WO1993015264A1 - Delignification en phase gazeuse de matieres lignocellulosiques - Google Patents

Delignification en phase gazeuse de matieres lignocellulosiques Download PDF

Info

Publication number
WO1993015264A1
WO1993015264A1 PCT/US1993/000408 US9300408W WO9315264A1 WO 1993015264 A1 WO1993015264 A1 WO 1993015264A1 US 9300408 W US9300408 W US 9300408W WO 9315264 A1 WO9315264 A1 WO 9315264A1
Authority
WO
WIPO (PCT)
Prior art keywords
chlorine dioxide
pulp
ozone
lignocellulosic material
delignification
Prior art date
Application number
PCT/US1993/000408
Other languages
English (en)
Inventor
Sudhir K. Mendiratta
David W. Cawlfield
Glenn F. Rudie
Venketa R. Parthasarathy
Original Assignee
Olin Corporation
Mead Corporation
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Olin Corporation, Mead Corporation filed Critical Olin Corporation
Priority to BR9305760A priority Critical patent/BR9305760A/pt
Priority to JP5513284A priority patent/JPH07502082A/ja
Priority to AU34769/93A priority patent/AU656658B2/en
Priority to EP93903543A priority patent/EP0705361A1/fr
Publication of WO1993015264A1 publication Critical patent/WO1993015264A1/fr
Priority to FI943466A priority patent/FI943466A0/fi

Abstract

Permettant de délignifier des matières lignocellulosiques telles que la pâte de bois, un procédé consiste à traiter ces matières de façon séquentielle ou simultanée avec un gaz, le dioxide de chlore, et de l'ozone, ce qui donne la matière cellulosique délignifiée et des rejets d'effluents dont la teneur en halogénures organiques adsorbés (HOA) est réduite.
PCT/US1993/000408 1992-01-22 1993-01-19 Delignification en phase gazeuse de matieres lignocellulosiques WO1993015264A1 (fr)

Priority Applications (5)

Application Number Priority Date Filing Date Title
BR9305760A BR9305760A (pt) 1992-01-22 1993-01-19 Processo para deslignificaçao de material lignocelulósico
JP5513284A JPH07502082A (ja) 1992-01-22 1993-01-19 リグノセルロール材料の気相脱リグニン化
AU34769/93A AU656658B2 (en) 1992-01-22 1993-01-19 Gas phase delignification of lignocellulosic material
EP93903543A EP0705361A1 (fr) 1992-01-22 1993-01-19 Delignification en phase gazeuse de matieres lignocellulosiques
FI943466A FI943466A0 (fi) 1992-01-22 1994-07-21 Lignoselluloosamateriaalin kaasufaasidelignifiointi

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US82379592A 1992-01-22 1992-01-22
US823,795 1992-01-22

Publications (1)

Publication Number Publication Date
WO1993015264A1 true WO1993015264A1 (fr) 1993-08-05

Family

ID=25239744

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US1993/000408 WO1993015264A1 (fr) 1992-01-22 1993-01-19 Delignification en phase gazeuse de matieres lignocellulosiques

Country Status (10)

Country Link
EP (1) EP0705361A1 (fr)
JP (1) JPH07502082A (fr)
AU (1) AU656658B2 (fr)
BR (1) BR9305760A (fr)
CA (1) CA2128408A1 (fr)
FI (1) FI943466A0 (fr)
NZ (1) NZ245712A (fr)
RU (1) RU94036007A (fr)
WO (1) WO1993015264A1 (fr)
ZA (1) ZA93224B (fr)

Cited By (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
FR2743094A1 (fr) * 1995-12-27 1997-07-04 Centre Tech Ind Papier Procede de blanchiment des pates a papier chimiques
WO2002016691A1 (fr) * 2000-08-25 2002-02-28 Akzo Nobel N.V. Procede chimique
US6579412B2 (en) * 1998-05-08 2003-06-17 L'air Liquide - Societe' Anonyme A' Directoire Et Conseil De Surveillance Pour L'etude Et L'exploitation Des Procedes Georges Claude Process for ozone bleaching of low consistency pulp
US6773547B2 (en) * 1998-05-08 2004-08-10 American Air Liquide, Inc. Process for the bleaching of low consistency pulp using high partial pressure ozone
US8524038B2 (en) 2006-03-31 2013-09-03 Oy Lannen Tutkimus—Western Research Inc. Bleaching process of chemical pulp
CN111315802A (zh) * 2017-11-07 2020-06-19 英格维蒂南卡罗来纳有限责任公司 制备低色木质素的方法

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN111253424B (zh) 2014-08-06 2023-06-20 加州理工学院 芳族杂环通过地球丰富的无过渡金属的催化剂的甲硅烷基化

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US1957937A (en) * 1930-10-10 1934-05-08 Int Paper Co Process of bleaching fibrous cellulose material
US3725193A (en) * 1969-11-26 1973-04-03 Pulp Paper Res Inst Process and apparatus for the chemical reaction between a gas and a wood pulp
US3810969A (en) * 1971-06-22 1974-05-14 Hooker Chemical Corp Process for the production of chlorine dioxide
US4902381A (en) * 1988-12-09 1990-02-20 Kamyr, Inc. Method of bleaching pulp with ozone-chlorine mixtures
US4959124A (en) * 1989-05-05 1990-09-25 International Paper Company Method of bleaching kraft pulp in a DZED sequence
US5034095A (en) * 1989-06-01 1991-07-23 Oji Paper Co., Ltd. Apparatus and process for the delignification of cellulose pulp

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US4216054A (en) * 1977-09-26 1980-08-05 Weyerhaeuser Company Low-consistency ozone delignification
DE69128287T2 (de) * 1990-08-14 1998-03-19 Int Paper Co Bleichen von chemischem zellstoff mittels chlor/chlordioxid dann durch ozon

