US20060272939A1 - Electrolyzing electrode and production method of persulfuric acid-dissolving liquid by use of the electrode - Google Patents

Electrolyzing electrode and production method of persulfuric acid-dissolving liquid by use of the electrode Download PDF

Info

Publication number
US20060272939A1
US20060272939A1 US11/447,203 US44720306A US2006272939A1 US 20060272939 A1 US20060272939 A1 US 20060272939A1 US 44720306 A US44720306 A US 44720306A US 2006272939 A1 US2006272939 A1 US 2006272939A1
Authority
US
United States
Prior art keywords
electrode
substrate
electrolyzing
surface layer
ozone
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Abandoned
Application number
US11/447,203
Other languages
English (en)
Inventor
Kazuhiro Kaneda
Mineo Ikematsu
Masahiro Iseki
Tsuyoshi Rakuma
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sanyo Electric Co Ltd
Original Assignee
Sanyo Electric Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sanyo Electric Co Ltd filed Critical Sanyo Electric Co Ltd
Assigned to SANYO ELECTRIC CO., LTD. reassignment SANYO ELECTRIC CO., LTD. ASSIGNMENT OF ASSIGNORS INTEREST (SEE DOCUMENT FOR DETAILS). Assignors: IKEMATSU, MINEO, ISEKI, MASAHIRO, KANEDA, KAZUHIRO, RAKUMA, TSUYOSHI
Publication of US20060272939A1 publication Critical patent/US20060272939A1/en
Abandoned legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C02—TREATMENT OF WATER, WASTE WATER, SEWAGE, OR SLUDGE
    • C02F—TREATMENT OF WATER, WASTE WATER, SEWAGE, OR SLUDGE
    • C02F1/00—Treatment of water, waste water, or sewage
    • C02F1/46—Treatment of water, waste water, or sewage by electrochemical methods
    • C02F1/461—Treatment of water, waste water, or sewage by electrochemical methods by electrolysis
    • C02F1/467—Treatment of water, waste water, or sewage by electrochemical methods by electrolysis by electrochemical disinfection; by electrooxydation or by electroreduction
    • C02F1/4672—Treatment of water, waste water, or sewage by electrochemical methods by electrolysis by electrochemical disinfection; by electrooxydation or by electroreduction by electrooxydation
    • C—CHEMISTRY; METALLURGY
    • C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
    • C25B—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES FOR THE PRODUCTION OF COMPOUNDS OR NON-METALS; APPARATUS THEREFOR
    • C25B1/00—Electrolytic production of inorganic compounds or non-metals
    • C25B1/01—Products
    • C25B1/13—Ozone
    • C—CHEMISTRY; METALLURGY
    • C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
    • C25B—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES FOR THE PRODUCTION OF COMPOUNDS OR NON-METALS; APPARATUS THEREFOR
    • C25B1/00—Electrolytic production of inorganic compounds or non-metals
    • C25B1/01—Products
    • C25B1/28—Per-compounds
    • C25B1/29—Persulfates
    • C—CHEMISTRY; METALLURGY
    • C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
    • C25B—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES FOR THE PRODUCTION OF COMPOUNDS OR NON-METALS; APPARATUS THEREFOR
    • C25B11/00—Electrodes; Manufacture thereof not otherwise provided for
    • C25B11/04—Electrodes; Manufacture thereof not otherwise provided for characterised by the material
    • C25B11/051—Electrodes formed of electrocatalysts on a substrate or carrier
    • C25B11/073—Electrodes formed of electrocatalysts on a substrate or carrier characterised by the electrocatalyst material
    • C25B11/075—Electrodes formed of electrocatalysts on a substrate or carrier characterised by the electrocatalyst material consisting of a single catalytic element or catalytic compound
    • C25B11/077—Electrodes formed of electrocatalysts on a substrate or carrier characterised by the electrocatalyst material consisting of a single catalytic element or catalytic compound the compound being a non-noble metal oxide
    • C—CHEMISTRY; METALLURGY
    • C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
    • C25B—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES FOR THE PRODUCTION OF COMPOUNDS OR NON-METALS; APPARATUS THEREFOR
    • C25B11/00—Electrodes; Manufacture thereof not otherwise provided for
    • C25B11/04—Electrodes; Manufacture thereof not otherwise provided for characterised by the material
    • C25B11/051—Electrodes formed of electrocatalysts on a substrate or carrier
    • C25B11/073—Electrodes formed of electrocatalysts on a substrate or carrier characterised by the electrocatalyst material
    • C25B11/091—Electrodes formed of electrocatalysts on a substrate or carrier characterised by the electrocatalyst material consisting of at least one catalytic element and at least one catalytic compound; consisting of two or more catalytic elements or catalytic compounds
    • C—CHEMISTRY; METALLURGY
    • C02—TREATMENT OF WATER, WASTE WATER, SEWAGE, OR SLUDGE
    • C02F—TREATMENT OF WATER, WASTE WATER, SEWAGE, OR SLUDGE
    • C02F1/00—Treatment of water, waste water, or sewage
    • C02F1/46—Treatment of water, waste water, or sewage by electrochemical methods
    • C02F1/461—Treatment of water, waste water, or sewage by electrochemical methods by electrolysis
    • C02F1/46104—Devices therefor; Their operating or servicing
    • C02F1/46109—Electrodes
    • C02F2001/46133—Electrodes characterised by the material
    • C02F2001/46138—Electrodes comprising a substrate and a coating

