of a layer, which is next to another layer of the same or of a different material
- B32B27/08—Layered products comprising a layer of synthetic resin as the main or only constituent of a layer, which is next to another layer of the same or of a different material of synthetic resin
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/18—Layered products comprising a layer of synthetic resin characterised by the use of special additives
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B5/00—Layered products characterised by the non- homogeneity or physical structure, i.e. comprising a fibrous, filamentary, particulate or foam layer; Layered products characterised by having a layer differing constitutionally or physically in different parts
- B32B5/02—Layered products characterised by the non- homogeneity or physical structure, i.e. comprising a fibrous, filamentary, particulate or foam layer; Layered products characterised by having a layer differing constitutionally or physically in different parts characterised by structural features of a fibrous or filamentary layer
- B32B5/10—Layered products characterised by the non- homogeneity or physical structure, i.e. comprising a fibrous, filamentary, particulate or foam layer; Layered products characterised by having a layer differing constitutionally or physically in different parts characterised by structural features of a fibrous or filamentary layer characterised by a fibrous or filamentary layer reinforced with filaments
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
- C08J5/04—Reinforcing macromolecular compounds with loose or coherent fibrous material
- C08J5/0405—Reinforcing macromolecular compounds with loose or coherent fibrous material with inorganic fibres
- C08J5/042—Reinforcing macromolecular compounds with loose or coherent fibrous material with inorganic fibres with carbon fibres
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
- C08J5/24—Impregnating materials with prepolymers which can be polymerised in situ, e.g. manufacture of prepregs
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
- C08J5/24—Impregnating materials with prepolymers which can be polymerised in situ, e.g. manufacture of prepregs
- C08J5/241—Impregnating materials with prepolymers which can be polymerised in situ, e.g. manufacture of prepregs using inorganic fibres
- C08J5/243—Impregnating materials with prepolymers which can be polymerised in situ, e.g. manufacture of prepregs using inorganic fibres using carbon fibres
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L101/00—Compositions of unspecified macromolecular compounds
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29K—INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR MOULDS, REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29K2101/00—Use of unspecified macromolecular compounds as moulding material
- B29K2101/10—Thermosetting resins
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29K—INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR MOULDS, REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29K2101/00—Use of unspecified macromolecular compounds as moulding material
- B29K2101/12—Thermoplastic materials
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29K—INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR MOULDS, REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29K2105/00—Condition, form or state of moulded material or of the material to be shaped
- B29K2105/06—Condition, form or state of moulded material or of the material to be shaped containing reinforcements, fillers or inserts
- B29K2105/08—Condition, form or state of moulded material or of the material to be shaped containing reinforcements, fillers or inserts of continuous length, e.g. cords, rovings, mats, fabrics, strands or yarns
- B29K2105/0872—Prepregs
- B29K2105/0881—Prepregs unidirectional
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B2262/00—Composition or structural features of fibres which form a fibrous or filamentary layer or are present as additives
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B2307/00—Properties of the layers or laminate
- B32B2307/50—Properties of the layers or laminate having particular mechanical properties
- B32B2307/54—Yield strength; Tensile strength
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B2307/00—Properties of the layers or laminate
- B32B2307/50—Properties of the layers or laminate having particular mechanical properties
- B32B2307/542—Shear strength
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B2307/00—Properties of the layers or laminate
- B32B2307/70—Other properties
- B32B2307/732—Dimensional properties
- B32B2307/737—Dimensions, e.g. volume or area
- B32B2307/7375—Linear, e.g. length, distance or width
- B32B2307/7376—Thickness
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2300/00—Characterised by the use of unspecified polymers
- C08J2300/22—Thermoplastic resins
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2300/00—Characterised by the use of unspecified polymers
- C08J2300/24—Thermosetting resins
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2323/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
- C08J2323/26—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers modified by chemical after-treatment
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2363/00—Characterised by the use of epoxy resins; Derivatives of epoxy resins
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2363/00—Characterised by the use of epoxy resins; Derivatives of epoxy resins
- C08J2363/02—Polyglycidyl ethers of bis-phenols
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2365/00—Characterised by the use of macromolecular compounds obtained by reactions forming a carbon-to-carbon link in the main chain; Derivatives of such polymers
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2371/00—Characterised by the use of polyethers obtained by reactions forming an ether link in the main chain; Derivatives of such polymers
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2377/00—Characterised by the use of polyamides obtained by reactions forming a carboxylic amide link in the main chain; Derivatives of such polymers
- C08J2377/02—Polyamides derived from omega-amino carboxylic acids or from lactams thereof
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2423/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
- C08J2423/26—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers modified by chemical after-treatment
- C08J2423/30—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers modified by chemical after-treatment by oxidation
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2471/00—Characterised by the use of polyethers obtained by reactions forming an ether link in the main chain; Derivatives of such polymers
- C08J2471/08—Polyethers derived from hydroxy compounds or from their metallic derivatives
- C08J2471/10—Polyethers derived from hydroxy compounds or from their metallic derivatives from phenols
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2477/00—Characterised by the use of polyamides obtained by reactions forming a carboxylic amide link in the main chain; Derivatives of such polymers
- C08J2477/02—Polyamides derived from omega-amino carboxylic acids or from lactams thereof
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2481/00—Characterised by the use of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing sulfur with or without nitrogen, oxygen, or carbon only; Polysulfones; Derivatives of such polymers
- C08J2481/06—Polysulfones; Polyethersulfones
Definitions
- the present invention relates to a prepreg in which a reinforcing fiber is impregnated with a thermosetting resin and a thermoplastic resin is present on at least a part of its surface.
- Fiber-reinforced composite materials which use a thermosetting resin as a matrix and are combined with reinforcing fibers such as carbon fiber and glass fiber, are lightweight and have excellent mechanical properties such as strength and rigidity, as well as heat resistance and corrosion resistance. • Has been applied in many fields such as space, automobiles, railroad vehicles, ships, civil engineering and sports equipment. However, these fiber-reinforced composite materials are not suitable for manufacturing parts or structures having complex shapes in a single molding process. Therefore, in the above applications, it is often necessary to fabricate a member made of a fiber-reinforced composite material and then integrate it with members of the same or different type.
- Mechanical joining methods such as bolts, rivets, screws, etc., and joining methods using adhesives are used as methods for integrating fiber-reinforced composite materials made of reinforcing fibers and thermosetting resins with members of the same or different types.
- the mechanical joining method requires a process to process the joining part such as drilling in advance, which leads to a longer manufacturing process, an increase in manufacturing cost, and a decrease in material strength due to the drilling of holes.
- Bonding methods that use adhesive require a bonding process that includes preparation and application of the adhesive, as well as a curing process. There was a problem of not being satisfied.
- Patent Document 1 discloses a method of bonding a fiber-reinforced composite material composed of reinforcing fibers and a thermosetting resin via an adhesive.
- Patent Document 2 discloses a method of providing a thermoplastic resin on the surface of a fiber-reinforced composite material composed of reinforcing fibers and a thermosetting resin, and integrating members formed of the thermoplastic resin by injection molding.
- the method of bonding members together with an adhesive requires time for the adhesive to harden, and in some cases, the bonding strength depends on the strength of the adhesive itself. .
- Patent Document 2 discloses a fiber-reinforced composite material in which a thermoplastic resin film is laminated on the surface of a prepreg made of reinforcing fibers and a thermosetting resin, and then the prepreg and the thermoplastic resin layer are integrated by heating and pressure curing. discloses a method of integrally molding a member containing a thermoplastic resin onto a thermoplastic resin layer on the surface thereof by injection molding.
- the fiber-reinforced composite material obtained by this method is rigid because the thermosetting resin is hardened, and it is difficult to shape using a mold having a complicated surface shape.
- the hardened thermosetting resin loses its surface adhesiveness, it cannot be accurately fixed to the desired location in the mold. . For this reason, the technology described in Patent Document 2 is considered to be limited to application within a mold having a simple planar shape.
- An object of the present invention is to provide a prepreg having a thermoplastic resin on its surface, which has moderate flexibility and adhesiveness, excellent formability to a complicated mold surface and excellent adhesion to the mold surface. That is.
