JPS5915407A - Polymerization of 1-olefin - Google Patents
Polymerization of 1-olefinInfo
- Publication number
- JPS5915407A JPS5915407A JP12301482A JP12301482A JPS5915407A JP S5915407 A JPS5915407 A JP S5915407A JP 12301482 A JP12301482 A JP 12301482A JP 12301482 A JP12301482 A JP 12301482A JP S5915407 A JPS5915407 A JP S5915407A
- Authority
- JP
- Japan
- Prior art keywords
- compound
- polymerization method
- polymerization
- catalyst
- group
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【発明の詳細な説明】
本発明は、エチレンもしくけエチレンと他の1−オレフ
ィンを重合する方法に関するものである。DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for polymerizing ethylene and other 1-olefins.
さらに詳しくは、特定のクロム成分、マグネシウム成分
、チタン(もしくはバナジウム、ジルコニウム)成分の
反応生成物をシリカなどの無機酸化物に担持し焼成した
固体成分(ホ)と、有機アルミニウムなどの有機金属化
合物Q3)とを組み合わせた新規で、活性が高く、かつ
生成ポリマーの分子量分布の広い触媒を用いることを特
徴とするオレフィン重合方法に関するものである。More specifically, solid components (e) are made by supporting reaction products of specific chromium components, magnesium components, and titanium (or vanadium, zirconium) components on inorganic oxides such as silica and firing them, and organometallic compounds such as organoaluminum. Q3) This relates to an olefin polymerization method characterized by using a novel catalyst with high activity and a wide molecular weight distribution of the produced polymer.
酸化クロム等のクロム化合物をシリカ、シリカ−アルミ
ナ等の無機酸化物担体に担持させ焼成することによって
得られるエチレーン重合用触媒は、いわゆるフィリップ
ス型触媒として広く知られておシ、一般に生成ポリマー
の分子量分布が広いことから、例えば中空成形、押出成
形用途に適したポリマーを製造するために賞月されてい
る。The ethylene polymerization catalyst obtained by supporting a chromium compound such as chromium oxide on an inorganic oxide support such as silica or silica-alumina and firing it is widely known as a so-called Phillips type catalyst, and generally the molecular weight of the produced polymer is low. Because of its wide distribution, it is prized for producing polymers suitable for blow molding and extrusion applications, for example.
しかし、この触媒を使用する場合、触媒の活性および重
合体の平均分子−量は、重合温度に大きく依存し、市販
に適した分子量数万〜数十万の重合体を十分な触媒活性
のもとで製造するためには、一般に重合温度を1oo〜
200℃にする必要があった。このような温度範囲で重
合を行なう場合、生成する重合体は反応溶媒に溶解した
状態となるため、反応系の粘度が著しく上昇し、その結
果として、生成重合体濃度を20%以上に上げることが
困難であった。したがって、重合がいわゆるスラリー重
合となる100℃以下の重合温度において、高い触媒活
性を示す触媒の開発が強く求められていた。さらに加え
て、近時は生産コストの低減のため、重合後工程におい
ての触媒除去工程を省略でき′ることか重要であり、こ
のためにはさらに高い活性を示す触媒の開発が必要とさ
れ1きている。However, when using this catalyst, the activity of the catalyst and the average molecular weight of the polymer greatly depend on the polymerization temperature. In order to produce with
It was necessary to raise the temperature to 200°C. When polymerization is carried out in such a temperature range, the produced polymer will be dissolved in the reaction solvent, so the viscosity of the reaction system will increase significantly, and as a result, the concentration of the produced polymer will increase to 20% or more. was difficult. Therefore, there has been a strong demand for the development of a catalyst that exhibits high catalytic activity at a polymerization temperature of 100° C. or lower, at which polymerization becomes so-called slurry polymerization. In addition, in order to reduce production costs, it is important these days to be able to omit the catalyst removal step in the post-polymerization process, and this requires the development of catalysts that exhibit even higher activity. coming.
本発明者らは、上記の観点から種々検討を重ねた結果、
特定のクロム成分、マグネシウム成分、−Flン(もし
くはバナジウム、ジルコニウム)成分の反応生成物をシ
リカなどの担体に担持し焼成活性化した固体と、有機金
属化合物とを組み合わせた触媒が、100℃以上のみで
なく100℃以下の低温における重合においても極めて
高い触媒活性を示し、かつ成形加工容易な分子量および
広い分子量分布を持つポリマーを容易に製造できること
を見出し1本発明に到達した。As a result of various studies from the above viewpoint, the present inventors found that
A catalyst is a combination of a reaction product of a specific chromium component, magnesium component, -Flin (or vanadium, zirconium) component supported on a carrier such as silica and activated by firing, and an organometallic compound. The present inventors have discovered that it is possible to easily produce a polymer that exhibits extremely high catalytic activity not only in polymerization at low temperatures of 100° C. or lower, but also has a molecular weight that is easily molded and has a wide molecular weight distribution, and has thus arrived at the present invention.