Definitions

  • the present invention relates to an electrolyzing electrode for use in an industrial or household electrolysis process and a method of producing a persulfuric acid-dissolving liquid by use of the electrolyzing electrode.
  • ozone is a substance having a very strong oxidizing power.
  • ozone water in a cleaning and sterilizing treatment, such as application of ozone water to water supply and sewage systems or foods or application of ozone water to a cleaning treatment in a semiconductor device manufacturing process or the like.
  • a method of producing ozone water there are known: a method of dissolving, in water, ozone produced by ultraviolet irradiation or electric discharge; a method of producing ozone in water by electrolysis of water and the like.
  • an ozone water producing device including: ozone producing means for producing an ozone gas by use of an ultraviolet lamp; and a tank which stores water. In the device, the produced ozone gas is supplied to water in the tank to thereby produce ozone water.
  • an ozone water producing device which mixes, at a predetermined ratio by a mixing pump, an ozone gas produced by an electric discharge type of ozone gas producing device and water in order to dissolve the ozone gas in water with a good efficiency.
  • an ozone producing electrode including: an electrode substrate constituted of a porous or net-like material; and an electrode catalyst containing an oxide of a platinum group element or the like.
  • a persulfuric acid is an oxidizing agent which is broadly used in cleaning a semiconductor or as a polymerization initiator, an oxidizing agent, a bleaching agent, a photograph treating agent, an oxidizing agent for a reagent chemical such as manganese or chromium, an analysis reagent or the like.
  • a sulfuric acid is used in cleaning a semiconductor.
  • the persulfuric acid has an oxidizing power which is stronger than that of the sulfuric acid. Therefore, the cleaning can efficiently be performed with a less amount of persulfuric acid having a concentration which is lower than that of the sulfuric acid.
  • a method of manufacturing the persulfuric acid is generally performed by an electrochemical technology in many cases, and a platinum ribbon is used as, for example, an electrode for manufacturing the persulfuric acid.
  • a platinum ribbon is used as, for example, an electrode for manufacturing the persulfuric acid.
  • wear on the electrode increases in accordance with electrolysis conditions.
  • the treatment also has a disadvantage due to mixed impurities or a disadvantage that the electrode has to be changed frequently.
  • the platinum group element is a standard anode material, and has a characteristic that the element is hardly dissolved in an aqueous solution which does not contain any organic substance.
  • the element has a low ozone production efficiency for the ozone producing electrode, and it is difficult to produce ozone water by a high-efficiency electrolysis method.
  • electrolysis at a high current density is required for producing ozone, and there is a problem in energy consumption or electrode life.
  • an electrolyzing electrode capable of producing ozone water with a high efficiency by electrolysis of water at a low current density
  • a production method of a persulfuric acid-dissolving liquid by use of the electrode
  • an electrolyzing electrode comprises: a substrate; and a surface layer formed on the surface of the substrate and including a dielectric material, the surface layer being formed to have a thickness which is larger than 0 and is 2000 nm or less.
  • the substrate is a conductive substrate.
  • an intermediate layer positioned on an inner side of the surface layer, formed on the surface of the substrate, and containing at least one of an oxidization retarding metal, a metal oxide having conductivity and a metal having conductivity even when oxidized.
  • the dielectric material included in the surface layer is an oxide.
  • the oxide is tantalum oxide or aluminum oxide.
  • the surface layer is constituted by forming a surface layer constituting material on the surface of the substrate by a sputtering process.
  • the intermediate layer is constituted by forming an intermediate layer constituting material on the surface of the substrate by the sputtering process.
  • a method of producing a persulfuric acid-dissolving liquid in an eighth aspect of the present invention is a production method of a persulfuric acid-dissolving liquid by electrolyzing an aqueous solution containing sulfate ions to produce a persulfuric acid-dissolving liquid, wherein the electrolyzing electrode of each of the above inventions is used as an anode.
  • the electrolyzing electrode comprises: the substrate; and the surface layer formed on the surface of the substrate and including the dielectric material, and the surface layer is formed to have a thickness which is larger than 0 and is 2000 nm or less. Therefore, when electrolysis is performed by the electrolyzing electrode, ozone can be produced efficiently at a low current density.
  • the surface layer constituted of the dielectric material formed on the surface of the substrate has a thickness which is larger than 0 and is 2000 um or less. Therefore, electrons can move in the electrode via an impurity level in the surface layer or the Fowler-Nordheim tunneling. Accordingly, in an electrode reaction in the anode, an empty level in the vicinity of a bottom of a conduction band in an energy level can receive the electrons from an electrolyte, the energy level being higher as much as about a half of a band gap than the Fermi level. When the movement of the electrons is excited in a higher energy level, ozone can efficiently be produced at a lower current density.
  • the electrode reaction can be excited by the electrons which have moved in the surface layer. In consequence, ozone can efficiently be produced.
  • the electrolyzing electrode of the third aspect of the present invention in the above invention, on the substrate, there is formed the intermediate layer positioned on the inner side of the surface layer, formed on the surface of the substrate, and containing at least one of the oxidization retarding metal, the metal oxide having conductivity and the metal having the conductivity even when oxidized. Therefore, the electrons can effectively move in the surface layer as described above. Therefore, the electrode reaction can occur in the high energy level on the surface of the surface layer. In consequence, ozone can efficiently be produced with a lower current density.
  • the intermediate layer including any of the oxidization retarding metal, the metal oxide having the conductivity and the metal having the conductivity even when oxidized. Therefore, in a case where the electrolysis is performed by the electrode, it is possible to avoid a disadvantage that the intermediate layer is oxidized and become an insulator. This can improve durability of the electrode. Moreover, as compared with a case where the whole substrate is constituted of a material constituting the intermediate layer, production costs can reduced, and ozone can similarly efficiently be produced.
  • the dielectric material included in the surface layer is an oxide.