- a further object of the present invention is to use the prepreg to produce a high-quality fiber-reinforced composite material molded article, especially a molded article having a complicated shape without difficulty.
- thermosetting resin has a peak in the temperature range of more than 100° C. and 180° C. or less in the loss tangent tan ⁇ curve obtained by isokinetic heating measurement by dynamic viscoelasticity measurement (DMA method).
- the prepreg has a point showing a maximum value in a loss angle ⁇ curve obtained by isothermal measurement by dynamic viscoelasticity measurement (DMA method), and There is a point at which the loss angle ⁇ is 5° or more smaller than the maximum value on the short-time side of the point showing the maximum value.
- the prepreg has a loss angle ⁇ curve obtained by isothermal measurement by dynamic viscoelasticity measurement (DMA method), even if the loss angle ⁇ curve has a maximum value There is no point on the short-time side of the point where the loss angle ⁇ is 5° or more smaller than the maximum value, or there is no point showing the maximum value, and the loss angle ⁇ is -1.4°/min or more. has a section that exhibits a descent behavior that decreases by 5° or more with an inclination of .
- the prepreg of the present invention it is possible to obtain a prepreg having a thermoplastic resin on its surface, which has moderate flexibility and adhesiveness, excellent moldability to a complicated mold surface and excellent adhesion to the mold surface. can be done.
- the prepreg of the present invention it is possible to obtain a molded body of a fiber-reinforced composite material of excellent quality. Furthermore, even when applied to reinforcement and stiffening, the prepreg of the present invention is less likely to be misaligned and can be efficiently arranged at the target location.
- FIG. 4 is a diagram for explaining a loss angle ⁇ curve measured for a region in which (A) a reinforcing fiber is impregnated with (B) a thermosetting resin. It is a cross-sectional schematic diagram of one embodiment of the prepreg according to the present invention. It is a schematic diagram for demonstrating the drape evaluation method. BRIEF DESCRIPTION OF THE DRAWINGS It is a schematic diagram for demonstrating the preparation procedure of the sample for tensile shear strength evaluation used by the section of an Example.
- FIG. 1 shows one embodiment of the prepreg of the present invention.
- a thermosetting resin is impregnated into (A) reinforcing fibers, and
- a thermoplastic resin is provided on one surface of the sheet-shaped prepreg. is provided.
- the thermoplastic resin Since the thermoplastic resin has heat-welding properties, by allowing it to exist on the surface, it is possible to perform good welding and joining in a short time with another member, particularly a member on which the thermoplastic resin exists on the surface.
- the form in which (C) the thermoplastic resin is present is not particularly limited, and it may cover all or part of the surface of the prepreg.
- thermoplastic resin regions may be provided in the form of islands.
- the proportion of the thermoplastic resin present on the surface is 50% or more, with the area of the prepreg surface on the side where the (C) thermoplastic resin exists as 100%, from the viewpoint of ensuring stable heat-welding properties. is preferably 80% or more. Among these, it is more preferable to cover 100% of one surface of the prepreg, that is, to form a layer on the surface.
- (A) reinforcing fibers and sides that are not actually visible from a perspective view are also indicated by solid lines in order to facilitate understanding of the invention, but they actually exist in the prepreg. Note that FIG. 1 is a perspective view.
- the (C) thermoplastic resin does not exist on the surface opposite to the surface on which the (C) thermoplastic resin exists. That is, the (C) thermoplastic resin is present only on one surface of the prepreg, and the other surface is formed by a layer of (A) reinforcing fibers impregnated with (B) a thermosetting resin.
- a general mold temperature 60 to 160 ° C.
- thermosetting resin exceeds 100 ° C. and is 180 ° C. or less in the loss tangent tan ⁇ curve measured at a constant rate of temperature rise by dynamic viscoelasticity measurement (DMA method). have a peak.
- the (B) loss tangent tan ⁇ curve of the thermosetting resin measured by the dynamic viscoelasticity measurement method (DMA method) in the present invention is obtained by the following method. i.e. i) Remove the thermoplastic portion from the prepreg to prepare a piece of sample consisting only of thermoset resin and reinforcing fibers. The sample amount is about 1 g.
- the peak temperature of the tan ⁇ curve is determined by isokinetic heating measurement in accordance with JIS C6481.
- the peak temperature plots a curve with temperature on the horizontal axis and tan ⁇ obtained as the ratio (G′′/G′) of the storage elastic modulus G′ and the loss elastic modulus G′′ of the prepreg on the vertical axis. Measurement conditions are as follows.
- Heating rate 5°C/min Frequency: 1Hz.
- the peak temperature of the tan ⁇ curve obtained from the relationship between temperature and tan ⁇ is higher than 100 ° C., so that the tackiness of the thermosetting resin is suppressed and the handleability is improved. Arrangement in the mold is facilitated.
- the peak temperature of the tan ⁇ curve is 100° C. or less, the prepreg exhibits adhesiveness in a room temperature environment (23° C.), resulting in poor handleability and difficulty in placement in a molding die. .
- the peak temperature of the tan ⁇ curve by setting the peak temperature of the tan ⁇ curve to 180°C or less, it exhibits appropriate flexibility and adhesiveness at a general mold temperature (60 to 160°C), and can be shaped into complex mold surfaces.
- thermosetting resin in a prepreg with a high heat-resistant resin as a matrix, if the peak temperature of the tan ⁇ curve of the thermosetting resin exceeds 100°C and is outside the range of 180°C or less, the member containing the thermoplastic resin is efficiently reinforced and It is not possible to obtain an integrally molded body that is stiffened and has excellent appearance characteristics.
- a preferable range of the peak temperature of the tan ⁇ curve of the thermosetting resin is over 105° C. and 160° C. or less, more preferably over 110° C. and 140° C. or less.
- thermosetting resin It is known that the peak temperature of the tan ⁇ curve of thermosetting resin depends on the degree of cure of the thermosetting resin.
- a prepreg that satisfies the condition [I] can be obtained, for example, by adjusting the curing temperature and time of the thermosetting resin used to adjust the degree of curing of the thermosetting resin in the prepreg.
- condition [II] or condition [III] satisfies condition [II] or condition [III].
- condition [II] or condition [III] is determined by measuring the region in which (A) reinforcing fibers are impregnated with (B) thermosetting resin.
- Condition [II] is that the area where (A) the reinforcing fiber is impregnated with (B) the thermosetting resin is isothermally measured by the dynamic viscoelasticity measurement method (DMA method), and in the loss angle ⁇ curve,
- the loss angle ⁇ curve has a point indicating a maximum value, and has a point on the short-time side of the point indicating the maximum value at which the loss angle ⁇ is 5° or more smaller than the maximum value. be.
- the loss angle ⁇ curve is obtained by the following method. i.e. i) Remove any thermoplastic resin present in the prepreg and prepare a strip of sample consisting only of thermoset resin and reinforcing fibers. Furthermore, a sample is obtained by laminating such that the thickness is about 0.5 to 3 mm, typically about 1 mm. In addition, when the sample is a unidirectional material, it is assumed to be symmetrical lamination.
- the measurement conditions are as follows. As the measurement temperature, the measurement is performed at the following three measurement temperatures, and any one of the obtained loss angle ⁇ curves may satisfy the conditions of the preferable loss angle ⁇ curve described above or described later. . It should be noted that the mold temperature employed during molding should be selected to satisfy this condition or a temperature in the vicinity thereof. Incidentally, since the thermosetting resins used in the examples can be integrally molded at an injection mold temperature of 140°C, the results obtained are shown at a measurement temperature of 140°C. In addition, since a lower mold temperature is preferable in terms of energy efficiency, it is preferable to use a prepreg that gives the above-described or later-described preferable loss angle ⁇ curve at a measurement temperature of 140°C.
- Heating rate 5°C/min Start rate: 30°C Measurement temperature: 80°C, 110°C, or 140°C Frequency: 10Hz.
