WO1995004837A1 - Al-cu-li alloys with improved cryogenic fracture toughness - Google Patents
Al-cu-li alloys with improved cryogenic fracture toughness Download PDFInfo
- Publication number
- WO1995004837A1 WO1995004837A1 PCT/US1994/008876 US9408876W WO9504837A1 WO 1995004837 A1 WO1995004837 A1 WO 1995004837A1 US 9408876 W US9408876 W US 9408876W WO 9504837 A1 WO9504837 A1 WO 9504837A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- alloy
- weight percent
- cryogenic
- fracture toughness
- aluminum
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22F—CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS
- C22F1/00—Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working
- C22F1/04—Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working of aluminium or alloys based thereon
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C21/00—Alloys based on aluminium
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C21/00—Alloys based on aluminium
- C22C21/12—Alloys based on aluminium with copper as the next major constituent
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22F—CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS
- C22F1/00—Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working
- C22F1/04—Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working of aluminium or alloys based thereon
- C22F1/057—Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working of aluminium or alloys based thereon of alloys with copper as the next major constituent
Definitions
- Patent Application No. 08/032,158 filed March 12, 1993, which is a continuation of U.S. Application No. 07/493,255 filed March 14, 1990, which is a
- the present invention relates to
- alloys are provided that exhibit improved fracture toughness and strength at low
- Aluminum-copper-lithium alloys are under
- launch vehicles are constructed primarily from Aluminum Association registered alloys 2014 (Titan) and 2219 (Space Shuttle External Tank). Most of the dry weight of such launch systems, i.e., excluding propellent, is in propellant containment.
- the preferred propellant system is liquid hydrogen and liquid oxygen, which are each cryogenic liquids. It is therefore important for the structural alloy for such propellant containment to have both high strength and high toughness at cryogenic service temperatures. Furthermore, it is particularly advantageous for the alloy to have substantially equal or greater strength and toughness at cryogenic
- AA Aluminum Association
- Alloy 2020 has a nominal composition, in weight percent, of Al - 4.5Cu - 1.1Li - 0.5Mn - 0.2Cd and was registered in the 1950's. Although the alloy possessed a relatively low density and developed high strength, it also possessed very low levels of fracture toughness and ductility. These problems along with processing difficulties led to the withdrawal of the alloy from the Aluminum Association register.
- Alloy 2090 comprising Al - (2.4-3.0)Cu - (1.9-2.6)Li - (0-0.25)Mg - 0.12Zr was designed as a low density replacement for high strength alloys such as 2024 and 7075. Although this alloy develops relatively high strength, it also possesses poor short transverse fracture toughness and poor short transverse ductility associated with delamination problems and has not yet had wide range commercial success.
- Alloy 2091 comprising Al - (1.8-2.5)Cu -
- Alloy 8090 comprising Al - (1.0-1.6)Cu - (2.2-2.7) Li - (0.6-1.3)Mg - 0.12Zr was designed for aircraft applications in which exfoliation corrosion resistance and damage tolerance were required.
- alloy 8090's limited strength capability and poor fracture toughness have prevented the alloy from becoming a widely accepted alloy for aerospace and aircraft applications.
- Alloy 2094 comprises Al - (4.4-5.2)Cu - (0.8- 1.5)Li - (0.25-0.6)Mg - (0.25-0.6)Ag - 0.25max.Zn - O.lmax.Mn - (0.04-0.18) Zr, while alloy 2095 comprises Al - (3.9-4.6)CU - (1.0-1.6)Li - (0.25-0.6)Mg - (0.25-0.6)Ag - 0.25max.Zn - O.lOmax.Mn - (0.04-0.18) Zr. Alloy 2195 is similar to alloy 2095, but has slightly lower Cu and Li limits. These alloys possess
- compositional ranges that exhibit improved combinations of cryogenic fracture toughness and strength when processed in accordance with the method
- An object of the present invention is to provide a method of producing an aluminum-copper-lithium alloy that possesses improved fracture toughness and strength at cryogenic temperatures in comparison to room
- Another object of the present invention is to provide a method of increasing the cryogenic fracture toughness and strength of an aluminum-base alloy, the method comprising the steps of providing a solution heat treated and quenched aluminum-base alloy within certain compositional ranges, working the alloy and artificially aging the alloy a sufficient amount to produce the desired increase in strength and fracture toughness at cryogenic temperatures.
- Another object of the present invention is to provide an aluminum-copper-lithium alloy having improved fracture toughness and strength at cryogenic temperatures in comparison to room temperature.
- Another object of the present invention is to provide a wrought aluminum-base alloy having increased cryogenic fracture toughness and strength, wherein the alloy is worked and artificially aged a sufficient amount to achieve the desired increase in fracture toughness and strength at cryogenic temperatures.
- the amounts of copper, lithium and other elements present in the alloy are controlled in order to achieve the desired improvement in properties at cryogenic temperatures.
- Another object of the present invention is to provide a container for holding cryogenic materials such as liquid hydrogen, liquid oxygen, and liquid nitrogen, wherein the container is made of an aluminum-copper-lithium alloy that possesses improved fracture toughness and strength at cryogenic service
- a method for producing an improved aluminum-based alloy comprising the steps of: a) providing a solution heat treated and
- quenched aluminum-base alloy consisting essentially of from 2.0 to 6.5 weight percent Cu, from 0.2 to 2.7 weight percent Li, and the balance aluminum and incidental impurities; and b) at least one of working and artificially aging said alloy in an amount sufficient to provide strength and fracture toughness to said alloy at cryogenic temperature substantially equal to or greater than the strength and fracture toughness at room temperature.
- a wrought aluminum-base alloy consisting essentially of from 2.8 to 4.8 weight percent Cu, from 0.4 to 1.5 weight percent Li, from 0.2 to 1.0 weight percent Mg, and the balance aluminum and incidental impurities, wherein said alloy is worked, artificially aged, or worked and artificially aged an amount sufficient to provide strength and fracture toughness to said alloy at cryogenic temperature substantially equal to or greater than the strength and fracture toughness at room temperature.
- a cryogenic material-holding container made from an alloy
- alloy consisting essentially of from 2.8 to 4.5 weight percent Cu, from 0.4 to 1.5 weight percent Li, from 0.2 to 1.0 weight percent Mg, and the balance aluminum and incidental impurities, wherein said alloy is worked, artificially aged, or worked and artificially aged an amount sufficient to provide strength and fracture toughness to said alloy at cryogenic temperature substantially equal to or greater than the strength and fracture toughness at room temperature.
- Figure 1 is a graph of fracture toughness versus yield strength for an alloy at room temperature and at cryogenic temperature. The graph demonstrates that fracture toughness of the alloy increases at cryogenic temperature when the alloy is artificially aged to a lower yield strength, but cryogenic fracture toughness decreases relative to that at room temperature when the alloy is artificially aged to a higher yield strength.
- Figure 2 is a graph of fracture toughness versus lithium content for alloys at room temperature and at cryogenic temperature. The graph shows an increase in cryogenic versus room temperature fracture toughness for alloys having a lower lithium content, but no discernable increase in cryogenic fracture toughness for alloys having a higher lithium content.
- Figure 3 is a graph of fracture toughness versus magnesium (Mg) content for alloys at room temperature and at cryogenic temperature. The graph shows an increase in cryogenic versus room temperature fracture toughness for all of the alloys.