すなわち、本発明は、■(1−1)結晶水含有3価クロ
ト化合物と、(1=+)マグネシウムアルコラードと、
(1−iii)チタン、バナジウム、/
ジルコニウムから成る群よシ選ばれた遷移金属のアルコ
ラ−トもしくはオキジアルコラードとの反応生成物を、
ρ)無機酸化物担体に担持髪し焼成した固体成分と、偉
)有機金属化合物とから成る触媒を用いることを特徴と
するオレフィンの重合方法に係るものである。That is, the present invention comprises: (1-1) a trivalent croto compound containing water of crystallization; (1=+) magnesium alcoholade;
(1-iii) a reaction product of a transition metal selected from the group consisting of titanium, vanadium, and/or zirconium with an alcoholate or oxyalcoholade;
This invention relates to an olefin polymerization method characterized by using a catalyst consisting of ρ) a solid component supported on an inorganic oxide carrier and fired, and ρ) an organometallic compound.
特定のクロム成分、マグネシウム成分、チタン(もしく
はバナジウム、ジルコニウム)成分の反応生成物をシリ
カなどの担体に担持し焼成活性化した固体と、有機金属
化合物とを糾み合わせた本発明の触媒を用いる重合方法
においては、後述の実施例ならびに比−例から明らかな
通り、マグネシウム成分が含まれていない場合に比べて
分子量が下がって(MIが上がって)、成形加工に適し
た分子量となっておシ、またマグネシウム成分およびチ
タン成分の双方が含まれていない場合に比べて分子量分
布が広<(P几が土がって)、中空成形や押出成形に、
より適した流動性となっている。そして、いずれの場合
においても、本発明の触媒を用いる方がさらに活性が高
く、まことに好適である。The catalyst of the present invention is a combination of a solid obtained by supporting a reaction product of a specific chromium component, magnesium component, titanium (or vanadium, zirconium) component on a carrier such as silica and activated by firing, and an organometallic compound. In the polymerization method, as is clear from the examples and proportions described later, the molecular weight is lower (MI is higher) than when no magnesium component is included, and the molecular weight is suitable for molding. In addition, the molecular weight distribution is wider than when both magnesium and titanium components are not included.
It has more suitable liquidity. In any case, the use of the catalyst of the present invention has even higher activity and is therefore suitable.
以下、本発明の詳細な説明する。The present invention will be explained in detail below.
本発明に用いる無機酸化物担体としては、シリカ、アル
ミナ、シリカ−アルミナ、ドリア、ジルコニア等を用い
ることができるが、シリカ、シリカ−アルミナが好まし
く、特にシリカが好ましい。As the inorganic oxide carrier used in the present invention, silica, alumina, silica-alumina, doria, zirconia, etc. can be used, but silica and silica-alumina are preferable, and silica is particularly preferable.
本発明の(1−1)に用いる結晶水含有3価クロム化合
物としては、酢酸クロム、シュウ酸クロム、塩化クロム
、硝酸クロムなどの水和塩ならびに複塩などが挙げられ
、好ましくは(C)I、c、’oo )aCr・11−
1.0、Cr(NO3)、 −9H,0、CrCt、−
6H,0カ挙けられる。本発明に(マグネシウムアルコ
ラードとともに)用いるクロム化合物は、結晶水を含有
しているものであることが重要である。無水のものでは
本発明の効果は発揮されない。Examples of the crystal water-containing trivalent chromium compound used in (1-1) of the present invention include hydrated salts and double salts such as chromium acetate, chromium oxalate, chromium chloride, and chromium nitrate, and preferably (C) I, c, 'oo) aCr・11-
1.0, Cr(NO3), -9H,0, CrCt, -
6H, 0 can be mentioned. It is important that the chromium compound used in the present invention (along with the magnesium alcoholade) contains water of crystallization. The effects of the present invention cannot be achieved with anhydrous materials.
本発明の(1−It )に用いるマグネシウムアルコラ
ードとしては、Mg(QC搗)7、Mg(OCj(s
)y、M5((Q i s o −C,H,)、などの
各種アルコラードを挙げることができ、好ましくはMg
(OCtHs )tが用いられる。The magnesium alcoholade used in (1-It) of the present invention includes Mg(QC)7, Mg(OCj(s)
)y, M5((Q i s o -C,H,), etc., and preferably Mg
(OCtHs)t is used.
本発明の(1−tri )に用いるチタン、バナジウム
、ジルコニウムから成る群より選ばれた遷移金属のアル
コラードもしくはオキシアルコラ−トドしては、例えば
、’l’i (On −C4H,)、 、 Ti (U
i 5o−C,IA、f)、 。The transition metal alcoholade or oxyalcoholate selected from the group consisting of titanium, vanadium, and zirconium used in (1-tri) of the present invention is, for example, 'l'i (On -C4H,), Ti ( U
i5o-C,IA,f),.
