JPS62278029A - Manufacture of gypsum board composite body - Google Patents

Manufacture of gypsum board composite body

Info

Publication number
JPS62278029A
JPS62278029A JP61121431A JP12143186A JPS62278029A JP S62278029 A JPS62278029 A JP S62278029A JP 61121431 A JP61121431 A JP 61121431A JP 12143186 A JP12143186 A JP 12143186A JP S62278029 A JPS62278029 A JP S62278029A
Authority
JP
Japan
Prior art keywords
gypsum board
reinforcing paper
paper
composite
shaped cross
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP61121431A
Other languages
Japanese (ja)
Inventor
浅井 規雄
治 山本
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nitto Boseki Co Ltd
Original Assignee
Nitto Boseki Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Boseki Co Ltd filed Critical Nitto Boseki Co Ltd
Priority to JP61121431A priority Critical patent/JPS62278029A/en
Publication of JPS62278029A publication Critical patent/JPS62278029A/en
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 3、発明の詳細な説明 〔産業上の利用分野〕 本発明はシート状の熱硬化性樹脂発泡層と石膏ボードと
からなる主として建造物内装材として利用される石膏ボ
ード複合体の製造方法に関するものである。
[Detailed Description of the Invention] 3. Detailed Description of the Invention [Field of Industrial Application] The present invention relates to a gypsum board, which is mainly used as an interior material for buildings, and is composed of a sheet-shaped thermosetting resin foam layer and a gypsum board. The present invention relates to a method for manufacturing a composite.

〔従来の技術〕[Conventional technology]

シート状の熱硬化性樹脂発泡層と石膏ボードとの積層体
たる石膏ボード複合体は、第2図に符号1で表示される
ような補強紙付き石膏ポード、すなわち、石膏ボード2
の上面、下面及び長手方向における両側面の四周面に補
強紙3が貼着されている石膏ボード1を50〜608C
程度に予熱し、次いで前記補強紙付き石膏ボード1の上
面に熱硬化性の発泡性樹脂液を供給し、更に必要に応じ
て前記発泡性樹脂液の」二面に不織布、金属箔2合成樹
脂フィルム等の面材を供給し、これを加熱硬化炉中の上
、下2段のスチール製エンドレスベルトコンベヤー間ニ
て加熱することにより、前記熱硬化性の発泡性樹脂を発
泡・硬化させてシート状の熱硬化性樹脂発泡層を形成し
た後、所定の大きさに切断することによって得られてい
た。尚、第2図に示される補強紙付き石膏ボード1にお
いて、符号4で表示される部分は接着剤層である。
A gypsum board composite, which is a laminate of a sheet-like thermosetting resin foam layer and a gypsum board, is a gypsum board with reinforcing paper as shown by reference numeral 1 in FIG. 2, that is, a gypsum board 2.
A gypsum board 1 with reinforcing paper 3 pasted on the upper surface, lower surface, and both sides in the longitudinal direction is 50 to 608C.
Then, a thermosetting foaming resin liquid is supplied to the upper surface of the gypsum board with reinforcing paper 1, and if necessary, non-woven fabric, metal foil 2 and synthetic resin are applied to the two sides of the foaming resin liquid. By supplying a surface material such as a film and heating it between two upper and lower steel endless belt conveyors in a heat curing furnace, the thermosetting foamable resin is foamed and hardened to form a sheet. It was obtained by forming a thermosetting resin foam layer and then cutting it into a predetermined size. In addition, in the reinforced paper-covered gypsum board 1 shown in FIG. 2, the portion indicated by the reference numeral 4 is an adhesive layer.

然しなから、前記方法による石膏ボード複合体の製造方
法においては、石膏ボードの長手方向における両側面に
前述の熱硬化性樹脂液が漏れることか多く、得られる石
膏ボード複合体の木口に汚れを有することとなる。
However, in the method for producing a gypsum board composite using the above method, the thermosetting resin liquid often leaks from both sides in the longitudinal direction of the gypsum board, and the end of the resulting gypsum board composite may be contaminated. It will be held.