- Figure 4 is a graph of fracture toughness versus temperature for an alloy that has been stretched various amounts. The graph demonstrates a decrease in cryogenic versus room temperature fracture toughness when the alloy is stretched a lesser amount, but an increase in cryogenic fracture toughness when the alloy is stretched a greater amount.
- Figure 5 is a graph of fracture toughness versus percentage of stretch for an alloy at room temperature and at cryogenic temperature. The graph shows a decrease in cryogenic versus room temperature fracture toughness at lower stretch levels, but an increase in cryogenic fracture toughness at higher stretch levels.
- Figure 6 is a graph of fracture toughness versus aging temperature for an alloy at room temperature and at cryogenic temperature. The graph shows that both room temperature and cryogenic fracture toughness increase as aging temperature decreases.
- Figure 7 is a graph of fracture strength versus temperature for an alloy of the present invention that has been stretched varying amounts.
- fracture strength versus temperature for a conventional alloy is shown.
- the graph demonstrates an increased improvement in cryogenic fracture strength when this alloy of the present invention is stretched a greater amount.
- a significant improvement in both strength and fracture toughness of the present alloy in comparison to the conventional alloy is shown.
- the present invention relates to the control of composition, fabrication and heat treating of
- a wrought aluminum-copper-lithium alloy in which fracture toughness at cryogenic temperatures is higher than, or equal to, that at room temperature.
- strength at cryogenic temperatures is higher than that at room temperature.
- the desirable trend can be attained by controlling the levels of copper and lithium in the alloys, and by controlling processing parameters such as stretch, aging and recrystallization of the alloys.
- cryogenic temperature is defined in accordance with the present invention to include temperatures significantly below room temperature and typically below 0°C. Thus, the temperatures at which hydrogen (-253°C), oxygen (-183°C) and nitrogen
- cryogenic temperatures For purposes of experimental evaluation, a temperature of -196°C is considered as a cryogenic temperature. Room temperature is defined in accordance with its common usage and includes temperatures of from about 20 to about 25°C. For purposes of experimental evaluation, a .temperature of 25°C is considered to be room temperature.
- the alloys of the present invention may, in certain aspects, in certain
- preferred embodiments contain magnesium, silver, zinc, and combinations thereof, along with other alloying elements such as grain refiners, dispersoid forming elements and nucleation aids.
- alloying elements such as grain refiners, dispersoid forming elements and nucleation aids.
- Compositional ranges of the alloying additions of the present alloys are given below in Table 1. Unless stated otherwise, all
- composition values herein are in weight percent.
- alloying additives such as Zr, Ti, Cr, Mn, Hf, Nb, B, Fe, Y, La, V, Mo, Se, Co, Ni, Cd, In, Sn, Ge and combinations thereof may be included in amounts up to a total of about 10 weight percent as long as such additions do not significantly impair the attainment of the desirable cryogenic fracture toughness trend.
- Grain refiners such as Zr, Ti, Cr, Mn, Hf, Nb, B, V and TiB 2 may be included in a preferred total amount of from about 0.01 to about 1.0 weight percent and more
- grain refining elements and/or dispersoid forming elements may be increased in excess of 1.0% when powder metallurgy processing is employed, e.g., rapid solidification, mechanical alloying, and reaction milling.
- Zirconium and titanium are particularly preferred as grain refining additions, with Zr also being beneficial as a recrystallization inhibitor.
- alloys were prepared having compositions as set forth in Table 2. Although not listed in Table 2, aluminum makes up the balance of each composition.
- each of the above listed compositions was prepared as follows.
- the alloys were cast as 23 kilogram (50 lb.), 16.5-cm
- alloys range from about 3 to about 9 percent, with from about 4.5 to about 7 percent generally being more preferred, depending on the alloy composition, the geometry of the part, and other processing parameters.
- Working of the alloys is typically carried out at room temperature (cold work), but both cryogenic and warm temperatures may be suitable.
- Artificial aging temperatures may vary, with temperatures of less than about 120°C to greater than about 180°C being satisfactory for most alloys.
- Aging times are dependent on aging temperature and may extend up to a point at which the length of time becomes impractical. Aging times of from about 0.25 to about 500 hours may typically be used, with from about 2 to about 48 hours being preferred, and about 4 to about 24 hours being most preferred, depending on the alloy composition and other processing parameters.
- the alloys of the present invention are typically cast into ingot form or billet form.
- the term "ingot” as used herein is broadly defined as a solid mass of alloy material.
- the term “billet” as used herein includes hot worked, semi-finished products suitable for subsequent working by such methods as rolling, extruding, forging, etc. While the formation of ingots or billets of the present alloys by casting techniques is preferred, the alloys may also be provided in ingot or billet form consolidated from fine powders or particulates.
- the powder or particulate material can be produced by such processes as atomization,
- the alloys of the present invention may be any alloys of the present invention.
- wrought alloy as used herein is defined as a product that has been subjected to mechanical working by such processes as extruding, rolling, forging, spin-forming and the like.
- sheet is defined in accordance with the present invention as a rolled product having a generally rectangular cross section with a thickness of from about 0.006 to about 0.249 inch, and having sheared, slit or sawed edges.
- plate is defined in a similar manner as sheet, with the exception that the thickness is about 0.250 inches or greater.
- Alloy A was aged to a higher strength level than in Example 1, i.e., aged at 160°C for 24 hours, giving a 20°C YS of 98.7 ksi, UTS of 101.5 ksi and elongation of 5.4%. Fracture toughness at 20°C at this higher strength level is quite low at 13.4 ksivin. This toughness is sufficiently low such that the alloy would not be competitive for toughness-critical applications at this strength level. Consequently, toughness at -196°C was not measured, but the cryotoughness trend would be expected to be undesirable.
- Alloy B was processed similarly to Alloy A in the preceeding examples. Alloy B has a similar composition to that of Alloy A, except that Cu content is
- Alloy B's 20°C fracture toughness is also higher at a K Ic of 22.3 ksivin at this higher strength level. This is significant because the alloy was aged 5 ksi stronger than Alloy A in Example 1, where the toughness at 20°C was only 18.6 ksivin.
- Alloy B was aged for 16 hours at 160°C as in
- Example 3 but was stretched 5% instead of 3%. By stretching 5%, aging kinetics are increased such that artificial aging for 16h at 160°C now gives peak strength (103 ksi YS, 105 ksi UTS with 6% el).
- Fracture toughness at 20°C is 20.2 ksivin at this ultra-high strength level.
- the desirable trend is achieved at an extremely high strength level by lowering the Cu to 4.52% and increasing the stretch level to 5%.
- Alloy C is similar to Alloys A and B but has a Cu content of 4.13%.
- SHT 511°C for 1h, WQ, stretched 3% and aged for 12h at 160°C it is slightly weaker in the T8 temper at 94 ksi YS and 98 ksi UTS, but has better 20°C fracture toughness than that of the 4.52% Cu Alloy B, i.e., 24.5 instead of 22.3 ksivin.
- YS increases to 115 ksi, but fracture toughness decreases to 19.3 ksivin (see Figure 1).
- the decrease in Cu to 4.13% increases toughness at 20°C at the 3% stretch level
- the desirable cryogenic fracture toughness trend is not achieved at the 94 ksi YS level.