VO(On C4HO)s、zr (On −C4H
o )4、Z ro (n C4搗)tなどが挙げら
れ、好ましくはTi (On −04H,)4、VO(
OnC4H9)!、7.r(Qn−C4H,)4が用い
られる。VO(On C4HO)s,zr(On -C4H
o ) 4, Z ro (n C4 搗) t, etc., preferably Ti (On -04H,) 4, VO (
OnC4H9)! ,7. r(Qn-C4H,)4 is used.
不発明細に用いる有機金属化合物としては、有機アルミ
ニウム化合物、有機ホウ素化合物、有機亜鉛化合物、有
機リチウム化合物、炭化水累司溶性有機マグネシウム化
合物もしくは錯化介物などが挙げられ、例えば、トリエ
チルアルミニウム、トリイソブチルアルミニウム、トリ
r1−−−\ギソルアルミニウム、トリデシルアルミニ
ウム、ジエチルアルミニウムハイドライド、アルミニラ
j・イソプレニル、ジェチルアルミニウムエトギンド、
メチルエチルヒドロシロキシアルミニウムジエチルなら
び忙これらの混合物、トリエチルボウ素、ジエチル咀鉛
、n−ブチルリチウム、ジ11− ブチ/l/マグネシ
ウム−トリエチルアルミニウム錯化合物、n−ブチル5
ec−フ゛デルマグネシウム、11−ブJルエチルマグ
ネシウノ、などが挙げられる。vr−iしくけアルコキ
シ基またはシロキシ基の少なくとも一方を含有するイ1
機アルミニウム化合I吻が用いられる。Examples of organometallic compounds used in the invention include organoaluminum compounds, organoboron compounds, organozinc compounds, organolithium compounds, hydrocarbon-soluble organomagnesium compounds, and complex inclusions, such as triethylaluminum, triethylaluminum, isobutylaluminum, trir1--\gysolaluminum, tridecylaluminum, diethylaluminum hydride, aluminiraj isoprenyl, diethylaluminum etogindo,
Diethyl methyl ethylhydrosiloxyaluminum and mixtures thereof, triethyl boron, diethyl masticate, n-butyl lithium, di11-buty/l/magnesium-triethyl aluminum complex, n-butyl 5
Examples include ec-ferdelmagnesium, 11-butyl ethylmagnesium, and the like. vr-i containing at least one of an alkoxy group or a siloxy group
A aluminum compound I proboscis is used.
次に、(1−1)のクロム化合物と(1−it)のマグ
ネシウム化合物と(1−i*)のチタン化合物(または
バナジウム、ジルコニウム化合物)トを反応させ、続い
て無機酸化物担体にJ[1持−)る仁とについて説明す
る。Next, the chromium compound (1-1), the magnesium compound (1-it), and the titanium compound (or vanadium or zirconium compound) (1-i*) are reacted, and then J I will explain about [1 have-)ru jin.
(1−i)の結晶水含有3価クロム化合物と、(1−1
+ )のマグネシウムアルコラードと、(1=t+)の
チタン(もしくはバナジウム、ジルコニウム)のアルコ
ラード(もしくはオキジアルコラード)との反応は、四
塩化炭素、クロロホルム、メチレンクロライドなどの塩
素化炭化水素、ベンゼン、トルエン、キシレンなどの芳
香族炭化水素、ヘキサン、ヘプタン、イソオクタンなど
の脂肪族炭化水素、シクロヘキサン、メチルシクロヘキ
サンなどの脂環式炭化水素などの媒体中、もしくはこれ
らの媒体にエタノール、イソプロパツールなどのアルコ
ール類を混合した媒体中で行なうことができる。好まし
くは四塩化炭素、クロロホルムなどの塩素化炭化水素中
で反応を行なう。反応させる順序には制限はないが、好
1しくは(1−1+)のマグネシウム化合物と(1−+
++ )のチタン(またtまバナジウム、ジルコニウム
)化合物を先に混合、攪拌し、その後に(1−i)のク
ロム化合物を加える方法か、もしくは(1−1)のクロ
ム化合物と(1−++)のマグネシウム化合物を先に混
合、攪拌し、その後に(1−tri )のチタン(゛ま
たはバナジウム、ジルコニウム)化合物を加える方法が
採用される。混合反応のモル比については、特に制限は
ないが、好ましくは(1−1)のCrと(1−H)の鳩
と(1−+++ >のTI(もしくし↓V、Zr )の
モ/L/比がMg/Cr ”=1〜l O1’l”i(
V、Z[)/Cr二0.25〜10の範囲にあることが
推奨される。反応温度、反応時間についても特に制限は
ないが、反応の進行上好ましくは0〜200℃、l薩に
好ましくは30〜120℃の温ノ蔓で、0.5〜121
寺1川反応させる。反応混合物の状態は、溶媒や反+、
=、条件によるが、クロム、マグネシ−ラム、チタン等
が一部または大部分溶解したスラリー状態もしくは溶液
となる。(1-i) trivalent chromium compound containing crystal water;
The reaction between the magnesium alcolade (+) and the titanium (or vanadium, zirconium) alcolade (or oxyalcolade) (1=t+) can be performed using carbon tetrachloride, chloroform, chlorinated hydrocarbons such as methylene chloride, benzene, etc. , aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as hexane, heptane, and isooctane, and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane. It can be carried out in a medium mixed with alcohols. Preferably, the reaction is carried out in a chlorinated hydrocarbon such as carbon tetrachloride or chloroform. There is no restriction on the order of reaction, but preferably (1-1+) magnesium compound and (1-+
++ ) titanium (or vanadium, zirconium) compound is first mixed and stirred, and then (1-i) chromium compound is added, or (1-1) chromium compound and (1-++ ) is first mixed and stirred, and then (1-tri) of titanium (or vanadium, zirconium) compound is added. There is no particular restriction on the molar ratio of the mixed reaction, but preferably (1-1) Cr, (1-H) and (1-+++ > TI (or ↓V, Zr) mo/ L/ratio is Mg/Cr"=1~l O1'l"i(
It is recommended that V, Z[)/Cr2 be in the range of 0.25 to 10. There are no particular restrictions on the reaction temperature and reaction time, but in view of the progress of the reaction, preferably 0 to 200 °C, preferably 30 to 120 °C, and 0.5 to 120 °C.