このため、第3図に示されるように、断面り字形及び断
面逆り字形のゴムまたは軟質プラスチック製のサイドシ
ールベルト5,5が長手方向の両側縁辺に接触もしくは
固定されているスチール製の下段エンドレスベルトコン
ベヤー6を使用することにより、前述の熱硬化性樹脂液
の漏れを防止するようにした石膏ボード複合体の製造方
法、すなわち、内側段部7を有するゴム(例えば、 S
BR等の一般ゴム、弗素樹脂等の耐熱ゴム、ナイロン繊
維やガラス繊維で補強されている補強ゴム等)!f、た
け軟質プラスチックからなるサイドシールベルト5がス
チール製ノ下段エンドレスベルトコンベヤー6 (7)
長手方向両側縁辺に接触もしくは固定されているサイド
シールベルト5付きの下段エンドレスベルトコンベヤー
6上に、前記補強紙付き石膏ボード8を載置し、次いで
前記石膏ボード8の上面に熱硬化性の発泡性樹脂液9を
供給し、更に、必要に応じて前記発泡性樹脂液9の上面
に面材10を供給した後、更に上段エンドレスベルトコ
ンベヤー11を接当し、加熱硬化炉中を通すことにより
前記熱硬化性の発泡性樹脂を発泡・硬化させるへ石膏ボ
ード複合体の製造方法が利用されている。
For this reason, as shown in FIG. 3, the lower stage made of steel has side seal belts 5, 5 made of rubber or soft plastic with an inverted-shaped cross section and an inverted-shaped cross section that are in contact with or fixed to both edges in the longitudinal direction. A method for manufacturing a gypsum board composite in which leakage of the aforementioned thermosetting resin liquid is prevented by using an endless belt conveyor 6, i.e. a rubber (for example, S
General rubber such as BR, heat-resistant rubber such as fluororesin, reinforced rubber reinforced with nylon fiber or glass fiber, etc.)! f. The lower end endless belt conveyor 6 (7) in which the side seal belt 5 made of soft plastic is made of steel.
The gypsum board 8 with reinforcing paper is placed on the lower endless belt conveyor 6 with side seal belts 5 that are in contact with or fixed to both edges in the longitudinal direction, and then thermosetting foam is applied to the top surface of the gypsum board 8. After supplying the foamable resin liquid 9 and, if necessary, supplying a face material 10 on the upper surface of the foamable resin liquid 9, the upper endless belt conveyor 11 is further brought into contact with the foamable resin liquid 9, and the foaming resin liquid 9 is passed through a heating curing furnace. A method for manufacturing a gypsum board composite is used in which the thermosetting foamable resin is foamed and hardened.

〔発明が解決しようとする問題点〕[Problem that the invention seeks to solve]

ところで、前記従来のサイドシールベルト付きの下段エ
ンドレスベルトコンベヤーヲ使用する石膏ボード複合体
の製造方法においては、サイドシールベルトの寸法精度
、経時寸法変化。
By the way, in the method of manufacturing a gypsum board composite using the conventional lower endless belt conveyor with side seal belts, the dimensional accuracy of the side seal belts and dimensional changes over time are limited.

更には蛇行等が原因で、石膏ボードの上面に供給した熱
硬化性の発泡性樹脂液を完全にシールすることが不可能
であり、依然として長手方向の木口に汚れを有し、石膏
ボード複合体同士を施工当接した際の当接部の密着性の
悪い石膏ボード複合体が得られ易いという欠点を有して
いる。
Furthermore, due to meandering, etc., it is impossible to completely seal the thermosetting foaming resin liquid supplied to the top surface of the gypsum board, and the end of the gypsum board still has stains in the longitudinal direction, making the gypsum board composite This has the disadvantage that a gypsum board composite tends to have poor adhesion at the abutting portions when they are brought into contact during construction.

然して、前記サイドシールベルトと石膏ボードとの間隙
からの発泡性樹脂液の漏れを無くすだめ、サイドシール
ベルトと石膏ボードとの間と、同じくサイドシールベル
トと得られる熱硬化性樹脂発泡層との間とに一連の合成
樹脂フィルムを接当する方法も考えられるが、依然とし
て発泡性樹脂液の漏れを完全に無くすることが出来ない
ばかりでなく、接当する合成樹脂フィルムの消費に伴な
う経費アップが生ずるという欠点を有している。
Therefore, in order to eliminate the leakage of the foaming resin liquid from the gap between the side seal belt and the gypsum board, a gap between the side seal belt and the gypsum board and between the side seal belt and the resulting thermosetting resin foam layer is required. A method of contacting a series of synthetic resin films between the two is considered, but not only is it still not possible to completely eliminate the leakage of the foaming resin liquid, but the synthetic resin film in contact is consumed. This method has the disadvantage of increasing costs.