- Alloy C is underaged to a 20°C YS of 89 ksi, at which point the onset of the desirable trend is
- Alloy D is similar in composition to alloy B except that the Li content is slightly lower. Part of this extrusion was stretched 3% and part 6%. The desirable trend is just about attained at a 20°C YS of 88 ksi at the 3% stretch level, but it is reached very easily at the 93 ksi 20°C YS level with 6% stretch (see Table 3). Furthermore, the desirable trend is almost achieved at 98.5 ksi YS. The desirable trend is more readily achieved because of the higher stretch level and, in addition, the lower Li content which will be further illustrated later.
- Alloy E is similar in composition to Alloy A except that Alloy E is Ag-free. Alloy E's peak 20°C strength with 3% stretch can be attained by aging for 16h at 160°C (95.2 ksi YS, 98.3 ksi UTS and 6% el). The peak strength of Alloy E is slightly lower than that of Alloy A because of the absence of Ag in Alloy
- Toughness at 20°C is 16.9 ksivin, decreasing slightly to 16.6 ksivin at -196°C.
- This toughness can be increased with only a slight strength penalty by underaging, e.g., aging for 6h at 160°C, producing a YS of 94.2 ksi, UTS of 98.6 ksi, elongation of 7.9% and Kg of 25.4 ksivin at 20°C.
- the properties at -196°C are 111 ksi YS, 123 ksi UTS, 7.5% el and K Q of 23.0 ksivin. The desirable trend is not quite achieved in either case.
- Alloy F is similar in composition to Alloy E, but is significantly lower in Cu and Li content (see Table 2).
- the decrease in solute produces a lower peak YS at 20°C of 90 ksi compared to that of Alloy E.
- 20°C properties are 88.1 ksi YS, 90.8 ksi UTS, 10.5% el and 39.4 ksivin toughness.
- toughness increases to 47.1 ksivin, an excellent example of the desirable trend.
- Alloy G is similar in composition to Alloy A (high Cu content) but has a lower Li content of 1.0% (see Table 2).
- Alloy A 370°C preheat temperature for extrusion, 504°C SHT, WQ, stretch 3% and age for 16h at 160°C
- similar tensile properties to those of Alloy A are obtained, but with higher toughness. That is, at 25°C, a YS of 103 ksi, UTS of 105 ksi, elongation of 3.8% and K Ic of 18.7 ksivin are obtained.
- This toughness is higher than the 13.4 ksivin attained for Alloy A at the ultra-high strength level (see Example 2).
- This example examines the effect of Li content on the desirable cryogenic toughness trend.
- the alloys were then tested for fracture toughness at various strength levels at 25 and -196°C. At 25°C, strength-toughness combinations clearly improve with increasing Mg content. At -196°C, strength-toughness combinations improve by raising the Mg content from 0.2 to 0.4wt%. At 0.6wt% Mg, the data vary more, but also show higher toughness and the desirable trend.
- Al-4.9Cu-1.15Li-0.4Ag-0.4Mg-0.14Zr was cast and extruded at a preheat temperature of 370°C (700°F) in a 16.2-cm (6.375-inch) diameter container at a nominal ram speed of 0.25 cm/s (0.1 in/s) into 5.1 ⁇ 1.9 cm (2 ⁇ 0075 inch) rectangular bar.
- the extrusion was solution heat treated at 504°C for 3/4h, water quenched at 25°C, and a portion of the bar was removed (with 0% stretch). The remaining bar was then stretched 1.5%, a piece was cut off, stretched again with material cut off, and this procedure was repeated giving sections with stretch levels of 0, 1.5, 4, 7 and 9.5%.
- the artificial aging response was determined for each stretch level and portions of each extrusion were heat treated to a 20°C YS of 88 ksi. Plane strain fracture toughness from fatigue precracked CT specimens was measured at each stretch level at 20°C and -196°C.
- the high 25°C toughness of 38.9 ksivin increases to 43.6 ksivin at -196°C, an excellent example of the desirable cryogenic toughness trend. Toughness could be increased further by lowering the Cu and/or Li content.
- Alloy T is similar in composition to Alloy S, except that the Zn content is roughly doubled to 0.40%.
- the alloy was aged for 28 hours at 143°C, which is slightly further along the aging curve than the
- Alloy K having a composition of Al-4.19Cu-1.21Li-0.37Ag-0.38Mg-0.14Zr-0.04Ti was cast, extruded, solutionized, quenched and stretched 6% as described in Example 11. Samples were then
- Another sample was aged at 143°C for 22 hours to attain a 25°C YS of 90.7 ksi, a UTS of 94.9 ksi, an elongation of 10.1% and a K Q of 31.9 ksivin.
- this sample attained a YS of 108.7 ksi, a UTS of 116.0 ksi, an elongation of 9.4% and a K Q of 31.0 ksivin.
- a third sample was aged at 160°C for 4.5 hours to attain a 25°C YS of 91.0 ksi, a UTS of 94.4 ksi, an elongation of 7.7% and a K Q of 28.4 ksivin.
- Alloy U having a composition of Al-4.0Cu-1.0Li-0.4 Ag-0.4Mg-0.14Zr (virtually the same as Alloy J) was cast and rolled to 9.5 mm (0.375 in.) plate, solution heated at 510°C (950°F), quenched in water at 20°C and either stretched 3% or 6%. Plate at each stretch level was aged at 143°C to a 20°C YS of 85 ksi. The plates were machined down to 2.0 mm to simulate anticipated flight gages for the External Tank of the Space
- both stretch levels display a significant toughness advantage over 2219-T87, the alloy currently used on the Space Shuttle External Tank.
- the variant with 6% stretch has a 69% advantage over 2219 at a test temperature of 4K, which could translate directly to a structural weight savings in the tank membranes of that gage. It is noted that both stretch levels show the desirable trend for the 2.0 mm gage and that toughness increases with stretch level as was shown in the previous examples for extrusions.
- Alloy V comprising Al-3.62Cu-0.99Li-0.35Ag- 0.36Mg-0.15Zr-0.04Ti, falls within the most preferred compositional range of the present invention.
- the alloy With 6% stretch and artificial aging at 143°C for 26 hours, the alloy attains room temperature properties of 90.0 ksi YS, 91.5 ksi UTS, 8.7% elongation and 38.7 ksivin K Ic .
- the alloy attains properties of 114.8 ksi YS, 120.0 ksi UTS, 9.6% elongation and 40.7 ksivin K Ic (see Table 3), i.e., the desirable cryogenic fracture toughness trend is obtained.
- Alloy W comprising Al-3.61Cu-0.91Li-0.33Mg-0.39Zn-0.15Zr-0.04Ti, was stretched 6% and artificially aged at 143°C for varying lengths of time as shown in Table 3.
- This alloy attains a peak strength of about 90 ksi, which is attained by aging for 26 hours at 143 °C.
- strength does not change significantly for longer aging times.
- increasing the aging time by about 70% to 44 hours only over-ages the alloy very slightly as 25°C YS decreases to about 89 ksi (See Table 3).
- this increased aging has an adverse effect on the cryogenic fracture toughness trend.
- Table 3 the desirable cryogenic fracture toughness trend is essentially attained at the shorter aging time but is not attained at the longer aging time.
- Alloys X and Y are Ag-free and contain Zn (see Table 2). As shown in Table 3, the room temperature strengths of these alloys are quite high, especially considering the relatively low alloying content of these alloys. Furthermore, the room temperature plane strain fracture toughnesses are well above 50 ksivin. The toughnesses of these alloys are so high that valid L-T K Ic toughness values are not obtained with the 2 ⁇ 3/4 inch extruded bar samples. Each of Alloys X and Y are capable of attaining the desirable cryogenic fracture toughness trend. EXAMPLE 21
- Alloy Z contains 2.16% Cu (see Table 2).