  • the oxide is tantalum oxide or aluminum oxide. Therefore, ozone can further effectively be produced at a low current density.
  • the surface layer is constituted by forming the surface layer constituting material on the surface of the substrate by the sputtering process. Therefore, the surface layer can uniformly be formed on the surface of the substrate. Since it is possible to constitute the surface layer having a homogeneous thickness on the whole surface of the substrate, electron can uniformly be conducted to the whole surface of the electrode, and it is possible to improve an ozone production efficiency.
  • the intermediate layer is constituted by forming the intermediate layer constituting material on the surface of the substrate by the sputtering process. Accordingly, the intermediate layer can uniformly be formed on the surface of the substrate. Therefore, it is possible to uniformly constitute even the surface layer to be formed on an outer side of the intermediate layer. In consequence, the electron can uniformly be conducted to the whole surface of the electrode, and it is possible to improve the ozone production efficiency.
  • a method of producing a persulfuric acid-dissolving liquid in the eighth aspect of the present invention is a production method of a persulfuric acid-dissolving liquid by electrolyzing the aqueous solution containing the sulfate ions to produce a persulfuric acid-dissolving liquid. Since the electrolyzing electrode of each of the above inventions is used as the anode, the persulfuric acid-dissolving liquid can efficiently be produced. That is, when the electrolyzing electrode of the present invention is used, an overvoltage rises with respect to an oxygen producing reaction. When the electrolytic treatment is performed in the presence of the sulfate ions, the production of persulfate ions by the oxidation of the sulfate ions proceeds in preference to the progress of the oxygen producing reaction.
  • FIG. 1 is a schematic sectional view of an electrolyzing electrode in the present invention
  • FIG. 2 is a flowchart of a method of manufacturing the electrolyzing electrode in the present invention
  • FIG. 3 is a schematic explanatory view of an ozone water producing device in the present invention.
  • FIG. 4 is a diagram showing an amount of ozone to be produced with respect to a thickness of a surface layer of the electrode of the present invention in the ozone water producing device of FIG. 3 ;
  • FIG. 5 is a diagram showing a current efficiency of an object which is ozone with respect to an annealing temperature of each electrolyzing electrode
  • FIG. 6 is a schematic sectional view of a persulfuric acid-dissolving liquid producing device
  • FIG. 7 is a current-potential curve in a case where an electrolytic solution including sulfate ions is electrolyzed.
  • FIG. 8 is a current-potential curve in a case where an electrolytic solution containing a perchloric acid is electrolyzed.
  • FIG. 1 is a cross sectional view of an electrolyzing electrode 1 in the present invention.
  • the electrolyzing electrode 1 is constituted of: a substrate 2 ; an intermediate layer 3 formed on the surface of the substrate 2 ; and a surface layer 4 formed on the surface of the intermediate layer 3 .
  • the substrate 2 is made of, as a conductive material, a valve metal such as tantalum (Ta), zirconium (Zr) or niobium (Nb), an alloy of two or more of the valve metals, silicon (Si) or the like. Since it is especially preferable that the surface of the substrate 2 for use in the present embodiment is flat, there is used silicon having its surface treated to be flat.
  • a valve metal such as tantalum (Ta), zirconium (Zr) or niobium (Nb), an alloy of two or more of the valve metals, silicon (Si) or the like. Since it is especially preferable that the surface of the substrate 2 for use in the present embodiment is flat, there is used silicon having its surface treated to be flat.
  • the intermediate layer 3 is made of: a metal which is difficult to oxidize, such as platinum or gold (Au); a metal oxide having conductivity, such as iridium oxide, palladium oxide or ruthenium oxide; a superconductive oxide; or a metal having conductivity even when oxidized, such as ruthenium (Ru), rhodium (Rh), palladium (Pd), iridium (Ir) or silver (Ag) included in platinum group elements.
  • a metal oxide having conductivity such as iridium oxide, palladium oxide or ruthenium oxide
  • a superconductive oxide such as ruthenium (Ru), rhodium (Rh), palladium (Pd), iridium (Ir) or silver (Ag) included in platinum group elements.
  • the metal oxide is not limited to the intermediate layer 3 formed beforehand as the oxide, and includes the metal oxide oxidized by electrolysis. In the present embodiment, it is assumed that the intermediate layer 3 is made of platinum.
  • the substrate 2 is made of platinum, needless to say, even the surface of the substrate 2 is made of platinum, and the intermediate layer 3 does not have to be especially constituted.
  • the substrate 2 is constituted of an inexpensive material, and the intermediate layer 3 made of a noble metal or the like is formed on the surface of the substrate 2 .
  • the surface layer 4 is constituted of a dielectric material into a layer on the surface of the substrate 2 together with the intermediate layer 3 so as to coat the intermediate layer 3 .
  • This surface layer 4 is formed into a predetermined thickness which is larger than 0 and is 2000 nm or less in the present embodiment. It is to be noted that the thickness of the surface layer 4 will be described later in detail. It is further preferable that the thickness is 40 nm or more and is less than 1000 nm.
  • the dielectric material constituting the surface layer 4 there is used tantalum oxide, aluminum oxide, titanium oxide, tungsten oxide or niobium oxide.
  • the surface layer 4 may be made of: an oxide containing two or more types of metal elements represented by a perovskite oxide such as barium titanate (BaTiO 3 ); or a mixture of two or more types of oxides having different crystal structure, such as a mixture of titanium oxide and tantalum oxide. In this case, instead of such oxide, there may be used an oxide containing the above noble metal or the noble-metal oxide.
  • a perovskite oxide such as barium titanate (BaTiO 3 )
  • a mixture of two or more types of oxides having different crystal structure such as a mixture of titanium oxide and tantalum oxide.
  • tantalum oxide indicates a general substance constituted by combining tantalum with oxygen
  • examples of tantalum oxide include: crystalline TaO or Ta 2 O 5 ; such oxide in which a slight oxygen defect is produced, such as TaO 1-X or Ta 2 O 5-x ; and amorphous TaO X .
  • aluminum oxide include Al 2 O 3 and AlO X .
  • titanium oxide include TiO 2 , Ti 2 O 3 and TiO X .
  • tungsten oxide include WO 3 and WO X .
  • dielectric material forming the surface layer 4 there is applicable Na 2 O, NaO X , MgO, MgO X , SiO 2 , SiO X , K 2 O, KO X , CaO, CaO X , Sc 2 O 3 , ScO X , V 2 O 5 , VO X , CrO 2 , CrO X , Mn 3 O 4 , MnO X , Fe 2 O 3 , FeO X , CoO, CoO X , NiO, NiO X , CuO, CuO X , ZnO, ZnO X , GaO, GaO X , GeO 2 , GeO X , Rb 2 O 3 , RbO X , SrO, SrO X , Y 2 O 3 , YO X , ZrO 2 , ZrO X , Nb 2 O 5 , NbO
  • silicon is used as the substrate 2 .
  • silicon having a very flat surface is used. It is to be noted that in the present embodiment, silicon is used as the substrate 2 .