Temple 1 River reacts. The state of the reaction mixture is the solvent, anti+,
= Depending on the conditions, it becomes a slurry state or solution in which chromium, magnesium, titanium, etc. are partially or mostly dissolved.
このようにして膨大したクロム、マグネシウム、チタン
等を含有する反応混合物jをシリカ、シリカ−アルミナ
等の無機酸化物担体と混合し、担持させる。この際には
、攪拌しつつ担持きせることか望ましい。担持させる際
の温度、時間等には特に制限はなく、溶剤はp過もしく
は蒸留によって除去する。溶剤を蒸留で留去してクロ太
等を付着担持させる場合、200℃以下の温度に1行な
うのが望ましい。担持させる金属の量については、担持
後の固体中のクロム含量が0.02〜2,5重量%。The reaction mixture j containing chromium, magnesium, titanium, etc. expanded in this way is mixed with an inorganic oxide support such as silica, silica-alumina, etc., and supported. At this time, it is preferable to support the particles while stirring. There are no particular restrictions on the temperature, time, etc. for supporting, and the solvent is removed by filtration or distillation. When the solvent is removed by distillation to deposit and support black fat, etc., it is desirable to carry out the reaction at a temperature of 200° C. or lower. Regarding the amount of metal to be supported, the chromium content in the solid after being supported is 0.02 to 2.5% by weight.
特KO,05〜1.5重量−の範囲にあることが好まし
い。なお、担体としで用いるシリカ、シリカ−アルミナ
等は事前に、例えば霊素気流下で加熱乾燥しておくこと
が好ましい。It is preferable that the weight is in the range of 05 to 1.5% by weight. Incidentally, it is preferable that silica, silica-alumina, etc. used as a carrier be heated and dried in advance, for example, under a stream of spirit gas.
次に、担持済同体の焼成活性化についで説明する。Next, firing activation of the supported body will be explained.
焼成活性化は、−・般に酸素の存在下、非還元性雰囲気
で行なうが、不活性ガスあるいは減圧下で行なうことも
oJ能である。好ましくは水分を実質的に宮まない空気
が用いられる。焼成温度は300℃以上、好ましくld
400〜900 ℃ノ温度範囲で数分〜数十時間、好ま
しくは30分〜lO時間行なわれる。焼成時には充分乾
燥空気を吹込み、流動状態)で焼成活性化を行なうこと
が推奨される。Firing activation is generally carried out in the presence of oxygen in a non-reducing atmosphere, but it can also be carried out under an inert gas or reduced pressure. Preferably, air substantially free of moisture is used. The firing temperature is 300°C or higher, preferably ld
The reaction is carried out at a temperature of 400 to 900° C. for several minutes to several tens of hours, preferably 30 minutes to 10 hours. During firing, it is recommended to blow in enough dry air to activate firing in a fluidized state.
なお、担持もしくは焼成時にフッ素含有塩類を添加して
、活性や分子量等を調節する公知の方法を併用すること
も勿論可能である。Of course, it is also possible to use a known method of controlling activity, molecular weight, etc. by adding fluorine-containing salts during supporting or firing.
次に、(イ)の固体成分(すなわち、担体に担持され焼
成活性化されたクロム、マグネシウム、チタンなどを含
有する固体)と8)の有機金属化合物とを組み合わせる
方法について説明する。Next, a method of combining the solid component (a) (ie, a solid containing chromium, magnesium, titanium, etc. supported on a carrier and activated by firing) with the organometallic compound of 8) will be described.
(ハ)の固体成分と63)の有機金属化合物とは、重合
条件下に重合系内に添加してもよいし、あらかじめ重合
に先立って組み合わせてもよい。また、固体成分をあら
かじめ該有機金属化合物にて処理した後に、さらに有機
金属化合物と組み合せて重合系内に送シ込むといっだ方
法も可能である。組み合せる両成分の比率は、(有機金
属)/C【の モル比で0.01〜3000、好壕しく
はo、1〜io。The solid component (c) and the organometallic compound 63) may be added to the polymerization system under polymerization conditions, or may be combined in advance prior to polymerization. It is also possible to carry out a method in which the solid component is previously treated with the organometallic compound and then combined with the organometallic compound and fed into the polymerization system. The ratio of both components to be combined is (organometallic)/C molar ratio of 0.01 to 3000, preferably o, 1 to io.