- compositional range of the present invention (see Table 2). As shown in Table 3, high strengths are obtained at room temperature, especially considering the
- the room temperature plane strain fracture toughness is above 50 ksivin. However, since the toughness is so high, valid L-T K Ic toughness values are not obtained with the 2 ⁇ 3/4 inch extruded bar samples. Alloy AA is readily capable of attaining the desirable cryogenic fracture toughness trend.
- Alloy BB and CC contain 0.29% Li and 0.56% Li, respectively. Otherwise, the alloys are very similar in composition (see Table 2). Alloy BB, containing the lower amount of Li, possesses significantly decreased room temperature strengths compared to Alloy CC, as shown in Table 3. Although each alloy could attain the desirable cryogenic fracture toughness trend, the lower Li content of alloy BB causes the alloy to have much lower strengths than alloy CC, and alloys in
- Alloy DD is similar in composition to alloy s, except that it is Zn free and has a lower Cu content of 3.41% and a higher Li content of 1.12%. It was
- Alloy EE is similar in composition to alloy D, and has the composition Al - 4.47 Cu - 0.95 Li - 0.43 Ag - 0.43 Mg - 0.14 Zr - 0.02 Ti. It was processed
- a section of the bar was stretched 3% and aged at 160°C for 6 hours, providing a 25°C longitudinal YS of 86.5 ksi and L-T K Ic of 40.7 ksi vin. These increased at -196°C to 106.2 ksi YS and 49.3 ksi K Ic ,
- composition FF Al - 4.99 Cu - 1.23 Li - 0.38 Ag - 0.46 Mg - 0.17 Zr - 0.04 Ti
- composition GG Al - 5.20 Cu - 1.00 Li - 0.40 Ag - 0.16 Zr. Plane strain fracture toughness was measured from compact tension specimens orientated with crack
- the desirable cryogenic fracture toughness trend can be achieved by controlling Cu and Li levels. Copper levels of from about 3.0 to about 4.5% and lithium levels of from about 0.7 to about 1.1% are most
- the desirable trend can be achieved for copper levels of from about 2.0 to about 6.5% and lithium levels of from about 0.2 to about 2.7%.
- Cu levels of 2.8 to 4.8% and Li levels of 0.4 to 1.5% are more preferred.
- the combined cryogenic fracture toughness and strength properties are maximized, making such alloys highly superior for cryogenic use.
- One particularly preferred alloy for cryogenic use comprises 4.0% Cu and 1.0% Li, while another highly preferred alloy comprises 4.5% Cu and 0.8% Li.
- the amounts of Cu and Li employed are interdependent.
- the level of lithium should be close to about 1.0% to achieve the desirable cryogenic fracture toughness trend at high strength levels
- the level of lithium should be close to about 1.0% to achieve the desirable cryogenic fracture toughness trend at high strength levels
- the level of lithium is at the low end of the broad range, e.g., 0.2%
- the level of copper can be relatively high and the desirable trend can be achieved, but strength will be lower than at higher Li levels of about 1%, as shown by Alloy BB (see Table 3).
- lower Cu levels such as 2% are preferred in order to attain the desirable trend.
- Copper and lithium levels have a significant effect on the strength levels attained in the present alloys. Copper levels above about 4% produce the highest strengths, with significant decreases in strength below about 3% (see Alloy Z in Table 3). In addition, the highest strengths are attained with Li levels of from about 1.05 to about 1.35%, with a peak at about 1.2% lithium. Significant decreases in strength result below about 0.5% and above about 1.5%
- the amount of copper and lithium used also affects the processing that must be employed to achieve the desired trend. For example, at the most preferred levels of about 4.0% copper and 1.0% lithium, little or no stretch may be required to achieve the desired trend at high strength levels. However, as the boundaries of the copper and lithium ranges are reached, optimal amounts of stretch and carefully controlled artificial aging treatments may be required in order to produce the desired cryogenic fracture toughness trend at technologically useful strength levels.
- the amount of magnesium used in the present alloys has only a minor effect on the cryogenic fracture toughness trend.
- the strength of the alloys is highly dependent on Mg content, with peak strengths being attained at Mg levels of from about 0.3 to about 0.6 percent.
- increasing the Mg content to levels of about 0.6 to about 1.0% increases the
- the presence or absence of silver in the alloys of the present invention does not significantly affect the cryogenic fracture toughness trend.
- Ag produces an improvement in strength.
- cryogenic fracture toughness trend, strength levels and aging kinetics may be increased with the addition of minor amounts of Zn (see Alloys S, T, W, X and Y in Table 3).
- additions of Zn and/or Ag do not adversely affect the ability to attain the
- the amount of stretch employed in accordance with the present invention has a significant effect on cryogenic fracture toughness and the ability to attain the desirable trend. In general, greater amounts of stretch result in an improved cryogenic fracture toughness trend.
- a given Al-Cu-Li alloy a
- the amount of stretch employed is also dependent upon the degree of artificial aging used, as more fully
- underaging The degree of underaging required is dependent upon alloy composition and processing history. For example, at a preferred copper level of 4% and lithium level of 1%, or 4.5% copper and 0.8% lithium, for a technologically wide range of stretch levels, underaging may not be required and the desirable trend can be achieved at peak
- underaging treatment is to artificially age the alloy to a yield strength that is at least about 5 ksi below the peak yield strength of the alloy. Such underaging has been found to significantly promote the desirable cryogenic fracture toughness trend. To attain the desirable trend with greater safety margin in a
- the alloys of the present invention can attain such high peak strengths because technologically useful strengths can still be achieved with significant underaging.
- cryogenic fracture toughness trend can be significantly affected by the amount of recrystallization.
- unrecrystallized plate tends to promote the desired cryogenic toughness trend while recrystallized plate tends to decrease the ease with which the desired trend can be attained after solution heat treatment,
- unrecrystallized microstructure is desirable for increased fracture toughness at a given temperature. It may therefore be desirable to, for example, roll the alloy at higher temperatures at which recrystallization is less likely to occur than at lower temperatures at which recrystallization may be induced. For products with higher amounts of recrystallization, a greater degree of underaging and/or a greater amount of stretch is generally necessary to attain the desirable
- Alloys of the present invention may be rolled, extruded and forged to the product forms necessary to fabricate a container for holding cryogenic materials.
- a cryogenic tank when used for holding cryogenic liquids such as liquid hydrogen, oxygen or nitrogen, generally consists of the barrel, which is a hollow cylinder, the domes, which are approximately
- the barrel may be fabricated from plate that has been processed in accordance with the present invention and which is subsequently machined so that it has longitudinal T- shaped or L-shaped stiffeners.
- the barrel may be fabricated from integrally-stiffened extrusions which have the T-shaped or L-shaped
- the ring can be formed from extrusions that are bent over a curved tool and welded into a ring, or roll-ring forged, an operation in which a billet is pierced to a doughnut shape and the wall thickness is worked to thinner gages as the diameter increases.
- the domes may be formed from gore panels of plate or sheet that are stretched over a tool and welded together. Alternatively, the dome can be spin-formed from plate at cold, warm, or hot working temperatures.