- the height when viewed from the short time side that is, the surface temperature of a general mold for injection molding and press molding ( 60 to 160°C)
- appropriate flexibility and adhesiveness can be expressed. Therefore, it is easy to shape even a mold curved surface with a small radius of curvature.
- prepreg can be easily attached to a vertical mold surface, so positional deviation occurs due to the effects of vibration when the mold is closed and pressure when resin is filled. Integral molding is possible without
- the shape of the loss angle ⁇ curve having a peak the shape (shape 1) shown in FIG.
- Condition [III] is that the region where (A) the reinforcing fiber is impregnated with (B) the thermosetting resin is isothermally measured by the dynamic viscoelasticity measurement method (DMA method), and in the loss angle ⁇ curve, Even if the loss angle ⁇ curve has a maximum value as shown in FIG. It has a section that does not have a point indicating a maximum value or does not have a point that indicates a maximum value, and exhibits a descending behavior in which the loss angle ⁇ decreases by 5° or more at an inclination of -1.4°/min or more.
- DMA method dynamic viscoelasticity measurement method
- this section is whether or not there is a section with a decrease width of 5° in the region where the loss angle ⁇ curve decreases with the passage of time, and the slope in that section is -1.4°/min or more. is judged by As a result, it has excellent handleability in a room temperature environment (23° C.), and exhibits flexibility and adhesiveness at the surface temperature (60 to 160° C.) of general molds for injection molding and press molding. Therefore, it is possible to shape a flat plate or a mold curved surface with a large radius of curvature. In particular, during high-pressure molding of a large area, it has excellent shape retention that can withstand high pressure.
- a prepreg having a peak with a height of 5° or more when viewed from the short time side has moderate flexibility at the surface temperature (60 to 160°C) of a general mold for injection molding and press molding. It is suitable for mold curved surfaces with small curvature radii because it is easy to shape in order to develop properties and adhesiveness. Prepreg without peaks is slightly rigid compared to prepregs with peaks, but it has excellent shape retention that can withstand high pressure, so it is suitable for high-pressure molding of flat plates and curved mold surfaces with large curvature radii. It is preferably used.
- the prepreg of the present invention has (A) reinforcement that exists across the boundary between (B) a resin region containing a thermosetting resin and (C) a resin region containing a thermoplastic resin. It preferably has fibers.
- (A) reinforcing fibers present across the interface between (B) a resin region containing a thermosetting resin and (C) a resin region containing a thermoplastic resin are defined as A state in which both the (B) thermosetting resin and (C) the thermoplastic resin are in contact with the entire circumference, and/or the entire circumference is in contact with the (B) thermosetting resin in a portion with a fiber cross section, In addition, it refers to (A) reinforcing fibers in a state where the entire circumference of another portion of the fiber cross section is in contact with the (C) thermoplastic resin.
- both (B) the resin region containing the thermosetting resin and (C) the resin region containing the thermoplastic resin are bonded via (A) the reinforcing fiber.
- (B) The resin region containing a thermosetting resin and the (C) resin region containing a thermoplastic resin are improved in bonding strength, making it difficult for the two to separate. Therefore, even if the (C) resin region containing a thermoplastic resin is integrated with another thermoplastic resin member to form a molded product, the (B) resin region containing a thermosetting resin of the prepreg of the present invention can be used.
- thermoplastic resin is also impregnated in (A) the reinforcing fiber.
- thermosetting resin As a method for forming a state in which (A) reinforcing fibers exist across the interface between (B) a resin region containing a thermosetting resin and (C) a resin region containing a thermoplastic resin, (A) reinforcing fibers (C) A method in which a thermoplastic resin is melted and coated from one side, and then (B) a thermosetting resin is impregnated from the opposite side, and (A) a reinforcing fiber is coated with (B) a thermosetting resin.
- thermoplastic resin is attached to the surface in the form of a sheet, a nonwoven fabric, or a particle, and heated and pressed to form (B) the thermosetting resin and (C )
- the heating temperature is (C) the melting point + 30 ° C. or higher when the thermoplastic resin is crystalline, and (B) the glass transition temperature of the thermosetting resin + 30 ° C. or higher when amorphous. can.
- the thermoplastic resin (C) it is preferable to first cover one side with the thermoplastic resin (C) because the melting point of the thermoplastic resin is high.
- the prepreg of the present invention is obtained by a test based on JIS K6850 (1994), and the tensile strength at the interface between the thermoset (B) resin region containing the thermosetting resin and the (C) resin region containing the thermoplastic resin.
- the shear strength is preferably 10 MPa or more at room temperature (23° C.).
- the tensile shear strength at the interface between (B) the resin region containing the thermosetting resin and (C) the resin region containing the thermoplastic resin is more preferably 20 MPa or more, and still more preferably 30 MPa or more. Although the upper limit of the tensile shear strength is not particularly limited, 100 MPa or less is practically sufficient.
- the prepreg of the present invention preferably has a drape property of 3° or more as defined below. As a result, it is possible to obtain good shapeability when arranging in a mold having a complicated shape with curved surfaces and corners for injection molding or press molding.
- the drapeability is more preferably 10° or more.
- the upper limit is not particularly limited, it is preferable to set the angle to 90° or less because even if the degree of curvature is large, the handleability may be poor.
- Drapability is an index that expresses the flexibility of the prepreg, that is, the ease with which it can be shaped into a mold.
- a sample for evaluation is obtained by cutting out a piece having a width of 25 mm and a length of 300 mm. In a room temperature environment (23° C.), as shown in FIG. 4, 100 mm from the edge of the sample is fixed to the upper surface of a horizontal test stand with adhesive tape, and further fixed with cellophane tape from above.
- the remaining 200 mm part is arranged to protrude from the test table in the air, hold the sample horizontally, remove the hold and let it hang down, 5 minutes after releasing the sample, by its own weight
- the drape angle is evaluated based on the tip of the bent sample and the horizontal plane of the test table.
- the drape angle is set vertically from point a and horizontally from point b, with point a being the lowest point of the tip of the sample bent by its own weight and point b being the root protruding into the air.
- the drape angle (.theta.; reference numeral 21 in FIG. 4) is given by the following equation. This measurement is performed at 5 points, and the arithmetic average value is taken as Trape's property.
- Drape angle ⁇ (°) ⁇ tan ⁇ 1 (lac/lbc) ⁇ (180/ ⁇ )
- lac is the distance between points a and c
- lbc is the distance between points b and c.
- the average thickness of the entire prepreg is 50 ⁇ m or more and 400 ⁇ m or less, and the average thickness of the resin region containing (C) the thermoplastic resin is 2% or more and 55% or less when the average thickness is 100%.
- the ratio of the average thickness of the (C) thermoplastic resin-containing resin region to the average thickness of the entire prepreg within the above range, drapeability is improved and shaping into a mold is facilitated.
- This ratio is more preferably 10% or more and 40% or less, and still more preferably 10% or more and 25% or less. , a prepreg having excellent unwindability can be obtained.
- the average thickness of the entire prepreg and the average thickness of (C) the resin region containing the thermoplastic resin can be measured as follows by observing the cross section of the prepreg using an optical microscope.
- a 20 mm long x 25 mm wide sample was taken from the prepreg, and the thickness of each part was measured as follows.
- the cross section of the sample is magnified 200 times with a laser microscope (manufactured by Keyence Corporation, VK-9510), randomly selected except for the part where the thickness of the thermoplastic resin is 0 mm, and the fields of view overlap each other Photographs were taken at 10 locations that were not exposed (observed, for example, as shown in FIG. 3).
- 10 measurement positions were determined at equal intervals, and the thickness of the entire prepreg and the thickness of the thermoplastic resin were measured.
- the average value of the measurement data for a total of 100 points was determined as the typical average thickness T of the entire prepreg and the average thickness Tp of the resin region containing the thermoplastic resin. The difference was defined as the average thickness Ts of the thermosetting resin.
- (A) reinforcing fibers are preferably arranged in one direction.
- (A) the portion containing the thermoplastic resin can be efficiently reinforced and stiffened.
- the tensile strength in the direction perpendicular to the direction in which the reinforcing fibers are arranged and parallel to the sheet surface is preferably 0.3 MPa or more.