の範囲が推奨される。range is recommended.
次に、本発明の触媒を用いてメレフィンを重合する方法
に関して説明する。Next, a method for polymerizing melefin using the catalyst of the present invention will be explained.
本発明の触媒を用いて重合しうるオレフィンはα−オレ
フィンであり、特にエチレンである1、さらに本発明の
触媒はエチレンとプロピレン、ププーン・−11ヘキセ
ン−1等のモノオレフィンとの共重合、あるいはさらに
ブタジェン、インプレン等のジエンの共存下での重合に
用いることも可能である。The olefins that can be polymerized using the catalyst of the present invention are α-olefins, particularly ethylene1, and the catalyst of the present invention can also be used to copolymerize ethylene with monoolefins such as propylene, pupoon-11hexene-1, etc. Alternatively, it is also possible to use it for polymerization in the coexistence of a diene such as butadiene or imprene.
本発明の触媒を用い、共重合を実施することによって密
度0.91〜0.97 y/atlの範囲のポリマーを
製造することが可能である。By carrying out copolymerization using the catalyst of the present invention, it is possible to produce a polymer having a density in the range of 0.91 to 0.97 y/atl.
重合方法としては、通常の懸濁重合、溶液重合、気相重
合が可能である。懸濁重合、溶液重合の場合は触媒を重
合溶媒、たとえは、プロパン、ブタン、ペンタン、ヘキ
サン、ヘプタンのごとき脂肪族炭化水i 、ベンゼン、
トルエン、キシレンのごとき芳香族炭化水素、シクロヘ
キサン、メチルシクロヘキサンのごとき脂環式炭化水嵩
と\もに反応器に導入し、不活性雰囲気下にエチレンを
1〜200に/Iに圧入して、室温ないし320℃の温
度で重合を進めることができる。また、チューブラ−反
応器、オートクレーブ反応器、オートクレープルチュー
ブラ−反応器などを用いて、たとえば圧力200〜20
00kf/d、温度150〜300℃なる条件で重合を
行なう、いわゆる高圧重合法も適用することが可能であ
る、
一方、気相重合はエチレンを1〜501薗の圧力で室温
ないし120℃の温度条件下で、エチレンと触媒の接触
が良好となるよう流動床、移動床、あるいは攪拌によっ
て混合を行なう等の手段を講じて重合を行なうことが■
J能である。As the polymerization method, usual suspension polymerization, solution polymerization, and gas phase polymerization are possible. In the case of suspension polymerization and solution polymerization, the catalyst is used as a polymerization solvent, such as aliphatic hydrocarbons such as propane, butane, pentane, hexane, and heptane, benzene,
Aromatic hydrocarbons such as toluene and xylene, and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane were introduced into a reactor, and ethylene was injected to a concentration of 1 to 200/I under an inert atmosphere, and the mixture was heated to room temperature. Polymerization can proceed at temperatures between 320°C and 320°C. In addition, using a tubular reactor, an autoclave reactor, an autoclave tubular reactor, etc., a pressure of 200 to 200
It is also possible to apply the so-called high-pressure polymerization method in which polymerization is carried out under conditions of 00 kf/d and a temperature of 150 to 300°C.On the other hand, in gas phase polymerization, ethylene is polymerized at a pressure of 1 to 501 kf at a temperature of room temperature to 120°C. Polymerization can be carried out under the following conditions, using methods such as a fluidized bed, moving bed, or stirring to ensure good contact between ethylene and the catalyst.
It is J-Noh.
本発明の触媒は高性能であり、80℃、10ks/m程
度の比較的低温低圧の重合条件下においても充分に高い
活性を示す。この場合には、生成する重合体岐重合系に
スラリー状態で存在するため、重合系の粘度上昇がきわ
めて少ない。したがって、重合系の重合体濃度を30チ
以上にもすることができ、生産効率面上等の利点が大き
い。また高活性のため、生成ポリマーからの触媒残渣除
去工程は省略できる。The catalyst of the present invention has high performance and exhibits sufficiently high activity even under relatively low temperature and low pressure polymerization conditions of about 80° C. and 10 ks/m. In this case, since it exists in a slurry state in the branched polymer system to be produced, the increase in viscosity of the polymer system is extremely small. Therefore, the polymer concentration in the polymerization system can be increased to 30% or more, which has great advantages in terms of production efficiency and the like. Furthermore, due to its high activity, the step of removing catalyst residue from the produced polymer can be omitted.