  • the above-described conductive material preferably having its surface treated to be flat.
  • step S 1 the silicon substrate 2 is pretreated with 5% hydrofluoric acid, and a natural silicon oxide film formed on the surface of the substrate 2 is removed. This brings the surface of the substrate 2 into a flatter state. Thereafter, in step S 2 , the surface of the substrate 2 is rinsed with pure water. Subsequently, in steps S 3 and S 4 , the substrate is introduced into a chamber of an existing sputtering device, and films are formed on the substrate.
  • the intermediate layer 3 and the surface layer 4 are formed onto the substrate 2 by an RF sputtering process.
  • the intermediate layer 3 is made of platinum, Pt (80 mm ⁇ ) which is an intermediate layer constituting material is used as a first target.
  • An RF power is set to 100 W
  • an Ar gas pressure is set to 0.9 Pa
  • a distance between the substrate 2 and the target is set to 60 mm
  • the film is formed at room temperature for 20 minutes (step S 3 ). Accordingly, the intermediate layer 3 having a thickness of about 100 nm is formed on the surface of the substrate 2 .
  • the surface layer 4 is formed on the surface of the substrate 2 on which the intermediate layer 3 has been formed.
  • the target is changed to Ta which is a surface layer constituting material.
  • Conditions similar to the above conditions are set. That is, the RF power is set to 100 W, the Ar gas pressure is set to 0.9 Pa, the distance between the substrate 2 and the target is set to 60 mm, and the film is formed at room temperature for 5 to 180 minutes (step S 4 ). Accordingly, the surface layer 4 having a thickness of about 7 nm to 1000 nm is formed on the surface of the intermediate layer 3 of the substrate 2 . It is to be noted that film thicknesses of the intermediate layer 3 and the surface layer 4 are obtained by acquiring carried amounts of Pt and Ta by evaluation with a X-ray fluorescence and converting the amounts into the thicknesses.
  • the intermediate layer 3 and the surface layer 4 are formed into appropriate thicknesses and amounts with high in-plane homogeneity.
  • the intermediate layer 3 and the surface layer 4 can be formed with a high adhesion. In consequence, durability of the electrolyzing electrode 1 can be improved.
  • step S 5 the substrate 2 , on which the intermediate layer 3 and the surface layer 4 have been formed, is thermally annealed at 600° C. in a muffle furnace for 30 minutes in air atmosphere, and the electrolyzing electrode 1 is obtained. Accordingly, the tantalum metal constituting the surface layer 4 formed on the surface of the intermediate layer 3 is homogeneously oxidized. It is to be noted that the tantalum metal is oxidized by the annealing to constitute tantalum oxide. Therefore, the surface layer 4 has a thickness of about 14 nm to 2000 nm. In the present embodiment, after forming the intermediate layer 3 and the surface layer 4 by the sputtering process, the layers are annealed, and the surface of the electrode 1 is oxidized. However, when the electrode 1 is used in electrolysis, the surface of the electrode is oxidized. Therefore, it is assumed that the annealing does not have to be executed.
  • the surface layer 4 of the electrolyzing electrode 1 obtained as described above is entirely oxidized.
  • the intermediate layer 3 forms platinum silicide together with silicon of the substrate 2 .
  • silicon stops at the intermediate layer 3 and is not diffused in the surface layer 4 .
  • platinum constituting the intermediate layer 3 does not reach the inside of the surface layer 4 .
  • the surface layer 4 is very homogeneously distributed on the surface of the intermediate layer 3 , and the layer is uniformly on the whole surface of the intermediate layer 3 . Since the surface of the electrolyzing electrode 1 is thus uniformly coated with the surface layer 4 , the substrate 2 and the intermediate layer 3 are not exposed.
  • any gap or crack is not formed in the surface layer 4 , an electrolyte as an object of an electrolysis treatment does not directly reach the intermediate layer 3 or the substrate 2 under the surface layer. Therefore, it is possible to avoid a disadvantage that the substrate 2 is corroded during the electrolysis.
  • the surface layer 4 is constituted of the only dielectric material, the use of a noble metal or a noble-metal oxide in the surface layer 4 can be reduced. This can reduce costs.
  • FIG. 3 is a schematic explanatory view of an ozone water producing device 20 to which the electrolyzing electrode 1 of the present embodiment has been applied.
  • the ozone water producing device 20 includes: a treatment tank 21 ; the above-described electrolyzing electrode 1 as the anode; an electrode 22 ; a cation exchange film 24 ; and a power supply 25 which applies a direct current to the electrodes 1 and 22 .
  • model tap water 23 is pooled as an electrolytic solution.
  • the electrolyzing electrode 1 is prepared by the above manufacturing method.
  • the electrolyzing electrodes 1 for use in the ozone water producing device 20 there are used electrodes having five types of thicknesses of the surface layers 4 in total: about 14 nm; about 56 nm; about 170 nm; about 730 nm; and about 1800 nm. Accordingly, there are measured amounts of ozone to be produced in a case where the electrolyzing electrodes 1 are used as the anodes, respectively, and each electrolyzing electrode 1 is evaluated.
  • platinum is used in the electrode 22 as a cathode.
  • an insoluble electrode obtained by platinum on the substrate of the silicon substrate 2 a platinum-iridium based electrolyzing electrode; a carbon electrode or the like.
  • the cation exchange film 24 is a fluororesin-based film having durability against an oxidizing agent such as hydrogen peroxide.
  • an oxidizing agent such as hydrogen peroxide.
  • a typical cation exchange film there is a perfluoro sulfonic acid-based film such as trade name Nafion 115, 117, 315 or 350 manufactured by DuPont. It is assumed that in the present embodiment, Nafion is used as the cation exchange film 24 .
  • the electrolytic solution to be electrolyzed is an aqueous solution obtained by simulating tap water.
  • a component composition of model tap water 23 is: 5.75 ppm of Na + ; 10.02 ppm of Ca 2+ ; 6.08 ppm of Mg 2+ ; 0.98 ppm of K + ; 17.75 ppm of Cl ⁇ ; 24.5 ppm of SO 4 ; and 16.5 ppm of CO 3 2 ⁇ .
  • each of areas of the electrolyzing electrode 1 and the electrode 22 is 40 mm ⁇ 20 mm (submerged portion of 35 mm ⁇ 15 mm), and a distance between the electrodes is set to 10 mm.
  • the power supply 25 applies each constant current of 100 mA to the electrolyzing electrode 1 and the electrode 22 at a current density of about 20 mA/cm 2 .
  • the amount of ozone to be produced by the electrolyzing electrode 1 is obtained by measuring, by a colorimetric method, a concentration of ozone in model tap water 23 after the electrolysis performed for one minute on the above conditions.
  • FIG. 4 shows the amount of ozone to be produced by each electrolyzing electrode 1 on the same conditions among the five types of electrolyzing electrodes in the present embodiment.
  • the ordinate indicates the amount of ozone to be produced (mg/l)