- cryogenic toughness trend can be introduced during the forming operation after solution heat treatment and quench.
- the plate and extrusion can be simply stretch straightened.
- cold work can be introduced when the gore panels are stretched over a mandrel, the barrel panels are bump formed over a tool, the ring extrusions are bent and stretched over a tool to introduce
- the artificial aging conditions are selected as previously disclosed to ensure that the desirable trend is achieved.
- the tank components may be welded together by virtually any of the conventional welding techniques, including gas tungsten arc welding, dual torch gas tungsten arc welding, metal inert gas welding, variable polarity plasma arc welding, variable polarity gas tungsten arc welding, electron beam welding and others.
- Conventional filler alloys such as 2319 are acceptable, as are parent filler alloys of the present invention.
- parent alloys containing greater amounts of grain refiners, e.g., Zr and Ti, and slightly greater Cu content are often preferred to increase weldment strength.
- the barrel panels are welded together forming a right circular cylinder which is then welded to the ring.
- cryogenic tank typically also has secondary hardware that may be fabricated by forging to asymmetric shapes, i.e., that cannot be stretched.
- These components should contain the more preferred amounts of Cu and Li, e.g., 2.8 - 4.8 Cu and 0.7 - 1.1 Li, to enable the desirable trend to be attained with no stretch, while still maintaining high strength levels. For some forgings, cold work could be practically introduced by shot peening.
- the components of the cryogenic tank can be welded by various parameters depending upon the technique selected.
- a preferred route is to weld the components using conventional gas tungsten arc welding with conventional 2319 filler.
- the surfaces to be welded should preferably be mechanically milled or chemically milled in a 100 g/1 NaOH aqueous solution such that about 0.5 mm of the surface is removed.
- a 75% Ar/25% He inert gas cover at 14 1/min can be used.
- the tank so fabricated can be cost effectively proof tested at room temperature.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Materials Engineering (AREA)
- Mechanical Engineering (AREA)
- Metallurgy (AREA)
- Organic Chemistry (AREA)
- Physics & Mathematics (AREA)
- Thermal Sciences (AREA)
- Crystallography & Structural Chemistry (AREA)
- Materials For Medical Uses (AREA)
- Extrusion Of Metal (AREA)
- Forging (AREA)
- Powder Metallurgy (AREA)
- Heat Treatment Of Steel (AREA)
Priority Applications (7)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| RU96105399A RU2128241C1 (ru) | 1993-08-10 | 1994-08-08 | Al-cu-li-сплавы с улучшенной криогенной вязкостью при разрушении |
| DE69422630T DE69422630T2 (de) | 1993-08-10 | 1994-08-08 | Al-cu-li legierung mit guter bruchzähigkeitseigentschaften bei kryogenischen temperaturen |
| KR1019960700671A KR100330990B1 (ko) | 1993-08-10 | 1994-08-08 | 극저온파괴인성이개선된알루미늄-구리-리튬합금 |
| EP94925755A EP0714453B1 (en) | 1993-08-10 | 1994-08-08 | Al-cu-li alloys with improved cryogenic fracture toughness |
| JP50654295A JP3742884B2 (ja) | 1993-08-10 | 1994-08-08 | 極低温破壊靭性の改良されたAl‐Cu‐Li合金 |
| AU75560/94A AU683296B2 (en) | 1993-08-10 | 1994-08-08 | AL-CU-LI alloys with improved cryogenic fracture toughness |
| NO19960515A NO313641B1 (no) | 1993-08-10 | 1996-02-08 | Anvendelse av Al-Cu-Li legeringer med forbedret kryogen bruddseighet |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US08/103,662 | 1993-08-10 | ||
| US08/103,662 US5455003A (en) | 1988-08-18 | 1993-08-10 | Al-Cu-Li alloys with improved cryogenic fracture toughness |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1995004837A1 true WO1995004837A1 (en) | 1995-02-16 |
Family
ID=22296371
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US1994/008876 Ceased WO1995004837A1 (en) | 1993-08-10 | 1994-08-08 | Al-cu-li alloys with improved cryogenic fracture toughness |
Country Status (13)
| Country | Link |
|---|---|
| US (1) | US5455003A (enExample) |
| EP (1) | EP0714453B1 (enExample) |
| JP (1) | JP3742884B2 (enExample) |
| KR (1) | KR100330990B1 (enExample) |
| AU (1) | AU683296B2 (enExample) |
| BR (1) | BR9407224A (enExample) |
| CA (1) | CA2167847A1 (enExample) |
| DE (1) | DE69422630T2 (enExample) |
| ES (1) | ES2141250T3 (enExample) |
| NO (1) | NO313641B1 (enExample) |
| PT (1) | PT714453E (enExample) |
| RU (1) | RU2128241C1 (enExample) |
| WO (1) | WO1995004837A1 (enExample) |
Cited By (10)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1995028250A1 (en) * | 1994-04-13 | 1995-10-26 | Lockheed Martin Corporation | Al-cu-li weld filler alloy, process for the preparation thereof and process for welding therewith |
| WO2005035810A1 (en) * | 2003-10-03 | 2005-04-21 | Alcoa Inc. | Aluminum-copper-magnesium alloys having ancillary additions of lithium |
| WO2009073794A1 (en) * | 2007-12-04 | 2009-06-11 | Alcoa Inc. | Improved aluminum-copper-lithium alloys |
| WO2010149873A1 (fr) * | 2009-06-25 | 2010-12-29 | Alcan Rhenalu | Alliage aluminium cuivre lithium a resistance mecanique et tenacite ameliorees |
| FR2969177A1 (fr) * | 2010-12-20 | 2012-06-22 | Alcan Rhenalu | Alliage aluminium cuivre lithium a resistance en compression et tenacite ameliorees |
| EP2561109A4 (en) * | 2010-04-20 | 2014-08-27 | Alcoa Inc | HIGH-FIXED FORGED ALUMINUM ALLOY PRODUCTS |
| KR101437243B1 (ko) | 2009-09-04 | 2014-09-03 | 알코아 인코포레이티드 | 방탄 성능을 개선하기 위한 알루미늄 합금 에이징 방법 |
| EP3012338A1 (en) * | 2014-10-26 | 2016-04-27 | Kaiser Aluminum Fabricated Products, LLC | High strength, high formability, and low cost aluminum lithium alloys |
| EP2766503B1 (fr) | 2011-10-14 | 2016-12-07 | Constellium Issoire | Procédé de transformation amélioré de tôles en alliage al-cu-li |
| EP3384061B1 (fr) | 2015-12-04 | 2020-02-05 | Constellium Issoire | Alliage aluminium cuivre lithium à resistance mécanique et tenacité ameliorées |