これに対して本発明の石膏ボード複合体の製造方法は、
長手方向の木口に汚れを存することのない外観の美麗な
石膏ボード複合体で、石膏ボード複合体同士を施工当接
した際の当接部の密着性の良好な石膏ボード複合体を、
容易、且つ確実に得る方法を提供するものである。
On the other hand, the method for manufacturing a gypsum board composite of the present invention,
A gypsum board composite with a beautiful appearance without any dirt on the longitudinal ends, and with good adhesion at the contact area when the gypsum board composites are brought into contact with each other during construction.
This provides a method for easily and reliably obtaining the information.

〔問題点を解決するだめの手段〕[Failure to solve the problem]

本発明の石膏ボード複合体の製造方法は、石膏ボードの
上面に貼着されている補強紙が該石膏ボードの上面長手
方向における両側縁辺から突出する延設部を具備してい
るところの補強紙付き石膏ボードを使用するものであり
、前記補強紙付き石膏ボードを、ベルトコンベヤーの長
手方向両側縁辺に断面り字形及び断面逆り字形のゴムま
たは軟質プラスチック製サイドシールベルトが接触もし
くは固定されている下段エンドレスベルトコンベヤー上
に、前記石膏ボードの上面に貼着されている補強紙の延
設部が前記サイドシールベルトの互いに対向する内側段
部の上面と接当するようにして載置することにより、石
膏ボードの上面に供給される熱硬化性の発泡性樹脂液が
サイドシールベルトと石膏ボードの長手方向における側
面との間に漏れるのを防止するものである。
The method for manufacturing a gypsum board composite of the present invention is such that the reinforcing paper attached to the top surface of the gypsum board has extending portions protruding from both edges in the longitudinal direction of the top surface of the gypsum board. The gypsum board with reinforcing paper is in contact with or is fixed to the gypsum board with reinforcement paper, and side seal belts made of rubber or soft plastic having an inverted cross section and an inverted cross section are in contact with or are fixed to both edges of the belt conveyor in the longitudinal direction. By placing the reinforcing paper on the lower endless belt conveyor so that the extending portion of the reinforcing paper affixed to the upper surface of the gypsum board is in contact with the upper surface of the mutually opposing inner step portion of the side seal belt. This prevents the thermosetting foamable resin liquid supplied to the upper surface of the gypsum board from leaking between the side seal belt and the side surface in the longitudinal direction of the gypsum board.

従って、本発明方法においては、補強紙付き石膏ボード
の上面に供給した熱硬化性の発泡性樹脂液を加熱・硬化
して熱硬化性樹脂発泡層を形成した後に、該発泡層の耳
揃えのための切断工程や、あるいは得られた石膏ボード
複合体を所定のサイズに切断する工程で、前記補強紙付
き石膏ボードにおける補強紙の延設部を切断。
Therefore, in the method of the present invention, after heating and curing the thermosetting foaming resin liquid supplied to the upper surface of the gypsum board with reinforcing paper to form a thermosetting resin foam layer, the edges of the foam layer are aligned. In the step of cutting the obtained gypsum board composite into a predetermined size, the extending portion of the reinforcing paper in the gypsum board with reinforcing paper is cut.

除去するものである。It is to be removed.

〔実施例〕〔Example〕

以下本発明の石膏ボード複合体の製造方法の具体的な構
成を図面実施例工程に基いて説明する。
The specific structure of the method for manufacturing a gypsum board composite of the present invention will be explained below based on drawings and embodiment steps.

第4図にて符号12で表示される補強紙付き石膏ボード
、すなわち、下面及び長手方向における両側面に補強紙
14が貼着されている厚さ9闘の石膏ボード13の上面
に、更に、前記石膏ボード13の上面長手方向における
両側縁辺から突出する延設部15.15を具備している
上面補強紙16が貼着されている補強紙付き石膏ボード
12を得た。
Further, on the upper surface of the gypsum board 13 with reinforcing paper indicated by reference numeral 12 in FIG. A gypsum board 12 with reinforcing paper was obtained, to which a top reinforcing paper 16 was attached, which had extensions 15.15 projecting from both edges in the longitudinal direction of the top surface of the gypsum board 13.