- the tensile strength is more preferably 1.2 MPa or more, and by setting it in this range, it is possible to withstand the injection pressure during injection molding, which is accompanied by the fluidity of the resin and generates high pressure.
- the upper limit is not particularly limited, and the higher the pressure, the better, but about 1.5 MPa is preferable.
- the tensile strength in the direction perpendicular to the fiber is measured by the method described below.
- a prepreg in which reinforcing fibers are arranged in one direction is cut into a width of 50 mm and a length of 150 mm with the direction perpendicular to the fibers as the longitudinal direction, and used as an evaluation sample.
- the sample for evaluation is set in a desktop precision universal testing machine (Autograph AGS: manufactured by Shimadzu Corporation) so that the distance between the gripping jigs is 100 mm, and the speed is 100 mm / min in a room temperature environment (23 ° C.). Perform a tensile test.
- the tensile strength in the direction perpendicular to the fiber (MPa) from the following formula, where Pmax is the maximum load until the sample breaks, and A is the horizontal cross-sectional area perpendicular to the longitudinal direction of the sample.
- the number of evaluation samples shall be 5 or more, and the arithmetic mean value shall be adopted.
- the tensile strength is a value obtained as a yield stress during a tensile test.
- the molded article of the present invention is a molded article obtained by heating and curing the prepreg described above on a mold.
- the molded body is heated and hardened on the mold so that it has the same shape as the desired reinforcement/stiffening part on the existing part. do.
- it is a compact that can efficiently reinforce and stiffen large parts that are difficult to reinsert into the mold.
- the peak temperature of the tan ⁇ curve of the molded body obtained is 195° C. or higher.
- the integrated molded body of the present invention is a molded body obtained by integrating the prepreg with a thermoplastic resin by injection molding or press molding. By using the prepreg, it is possible to efficiently reinforce and stiffen the target portion of the thermoplastic resin member.
- thermosetting resin thermosetting resin
- thermoplastic resin thermoplastic resin
- reinforcing fibers include carbon fibers, glass fibers, metal fibers, aromatic polyamide fibers, polyaramid fibers, alumina fibers, silicon carbide fibers, boron fibers, basalt fibers, and the like. These may be used alone or in combination of two or more. These reinforcing fibers may be surface-treated. Surface treatments include metal adhesion treatment, coupling agent treatment, sizing agent treatment, and additive adhesion treatment. These reinforcing fibers also contain conductive reinforcing fibers. Carbon fibers are preferably used as the reinforcing fibers because of their low specific gravity, high strength, and high elastic modulus.
- (A) reinforcing fibers are arranged in one direction. Continuous fibers such as aligned long fibers (fiber bundles) and woven fabrics, and discontinuous fibers such as mats and non-woven fabrics may be used.
- the reinforcing fiber may be used to mean an aggregate of such reinforcing fibers.
- the reinforcing fibers may be composed of a plurality of fibers of the same form, or may be composed of a plurality of fibers of different forms.
- the number of reinforcing fibers constituting one reinforcing fiber bundle is usually 300 to 60,000, preferably 300 to 48,000, more preferably 300 to 48,000 in consideration of the production of the base material. , 1,000 to 24,000.
- the range may be a combination of any of the above upper limits and any of the above lower limits.
- Carbon fibers include “Torayca (registered trademark)” T800G-24K, “Torayca (registered trademark)” T800S-24K, “Torayca (registered trademark)” T700G-24K, “Torayca (registered trademark)” T700S- 24K, “Torayca (registered trademark)” T300-3K, and “Torayca (registered trademark)” T1100G-24K (manufactured by Toray Industries, Inc.).
- Thermosetting resins include, for example, unsaturated polyester resins, vinyl ester resins, epoxy resins, phenol resins, urea resins, melamine resins, polyimide resins, cyanate ester resins, bismaleimide resins, benzoxazine resins, or these. and a resin blended with at least two of these.
- An elastomer or rubber component may be added to the thermosetting resin to improve impact resistance.
- epoxy resins are preferable because of their excellent mechanical properties, heat resistance, and adhesiveness to reinforcing fibers.
- Examples of the main agent of the epoxy resin include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, bisphenol S type epoxy resin, and brominated epoxy such as tetrabromobisphenol A diglycidyl ether.
- bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, bisphenol S type epoxy resin, and brominated epoxy such as tetrabromobisphenol A diglycidyl ether.
- Curing agents for epoxy resins include, for example, dicyandiamide, aromatic urea compounds, aromatic amine compounds, phenol novolak resins, cresol novolak resins, polyphenol compounds, imidazole derivatives, tetramethylguanidine, thiourea-added amines, carboxylic acid hydrazides, carboxylic acid acid amides, polymercaptans and the like.
- an epoxy resin having good heat resistance can be obtained by using an aromatic amine compound as the amine compound.
- aromatic amine compounds examples include 3,3′-diisopropyl-4,4′-diaminodiphenylsulfone, 3,3′-di-t-butyl-4,4′-diaminodiphenylsulfone, 3,3′- Diethyl-5,5'-dimethyl-4,4'-diaminodiphenylsulfone, 3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenylsulfone, 3,3'-di-t- Butyl-5,5'-dimethyl-4,4'-diaminodiphenylsulfone, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenylsulfone, 3,3'-diisopropyl-5,5' -diethyl-4,4'-diaminodiphenylsulfone, 3,
- the epoxy resin preferably contains a thermoplastic resin component that is soluble in the epoxy resin in a dissolved state as a viscosity modifier. Since such a thermoplastic resin component dissolves in an epoxy resin and exhibits thermosetting properties as a whole, it is considered to be one component of the thermosetting resin (B).
- the term "soluble in epoxy resin” refers to the presence of a temperature range in which a homogeneous phase is formed by heating or heating and stirring a mixture of a thermoplastic resin component and an epoxy resin.
- form a homogeneous phase means that a state without separation can be visually observed.
- the "dissolved state” refers to a state in which an epoxy resin containing a thermoplastic resin component is brought to a certain temperature range and forms a homogeneous phase. Once a homogeneous phase is formed in a certain temperature range, separation may occur outside that temperature range, eg, at room temperature.
- the thermoplastic resin component soluble in the epoxy resin generally has a carbon-carbon bond, an amide bond, an imide bond, an ester bond, an ether bond, a carbonate bond, a urethane bond, a thioether bond, a sulfone bond and a carbonyl bond in the main chain. It is preferably a thermoplastic resin having a bond selected from the group consisting of Further, this thermoplastic resin component may have a partially crosslinked structure, and may be crystalline or amorphous.
- polyamides, polycarbonates, polyacetals, polyphenylene oxides, polyphenylene sulfides, polyarylates, polyesters, polyamideimides, polyimides, polyetherimides, polyimides having a phenyltrimethylindane structure, polysulfones, polyethersulfones, polyetherketones, polyetheretherketones , polyaramid, polyvinyl formal, polyvinyl butyral, phenoxy resin, polyethernitrile and polybenzimidazole are preferred.
- it is preferable to have a glass transition temperature of over 180°C from the viewpoint of resistance to thermal deformation when used as a molded article and polyetherimide and polyethersulfone are suitable examples. It is mentioned as.
- thermoplastic resin is not particularly limited as long as it can be melted by heating.
- examples include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and liquid crystal polyester Polyolefins such as polyethylene, polypropylene, and polybutylene, styrene resins, urethane resins, polyoxymethylene, polyamides such as polyamide 6 and polyamide 66, polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyphenylene sulfide, and polyphenylene ether , modified polyphenylene ether, polyimide, polyamideimide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetherketoneketone, polyarylene ether ketone, polyarylate, poly Ether
- thermoplastic resins may be copolymers or modified products of the above resins, or may be blends of two or more selected from the above resins and their copolymers and modified products.
- one or more selected from polyarylene ether ketone, polyphenylene sulfide or polyetherimide is (C) a resin or resin containing 60% by weight or more of the thermoplastic resin A composition is preferred.
- An elastomer or rubber component may be added to improve impact resistance.
- other fillers and additives may be contained as appropriate depending on the intended use, etc., as long as the object of the present invention is not impaired.