  • the abscissa indicates the thickness (nm) of the surface layer 4 of the electrolyzing electrode 1 .
  • the amount of ozone to be produced was 0.05 mg/l.
  • the amount of ozone to be produced was as small as 0.12.
  • the amount of ozone to be produced rapidly increased in a case where the thickness as 40 nm or more and below 1000 nm.
  • the amount of ozone to be produced was 0.275 mg/l.
  • the thickness was about 170 nm, the amount was 0.28 mg/l.
  • the thickness was about 730 nm, the amount was 0.25 mg/l.
  • FIG. 5 shows experimental results of the five types of substances, indicating a current efficiency with respect to ozone as an object at an annealing (the step S 5 ) temperature.
  • the annealing temperatures are 300° C., 400° C., 500° C. and 600° C. while the thickness of each surface layer 4 is around 50 nm.
  • Four types of each substance are used, and the current efficiency with respect to ozone as the object is measured in a case where each electrolyzing electrode 1 is used as the anode, whereby evaluating each electrolyzing electrode 1 .
  • platinum is used in the electrode 22 as the cathode in the same manner as in the experiment of FIG. 4
  • Nafion is used in the cation exchange film 24 .
  • model tap water 23 is used in the same manner as in the aqueous solution.
  • each of areas of the electrolyzing electrode 1 and the electrode 22 is 2.25 cm 2 , and a distance between the electrodes is set to 10 mm.
  • the power supply 25 applies each constant current of 50 mA to the electrolyzing electrode 1 and the electrode 22 at a current density of about 20 mA/cm 2 .
  • the electrolysis is performed for one minute on the above conditions, and there is measured each current efficiency with respect to ozone as the object, whereby evaluating each electrolyzing electrode 1 .
  • the current efficiency was 8.4% with respect to ozone as the object at an annealing temperature of 300° C.
  • the current efficiency at 400° C. was 9.6%
  • the current efficiency at 500° C. was 9.6%
  • the current efficiency at 600° C. was 10.8%.
  • the current efficiency was 6.0% with respect to ozone as the object at an annealing temperature of 300° C.
  • the current efficiency at 500° C. was 6.0%
  • the current efficiency at 600° C. was 7.2%.
  • the current efficiency was 7.8% with respect to ozone as the object at an annealing temperature of 300° C.
  • the current efficiency at 400° C. was 5.4%
  • the current efficiency at 500° C. was 6.6%
  • the current efficiency at 600° C. was 7.2%
  • the current efficiency at 400° C. was 3.6%
  • the current efficiency at 500° C. was 6.0%
  • the current efficiency at 600° C. was 8.4%.
  • the current efficiency was 7.2% with respect to ozone as the object at an annealing temperature of 300° C.
  • the current efficiency at 400° C. was 10.2%
  • the current efficiency at 500° C. was 9.6%
  • the current efficiency at 600° C. was 0.6%.
  • the electrolytic solution can be electrolyzed as described above even in a case where the surface layer 4 constituting the surface of the electrolyzing electrode 1 is made of tantalum oxide, niobium oxide, zirconium oxide, titanium oxide or tungsten oxide which is not a metal.
  • the surface layer 4 made of tantalum oxide, niobium oxide, zirconium oxide, titanium oxide or tungsten oxide has a comparatively small thickness of, for example, about 40 nm, and therefore the electrons in the surface layer 4 move via the impurity level or the Fowler-Nordheim tunnel to the intermediate layer 3 constituted of the conductive material.
  • the voltage between the electrodes during the electrolysis was about 90 V (there was used the electrode including the surface layer 4 having a thickness of 56 nm). This does not indicate a remarkably large value, where as the voltage between the electrodes during the electrolysis is about 75 V in a case where the electrolyzing electrode 1 is made of platinum silicide.
  • the ozone production efficiency is high as compared with a case where the electrode made of platinum silicide is used.
  • the electrode reaction in the anode occurs, when the empty level directly above the Fermi level receives the electrons from the electrolyte.
  • the electrolyzing electrode 1 including the surface layer 4 constituted of the dielectric material in the present invention is used, the reaction occurs, when the empty level in the vicinity of the bottom of the conduction band receives the electrons from the electrolyte, the bottom of the conduction band being located at an energy level which is higher as much as about a half of a band gap than the Fermi level.
  • the electrolyzing electrode 1 of the present invention the movement of the electron in a higher energy level is caused to excite the electrode reaction as compare with a case where the platinum silicide electrode is used. Therefore, it is considered that the ozone production efficiency rises.
  • the electrode capable of producing ozone at a high efficiency even with a low current density, in a case where the surface layer 4 constituted of the dielectric material in the electrolyzing electrode 1 is formed to have a thickness which is larger than 0 and is 2000 nm or less. Especially in a case where the surface layer 4 is formed to have a thickness which is 40 nm or more and is below 1000 nm, even when the current density is remarkably low, ozone can be produced with a high efficiency.
  • the substrate 2 on which the intermediate layer 3 and the surface layer 4 are to be formed is constituted of a material having a flat surface
  • the intermediate layer 3 and the surface layer 4 can homogeneously be formed on the surface of the substrate 2 . Therefore, since the thickness of each layer 3 or 4 is set to be homogeneous with respect to the surface of the electrode, uniform electric conduction can be realized with respect to the whole surface of the electrolyzing electrode 1 . In consequence, fluctuations of the electric conduction to the whole surface of the electrode can be reduced, and the ozone production efficiency can be improved.
  • the intermediate layer 3 and the surface layer 4 are formed on the surface of the substrate 2 by the sputtering process, the layers can more homogeneously be formed on the surface of the substrate 2 . Accordingly, the intermediate layer 3 and the surface layer 4 having a uniform thickness can be formed on the whole surface of the substrate 2 . Therefore, electron can uniformly be conducted to the whole surface of the electrode, and the ozone production efficiency can be improved. In this case, even if the treatment for flattening the surface of the substrate 2 is slightly insufficient, the sputtering process can form the layer having a uniform thickness on the whole surface on which the layer is to be formed. Therefore, the electron can uniformly be conducted to the whole surface of the electrode.
  • a method of forming the intermediate layer 3 and the surface layer 4 is not limited to the sputtering process as in the present embodiment, and there may be used, for example, a CVD process, an evaporation process, an ion plating process, a plating process or the like.
  • the intermediate layer 3 containing any of at least an oxidation retarding metal, a metal oxide having conductivity and a metal having the conductivity even when oxidized.