次いで、前記補強紙付き石膏ボード12を約55℃に予
熱した後、第1図に示される断面り字形及び断面逆り字
形のゴム(ナイロン繊維強化SBR)製サイドシールベ
ル)17.17付きのスチール製下段エンドレスベルト
コンベヤー18上に、前記補強紙付き石膏ボード12に
おける上面補強紙16の延設部15,15が前記ゴム製
サイドシールペル)17.17における互いに対向する
内側段部19,19の上面と接当するようにして載置し
、更に、前記補強紙付き石膏ボード12の上面に下記組
成の熱硬化性の発泡性樹脂液を供給して発泡性樹脂液層
20を形成した。
Next, after preheating the reinforced paper-covered gypsum board 12 to about 55° C., a rubber (nylon fiber-reinforced SBR) side seal bell 17. On the steel lower endless belt conveyor 18, the extending portions 15, 15 of the upper reinforcing paper 16 of the gypsum board with reinforcing paper 12 are attached to the mutually opposing inner step portions 19, 19 of the rubber side seal pel 17.17. It was placed so as to be in contact with the upper surface of the gypsum board 12 with reinforcing paper, and a thermosetting foamable resin liquid having the following composition was further supplied to the upper surface of the gypsum board 12 with reinforcing paper to form a foamable resin liquid layer 20.

発泡性樹脂液組成 (1)  レゾール樹脂・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・100重量部(2)
気泡安定剤・・・・・・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・・・・・・・2重量
部〔UCC■製:品番L−53403 (3)発泡剤・・・・・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・・・・・・・・・・
・20重量部[デュポン■製:品番フレオンR−133
](4)難燃添加剤         10重量部〔ポ
リリン酸アンモニウム粉末〕 (5)硬化剤・・・・・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・・・・・・・・・・
・20重量部〔60チフエノールスルホン酸〕 更に、前記発泡性樹脂液層20の上面に面材(石綿紙、
目付150f/m’)21を載置した後、スチール製の
上段エンドレスベルトコンベヤー22を接当し、これを
80℃に加熱されている硬化炉中に導いて80℃、6分
間の発泡成形に付し、厚さ16朋、フオーム密度40に
97m3の熱硬化性樹脂発泡層を形成し、熱硬化性樹脂
発泡層を有する石膏ボード複合体を得だ。
Foaming resin liquid composition (1) Resole resin・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・100 parts by weight (2)
Bubble stabilizer・・・・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・・・・・・ 2 parts by weight [Manufactured by UCC ■: Product number L-53403 (3) Foaming agent・・・・・・・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・・・・・・・・・
・20 parts by weight [manufactured by DuPont ■: Product number Freon R-133
](4) Flame retardant additive 10 parts by weight [ammonium polyphosphate powder] (5) Hardening agent・・・・・・・・・・・・・・・・・・
・・・・・・・・・・・・・・・・・・・・・・・・
・20 parts by weight [60 thiphenolsulfonic acid] Furthermore, a facing material (asbestos paper,
After placing the sheet (with a basis weight of 150 f/m') 21, an upper endless belt conveyor 22 made of steel is brought into contact with the sheet, and the sheet is introduced into a curing furnace heated to 80° C. for foam molding at 80° C. for 6 minutes. Then, a thermosetting resin foam layer of 97 m 3 with a thickness of 16 mm and a foam density of 40 was formed to obtain a gypsum board composite having a thermosetting resin foam layer.

次いで、前記熱硬化性樹脂発泡層を有する石膏ボード複
合体について、その長手方向については、熱硬化性樹脂
発泡層と面材との耳部と補強紙付き石膏ボードの」二面
補強紙における延設部とを切断、除去するトリミング処
置を行なうと共に、所定の長さの石膏ボード複合体を得
るための短手方向における発泡層の切断を実施し、目的
製品たる石膏ボード複合体を得た。
Next, regarding the gypsum board composite having the thermosetting resin foam layer, in the longitudinal direction, the edges of the thermosetting resin foam layer and the facing material, and the extension of the two-sided reinforced paper of the gypsum board with reinforcing paper. A trimming process was carried out to cut and remove the installed parts, and the foam layer was cut in the transverse direction to obtain a gypsum board composite of a predetermined length, thereby obtaining the desired product, the gypsum board composite.

尚、前記得られた石膏ボード複合体を、前記第2図に示
されるような構造からなる補強紙付き石膏ボード1を利
用して以下同一工程を実施することによって得られた比
較のだめの石膏ボード複合体と比較したところ、本発明
の実施例品における石膏ボードの側面には汚れの付着は
なかったが、比較のだめの石膏ボード複合体の長手方向
における両側面には発泡樹脂による汚れが多く付着して
おシ、この石膏ボード複合体同士を施工し当接した際の
当接部の密着性が不良であった。
A comparative gypsum board was obtained by subjecting the obtained gypsum board composite to the same process using a reinforced paper-covered gypsum board 1 having the structure shown in FIG. 2. When compared with the composite, there was no dirt adhering to the side surfaces of the gypsum board in the example product of the present invention, but there was a lot of dirt adhering to the foamed resin on both longitudinal sides of the comparative gypsum board composite. However, when these gypsum board composites were constructed and abutted against each other, the adhesion of the abutting portions was poor.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明の石膏ボード複合体の製造方法の途中工
程要部を示す断面模型図、第2図は従来の石膏ボード複
合体の製造方法に使用されている補強紙付き石膏ボード
の断面模型図、第3図は前記第2図に示される構成の補
強紙付き石膏ボードを利用して石膏ボード複合体を得る
場合の途中工程要部を示す断面模型図、第4図は本発明
の石膏ボード複合体の製造方法に使用される補強紙付き
石膏ボードの断面模型図である。 12:補強紙付き石膏ボード、13:石膏ボード、14
:補強紙、15:上面補強紙16における延設部、17
.17’ゴムまたは軟質プラスチック製ザイドシールベ
ルト、18:下段エンドレスベルトコンベヤー、19.
19  サイドシールベルト17における内側段部、2
0発泡性樹脂液層、22°」二段エンドレスベノトトコ
ンベヤー。
Fig. 1 is a cross-sectional model diagram showing the main steps in the process of manufacturing a gypsum board composite according to the present invention, and Fig. 2 is a cross-section of a gypsum board with reinforcing paper used in the conventional method for manufacturing a gypsum board composite. A model diagram, FIG. 3 is a cross-sectional model diagram showing a main part of the intermediate process when obtaining a gypsum board composite using the reinforced paper-covered gypsum board having the structure shown in FIG. 2, and FIG. FIG. 2 is a cross-sectional model diagram of a gypsum board with reinforcing paper used in the method for manufacturing a gypsum board composite. 12: Gypsum board with reinforced paper, 13: Gypsum board, 14
: Reinforcement paper, 15: Extension portion of upper surface reinforcement paper 16, 17
.. 17' Rubber or soft plastic Zyde seal belt, 18: Lower endless belt conveyor, 19.
19 Inner step portion in side seal belt 17, 2
0 foamable resin liquid layer, 22°" two-stage endless benototo conveyor.

Claims (1)

【特許請求の範囲】[Claims]  補強紙が石膏ボードの上面と下面と長手方向における
両側面との四周面に貼着されており、しかも前記石膏ボ
ードの上面に貼着されている上面補強紙が石膏ボードの
上面長手方向における両側縁辺から突出する延設部を具
備しているところの補強紙付き石膏ボードを、断面L字
形及び断面逆L字形のゴム又は軟質プラスチック製サイ
ドシールベルトがベルトコンベヤーの長手方向両側縁辺
に接触もしくは固定されている下段エンドレスベルトコ
ンベヤー上に、前記補強紙付き石膏ボードにおける上面
補強紙の延設部が前記断面L字形及び断面逆L字形のサ
イドシールベルトにおける互いに対向する内側段部の上
面と接当するようにして載置し、次いで前記補強紙付き
石膏ボードの上面に熱硬化性の発泡性樹脂液を供給し、
更に、上段エンドレスベルトコンベヤーを接当し、これ
を加熱硬化炉中に導いて熱硬化性樹脂発泡層を形成して
から前記補強紙付き石膏ボードにおける前記補強紙の延
設部を切断すると共に得られた石膏ボード複合体を所定
のサイズに切断することを特徴とする石膏ボード複合体
の製造方法。
Reinforcing paper is affixed to the four circumferential surfaces of the gypsum board, including the top surface, the bottom surface, and both sides in the longitudinal direction, and the top reinforcing paper affixed to the top surface of the gypsum board is attached to both sides of the top surface of the gypsum board in the longitudinal direction. A rubber or soft plastic side seal belt with an L-shaped cross section and an inverted L-shaped cross section contacts or fixes the gypsum board with reinforcing paper, which has an extension part protruding from the edge, on both longitudinal edges of the belt conveyor. The extending portion of the upper reinforcing paper in the gypsum board with reinforcing paper is in contact with the upper surface of the mutually opposing inner step portions of the side seal belts having an L-shaped cross section and an inverted L-shaped cross section. and then supplying a thermosetting foaming resin liquid to the upper surface of the gypsum board with reinforcing paper,
Furthermore, an upper endless belt conveyor is brought into contact with the conveyor belt, and this is guided into a heating curing furnace to form a thermosetting resin foam layer, and then the extending portion of the reinforcing paper in the gypsum board with reinforcing paper is cut, and the A method for manufacturing a gypsum board composite, comprising cutting the gypsum board composite into a predetermined size.
JP61121431A 1986-05-27 1986-05-27 Manufacture of gypsum board composite body Pending JPS62278029A (en)