- inorganic fillers for example, inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, release agents , antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foam control agents, coupling agents and the like.
- thermoplastic resin when the (C) thermoplastic resin is applied to the sheet-like material in which the (A) reinforcing fibers are preliminarily impregnated with the (B) thermosetting resin, various application forms can be employed.
- (C) a method of forming a thermoplastic resin into a sheet or non-woven fabric and laminating it, or a method of dispersing particulate (C) thermoplastic resin on the sheet and applying heat to integrate it. There is a method to make it possible.
- the integrally molded article of the present invention can be obtained by placing a prepreg in a mold for injection molding or press molding and integrating it with a member containing a thermoplastic resin by insert molding.
- the integrally molded product of the present invention is preferably used for aircraft structural members, wind turbine blades, automobile outer panels and sheets, computer applications such as IC trays and laptop computer cases, and sports applications such as golf shafts and tennis rackets.
- A Materials used (A) Reinforcing fibers
- A-1 Carbon fibers (“Torayca (registered trademark)” T700S-24K, manufactured by Toray Industries, Inc., strand tensile strength: 4.9 GPa) are arranged in parallel at regular intervals. What I did.
- A-2 A woven fabric obtained by plain weaving carbon fibers (basis weight: 193 g/m 2 ).
- ⁇ Curing agent for epoxy resin d) 4,4'-diaminodiphenylsulfone (Seikacure S, manufactured by Wakayama Seika Kogyo Co., Ltd., active hydrogen equivalent: 62 (g/eq.)).
- ⁇ Viscosity modifier e) Polyethersulfone (“Sumika Excel” (registered trademark) PES5003P, manufactured by Sumitomo Chemical Co., Ltd.).
- thermosetting resins B-1 and B-2 were produced according to the following method.
- B-1 a) tetraglycidyldiaminodiphenylmethane (60 parts by mass), b) bisphenol A type epoxy resin (40 parts by mass), and e) polyethersulfone (10 parts by mass) are put into a kneading device and heated and kneaded. was performed to dissolve the viscosity modifier. Next, the temperature was lowered to 100° C. or lower while kneading was continued, and d) 4,4′-diaminodiphenylsulfone (45 parts by mass) was added and stirred to obtain a thermosetting resin B-1.
- thermosetting resin B-2 a) tetraglycidyldiaminodiphenylmethane (60 parts by mass), c) bisphenol F type epoxy resin (40 parts by mass), and e) polyethersulfone (10 parts by mass) are put into a kneading device and heated and kneaded. was performed to dissolve the viscosity modifier. Next, the temperature was lowered to 100° C. or lower while kneading was continued, and d) 4,4′-diaminodiphenylsulfone (45 parts by mass) was added and stirred to obtain a thermosetting resin B-2.
- Thermoplastic resin C-1 A film made of polyamide 6 (“Amilan” (registered trademark) CM1007 (manufactured by Toray Industries, Inc., melting point 225° C.)) and having a basis weight of 10 g/m 2 was used.
- C-2 A film having a basis weight of 30 g/m 2 made of polyamide 6 (“Amilan” (registered trademark) CM1007 (manufactured by Toray Industries, Inc., melting point: 225°C)) was used.
- C-3 A film having a basis weight of 85 g/m 2 made of polyamide 6 (“Amilan” (registered trademark) CM1007 (manufactured by Toray Industries, Inc., melting point: 225°C)) was used.
- C-4 A film made of acid-modified polypropylene (“ADMER” (registered trademark) QB510 (manufactured by Mitsui Chemicals, Inc., melting point 165° C.)) and having a basis weight of 30 g/m 2 was used.
- ADMER acid-modified polypropylene
- D-1 80 parts of polyamide 6 and 20 parts of T700S were put into a twin-screw extruder and heated and kneaded at 250° C. to obtain pellets for injection molding.
- the average fiber length of T700S in the pellet was 0.1 mm.
- D-2 80 parts of acid-modified polypropylene and 20 parts of T700S were put into a twin-screw extruder and heated and kneaded at 250° C. to obtain pellets for injection molding.
- the average fiber length of T700S in the pellet was 0.1 mm.
- D-3 80 parts of polyether ketone ketone and 20 parts of T700S were put into a twin-screw extruder and heated and kneaded at 360° C. to obtain pellets for injection molding.
- the average fiber length of T700S in the pellet was 0.1 mm.
- E Thermoplastic Plate
- E-1 A randomly oriented fiber-reinforced thermoplastic resin composed of 80 parts of polyamide 6 and 20 parts of T700S was used. The plate thickness was 5 mm.
- E-2 A randomly oriented fiber-reinforced thermoplastic resin composed of 80 parts of acid-modified polypropylene and 20 parts of T700S was used. The plate thickness was 5 mm.
- E-3 A randomly oriented fiber-reinforced thermoplastic resin composed of 80 parts of polyether ketone ketone and 20 parts of T700S was used. The plate thickness was 5 mm.
- Method I A reinforcing fiber sheet having a basis weight of 193 g/m 2 made of reinforcing fibers (described in the sections of Examples and Comparative Examples; the same applies to methods II and III) is pulled out, and while the reinforcing fiber sheet is running, A predetermined (C) thermoplastic resin film (described in the sections of Examples and Comparative Examples; the same applies to methods II and III) is placed on the reinforcing fiber sheet and heated with an IR heater ( C) Melt the thermoplastic resin and attach it to the entire surface of one side of the reinforcing fiber sheet, and (C) pressurize with a nip roll maintained at a melting temperature of the thermoplastic resin or less to cool the impregnated reinforcing fiber sheet.
- thermosetting resin (described in the section of each example and comparative example, the same applies to methods II and III) is applied on release paper with a resin basis weight of 100 g / m 2 using a knife coater. After coating to produce a thermosetting resin film, the thermosetting resin film is superimposed on the surface of the intermediate (C) opposite to the surface impregnated with the thermoplastic resin, and heated with a heat roll.
- a prepreg was obtained by impregnating the fiber-reinforced resin intermediate while pressurizing. At this time, the peak temperature of the tan ⁇ curve of the prepreg is adjusted by the contact time between the fiber bundle passing through the heat roll and the roll and the roll temperature.
- the contact time between the fiber bundle and the roll was adjusted by the number of roll stages and the passing speed of the fiber bundle.
- the running direction of the reinforcing fiber sheet during impregnation is the longitudinal direction with respect to the reinforcing fibers in the case of a prepreg in which the reinforcing fibers are arranged in one direction, and the longitudinal direction of the fabric in the case of a prepreg made of reinforcing fiber fabric. is.
- thermosetting resin was coated on release paper with a resin basis weight of 50 g/m 2 using a knife coater to prepare a thermosetting resin film. This resin film is superimposed on both sides of (A) a reinforcing fiber sheet having a basis weight of 193 g/m 2 made of reinforcing fibers, and using a heat roll, the reinforcing fiber sheet is impregnated with a thermosetting resin while being heated and pressed to reinforce the fiber. A resin intermediate was obtained. A (C) thermoplastic resin film was placed on the surface of the fiber-reinforced resin intermediate, and the (C) thermoplastic resin was impregnated with heat and pressure to obtain a prepreg. The peak temperature of the tan ⁇ curve of the prepreg was adjusted by the contact time between the fiber bundle passing through the heat roll and the roll and the roll temperature in the same manner as described above.
- thermosetting resin was coated on release paper with a resin basis weight of 50 g/m 2 using a knife coater to prepare a thermosetting resin film.
- This resin film is superimposed on both sides of (A) a reinforcing fiber sheet having a basis weight of 193 g/m 2 made of reinforcing fibers, and using a heat roll, the reinforcing fiber sheet is impregnated with a thermosetting resin while being heated and pressurized to form a prepreg. Obtained.
- the peak temperature of the tan ⁇ curve of the prepreg was adjusted by the contact time between the fiber bundle passing through the heat roll and the roll and the roll temperature in the same manner as described above.
- the prepreg was cut into a width of 25 mm and a length of 300 mm to obtain an evaluation sample.