Families Citing this family (47)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5983099A (en) * | 1996-06-11 | 1999-11-09 | Qualcomm Incorporated | Method/apparatus for an accelerated response to resource allocation requests in a CDMA push-to-talk system using a CDMA interconnect subsystem to route calls |
| US6168067B1 (en) * | 1998-06-23 | 2001-01-02 | Mcdonnell Douglas Corporation | High strength friction stir welding |
| RU2163940C1 (ru) * | 1999-08-09 | 2001-03-10 | Государственное предприятие "Всероссийский научно-исследовательский институт авиационных материалов" | Сплав на основе алюминия и изделие, выполненное из него |
| US6562154B1 (en) | 2000-06-12 | 2003-05-13 | Aloca Inc. | Aluminum sheet products having improved fatigue crack growth resistance and methods of making same |
| US6869490B2 (en) * | 2000-10-20 | 2005-03-22 | Pechiney Rolled Products, L.L.C. | High strength aluminum alloy |
| DE10053664A1 (de) | 2000-10-28 | 2002-05-08 | Leybold Vakuum Gmbh | Mechanische kinetische Vakuumpumpe |
| CN100491579C (zh) * | 2003-03-17 | 2009-05-27 | 克里斯铝轧制品有限公司 | 制造整体单块铝结构的方法和由这种结构机加工的铝制件 |
| GB0425152D0 (en) * | 2004-11-15 | 2004-12-15 | Middlesex Silver Co Ltd | Fabric structure |
| CA2608971C (fr) | 2005-06-06 | 2014-09-16 | Alcan Rhenalu | Tole en aluminium-cuivre-lithium a haute tenacite pour fuselage d'avion |
| FR2889542B1 (fr) * | 2005-08-05 | 2007-10-12 | Pechiney Rhenalu Sa | Tole en aluminium-cuivre-lithium a haute tenacite pour fuselage d'avion |
| CN101189353A (zh) * | 2005-06-06 | 2008-05-28 | 爱尔康何纳吕公司 | 用于飞机机身的高韧度的铝-铜-锂合金板材 |
| US20100102049A1 (en) * | 2008-10-24 | 2010-04-29 | Keegan James M | Electrodes having lithium aluminum alloy and methods |
| FR2938553B1 (fr) * | 2008-11-14 | 2010-12-31 | Alcan Rhenalu | Produits en alliage aluminium-cuivre-lithium |
| US8333853B2 (en) * | 2009-01-16 | 2012-12-18 | Alcoa Inc. | Aging of aluminum alloys for improved combination of fatigue performance and strength |
| CA2793885C (en) | 2010-04-12 | 2016-03-15 | Howmet Aerospace Inc. | 2xxx series aluminum lithium alloys having low strength differential |
| FR2960002B1 (fr) | 2010-05-12 | 2013-12-20 | Alcan Rhenalu | Alliage aluminium-cuivre-lithium pour element d'intrados. |
| US9347558B2 (en) | 2010-08-25 | 2016-05-24 | Spirit Aerosystems, Inc. | Wrought and cast aluminum alloy with improved resistance to mechanical property degradation |
| KR101226484B1 (ko) | 2010-10-29 | 2013-01-25 | 국방과학연구소 | 인듐을 첨가한 2090 알루미늄 합금의 다단 열처리 방법 |
| US12565695B2 (en) * | 2011-02-17 | 2026-03-03 | Arconic Technologies Llc | 2XXX series aluminum lithium alloys |
| FR2989387B1 (fr) | 2012-04-11 | 2014-11-07 | Constellium France | Alliage aluminium cuivre lithium a resistance au choc amelioree |
| US9458528B2 (en) * | 2012-05-09 | 2016-10-04 | Alcoa Inc. | 2xxx series aluminum lithium alloys |
| US20140050936A1 (en) * | 2012-08-17 | 2014-02-20 | Alcoa Inc. | 2xxx series aluminum lithium alloys |
| US10266933B2 (en) | 2012-08-27 | 2019-04-23 | Spirit Aerosystems, Inc. | Aluminum-copper alloys with improved strength |
| FR3004197B1 (fr) | 2013-04-03 | 2015-03-27 | Constellium France | Toles minces en alliage d'aluminium-cuivre-lithium pour la fabrication de fuselages d'avion. |
| FR3004464B1 (fr) | 2013-04-12 | 2015-03-27 | Constellium France | Procede de transformation de toles en alliage al-cu-li ameliorant la formabilite et la resistance a la corrosion |
| FR3007423B1 (fr) | 2013-06-21 | 2015-06-05 | Constellium France | Element de structure extrados en alliage aluminium cuivre lithium |
| FR3014448B1 (fr) | 2013-12-05 | 2016-04-15 | Constellium France | Produit en alliage aluminium-cuivre-lithium pour element d'intrados a proprietes ameliorees |
| FR3026747B1 (fr) * | 2014-10-03 | 2016-11-04 | Constellium France | Toles isotropes en alliage d'aluminium-cuivre-lithium pour la fabrication de fuselages d'avion |
| CN105345308B (zh) * | 2015-10-29 | 2020-01-10 | 中国航发北京航空材料研究院 | 一种用于Al-Cu-Li系铝锂合金和Al-Cu系铝合金的焊丝 |
| FR3047253B1 (fr) | 2016-02-03 | 2018-01-12 | Constellium Issoire | Toles epaisses en alliage al - cu - li a proprietes en fatigue ameliorees |
| US20210207254A1 (en) | 2016-02-09 | 2021-07-08 | Aleris Rolled Products Germany Gmbh | Al-Cu-Li-Mg-Mn-Zn ALLOY WROUGHT PRODUCT |
| EP3577246A1 (en) | 2017-01-31 | 2019-12-11 | Universal Alloy Corporation | Low density aluminum-copper-lithium alloy extrusions |
| FR3065011B1 (fr) * | 2017-04-10 | 2019-04-12 | Constellium Issoire | Produits en alliage aluminium-cuivre-lithium |
| US20190233921A1 (en) * | 2018-02-01 | 2019-08-01 | Kaiser Aluminum Fabricated Products, Llc | Low Cost, Low Density, Substantially Ag-Free and Zn-Free Aluminum-Lithium Plate Alloy for Aerospace Application |
| FR3080861B1 (fr) | 2018-05-02 | 2021-03-19 | Constellium Issoire | Procede de fabrication d'un alliage aluminium cuivre lithium a resistance en compression et tenacite ameliorees |
| FR3080860B1 (fr) | 2018-05-02 | 2020-04-17 | Constellium Issoire | Alliage aluminium cuivre lithium a resistance en compression et tenacite ameliorees |
| FR3082210B1 (fr) | 2018-06-08 | 2020-06-05 | Constellium Issoire | Toles minces en alliage d’aluminium-cuivre-lithium pour la fabrication de fuselages d’avion |
| CN113039303A (zh) * | 2018-11-07 | 2021-06-25 | 奥科宁克技术有限责任公司 | 2xxx铝锂合金 |
| CN113661262B (zh) * | 2019-04-05 | 2023-10-03 | 奥科宁克技术有限责任公司 | 冷成型铝锂合金的方法 |
| CN110592448B (zh) * | 2019-08-27 | 2021-06-22 | 江苏大学 | 耐热耐腐蚀2219型铝合金及其制备方法 |
| JP7469072B2 (ja) * | 2020-02-28 | 2024-04-16 | 株式会社神戸製鋼所 | アルミニウム合金鍛造材及びその製造方法 |
| CN113373333B (zh) * | 2021-05-27 | 2022-03-11 | 湖南瀚德微创医疗科技有限公司 | 一种低弹高强铝合金变幅杆及其制备方法 |
| CN114438428B (zh) * | 2022-01-27 | 2023-02-28 | 湘潭大学 | 一种耐腐蚀铝合金的制备方法 |
| FR3132306B1 (fr) | 2022-01-28 | 2024-05-03 | Constellium Issoire | Tôle mince améliorée en alliage d’aluminium-cuivre-lithium |