  • the surface layer 4 is constituted as described above to thereby form the electrolyzing electrode 1 .
  • the substrate 2 is constituted of a material similar to that of the intermediate layer 3 , that is, the material containing any of at least the oxidation retarding metal, the metal oxide having the conductivity and the metal having the conductivity even when oxidized, if the intermediate layer 3 is not especially formed, it is possible to constitute an electrode similarly capable of efficiently producing ozone.
  • the substrate 2 is coated with the intermediate layer 3 constituted of the above material as in the present invention, it is possible to realize the electrode 1 similarly capable of efficiently producing ozone at a small production cost.
  • FIG. 6 is a schematic explanatory view of a persulfuric acid-dissolving liquid producing device 30 to which the electrolyzing electrode 1 of the present embodiment has been applied.
  • the persulfuric acid-dissolving liquid producing device 30 includes: a treatment tank 31 ; the above-described electrolyzing electrode 1 as an anode; an electrode 32 as a cathode; a cation exchange film 34 ; and a power supply 35 which applies a direct current to the electrodes 1 and 32 .
  • a 0.1 M sulfuric acid (electrolytic solution 33 ) is stored as an electrolytic solution containing sulfate ions on both anode and cathode sides with the cation exchange film 34 being sandwiched between opposite sides.
  • the electrolyzing electrode 1 is prepared by the above manufacturing method.
  • tantalum oxide is used as an oxide which is a dielectric material to be included in the surface layer 4
  • the surface layer 4 is formed into a film thickness which is larger than 0 and is 2000 nm or less, preferably 40 nm or more and below 1000 nm. It is to be noted that in the present embodiment, the surface layer having a thickness of about 56 nm is used.
  • platinum is used in the electrode 32 as the cathode.
  • an insoluble electrode obtained by platinum on the substrate of the silicon substrate 2 a platinum-iridium-based electrolyzing electrode; a carbon electrode or the like.
  • the cation exchange film 34 is a fluororesin-based film having durability against a predetermined oxidizing agent.
  • a typical cation exchange film there is a perfluoro sulfonic acid-based film such as trade name Nafion 115, 117, 315 or 350 manufactured by DuPont. It is assumed that in the present embodiment, Nafion is used as the cation exchange film 34 .
  • this treatment tank 31 a 0.1 M sulfuric acid (electrolytic solution 33 ) is stored on the anode side and the cathode side defined by the cation exchange film 34 , and the electrolyzing electrode 1 and the electrode 32 are submerged into the electrolytic solution 33 on the anode side and the electrolytic solution 33 on the cathode side, respectively, with the cation exchange film 34 being sandwiched between the opposite sides. Thereafter, the power supply 35 applies a direct current to the electrodes 1 and 32 to electrolyze the electrolytic solution 33 .
  • reaction A When water is electrolyzed using the electrolyzing electrode, an oxygen gas is usually produced on the anode side (reaction A).
  • reaction B When a material of the electrolyzing electrode is selected, in addition to oxygen, ozone or hydrogen peroxide is produced (reactions B and C). The reactions A to C will be described:
  • reaction D when the electrolytic solution 33 containing sulfate ions is electrolyzed using the electrolyzing electrode 1 , the persulfuric acid is produced (reaction D). It is to be noted that even in the electrolytic solution 33 contains sulfite ions, persulfate ions are similarly produced (reaction E). The reactions D and E will be described hereinafter.
  • the electrolyzing electrode usually has a small potential window, an anode-side reaction having a low theoretical electrolytic voltage, especially an oxygen producing reaction preferentially occurs.
  • the electrolyzing electrode 1 of the present embodiment has an excessively large potential window, and an active overvoltage is very high with respect to the oxygen producing reaction, a target oxidation reaction occurs in preference to the oxygen producing reaction. That is, in the present embodiment, the oxidation reaction of the sulfate ions contained in the electrolytic solution 33 proceeds. Accordingly, when the aqueous solution containing the sulfate ions is electrolyzed, a persulfuric acid-dissolving liquid can be obtained.
  • FIG. 7 shows a current-potential curve (cyclic voltammogram) at a time when a potential of the electrolyzing electrode 1 constituting the anode is changed with time by use of a potentiostatic electrolysis device (potentiostat), thereby electrolyzing the electrolytic solution 33 by the electrolyzing electrode 1 .
  • FIG. 8 shows, in contrast to FIG. 7 , a current-potential curve at a time when an electrolytic solution containing a perchloric acid is electrolyzed.
  • the potential of the electrolyzing electrode 1 constituting the anode is fixed in the vicinity of 2.5 V in which the chemical reaction peak is indicated, and the solution containing the sulfate ions, that is, the electrolytic solution 33 is electrolyzed. Accordingly, the persulfuric acid can be produced with a high current efficiency.
  • the persulfuric acid having a very strong oxidizing power when the aqueous solution containing the sulfate ions is electrolyzed, the persulfuric acid can efficiently be produced. Therefore, it is possible to avoid a risk in transporting or storing the persulfuric acid.
  • the persulfuric acid having an oxidizing power which is much stronger than that of the sulfuric acid or the like, can easily be used in cleaning a semiconductor or used as a polymerization initiator, an oxidizing agent, a bleaching agent, a photograph treating agent, an oxidizing agent for a reagent chemical such as manganese or chromium, an analysis reagent or the like.
  • a purpose can be achieved with a concentration and an amount which are less than those in a conventional method. In consequence, an amount of a solution required for the cleaning can be reduced, and waste water disposal can be simplified.
  • the electrolyzing electrode 1 which can realize the production of the persulfuric acid is made of silicon constituting the substrate 2 , platinum constituting the intermediate layer 3 , and tantalum oxide constituting the surface layer 4 . Therefore, the electrolyzing electrode can be manufactured inexpensively as compared with a conventional electrode using conductive diamond. In consequence, production costs can be reduced.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Electrochemistry (AREA)
  • Organic Chemistry (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Inorganic Chemistry (AREA)
  • General Chemical & Material Sciences (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Hydrology & Water Resources (AREA)
  • Environmental & Geological Engineering (AREA)
  • Water Supply & Treatment (AREA)
  • Electrodes For Compound Or Non-Metal Manufacture (AREA)
  • Electrolytic Production Of Non-Metals, Compounds, Apparatuses Therefor (AREA)
  • Water Treatment By Electricity Or Magnetism (AREA)
US11/447,203 2005-06-07 2006-06-06 Electrolyzing electrode and production method of persulfuric acid-dissolving liquid by use of the electrode Abandoned US20060272939A1 (en)