重合は1反応帯を用いる通常の1段重合で行なってもよ
いし、または複数個の反応帯を用いる、いわゆる多段重
合で行なってもよい。本発明の触媒を用いて重合したポ
リマーは1通常の1段重合でも広い分子量分布をもち、
中空成形や押出成形用途忙極めて適している″62個以
上の異なった反応条件下で重合を行なう多段重合では、
さらに広い分子量分布のポリマーの製造が可能である。The polymerization may be carried out in a conventional one-stage polymerization using one reaction zone, or in a so-called multi-stage polymerization using a plurality of reaction zones. The polymer polymerized using the catalyst of the present invention has a wide molecular weight distribution even in a normal one-stage polymerization,
It is extremely suitable for blow molding and extrusion molding applications. ``Multi-stage polymerization in which polymerization is carried out under more than 62 different reaction conditions''
It is possible to produce polymers with even wider molecular weight distributions.
ポリマーの分子量を調節するために、重合温度の調節、
重合系への水素の添加、あるいは連鎖移動を起こし易い
有機金属化合物の添加等の公知の技術を用いることも勿
論可能である。さらに、チタン酸エステルを添加して密
度調節、分子量調節を行なう等の方法を組み合わせて重
合を実施することもまた可能である。Adjustment of polymerization temperature to adjust the molecular weight of the polymer,
Of course, it is also possible to use known techniques such as adding hydrogen to the polymerization system or adding an organometallic compound that is likely to cause chain transfer. Furthermore, it is also possible to carry out the polymerization by combining methods such as adding a titanate ester to control density and molecular weight.
以下、本発明の実施例を示すが、本発明は、これらの実
施例によって何ら制限されるものではない。Examples of the present invention will be shown below, but the present invention is not limited to these Examples in any way.
なお、実施例中の触媒活性とは、モノマー圧力10唾−
において、触媒固体成分1f・1時間肖υのポリマー生
成j1 (r)を表わす。また、MIはメルトインデッ
クスを表わし、A、9TM・D−1238にしたがい、
温度190℃、荷重2.16 ktにて測定したもので
ある。Fl(、は温度190℃、荷重21.6輪にて測
定した偵をMIで除した商であり、分子量分布の広さを
表わす指標として当業者に知られているもの“である。In addition, the catalytic activity in the examples refers to monomer pressure of 10 mm.
represents the polymer production j1 (r) of the catalyst solid component 1f/1 hour time υ. Also, MI stands for melt index, and according to A, 9TM D-1238,
It was measured at a temperature of 190°C and a load of 2.16 kt. Fl (, is the quotient obtained by dividing the value measured at a temperature of 190° C. and a load of 21.6 wheels by MI, and is known to those skilled in the art as an index representing the breadth of molecular weight distribution.
実施例1゜
(1)固体成分翰の合成
窒素気流下、200−フラスコに四塩化炭素100−と
Mg(QC,H,ル11.4 W (100tnmol
)を仕込んだ。この懸濁液にTj (On −C4H,
)46.8 F (20mmoL )を添加し、加熱還
流下に5時間攪拌した。Example 1゜(1) Synthesis of solid components 100% carbon tetrachloride and 11.4 W (100 tnmol
) was prepared. Tj (On -C4H,
) 46.8 F (20 mmol) was added thereto, and the mixture was stirred for 5 hours while heating under reflux.
その後にcrcz、−6H405,3F (20mTn
ot )iJI]、j、さらに8時間加熱還流下に攪拌
した。次に、四塩化炭素80−を加えて稀釈17、Cr
、 Mg、 i’i ヲ含イ#する反応混合物を得た。Then crcz, -6H405,3F (20mTn
ot)iJI], j, and the mixture was further stirred under heating and reflux for 8 hours. Next, add 80 − of carbon tetrachloride to dilute 17, Cr
A reaction mixture containing , Mg, and i'i was obtained.
別の2tフラスコの内部を乾燥窒素で置換し、あらかじ
め300℃の乾燥窒素流通下で2時間乾燥したシリカゲ
ル(富士デヴイソン社與・グレード952)100Fと
脱水脱気した四塩化炭素1tを仕込み、この中へ攪拌し
つつ上記のCr、Mg、rlTi含有反応混合物の全景
を室温にで加え、1時間攪拌した。次に、蒸留により溶
媒の四塩化炭素を留去し、続いて60℃で5時間真空乾
燥して、クロム−マグネシウム−チタン相持済固体を得
た。The inside of another 2t flask was replaced with dry nitrogen, and 100F of silica gel (manufactured by Fuji Davison, grade 952), which had been previously dried under dry nitrogen flow at 300°C for 2 hours, and 1t of dehydrated and degassed carbon tetrachloride were charged. The entire reaction mixture containing Cr, Mg, and rlTi was added to the mixture at room temperature while stirring, and the mixture was stirred for 1 hour. Next, the solvent carbon tetrachloride was removed by distillation, followed by vacuum drying at 60° C. for 5 hours to obtain a chromium-magnesium-titanium phase-supported solid.