- the longitudinal direction of the fibers is taken as the longitudinal direction of the sample
- the longitudinal direction of the fabric is taken as the longitudinal direction of the sample.
- 100 mm from the edge of the sample is fixed to the upper surface of a horizontal test table with adhesive tape, and further fixed with cellophane tape from above.
- Drape angle ⁇ (°) ⁇ tan ⁇ 1 (lac/lbc) ⁇ (180/ ⁇ )
- lac is the distance between points a and c
- lbc is the distance between points b and c.
- Thickness of Prepreg, Thermoplastic Resin Layer, and Thermosetting Resin Layer A 20 mm long ⁇ 25 mm wide sample was obtained from the prepreg, and the thickness of each portion was measured as follows. The cross section of the sample is magnified 200 times with a laser microscope (VK-9510: manufactured by Keyence Corporation), randomly selected except for the part where the thickness of the thermoplastic resin is 0 mm, and the fields of view overlap each other Photographs were taken at 10 locations that were not exposed (observed, for example, as shown in FIG. 3). In each photographed image, 10 measurement positions (perpendicular base line for thickness measurement: 15) were set at equal intervals, and the overall thickness of the prepreg and the thickness of the thermoplastic resin layer were measured. The average value of the measurement data for a total of 100 points was defined as the representative prepreg thickness T and the thickness Tp of the thermoplastic resin layer, and the difference between them was defined as the thickness Ts of the thermosetting resin layer.
- Tensile strength in the direction perpendicular to the fiber A prepreg in which the reinforcing fibers are arranged in one direction is cut into a width of 50 mm and a length of 150 mm with the direction perpendicular to the direction of orientation of the reinforcing fibers as the longitudinal direction, and used as an evaluation sample. did.
- the sample for evaluation is set in a desktop precision universal testing machine (Autograph AGS: manufactured by Shimadzu Corporation) so that the distance between the gripping jigs is 100 mm, and the speed is 100 mm / min in a room temperature environment (23 ° C.).
- a tensile test was performed.
- the tensile strength in the direction perpendicular to the fiber (MPa) was calculated from the following formula, where Pmax is the maximum load until the sample breaks, and A is the horizontal cross-sectional area perpendicular to the longitudinal direction of the sample.
- the prepreg is inserted into a mold preheated to 140 ° C. so that the surface where the thermoplastic resin is not present (C) is in contact with the mold surface for injection molding, and (D) the injection molding material is placed in the mold.
- An integrally molded body reinforced and stiffened by the prepreg was obtained by injection filling into the prepreg.
- the injection molding material (D) was heated and melted in a heating cylinder to the melting point of the injection molding material + 30 ° C., and was injection molded at a screw rotation speed of 60 rpm, an injection speed of 90 mm / sec, an injection pressure of 200 MPa, and a back pressure of 0.5 MPa. .
- the injection mold used for the integral molding has a curved surface with an arc length of 302 mm in a cylinder with a radius of 225 mm and a height of 280 mm on a plane measuring 300 mm long by 300 mm wide.
- Formability on the curved surface of the mold when the prepreg is placed in the injection mold is relatively evaluated in the following four stages. evaluated.
- ⁇ Flexibility was exhibited in 3 seconds or more and less than 10 seconds after pressing the prepreg against the mold, but the flexibility was unstable, and the mold surface was curved in the range of 2 to 4 times in 5 molding times. I was able to shape along.
- ⁇ Flexibility is low even after 10 seconds or more have passed since the prepreg was pressed against the mold, so shaping along the curved mold surface was possible in the range of 0 to 1 in 5 molding times. .
- the formability of the prepreg of the present invention is expressed by relatively evaluating the adhesion to the mold and the formability to the curved surface of the mold.
- thermosetting resin used in the corresponding example or comparative example
- a release paper was coated with a resin basis weight of 50 g/m 2 using a knife coater to prepare a thermosetting resin film.
- This resin film is superimposed on both sides of the reinforcing fiber sheet (A) made of reinforcing fibers and having a basis weight of 193 g / m 2 used in the corresponding example or comparative example, and a heat roll is used to heat and press the thermosetting resin.
- the peak temperature of the tan ⁇ curve of the lower layer prepreg was adjusted to less than 30° C. by adjusting the contact time between the fiber bundle passing through the heat roll and the roll and the roll temperature.
- the direction in which the (A) reinforcing fibers are oriented is set to 0 °, and the direction orthogonal to the direction is set to 90 °, and the front and back surfaces are distinguished. [0°/90°] 2S (symbol S indicates specular symmetry).
- the prepreg prepared in the example or comparative example was placed in the injection mold for preparing the sample for tensile shear strength evaluation shown in FIG.
- the laminate was arranged so that the surface on the side opposite to the surface was formed.
- an injection molding machine J150EII-P: manufactured by JSW
- an injection molding material described in the section of each example and comparative example
- a width of 200 mm ⁇ length of 12.5 mm was introduced.
- An integrally molded body for tensile shear strength evaluation was produced in which the injection molding material and the laminate were joined in the region.
- the integrally molded body was placed in an oven, and the (B) thermosetting resin was completely cured by heat treatment.
- the injection molding material (D) was melted by heating to a melting point of +30°C in a heating cylinder, and injection molded at a screw rotation speed of 60 rpm, an injection speed of 90 mm/sec, an injection pressure of 200 MPa, and a back pressure of 0.5 MPa.
- the obtained integrated molded body for tensile shear strength evaluation was cut into a size of 180 mm in width ⁇ 172.5 mm in length so that the fiber direction of the surface was the longitudinal direction of the sample, and then placed in a vacuum oven for 24 hours. It was dried for a period of time, tab-bonded in accordance with ISO4587:1995 (JIS K6850 (1994)), and cut at a width of 25 mm to obtain a sample for tensile shear strength evaluation.
- the sample for tensile shear strength evaluation having the same uneven shape as shown in FIG.
- the laminate was arranged so that the prepreg was on the side opposite to the side facing the mold. Then, after adjusting the thickness by heat and pressure molding at a melting point of +30 ° C. so that it can be placed in the press molding die, the thermoplastic plate material cut into a width of 200 mm and a length of 150 mm (see the section of each example and comparative example) described) were prepared.
- thermoplastic plate material was placed in a press molding die so as to be joined to the laminate in a region of width 200 mm ⁇ length 12.5 mm, and an integrated molded body for evaluation of tensile shear strength was produced.
- the mold temperature was preheated to 140° C., and after placing the laminate and the thermoplastic plate material in the mold, the temperature was raised to +30° C. of the melting point of the thermoplastic plate material, and then the pressure was reduced to 0.5 MPa. ) and high pressure (5.0 MPa).
- the temperature was lowered and the integrated molded body for tensile shear strength evaluation was taken out, and the fiber direction of the surface was aligned with the longitudinal direction of the sample. , dried in a vacuum oven for 24 hours, tab-bonded according to ISO4587:1995 (JIS K6850 (1994)), and cut at a width of 25 mm to obtain a sample for tensile shear strength evaluation.
- the obtained sample for tensile shear strength evaluation was measured under a room temperature environment (23°C) based on ISO4587:1995 (JIS K6850 (1994)).
- the moldability was good, but the tensile shear strength of the obtained integrally molded products was extremely low.
- Example 1 (Example 1, Example 2) Using (A) A-1 as a reinforcing fiber, (B) B-1 as a thermosetting resin, and (C) C-4 as a thermoplastic resin, the tan ⁇ curve shown in Table 1 is produced by the preparation method II. A prepreg with a peak temperature was produced. After that, the prepreg was inserted into an injection mold, and insert injection molding was performed using D-2 as an injection molding material. Separately, the prepreg produced by the production method II was inserted into a press molding die, and press molding was performed using E-2 as a thermoplastic plate material. Table 1 summarizes the properties of the prepreg, the moldability, and the evaluation results of the integrally molded body after injection molding and the integrally molded body after press molding.
- the moldability was good, and all exhibited tensile shear strength that was satisfactory as an integrally molded product.
- Example 2 the fiber straightness of the integrally molded body was greatly disturbed, and in Comparative Example 4, the prepreg moved in the mold and could not be placed at the desired location.