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
JP2005-166786 2005-06-07
JP2005166786 2005-06-07
JP2006045693A JP4290169B2 (ja) 2005-06-07 2006-02-22 電解用電極及びその電極を用いた過硫酸溶解水の生成方法
JP2006-45693 2006-02-22

Publications (1)

Publication Number Publication Date
US20060272939A1 true US20060272939A1 (en) 2006-12-07

Family

ID=37493061

Family Applications (1)

Application Number Title Priority Date Filing Date
US11/447,203 Abandoned US20060272939A1 (en) 2005-06-07 2006-06-06 Electrolyzing electrode and production method of persulfuric acid-dissolving liquid by use of the electrode

Country Status (2)

Country Link
US (1) US20060272939A1 (enExample)
JP (1) JP4290169B2 (enExample)

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20080217168A1 (en) * 2007-03-07 2008-09-11 Sanyo Electric Co., Ltd. Electrode for electrolysis and electrolysis unit
US20120312682A1 (en) * 2006-09-05 2012-12-13 Jonathan James Wilman Solid electrode
US9353448B2 (en) 2010-09-17 2016-05-31 Tanaka Kikinzoku Kogyo K.K. Electrolytic electrode, anode for electrolytic production of ozone, anode for electrolytic production of persulfuric acid and anode for electrolytic oxidation of chromium
JP2017039981A (ja) * 2015-08-20 2017-02-23 国立研究開発法人産業技術総合研究所 過酸化水素の製造方法および製造装置

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2010001552A (ja) * 2008-06-23 2010-01-07 Sanyo Electric Co Ltd 電解用電極および電解ユニット