次に、との担持済固体を石英製焼成管に入れ、乾燥窒素
流通下800℃で5時間焼成して、触媒固体成分代を得
た。得られた固体成分へ)はクロムを1.0重挙チ含有
し、窒素雰囲気下室温にて貯蔵した。Next, the supported solid was placed in a quartz firing tube and fired at 800° C. for 5 hours under dry nitrogen flow to obtain a catalyst solid component. The obtained solid component contained 1.0 times chromium and was stored at room temperature under a nitrogen atmosphere.
(2)重合
0)で合成した固体成分(至)20■と、有機金属化合
物43)としてジエチルアルミニウムエトキシド0.1
mm01 とを、脱水脱酸素したヘキサン0.8tとと
もに、内部を真空脱気し窒素置換した1、5tのオート
クレーブに入れた。オートクレーブの内温を80℃に保
ち、エチレンを10に〜加え、水素を加えて全圧を14
ψ−としだ。エチレンを補給することによシ全圧を14
に〜の圧力に保ちつつ2時間重合を行ない、16 (l
fのポリマーを得た。(2) Solid component (to) 20■ synthesized in polymerization 0) and diethylaluminum ethoxide 0.1 as organometallic compound 43)
mm01 and 0.8 t of dehydrated and deoxygenated hexane were placed in a 1.5 t autoclave whose interior was vacuum degassed and replaced with nitrogen. Keep the internal temperature of the autoclave at 80℃, add ethylene to 10℃, and add hydrogen to bring the total pressure to 14℃.
ψ− Toshida. By replenishing ethylene, the total pressure was increased to 14
Polymerization was carried out for 2 hours while maintaining the pressure at ~16 (l
A polymer of f was obtained.
触媒活性は4000Fポリ? −/ y 5olid
e hr 。Is the catalyst activity 4000F poly? -/y 5olid
ehr.
ポリマーのMlは0.61、Fl(は102であった。The Ml of the polymer was 0.61 and Fl( was 102).
比較例人。Comparative example.
固体成分(転)の合成においでMg((疋J(s )z
を用いず、その他はすべて実施例1と全く同様にして、
触媒合成および重合を行なった。重合結果は1.l?
+17−収77102 f、触媒活性2550、八41
0.21、FR100であった。In the synthesis of solid components (conversion), Mg ((
was not used, and everything else was the same as in Example 1,
Catalyst synthesis and polymerization were performed. The polymerization results are 1. l?
+17-yield 77102 f, catalyst activity 2550, 841
It was 0.21 and FR100.
比較例B。Comparative example B.
固体成分(ホ)の合成においてMg(QC,H晶と’l
’1(On−〇4H,)、を用いず、その他はすべて実
施例1と全く同様にして触媒合成および重合を行なった
。屯仔結果は、ポリマー収納84り、触媒を古注210
0、Ml O,20、Fl(85であった。In the synthesis of the solid component (e), Mg (QC, H crystal and 'l
Catalyst synthesis and polymerization were carried out in the same manner as in Example 1 except that '1(On-04H,) was not used. The result is that the polymer storage is 84 and the catalyst is old note 210.
0, MlO, 20, Fl (85).
比較例C0
固体成分(イ)の合成において、担持後の焼成操作を行
なわず、その他はすべて実施例1と全く同様にして触媒
合成および重合を行なった(この触媒は特開昭50−1
28693号公報に記載されている)。重合結果は、ポ
リマー収態249、触媒活性600.Mlo、84、F
it 28であった、実施例2〜8
実施例1における固体成分(ホ)の合成条件を変え、オ
・1表の結果を得た。Comparative Example C0 In the synthesis of the solid component (a), the calcination operation after loading was not performed, and the catalyst synthesis and polymerization were carried out in the same manner as in Example 1.
28693). The polymerization results were as follows: polymer yield: 249, catalyst activity: 600. Mlo, 84, F
Examples 2 to 8 The synthesis conditions for the solid component (E) in Example 1 were changed, and the results shown in Table E.1 were obtained.
実施例9〜16゜
実施例1における有機金属化合物(13)の種類および
量を変え、オ・2表の結果を得た。なお、表中のシロキ
シ有機アルミニウム化合物については、本出願人の出願
に係る特公昭46−40334号公報に17たがって、
対比、する有機アルミニウムとアルキルヒト゛ロボ+1
シロキザンとから合成し、有機マグネシウム錯化合物に
ついては、本出願人の出願に係る特開昭50−1574
90号公報および特開昭50−154388号公報にし
たがって、対応する有機マグネシウムと有機アルミニウ
ムとから合成した1、
実施例17、
エチレンの代りにブテン−1を151110t%含有す
るエチレンおよびブテン−1の混合ガスを用い、ヘキサ
ノの代りにイソブチンを重合溶媒と1.てJtiい、8
0℃にて混合ガス分圧10 kp/m、水素外+−r:
1 kv/ffl、溶媒蒸気圧を含め全圧23 kg/
crlとし、子のほかは実施例1の触媒を用い、実施例
1と同様にして重合した。重合結果は、ポリマー収量1
181、触媒活性2950、ML O,67、ボ?ツマ
−の密度は0932てあった。Examples 9 to 16 The type and amount of organometallic compound (13) in Example 1 were changed to obtain the results shown in Table E.2. Regarding the siloxy organoaluminum compounds in the table, according to Japanese Patent Publication No. 46-40334 filed by the present applicant,
Comparison of organic aluminum and alkyl hydrogen robot +1
The organomagnesium complex compound synthesized from siloxane is disclosed in Japanese Unexamined Patent Publication No. 50-1574 filed by the present applicant.