- Examples 5 to 8 have high bonding strength, and Examples 6 and 7 in particular show good adhesion to the mold and moldability to the curved surface of the mold in addition to handleability at room temperature. The moldability was also good, and extremely high tensile shear strength was developed.
- Example 8 was more excellent in handleability in a room temperature environment (23 ° C.) and inferior in moldability to Examples 5 to 7, but even in an integrally molded body by high pressure press molding, the straightness of fibers was improved. There was no disturbance, and the appearance was better than those of Examples 6 and 7 press-molded under the same conditions.
- the fibers were disordered from the ends of the prepregs placed.
- Example 3 Using the (A) reinforcing fiber, (B) thermosetting resin, and (C) thermoplastic resin shown in Table 1, a prepreg having a peak temperature of the tan ⁇ curve shown in Table 1 is produced by the first production method. did. After that, the prepreg was inserted into an injection mold, and insert injection molding was performed using D-1 as an injection molding material. Separately, the prepreg produced by the above production method I was inserted into a press molding die, and press molding was performed using E-1 as a thermoplastic plate material. Table 1 summarizes the properties of the prepreg, the moldability, and the evaluation results of the integrally molded body after injection molding and the integrally molded body after press molding.
- Example 4 although the prepreg had high rigidity, it had good adhesion to the mold and could be integrally molded.
- Examples 3 and 4 exhibited excellent tensile shear strength, although the straightness of the fibers in the injection-molded articles was slightly impaired in some areas.
- the integrally molded product obtained by high-pressure press molding the straightness of the fibers was greatly disturbed and spread as the resin flowed, and the shape could not be maintained.
- Example 9 Using (A) A-2 as a reinforcing fiber, (B) B-1 as a thermosetting resin, and (C) C-2 as a thermoplastic resin, the tan ⁇ curve shown in Table 1 is produced by the first production method. A prepreg with a peak temperature was produced. After that, the prepreg was inserted into an injection mold, and insert injection molding was performed using D-1 as an injection molding material. Separately, the prepreg produced by the above production method I was inserted into a press molding die, and press molding was performed using E-1 as a thermoplastic plate material. Table 1 summarizes the properties of the prepreg, the moldability, and the evaluation results of the integrally molded body after injection molding and the integrally molded body after press molding.
- the injection-integrated molded article was superior in appearance with straightness of fibers maintained as compared with Comparative Example 3, but the appearance of the integrally molded article subjected to high-pressure press molding was disturbed in straightness of fibers from the prepreg end.
- Examples 10-12 Using (A) A-1 as a reinforcing fiber, (B) B-2 as a thermosetting resin, and (C) C-5 as a thermoplastic resin, the tan ⁇ curve shown in Table 2 is produced by the first production method. A prepreg with adjusted peak temperature was produced. After that, the prepreg was inserted into an injection mold, and insert injection molding was performed using D-3 as an injection molding material.
- the prepreg produced by the above production method I was inserted into a press molding die, and press molding was performed using E-3 as a thermoplastic plate material.
- Table 1 summarizes the properties of the prepreg, the moldability, and the evaluation results of the integrally molded body after injection molding and the integrally molded body after press molding.
- Example 10 was excellent in formability and exhibited extremely high tensile shear strength. On the other hand, in high-pressure press molding, the appearances of Examples 11 and 12 were better than that of Example 10.
- the tensile shear strength measured in the integrated molded body exceeded 10 MPa, so the resin region containing the cured (B) thermosetting resin of the prepreg produced in each example and (C) the resin region containing the thermoplastic resin is estimated to have a tensile shear strength of more than 10 MPa.
- Example 1 resulted in excellent tensile shear strength of the integrally molded body. This is because the surface of the prepreg of Example 1 is coated with the (C) thermoplastic resin having heat-welding properties, so that the prepreg can be integrated with the injection material. On the other hand, (C) the prepreg of Comparative Example 1, which was not coated with a thermoplastic resin, was seemingly integrated with the injection material, but had such a low tensile shear strength that it could be easily peeled off manually.
- the peak temperature of the tan ⁇ curve exceeds 100 ° C. and is 180 ° C. or less, so that the adhesion to the mold for injection molding and the shapeability are good. It was confirmed that the moldability was excellent. This is thought to be due to the development of appropriate adhesiveness and flexibility on the mold, and due to this effect, an integrally molded product excellent in appearance and tensile shear strength was obtained. In particular, Examples 6, 7, and 10 were excellent in the balance between the moldability and the appearance of the integrally molded product. This is because the peak temperature of the tan ⁇ curve is about 110 ° C. or higher and 140 ° C. or lower, (A) while maintaining the straightness of the reinforcing fibers, good adhesion and flexibility are obtained by heating from the mold surface. It was thought that it was possible.
- Example 9 was excellent in appearance of the integrally molded body. It is believed that this is because even when (A) the reinforcing fibers are woven fabrics, the (B) thermosetting resin has a specific peak temperature of the tan ⁇ curve, which makes it easier for the straightness of the fibers to be maintained. rice field.
- Example 3 By comparing Examples 3 to 12, it was confirmed that even if the prepreg manufacturing method is different, by adjusting the peak temperature of the tan ⁇ curve, the same degree of moldability and appearance of the integrally molded product can be obtained.
- Example 3 As a result of using layers of (C) thermoplastic resin with different thicknesses, Example 3 having a smaller thickness was found to be superior to Example 4 and Example 5. Compared with No. 5, the drape property was excellent, but the tensile shear strength was slightly inferior.
- Example 6 is a result that is even more excellent in tensile shear strength after integral molding, and (A) the reinforcing fiber is the interface between (B) the thermosetting resin and (C) the thermoplastic resin It was thought that strong bonding strength could be expressed by straddling the This tendency was also confirmed by comparing Example 2 and Example 7.
- Example 8 was less moldable than Example 6, which was attributed to the prepreg being less flexible and rigid. Furthermore, in Example 4, the moldability to the curved surface of the mold was inferior to that in Example 6, and it was considered that this was because the thermoplastic resin (C) was thick and had low flexibility. Although Example 3 was excellent in adhesion to the curved surface of the mold and formability, the appearance of the integrally molded product was slightly inferior to Example 6. It is thought that this is because the prepreg has a low tensile strength in the direction perpendicular to the fibers, so that the straightness of the fibers is impaired by the pressure and resin flow during hot-press molding. In comparing Example 11 and Example 12, although there was a difference in flexibility, both were within the range of appropriate condition [II], so it was confirmed that the prepreg is suitable for use.
- Example 6 By comparing Example 6 with Example 10, and Example 8 with Example 11, it was found that any prepreg made of different materials could be formed with the same degree of moldability and integrality by adjusting the peak temperature of the tan ⁇ curve. It was confirmed that the appearance of chemical molding can be obtained. It was also confirmed that a prepreg that does not have a peak with a height of 5° or more in the loss angle ⁇ curve is even more excellent in handleability in a room temperature environment (23° C.). On the other hand, although the formability, which is expressed by the adhesion to the mold and the ability to shape onto the curved surface of the mold, is inferior, it is suggested that the straightness of the fibers is less disturbed even during high-pressure press molding, and that the shape retention is excellent. was done.