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6200440B1 (en) * 1995-11-03 2001-03-13 Huron Tech Corp Electrolysis cell and electrodes
US6251254B1 (en) * 1998-09-30 2001-06-26 Permelec Electrode Ltd. Electrode for chromium plating
US20040011665A1 (en) * 2001-06-21 2004-01-22 Tomohito Koizumi Electrolyzing electrode and production method therefor and electrolysis method using electrolyzing electrode and electrolysis solution producing device
US20040226829A1 (en) * 2003-02-14 2004-11-18 Shao-An Cheng Device for and method of generating ozone
US20060042937A1 (en) * 2004-08-31 2006-03-02 Kazuhiro Kaneda Electrode for electrolysis and method of manufacturing electrode for electrolysis
US20070034505A1 (en) * 2005-08-11 2007-02-15 Mineo Ikematsu Electrode for electrolysis and method of manufacturing electrode for electrolysis

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6200440B1 (en) * 1995-11-03 2001-03-13 Huron Tech Corp Electrolysis cell and electrodes
US6251254B1 (en) * 1998-09-30 2001-06-26 Permelec Electrode Ltd. Electrode for chromium plating
US20040011665A1 (en) * 2001-06-21 2004-01-22 Tomohito Koizumi Electrolyzing electrode and production method therefor and electrolysis method using electrolyzing electrode and electrolysis solution producing device
US20040226829A1 (en) * 2003-02-14 2004-11-18 Shao-An Cheng Device for and method of generating ozone
US20060042937A1 (en) * 2004-08-31 2006-03-02 Kazuhiro Kaneda Electrode for electrolysis and method of manufacturing electrode for electrolysis
US20070034505A1 (en) * 2005-08-11 2007-02-15 Mineo Ikematsu Electrode for electrolysis and method of manufacturing electrode for electrolysis

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20120312682A1 (en) * 2006-09-05 2012-12-13 Jonathan James Wilman Solid electrode
US20080217168A1 (en) * 2007-03-07 2008-09-11 Sanyo Electric Co., Ltd. Electrode for electrolysis and electrolysis unit
US9353448B2 (en) 2010-09-17 2016-05-31 Tanaka Kikinzoku Kogyo K.K. Electrolytic electrode, anode for electrolytic production of ozone, anode for electrolytic production of persulfuric acid and anode for electrolytic oxidation of chromium
JP2017039981A (ja) * 2015-08-20 2017-02-23 国立研究開発法人産業技術総合研究所 過酸化水素の製造方法および製造装置

Also Published As

Publication number Publication date
JP4290169B2 (ja) 2009-07-01
JP2007016303A (ja) 2007-01-25

Similar Documents

Publication Publication Date Title
US20070034505A1 (en) Electrode for electrolysis and method of manufacturing electrode for electrolysis
Jerkiewicz Applicability of platinum as a counter-electrode material in electrocatalysis research
EP1900852A1 (en) Electrode for electrolysis, electrolytic process using the electrode, and electrolytic apparatus using them
TWI519679B (zh) The active cathode for hydrogen production
CN102770587B (zh) 电极基质和使用该电极基质的水溶液电解用阴极以及它们的制备方法
US20060042937A1 (en) Electrode for electrolysis and method of manufacturing electrode for electrolysis
JP2010042386A (ja) 電解処理装置
US11946151B2 (en) Electrolytic cell and electrolytic device
US20180022655A1 (en) Method for manufacturing ceramic material, capacitor, solid oxide fuel cell, water electrolysis device, and hydrogen pump
KR101600147B1 (ko) 전해용 전극, 오존 전해 생성용 양극, 과황산 전해 생성용 양극 및 크롬 전해 산화용 양극
US7919215B2 (en) Corrosion resistant metal oxide electrode catalyst for oxygen reduction
US20180086652A1 (en) Electrolysis electrode featuring nanotube array and methods of manufacture and using same for water treatment
CN105813985A (zh) 电解电极
JP4290169B2 (ja) 電解用電極及びその電極を用いた過硫酸溶解水の生成方法
CN100562606C (zh) 电解用电极及电解用电极的制造方法
JP2003331866A (ja) 固体酸化物型燃料電池
JP2010007144A (ja) 電解用電極および電解ユニット
CN1896319A (zh) 电解用电极及使用了该电极的过硫酸溶解水的生成方法
KR102512500B1 (ko) 오존 발생 전극, 그의 제조방법 및 그를 이용한 오존 제조방법
Godwin et al. Dimensionally Stable Anodes (DSA®) for Electrochemical Water Splitting: Redox Properties, OER Kinetics and Mechanism at RuO2/NiO Modified Electrodes in Aqueous Base
JP2007224351A (ja) 電解用電極及びその製造方法及びそれを用いた電解方法
JP7215727B2 (ja) 過酸化水素の製造方法及び過酸化水素の製造装置
CN101260536A (zh) 电解用电极及电解组件
EP1688516A1 (en) Electrode for electrochemical cell and electrochemical cell
KR20230055807A (ko) 페로브스카이트 화합물, 이를 포함하는 촉매, 및 이를 포함하는 전기 화학 소자

Legal Events

Date Code Title Description
AS Assignment

Owner name: SANYO ELECTRIC CO., LTD., JAPAN

Free format text: ASSIGNMENT OF ASSIGNORS INTEREST;ASSIGNORS:KANEDA, KAZUHIRO;IKEMATSU, MINEO;ISEKI, MASAHIRO;AND OTHERS;REEL/FRAME:017960/0661

Effective date: 20060601

STCB Information on status: application discontinuation

Free format text: ABANDONED -- FAILURE TO RESPOND TO AN OFFICE ACTION