JPH0834962A - Tacky agent composition and tacky processed article - Google Patents

Tacky agent composition and tacky processed article

Info

Publication number
JPH0834962A
JPH0834962A JP6170949A JP17094994A JPH0834962A JP H0834962 A JPH0834962 A JP H0834962A JP 6170949 A JP6170949 A JP 6170949A JP 17094994 A JP17094994 A JP 17094994A JP H0834962 A JPH0834962 A JP H0834962A
Authority
JP
Japan
Prior art keywords
weight
softening point
tackifying resin
acid value
tacky
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP6170949A
Other languages
Japanese (ja)
Inventor
Tetsuya Sasada
徹也 笹田
Motoi Nagano
基 長野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd filed Critical Sekisui Chemical Co Ltd
Priority to JP6170949A priority Critical patent/JPH0834962A/en
Publication of JPH0834962A publication Critical patent/JPH0834962A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To obtain a tacky agent composition having excellent heat resistance, adhesiveness to a curved surface, peel strength under fixed load and adhesiveness to a rough face at low temperature and to prepare a tacky processed article. CONSTITUTION:This tacky agent composition comprises 100 pts.wt. of an acrylic polymer, 10-40 pts.wt. of a tackifier resin and 0.01-2 pts.wt. of a curing agent except an isocyanate-based curing agent. The acrylic polymer is composed of 90-99.5 pts.wt. of a mixture of 60-100wt.% of a 2-18C alkyl group-containing (meth)acrylic alkyl ester monomer and 40-0wt.% of a vinyl-based monomer copolymerizable with the alkyl ester monomer and 10-0.5 pt.wt. of a carboxyl group-containing vinyl-based monomer. The tackifier resin has 125-160 deg.C softening point and 0-30 acid value.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、曲面接着性及び定荷重
剥離力に優れ、粘着力、保存力、ボールタック、粗面へ
の接着性、低温時の粘着性、オレフィンへの粘着性及び
初期タック等の物性のバランスに優れた粘着剤組成物及
びこれを塗工してなる粘着加工品に関する。
The present invention has excellent adhesiveness to curved surfaces and peeling force under constant load, adhesive strength, storage power, ball tack, adhesiveness to rough surface, adhesiveness at low temperature, adhesiveness to olefin and The present invention relates to a pressure-sensitive adhesive composition having an excellent balance of physical properties such as initial tack, and an adhesive processed product obtained by coating the same.

【0002】[0002]

【従来の技術】従来から、建材、家電製品、自動車用緩
衝材、隙間テープ等の用途に、両面テープ、フォームテ
ープ等として、表面を粘着で加工した粘着テープ、粘着
シート等の粘着加工品が広く用いられている。
2. Description of the Related Art Conventionally, adhesive products such as double-sided tapes, foam tapes, etc., whose surface has been processed with adhesive, adhesive processed products such as adhesive sheets, have been used for applications such as building materials, home appliances, cushioning materials for automobiles, gap tapes, etc. Widely used.

【0003】上記粘着加工品に用いる粘着剤組成物とし
ては、耐候性、耐久性、耐熱性、耐寒性、耐水性等に優
れることから、アクリル樹脂を主体とする溶剤型粘着剤
組成物が用いられている。近年、これら粘着加工品の用
途拡大に伴い、より高い耐熱性と他の物性とのバランス
に優れた粘着剤の要望が高まっている。
As the pressure-sensitive adhesive composition used for the above-mentioned pressure-sensitive adhesive processed product, a solvent-type pressure-sensitive adhesive composition mainly composed of an acrylic resin is used because it is excellent in weather resistance, durability, heat resistance, cold resistance, water resistance and the like. Has been. In recent years, as the applications of these adhesive processed products have expanded, there has been an increasing demand for adhesives having a better balance between higher heat resistance and other physical properties.