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US1957937A (en) * 1930-10-10 1934-05-08 Int Paper Co Process of bleaching fibrous cellulose material
US3725193A (en) * 1969-11-26 1973-04-03 Pulp Paper Res Inst Process and apparatus for the chemical reaction between a gas and a wood pulp
US3810969A (en) * 1971-06-22 1974-05-14 Hooker Chemical Corp Process for the production of chlorine dioxide
US4902381A (en) * 1988-12-09 1990-02-20 Kamyr, Inc. Method of bleaching pulp with ozone-chlorine mixtures
US4959124A (en) * 1989-05-05 1990-09-25 International Paper Company Method of bleaching kraft pulp in a DZED sequence
US5034095A (en) * 1989-06-01 1991-07-23 Oji Paper Co., Ltd. Apparatus and process for the delignification of cellulose pulp

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP0705361A4 *

Cited By (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
FR2743094A1 (fr) * 1995-12-27 1997-07-04 Centre Tech Ind Papier Procede de blanchiment des pates a papier chimiques
US6579412B2 (en) * 1998-05-08 2003-06-17 L'air Liquide - Societe' Anonyme A' Directoire Et Conseil De Surveillance Pour L'etude Et L'exploitation Des Procedes Georges Claude Process for ozone bleaching of low consistency pulp
US6773547B2 (en) * 1998-05-08 2004-08-10 American Air Liquide, Inc. Process for the bleaching of low consistency pulp using high partial pressure ozone
US6793771B2 (en) * 1998-05-08 2004-09-21 American Air Liquide, Inc. Ozone bleaching of low consistency pulp
WO2002016691A1 (fr) * 2000-08-25 2002-02-28 Akzo Nobel N.V. Procede chimique
US8524038B2 (en) 2006-03-31 2013-09-03 Oy Lannen Tutkimus—Western Research Inc. Bleaching process of chemical pulp
CN111315802A (zh) * 2017-11-07 2020-06-19 英格维蒂南卡罗来纳有限责任公司 制备低色木质素的方法

Also Published As

Publication number Publication date
RU94036007A (ru) 1996-06-10
CA2128408A1 (fr) 1993-08-05
FI943466A (fi) 1994-07-21
NZ245712A (en) 1994-09-27
BR9305760A (pt) 1997-01-28
AU3476993A (en) 1993-09-01
FI943466A0 (fi) 1994-07-21
EP0705361A1 (fr) 1996-04-10
AU656658B2 (en) 1995-02-09
JPH07502082A (ja) 1995-03-02
ZA93224B (en) 1993-08-18
EP0705361A4 (fr) 1995-09-27

Similar Documents

Publication Publication Date Title
US5770010A (en) Pulping process employing nascent oxygen
US4897156A (en) Process for activating cellulose pulp with NO and/or NO2 and oxygen in the presence of nitric acid and then delignifying bleaching the activated cellulose pulp
US5409570A (en) Process for ozone bleaching of oxygen delignified pulp while conveying the pulp through a reaction zone
US5366593A (en) Bleaching of lignocellulosic material with in-situ-generated dioxirane
AU656658B2 (en) Gas phase delignification of lignocellulosic material
EP0651832B1 (fr) Procede de delignification de pate de bois en phase gazeuse
EP0971066B1 (fr) Récupération de gaz riche en oxygène provenant de procédés de blanchiment avec ozone
US3755068A (en) Regeneration of chlorine dioxide for pulp treatment
Kuwabara et al. Impact on the filtrate from bleached pulp treated with peroxymonosulfuric acid for effective removal of hexenuronic acid
JPS6350464B2 (fr)
US6585880B1 (en) Method for recovering chemicals in a process of producing pulp by kraft process
EP0902120A1 (fr) Procédé de blanchissement d'une pâte à papier avec de l'ozone et du dioxyde de chlore
WO1995006772A1 (fr) Procede ameliore de blanchiment de pate lignocellulosique
CA1326112C (fr) Oxydation de l'effluent d'une usine de blanchiment par l'ajout de bioxyde de chlore
WO1993015263A1 (fr) Procede de delignification en phase gazeuse des matieres ligno-cellulosiques
Isaza Ferro Catalyzed and non-catalyzed hypochlorous acid bleaching of kraft pulps
WO1996015317A1 (fr) Processus de delignification a l'aide d'une phase gazeuse contenant du dioxyde de chlore
KR890002542B1 (ko) 안정화된 이산화염소의 제조방법
RU2097461C1 (ru) Способ газовой делигнификации древесной пульпы
WO1993006297A1 (fr) Procede de blanchiment de pate a l'ozone
Qin et al. Absorbable Organic Halide Reduction in Chlorine Dioxide Bleaching of Bagasse Pulp from the Addition of Ammonium Thiosulfate
CA1053860A (fr) Production de dioxyde de chlore et blanchiment de la pate a papier
Woodard Jr et al. Chloric acid-A new electrochemical product
CA2214957A1 (fr) Procede pour produire de la pate blanche dans un reacteur electrochimique
Hart Pulp bleaching

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): AU BB BG BR CA FI HU JP KP KR LK MG MN MW NO PL RO RU SD

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE BF BJ CF CG CI CM GA GN ML MR SN TD TG

DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
WWE Wipo information: entry into national phase

Ref document number: 1993903543

Country of ref document: EP

WWE Wipo information: entry into national phase

Ref document number: 2128408

Country of ref document: CA

WWE Wipo information: entry into national phase

Ref document number: 943466

Country of ref document: FI

WWP Wipo information: published in national office

Ref document number: 1993903543

Country of ref document: EP

WWW Wipo information: withdrawn in national office

Ref document number: 1993903543

Country of ref document: EP