1 synthesized from the corresponding organomagnesium and organoaluminium according to Japanese Patent Application No. 90 and JP-A-50-154388, Example 17. Using a gas mixture, add isobutyne instead of hexano as a polymerization solvent and 1. te Jti, 8
Mixed gas partial pressure 10 kp/m at 0°C, hydrogen outside +-r:
1 kv/ffl, total pressure including solvent vapor pressure 23 kg/
crl and polymerization was carried out in the same manner as in Example 1 using the catalyst of Example 1 except for the catalyst. The polymerization result shows that the polymer yield is 1
181, Catalytic activity 2950, ML O, 67, Bo? The density of Zuma was 0932.
Claims (1)
(1−1+ )マグネシウムアルコラードと、(l−i
)チタン、バナジウム、ジルコニウムから成る群よυ選
ばれた遷移金属のアルコラードもしくはオキジアルコラ
ードとの反応生成物を、(2)無機酸化物担体に担持し
焼成した固体成分と、CB)有機金属化合物とから成る
触媒を用いるオレフィンの重合方法。 2、 (2)の無機酸化物担体がシリカ、シリカ−ア
ルミナ、アルミナから成る群より選ばれたものである特
許請求の範囲、1’1項記載の重合方法。 3、(2)の無機酸化物担体がシリカである特許請求の
範囲第1項記載の重合方法。 4、(1−1)の結晶水含有3価クロム化合物が酢酸ク
ロム水利塩、硝酸クロム水利塩、塩化クロム水利塩から
成る群よシ選ばれたものである特許請求の範囲第1項な
いし】・3項記載の重合方法。 5、(1−I+)のマグネシウムアルコラードがMg
(QC!H1)tである特許請求の範囲第1項ないし牙
4項記載の重合方法。 6、(1−+i1)の遷移金属のアルコラードもしくは
オキジアルコラードがTi (On C4賜)いVO
(On−CaH,)s、 Zr(On−C4H,入から
成る群よυ選ばれたものである特許請求の範囲第1項な
いし牙5JJ記載の重合方法。 7、固体成分の焼成が非還元性雰囲気で行なわれる特許
請求の範囲第1項ないし、1−6項記載の重合方法。 8、[F])の有機金属化合物が有機アルミニウム化合
物、有機ホウ素化合物、有機亜鉛化合物、有機リチウム
化合物、炭化水素可溶性有機マグネシウム化合物もしく
は錯化合物から成る群より選ばれたものである特許請求
の範囲第1項ないしJ−7項記載の重合方法。 96卸の有機金属化合物がアルコキシ基またはシaキシ
基の少なくとも一方を含有する有機アルミニウム化合物
である特許請求の範囲矛8項記載の重合方法。[Claims] 1. (to) (1-1) a trivalent chromium compound containing crystal water;
(1-1+) magnesium alcoholade and (l-i
) A reaction product of a transition metal selected from the group consisting of titanium, vanadium, and zirconium with an alcollade or an oxyalcollade, (2) a solid component supported on an inorganic oxide carrier and fired, and CB) an organometallic compound. A method for polymerizing olefins using a catalyst comprising. 2. The polymerization method according to claim 1'1, wherein the inorganic oxide carrier in (2) is selected from the group consisting of silica, silica-alumina, and alumina. 3. The polymerization method according to claim 1, wherein the inorganic oxide carrier in (2) is silica. 4. Claims 1 to 4, wherein the crystal water-containing trivalent chromium compound of (1-1) is selected from the group consisting of chromium acetate aqueous salt, chromium nitrate aqueous salt, and chromium chloride aqueous salt; - Polymerization method described in Section 3. 5. (1-I+) magnesium alcoholade is Mg
(QC!H1)t. The polymerization method according to claims 1 to 4, wherein (QC!H1)t. 6. (1-+i1) transition metal alcoholade or oxidial alcoholade is Ti (On C4) VO
(On-CaH,)s, Zr(On-C4H, In) The polymerization method according to Claims 1 to 5JJ, wherein the polymerization method is selected from the group consisting of (On-CaH, )s, Zr(On-C4H, 8. The polymerization method according to claims 1 to 1-6, which is carried out in a neutral atmosphere. 8. The organometallic compound in [F]) is an organoaluminum compound, an organoboron compound, an organozinc compound, an organolithium compound, The polymerization method according to claims 1 to J-7, wherein the polymer is selected from the group consisting of hydrocarbon-soluble organomagnesium compounds or complex compounds. 9. The polymerization method according to claim 8, wherein the organometallic compound is an organoaluminum compound containing at least one of an alkoxy group and a hydroxyl group.