| FR3151859A1 (fr) | 2023-08-02 | 2025-02-07 | Constellium Issoire | Produit en alliage aluminium-cuivre-lithium pour element d’intrados a proprietes ameliorees |
| CN118186242A (zh) * | 2024-05-09 | 2024-06-14 | 中北大学 | 一种高强度铸造铝合金的制备方法 |
| FR3165018A1 (fr) | 2024-07-24 | 2026-01-30 | Constellium Issoire | Utilisation d’un alliage d’aluminium 4000 pour la fabrication de réservoir de stockage de liquides cryogéniques et son procédé de fabrication |
Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP0273600A2 (en) * | 1986-12-01 | 1988-07-06 | Comalco Aluminium, Ltd. | Aluminum-lithium alloys |
| US4797165A (en) * | 1984-03-29 | 1989-01-10 | Aluminum Company Of America | Aluminum-lithium alloys having improved corrosion resistance and method |
| US4844750A (en) * | 1984-03-29 | 1989-07-04 | Aluminum Company Of America | Aluminum-lithium alloys |
| EP0325937A1 (en) * | 1988-01-28 | 1989-08-02 | Aluminum Company Of America | Aluminum-lithium alloys |
| WO1990002211A1 (en) * | 1988-08-18 | 1990-03-08 | Martin Marietta Corporation | Ultrahigh strength al-cu-li-mg alloys |
| WO1991011540A1 (en) * | 1990-01-26 | 1991-08-08 | Martin Marietta Corporation | Ultra high strength aluminum-base alloys |
| US5116572A (en) * | 1983-12-30 | 1992-05-26 | The Boeing Company | Aluminum-lithium alloy |
| WO1992014855A1 (en) * | 1991-02-15 | 1992-09-03 | Reynolds Metals Company | Low density aluminum lithium alloy |
Family Cites Families (22)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US2381219A (en) * | 1942-10-12 | 1945-08-07 | Aluminum Co Of America | Aluminum alloy |
| US2915391A (en) * | 1958-01-13 | 1959-12-01 | Aluminum Co Of America | Aluminum base alloy |
| US3306717A (en) * | 1964-02-01 | 1967-02-28 | Svenska Metallverken Ab | Filler metal for welding aluminumbased alloys |
| US4526630A (en) * | 1982-03-31 | 1985-07-02 | Alcan International Limited | Heat treatment of aluminium alloys |
| JPS59118848A (ja) * | 1982-12-27 | 1984-07-09 | Sumitomo Light Metal Ind Ltd | 電気抵抗を高めた構造用アルミニウム合金 |
| EP0124286B1 (en) * | 1983-03-31 | 1986-08-27 | Alcan International Limited | Aluminium alloys |
| DE3466560D1 (en) * | 1983-11-24 | 1987-11-05 | Cegedur | Aluminium alloys containing lithium, magnesium and copper |
| DE3483607D1 (de) * | 1983-12-30 | 1990-12-20 | Boeing Co | Alterung bei relativ niedrigen temperaturen von lithium enthaltenden aluminiumlegierungen. |
| FR2561260B1 (fr) * | 1984-03-15 | 1992-07-17 | Cegedur | Alliages al-cu-li-mg a tres haute resistance mecanique specifique |
| FR2561261B1 (fr) * | 1984-03-15 | 1992-07-24 | Cegedur | Alliages a base d'al contenant du lithium, du cuivre et du magnesium |
| US5137686A (en) * | 1988-01-28 | 1992-08-11 | Aluminum Company Of America | Aluminum-lithium alloys |
| US4806174A (en) * | 1984-03-29 | 1989-02-21 | Aluminum Company Of America | Aluminum-lithium alloys and method of making the same |
| US4816087A (en) * | 1985-10-31 | 1989-03-28 | Aluminum Company Of America | Process for producing duplex mode recrystallized high strength aluminum-lithium alloy products with high fracture toughness and method of making the same |
| CH668269A5 (de) * | 1985-10-31 | 1988-12-15 | Bbc Brown Boveri & Cie | Aluminium-knetlegierung des typs al/cu/mg mit hoher festigkeit im temperaturbereich zwischen 0 und 250 c. |
| US4832910A (en) * | 1985-12-23 | 1989-05-23 | Aluminum Company Of America | Aluminum-lithium alloys |
| US4795502A (en) * | 1986-11-04 | 1989-01-03 | Aluminum Company Of America | Aluminum-lithium alloy products and method of making the same |
| US4812178A (en) * | 1986-12-05 | 1989-03-14 | Bruno Dubost | Method of heat treatment of Al-based alloys containing Li and the product obtained by the method |
| US5032359A (en) * | 1987-08-10 | 1991-07-16 | Martin Marietta Corporation | Ultra high strength weldable aluminum-lithium alloys |
| US5122339A (en) * | 1987-08-10 | 1992-06-16 | Martin Marietta Corporation | Aluminum-lithium welding alloys |
| US4848647A (en) * | 1988-03-24 | 1989-07-18 | Aluminum Company Of America | Aluminum base copper-lithium-magnesium welding alloy for welding aluminum lithium alloys |
| US4869870A (en) * | 1988-03-24 | 1989-09-26 | Aluminum Company Of America | Aluminum-lithium alloys with hafnium |
| US5151136A (en) * | 1990-12-27 | 1992-09-29 | Aluminum Company Of America | Low aspect ratio lithium-containing aluminum extrusions |
-
1993
- 1993-08-10 US US08/103,662 patent/US5455003A/en not_active Expired - Lifetime
-
1994
- 1994-08-08 BR BR9407224A patent/BR9407224A/pt not_active IP Right Cessation
- 1994-08-08 PT PT94925755T patent/PT714453E/pt unknown
- 1994-08-08 ES ES94925755T patent/ES2141250T3/es not_active Expired - Lifetime
- 1994-08-08 EP EP94925755A patent/EP0714453B1/en not_active Expired - Lifetime
- 1994-08-08 AU AU75560/94A patent/AU683296B2/en not_active Expired
- 1994-08-08 DE DE69422630T patent/DE69422630T2/de not_active Expired - Lifetime
- 1994-08-08 KR KR1019960700671A patent/KR100330990B1/ko not_active Expired - Lifetime
- 1994-08-08 RU RU96105399A patent/RU2128241C1/ru active
- 1994-08-08 JP JP50654295A patent/JP3742884B2/ja not_active Expired - Lifetime
- 1994-08-08 CA CA002167847A patent/CA2167847A1/en not_active Abandoned
- 1994-08-08 WO PCT/US1994/008876 patent/WO1995004837A1/en not_active Ceased
-
1996
- 1996-02-08 NO NO19960515A patent/NO313641B1/no not_active IP Right Cessation
Patent Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5116572A (en) * | 1983-12-30 | 1992-05-26 | The Boeing Company | Aluminum-lithium alloy |
| US4797165A (en) * | 1984-03-29 | 1989-01-10 | Aluminum Company Of America | Aluminum-lithium alloys having improved corrosion resistance and method |
| US4844750A (en) * | 1984-03-29 | 1989-07-04 | Aluminum Company Of America | Aluminum-lithium alloys |
| EP0273600A2 (en) * | 1986-12-01 | 1988-07-06 | Comalco Aluminium, Ltd. | Aluminum-lithium alloys |
| EP0325937A1 (en) * | 1988-01-28 | 1989-08-02 | Aluminum Company Of America | Aluminum-lithium alloys |