- the integrally molded product of the present invention is preferably used for computer applications such as aircraft structural members, wind turbine blades, automobile outer panels and sheets, IC trays and notebook computer cases, and sports applications such as golf shafts and tennis rackets.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Materials Engineering (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Health & Medical Sciences (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Manufacturing & Machinery (AREA)
- Inorganic Chemistry (AREA)
- Mechanical Engineering (AREA)
- Reinforced Plastic Materials (AREA)
- Laminated Bodies (AREA)
Priority Applications (5)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022502064A JP7088433B1 (ja) | 2021-01-21 | 2021-12-21 | プリプレグ、成形体および一体化成形体 |
| CN202180085543.6A CN116761713A (zh) | 2021-01-21 | 2021-12-21 | 预浸料坯、成型体及一体化成型体 |
| EP21921323.8A EP4282644B1 (en) | 2021-01-21 | 2021-12-21 | Prepreg, molded article, and integrally molded article |
| KR1020237022425A KR102763715B1 (ko) | 2021-01-21 | 2021-12-21 | 프리프레그, 성형체 및 일체화 성형체 |
| US18/270,013 US12558816B2 (en) | 2021-01-21 | 2021-12-21 | Prepreg, molded article, and integrally molded article |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021-007774 | 2021-01-21 | ||
| JP2021007774 | 2021-01-21 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2022158222A1 true WO2022158222A1 (ja) | 2022-07-28 |
Family
ID=82548285
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2021/047257 Ceased WO2022158222A1 (ja) | 2021-01-21 | 2021-12-21 | プリプレグ、成形体および一体化成形体 |
Country Status (7)
| Country | Link |
|---|---|
| US (1) | US12558816B2 (enExample) |
| EP (1) | EP4282644B1 (enExample) |
| JP (1) | JP7088433B1 (enExample) |
| KR (1) | KR102763715B1 (enExample) |
| CN (1) | CN116761713A (enExample) |
| TW (1) | TWI888690B (enExample) |
| WO (1) | WO2022158222A1 (enExample) |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN115697681B (zh) * | 2020-06-03 | 2026-04-28 | 东丽株式会社 | 纤维增强塑料、一体成型品、及预浸料坯 |
Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH10138354A (ja) | 1996-11-08 | 1998-05-26 | Yamaha Corp | 炭素繊維強化樹脂成形物とその製造方法 |
| JP2004315743A (ja) * | 2003-04-18 | 2004-11-11 | Mitsubishi Rayon Co Ltd | 熱硬化性樹脂組成物、プリプレグ及び繊維強化複合材料 |
| JP2012086578A (ja) * | 2004-02-27 | 2012-05-10 | Toray Ind Inc | 炭素繊維強化複合材料用エポキシ樹脂組成物、プリプレグ、一体化成形品、繊維強化複合材料板、および電気・電子機器用筐体 |
| JP2016113472A (ja) * | 2014-12-11 | 2016-06-23 | 本田技研工業株式会社 | マトリックス材 |
| JP2018161801A (ja) | 2017-03-27 | 2018-10-18 | 三菱ケミカル株式会社 | 接着構造部材 |
| WO2020235487A1 (ja) * | 2019-05-23 | 2020-11-26 | 東レ株式会社 | プリプレグ、積層体および成形品 |
Family Cites Families (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| KR960704977A (ko) * | 1994-07-18 | 1996-10-09 | 마에다 가쯔노스께 | 에폭시 수지 조성물, 프리프레그 및 섬유 강화 복합 재료(An Epoxy Resin Composition, a Prepreg and a Fiber Reinforced Composite Material) |
| TWI304321B (en) * | 2002-12-27 | 2008-12-11 | Toray Industries | Layered products, electromagnetic wave shielding molded articles and method for production thereof |
| WO2012147401A1 (ja) * | 2011-04-27 | 2012-11-01 | 東レ株式会社 | プリプレグ、繊維強化複合材料およびプリプレグの製造方法 |
| KR101596207B1 (ko) * | 2012-11-27 | 2016-02-19 | 미쯔비시 레이온 가부시끼가이샤 | 섬유 강화 열가소성 수지 프리프레그 및 그 성형체, 및 섬유 강화 열가소성 수지 프리프레그의 제조 방법 |
| EP3194466B1 (en) * | 2014-09-12 | 2019-11-06 | Drexel University | Toughening of anhydride cured thermosetting epoxy polymers using grafted triglycerides |
| JP7577931B2 (ja) * | 2019-05-23 | 2024-11-06 | 東レ株式会社 | 繊維強化樹脂基材、一体化成形品および繊維強化樹脂基材の製造方法 |
| JP2020193336A (ja) * | 2019-05-23 | 2020-12-03 | 東レ株式会社 | 成形材料および成形品 |
| US20230001651A1 (en) * | 2019-12-11 | 2023-01-05 | Toray Industries, Inc. | Prepreg, laminate, and integrated product |
-
2021
- 2021-12-21 CN CN202180085543.6A patent/CN116761713A/zh active Pending
- 2021-12-21 WO PCT/JP2021/047257 patent/WO2022158222A1/ja not_active Ceased
- 2021-12-21 US US18/270,013 patent/US12558816B2/en active Active
- 2021-12-21 JP JP2022502064A patent/JP7088433B1/ja active Active
- 2021-12-21 EP EP21921323.8A patent/EP4282644B1/en active Active
- 2021-12-21 KR KR1020237022425A patent/KR102763715B1/ko active Active
-
2022
- 2022-01-10 TW TW111100908A patent/TWI888690B/zh active
Patent Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH10138354A (ja) | 1996-11-08 | 1998-05-26 | Yamaha Corp | 炭素繊維強化樹脂成形物とその製造方法 |
| JP2004315743A (ja) * | 2003-04-18 | 2004-11-11 | Mitsubishi Rayon Co Ltd | 熱硬化性樹脂組成物、プリプレグ及び繊維強化複合材料 |
| JP2012086578A (ja) * | 2004-02-27 | 2012-05-10 | Toray Ind Inc | 炭素繊維強化複合材料用エポキシ樹脂組成物、プリプレグ、一体化成形品、繊維強化複合材料板、および電気・電子機器用筐体 |
| JP2016113472A (ja) * | 2014-12-11 | 2016-06-23 | 本田技研工業株式会社 | マトリックス材 |
| JP2018161801A (ja) | 2017-03-27 | 2018-10-18 | 三菱ケミカル株式会社 | 接着構造部材 |
| WO2020235487A1 (ja) * | 2019-05-23 | 2020-11-26 | 東レ株式会社 | プリプレグ、積層体および成形品 |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP4282644A4 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP7088433B1 (ja) | 2022-06-21 |
| TWI888690B (zh) | 2025-07-01 |
| US20240066758A1 (en) | 2024-02-29 |
| TW202241694A (zh) | 2022-11-01 |
| KR102763715B1 (ko) | 2025-02-07 |
| EP4282644B1 (en) | 2025-11-19 |
| EP4282644A1 (en) | 2023-11-29 |
| CN116761713A (zh) | 2023-09-15 |
| EP4282644A4 (en) | 2024-10-30 |
| KR20230135056A (ko) | 2023-09-22 |
| US12558816B2 (en) | 2026-02-24 |
| JPWO2022158222A1 (enExample) | 2022-07-28 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| TWI860362B (zh) | 預浸漬物、積層體及成形品 | |
| JP7803040B2 (ja) | プリプレグ、積層体および一体化成形品 | |
| JP7647099B2 (ja) | プリプレグ | |
| TWI861288B (zh) | 複合預浸漬物及其製造方法 | |
| JP7524763B2 (ja) | プリプレグ、積層体および成形品 | |
| JP7615683B2 (ja) | プリプレグ、積層体および成形品 | |
| TWI857059B (zh) | 纖維強化樹脂基材、一體成形品及纖維強化樹脂基材之製造方法 | |
| JP7180790B2 (ja) | プリプレグ、繊維強化樹脂成形体および一体化成形品 | |
| TWI871380B (zh) | 預浸漬物、成形體及一體成形體 | |
| JP7088433B1 (ja) | プリプレグ、成形体および一体化成形体 | |
| JP7088320B2 (ja) | プリプレグ、積層体および一体化成形品 | |
| JP7676777B2 (ja) | プリプレグ、積層体および一体化成形品 | |
| JP2020193336A (ja) | 成形材料および成形品 | |
| JP2026129247A (ja) | 中間基材、繊維強化樹脂成形体および繊維強化樹脂成形体の製造方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| ENP | Entry into the national phase |
Ref document number: 2022502064 Country of ref document: JP Kind code of ref document: A |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 21921323 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202180085543.6 Country of ref document: CN |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 18270013 Country of ref document: US |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| ENP | Entry into the national phase |
Ref document number: 2021921323 Country of ref document: EP Effective date: 20230821 |
|
| WWG | Wipo information: grant in national office |
Ref document number: 2021921323 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |