Prior art keywords
battery
gas
silicic acid
cracks
mixture
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP60296581A
Other languages
Japanese (ja)
Inventor
Mamoru Nishijima
西島 守
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Resonac Corp
Original Assignee
Shin Kobe Electric Machinery Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shin Kobe Electric Machinery Co Ltd filed Critical Shin Kobe Electric Machinery Co Ltd
Priority to JP60296581A priority Critical patent/JPS62154476A/en
Publication of JPS62154476A publication Critical patent/JPS62154476A/en
Pending legal-status Critical Current

Links

Classifications

    • HELECTRICITY
    • H01ELECTRIC ELEMENTS
    • H01MPROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
    • H01M10/00Secondary cells; Manufacture thereof
    • H01M10/06Lead-acid accumulators
    • H01M10/08Selection of materials as electrolytes
    • H01M10/10Immobilising of electrolyte
    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02EREDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E60/00Enabling technologies; Technologies with a potential or indirect contribution to GHG emissions mitigation
    • Y02E60/10Energy storage using batteries

Landscapes

  • Engineering & Computer Science (AREA)
  • Manufacturing & Machinery (AREA)
  • Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Electrochemistry (AREA)
  • General Chemical & Material Sciences (AREA)
  • Secondary Cells (AREA)

Abstract

PURPOSE:To prevent generation of cracks in gelled electrolyte by pouring a mixture of a silicic acid aqueous solution having a specified concentration and suffuric acid solution in a battery and vibrating the battery for a specified time. CONSTITUTION:A mixture of a silicic acid aqueous solution having a specified concentration and sulfuric acid solution is poured in a battery 1. Then, vibration by which the silicic acid gel is converted into the sol by thixotropy is applied to the battery with a vibrator 2 so that the electrolyte is kept in a sol state while gas is evolved for a specified time during which gas in the battery is sufficiently removed. Thereby, generation of cracks of gel caused by gas is prevented, and oxygen gas evolved in charge is transferred to the whole area of an anode plate to uniformly conduct oxygen gas reducing reaction in the anode, and the early deterioration in active material caused by ununiform specific gravity distribution is prevented.

Description

【発明の詳細な説明】 産業上の利用分野 本発明は密閉型鉛蓄電池の製造法に関するものである。[Detailed description of the invention] Industrial applications The present invention relates to a method for manufacturing a sealed lead-acid battery.

従来の技術 従来、ゲル電解液を用いた密閉型鉛蓄電池のケイ酸水溶
液と硫酸溶液の混合液の注液時において、セパレーター
、ガラスマット、極板等の空孔内へ前記混合液が浸入す
る時、多量のガスが発生するが、このガスは前記混合液
かゲル化する過程で連続し゛〔発生するため、ゲル化が
終了し、ガス発生がおさまった時点では、ゲル内にガス
が抜けたことによる亀裂が生じる。
Conventional Technology Conventionally, when a mixed solution of a silicic acid aqueous solution and a sulfuric acid solution is injected into a sealed lead-acid battery using a gel electrolyte, the mixed solution infiltrates into the pores of the separator, glass mat, electrode plate, etc. At this time, a large amount of gas is generated, but this gas is continuously generated during the gelation process of the mixed liquid, so by the time gelation has finished and gas generation has stopped, gas has escaped into the gel. Cracks occur due to this.

発明が解決しようとする問題点 この亀裂のために充電時に発生する酸素ガスは極板上部
へ容易に移動し、陰極での酸素ガスの還元反応は陰極上
部で起こり易くなる。これより寿命が進むに従い、上部
で比重が低く、下部で比重が高くなり、下部の方では活
物質の早期劣化が起こるという問題か生じる。
Problems to be Solved by the Invention Due to these cracks, oxygen gas generated during charging easily moves to the upper part of the electrode plate, and the reduction reaction of oxygen gas at the cathode tends to occur at the upper part of the cathode. As the life progresses beyond this point, the specific gravity becomes lower in the upper part and higher in the lower part, leading to the problem that early deterioration of the active material occurs in the lower part.

問題点を解決するための手段 本発明は上記欠点であるゲル電解液の亀裂の発生を防ぐ
もので、ケイ酸水溶液と硫酸溶液の混合液を電池内に注
入後、電池を所定時間振動させることを特徴とする。
Means for Solving the Problems The present invention prevents the occurrence of cracks in the gel electrolyte, which is the above-mentioned drawback, by injecting a mixture of a silicic acid aqueous solution and a sulfuric acid solution into the battery, and then vibrating the battery for a predetermined period of time. It is characterized by

実施例 本発明の一実施例を説明する。Example An embodiment of the present invention will be described.

図面は前記混合液を注入した電池lを振動発生機2の上
に載せた状態を示したものである。
The drawing shows a state in which a battery 1 injected with the liquid mixture is placed on a vibration generator 2.

ここで前記混合液りを注入した後、この振動発生機2を
用いて、一定時間、例えば該混合液がゲル化し、電池内
のガスが充分抜けるまでの間、ケイ酸ゲノソルによう変
する程度の振動を電池にかけることにより、ガスが発生
している間、電解液はゾル状態を保つようにする。
After injecting the liquid mixture, use the vibration generator 2 for a certain period of time, for example, until the liquid mixture gels and the gas inside the battery is sufficiently discharged, to the extent that it transforms into silicate Genosol. By applying vibrations to the battery, the electrolyte remains in a sol state while gas is generated.

発明の効果 上述したように、本発明によれば前記混合液を注入した
時に発生するガスによるゲルの亀裂発生は防止され、充
電時に発生した酸素ガスの上部へのみの移動は起こらな
く、陰極板の全域に移動する。これにより陰極での酸素
ガス還元反応は均一に生じるので、比重分布の不均一に
よる活物質の早期劣化は防止される。
Effects of the Invention As described above, according to the present invention, cracks in the gel due to the gas generated when the liquid mixture is injected are prevented, and the oxygen gas generated during charging does not move only to the upper part of the cathode plate. move to the entire area. This allows the oxygen gas reduction reaction to occur uniformly at the cathode, thereby preventing early deterioration of the active material due to non-uniform specific gravity distribution.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明の一実施例を示す説明図である。 【は電池、2は振動発生機 FIG. 1 is an explanatory diagram showing one embodiment of the present invention. [ is the battery, 2 is the vibration generator

Claims (1)

【特許請求の範囲】[Claims] 一定濃度のケイ酸水溶液と硫酸溶液の混合液を電池内に
注入した後、所定時間該電池に振動をかけることを特徴
とする密閉型鉛蓄電池の製造法。
1. A method for manufacturing a sealed lead-acid battery, which comprises injecting a mixture of a silicic acid aqueous solution and a sulfuric acid solution at a certain concentration into the battery, and then applying vibration to the battery for a predetermined period of time.
JP60296581A 1985-12-25 1985-12-25 Manufacture of sealed lead-acid battery Pending JPS62154476A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP60296581A JPS62154476A (en) 1985-12-25 1985-12-25 Manufacture of sealed lead-acid battery

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
JP60296581A JPS62154476A (en) 1985-12-25 1985-12-25 Manufacture of sealed lead-acid battery

Publications (1)

Publication Number Publication Date
JPS62154476A true JPS62154476A (en) 1987-07-09

Family

ID=17835396

Family Applications (1)

Application Number Title Priority Date Filing Date
JP60296581A Pending JPS62154476A (en) 1985-12-25 1985-12-25 Manufacture of sealed lead-acid battery

Country Status (1)

Country Link
JP (1) JPS62154476A (en)

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0736922A1 (en) * 1995-04-08 1996-10-09 Compagnie Européenne d'Accumulateurs Process for manufacturing a lead accumulator
US7682738B2 (en) 2002-02-07 2010-03-23 Kvg Technologies, Inc. Lead acid battery with gelled electrolyte formed by filtration action of absorbent separators and method for producing it

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0736922A1 (en) * 1995-04-08 1996-10-09 Compagnie Européenne d'Accumulateurs Process for manufacturing a lead accumulator
US7682738B2 (en) 2002-02-07 2010-03-23 Kvg Technologies, Inc. Lead acid battery with gelled electrolyte formed by filtration action of absorbent separators and method for producing it

Similar Documents

Publication Publication Date Title
SE8106554L (en) BLYACKUMULATOR AND WAY TO MAKE IT
GB1139082A (en) Gas-tight lead accumulator
JPS62154476A (en) Manufacture of sealed lead-acid battery
ATE152861T1 (en) METHOD FOR PRODUCING A LEAD BATTERY WITH A THIXOTROPIC GEL ELECTROLYTE
JPH06260208A (en) Sealed lead-acid battery
JPH06251759A (en) Separator for lead-acid battery
JPH0696793A (en) Manufacture of sealed lead-acid battery
KR100531545B1 (en) Manufacturing method for storage battery
JPS5956367A (en) Sealed lead-acid battery
JPS61124052A (en) Manufacture of pole plate for lead storage battery
JP2581237B2 (en) Manufacturing method of sealed lead-acid battery
JPH05217572A (en) Manufacture of lead-acid battery
JPH064536Y2 (en) Lead acid battery
JP2952374B2 (en) Sealed lead-acid battery
JPS62229666A (en) Manufacture of gel sell
JP2003178794A (en) Production process of sealed lead acid storage battery
JP2002134159A (en) Sealed lead-acid battery
JP2573094B2 (en) Manufacturing method of sealed lead-acid battery
JPS5727567A (en) Manufacture of battery
JPS6220242A (en) Manufacture of button type alkaline cell
JPS5951712B2 (en) Lead-acid battery manufacturing method
JPS62126565A (en) Manufacture of sealed lead-acid battery
JPS5818874A (en) Manufacture of lead storage battery
JPH04308666A (en) Gel type sealed lead-acid battery
JPS607069A (en) Manufacture of sealed lead-acid battery