| WO1990002211A1 (en) * | 1988-08-18 | 1990-03-08 | Martin Marietta Corporation | Ultrahigh strength al-cu-li-mg alloys |
| WO1991011540A1 (en) * | 1990-01-26 | 1991-08-08 | Martin Marietta Corporation | Ultra high strength aluminum-base alloys |
| WO1992014855A1 (en) * | 1991-02-15 | 1992-09-03 | Reynolds Metals Company | Low density aluminum lithium alloy |
Non-Patent Citations (2)
| Title |
|---|
| M. PETERS AND P.-J. WINKLER: "The Effect on Nucleation in Al-Cu-Li-Ag-Mg Alloy, Weldite 049(X2094)", ALUMINIUM-LITHIUM, vol. 1, 1991, pages 257 - 262 * |
| SLAVIK , BLANKENSHIP ET AL.: "Intrinsic Fatigue Crack Growth Rates for Al-Li-Cu-Mg Alloys in Vacuum", METALLURGURICAL TRANSACTIONS, vol. 24A, no. 8, August 1993 (1993-08-01), pages 1807 - 1817 * |
Cited By (23)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1995028250A1 (en) * | 1994-04-13 | 1995-10-26 | Lockheed Martin Corporation | Al-cu-li weld filler alloy, process for the preparation thereof and process for welding therewith |
| WO2005035810A1 (en) * | 2003-10-03 | 2005-04-21 | Alcoa Inc. | Aluminum-copper-magnesium alloys having ancillary additions of lithium |
| CN1878880B (zh) * | 2003-10-03 | 2012-01-25 | 阿尔科公司 | 含辅助添加物锂的铝-铜-镁合金 |
| WO2009073794A1 (en) * | 2007-12-04 | 2009-06-11 | Alcoa Inc. | Improved aluminum-copper-lithium alloys |
| KR101538529B1 (ko) * | 2007-12-04 | 2015-07-21 | 알코아 인코포레이티드 | 개선된 알루미늄-구리-리튬 합금 |
| EP2829623A1 (en) * | 2007-12-04 | 2015-01-28 | Alcoa Inc. | Improved aluminum-copper-lithium alloys |
| AU2013257457B2 (en) * | 2007-12-04 | 2016-03-31 | Arconic Inc. | Improved aluminum-copper-lithium alloys |
| EP2829623B1 (en) | 2007-12-04 | 2018-02-07 | Arconic Inc. | Improved aluminum-copper-lithium alloys |
| AU2008333796B2 (en) * | 2007-12-04 | 2013-08-22 | Arconic Inc. | Improved aluminum-copper-lithium alloys |
| US11111562B2 (en) | 2009-06-25 | 2021-09-07 | Constellium Issoire | Aluminum-copper-lithium alloy with improved mechanical strength and toughness |
| EP2449142B1 (fr) | 2009-06-25 | 2017-05-03 | Constellium Issoire | Alliage aluminium cuivre lithium a resistance mecanique et tenacite ameliorees |
| FR2947282A1 (fr) * | 2009-06-25 | 2010-12-31 | Alcan Rhenalu | Alliage aluminium cuivre lithium a resistance mecanique et tenacite ameliorees |
| WO2010149873A1 (fr) * | 2009-06-25 | 2010-12-29 | Alcan Rhenalu | Alliage aluminium cuivre lithium a resistance mecanique et tenacite ameliorees |
| KR101437243B1 (ko) | 2009-09-04 | 2014-09-03 | 알코아 인코포레이티드 | 방탄 성능을 개선하기 위한 알루미늄 합금 에이징 방법 |
| US9163304B2 (en) | 2010-04-20 | 2015-10-20 | Alcoa Inc. | High strength forged aluminum alloy products |
| EP2561109A4 (en) * | 2010-04-20 | 2014-08-27 | Alcoa Inc | HIGH-FIXED FORGED ALUMINUM ALLOY PRODUCTS |
| EP3354765A1 (en) * | 2010-04-20 | 2018-08-01 | Arconic Inc. | High strength forged aluminum alloy products |
| WO2012085359A3 (fr) * | 2010-12-20 | 2012-09-13 | Constellium France | Alliage aluminium cuivre lithium à résistance en compression et ténacité améliorées |
| FR2969177A1 (fr) * | 2010-12-20 | 2012-06-22 | Alcan Rhenalu | Alliage aluminium cuivre lithium a resistance en compression et tenacite ameliorees |
| EP2766503B1 (fr) | 2011-10-14 | 2016-12-07 | Constellium Issoire | Procédé de transformation amélioré de tôles en alliage al-cu-li |
| EP3012338A1 (en) * | 2014-10-26 | 2016-04-27 | Kaiser Aluminum Fabricated Products, LLC | High strength, high formability, and low cost aluminum lithium alloys |
| US10253404B2 (en) | 2014-10-26 | 2019-04-09 | Kaiser Aluminum Fabricated Products, Llc | High strength, high formability, and low cost aluminum-lithium alloys |
| EP3384061B1 (fr) | 2015-12-04 | 2020-02-05 | Constellium Issoire | Alliage aluminium cuivre lithium à resistance mécanique et tenacité ameliorées |
Also Published As
| Publication number | Publication date |
|---|---|
| DE69422630T2 (de) | 2000-08-31 |
| AU683296B2 (en) | 1997-11-06 |
| RU2128241C1 (ru) | 1999-03-27 |
| CA2167847A1 (en) | 1995-02-16 |
| NO960515D0 (no) | 1996-02-08 |
| NO313641B1 (no) | 2002-11-04 |
| PT714453E (pt) | 2000-04-28 |
| NO960515L (no) | 1996-02-08 |
| EP0714453A1 (en) | 1996-06-05 |
| AU7556094A (en) | 1995-02-28 |
| JPH09501203A (ja) | 1997-02-04 |
| EP0714453B1 (en) | 2000-01-12 |
| US5455003A (en) | 1995-10-03 |
| DE69422630D1 (de) | 2000-02-17 |
| ES2141250T3 (es) | 2000-03-16 |
| JP3742884B2 (ja) | 2006-02-08 |
| KR100330990B1 (ko) | 2002-08-27 |
| BR9407224A (pt) | 1994-08-08 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US5455003A (en) | Al-Cu-Li alloys with improved cryogenic fracture toughness | |
| US5462712A (en) | High strength Al-Cu-Li-Zn-Mg alloys | |
| US5512241A (en) | Al-Cu-Li weld filler alloy, process for the preparation thereof and process for welding therewith | |
| EP0656956B1 (en) | Tough aluminum alloy containing copper and magnesium | |
| US5211910A (en) | Ultra high strength aluminum-base alloys | |
| AU631137B2 (en) | Ultrahigh strength al based-cu-li-mg alloys | |
| AU750846B2 (en) | Exfoliation resistant aluminium-magnesium alloy | |
| EP0642598B1 (en) | Low density, high strength al-li alloy having high toughness at elevated temperatures | |
| US5320803A (en) | Process for making aluminum-lithium alloys of high toughness | |
| EP1078109B1 (en) | Formable, high strength aluminium-magnesium alloy material for application in welded structures | |
| US5422066A (en) | Aluminum-lithium, aluminum-magnesium and magnesium-lithium alloys of high toughness |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): AU BR CA JP KR NO RU |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 2167847 Country of ref document: CA |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1994925755 Country of ref document: EP |
|
| WWP | Wipo information: published in national office |
Ref document number: 1994925755 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1994925755 Country of ref document: EP |