【0004】例えば、家電製品等では、上記粘着加工品
をプラスチック等の曲面に貼合わせる必要があり、これ
に見合った粘着力及び粘着剤組成物自身の弾力性(以下
「曲面接着性」という)が要求されている。また、用途
によっては、プラスチック成形品に貼合わせられた粘着
加工品の端部に垂直に荷重が生じる場合があり、この荷
重に耐えうるだけの粘着性及び粘着剤組成物自身の弾力
性(以下「定荷重剥離力」という)が要求されている。
For example, in the case of home electric appliances and the like, it is necessary to stick the above-mentioned adhesive processed product to a curved surface of plastic or the like, and the adhesive force corresponding to this and the elasticity of the adhesive composition itself (hereinafter referred to as "curved surface adhesiveness"). Is required. In addition, depending on the application, a load may occur perpendicularly to the end of the adhesive processed product attached to the plastic molded product, and the adhesiveness and elasticity of the adhesive composition itself (hereinafter "Constant load peel force") is required.

【0005】上記曲面接着性及び定荷重剥離力等の粘着
力と応力変形追従性とのバランス力を満足させるため
に、上記粘着剤組成物を、極性モノマーや高凝集力モノ
マーを多く使用することにより、又は、粘着付与樹脂の
添加量を多くし若しくは硬化剤量を多くすることによる
工夫がなされてきた。
In order to satisfy the balance between the above-mentioned curved surface adhesiveness and the adhesive force such as the constant force peeling force and the stress deformation followability, the adhesive composition should be used with a large amount of polar monomers and high cohesive force monomers. Alternatively, or by increasing the amount of the tackifying resin added or the amount of the curing agent has been devised.

【0006】特開平3−281587号公報には、含有
させる粘着付与樹脂の水酸基価を50〜100とするこ
とにより、凝集力等の粘着特性を損なうことなく高い耐
剥離性及び低温タックに優れたアクリル系感圧接着剤組
成物に関する技術が開示されている。しかしながら、上
記公報開示の技術その他によっても、上記曲面接着性及
び定荷重剥離力を有しながら、かつ粘着力、保存力、ボ
ールタック、粗面への接着性、低温時の粘着性、オレフ
ィンへの粘着性及び初期タック等の諸物性のバランスを
満足させるものは、これまでに存在しなかった。
In JP-A-3-281587, by setting the hydroxyl value of the tackifying resin to be contained to 50 to 100, high peeling resistance and low temperature tack are excellent without impairing adhesive properties such as cohesive force. Techniques for acrylic pressure sensitive adhesive compositions are disclosed. However, also by the technique disclosed in the above publication, etc., while having the curved surface adhesiveness and the constant load peeling force, the adhesive force, the storage force, the ball tack, the adhesiveness to the rough surface, the adhesiveness at low temperature, the olefin Up to now, there has been no one satisfying the balance of various physical properties such as tackiness and initial tack.

【0007】特に各種用途に展開される両面テープの場
合には、低温時のプラスチックフォームの接着力等の粗
面難被着体への低温接着力と他の粘着物性を高度に満足
させることが必要であり、このような高性能汎用粘着剤
は、いまだ開発できていない。
Particularly, in the case of a double-sided tape which is developed for various uses, it is possible to highly satisfy the low-temperature adhesiveness to an adherend having a rough surface such as the adhesiveness of a plastic foam at a low temperature and other adhesive properties. It is necessary and such a high-performance general-purpose adhesive has not been developed yet.

【0008】[0008]

【発明が解決しようとする課題】本発明は、上記に鑑
み、特に耐熱性に優れ、かつ曲面接着性、定荷重剥離力
及び低温時の粗面接着性に優れた粘着剤組成物及び粘着
加工品を提供することを目的とする。
DISCLOSURE OF THE INVENTION In view of the above, the present invention has a pressure-sensitive adhesive composition having excellent heat resistance and excellent curved surface adhesiveness, constant load peeling force, and rough surface adhesiveness at low temperature, and an adhesive processing. The purpose is to provide goods.

【0009】[0009]

【課題を解決するための手段】本発明の要旨は、粘着剤
組成物を、アクリル系ポリマー100重量部、粘着付与
樹脂10〜40重量部及びイソシアネート系を除く硬化
剤0.01〜2重量部からなる粘着剤組成物であって、
上記アクリル系ポリマーは、アルキル基の炭素数が2〜
18の(メタ)アクリル酸のアルキルエステルモノマー
60〜100重量%と前記アルキルエステルモノマーと
共重合可能なビニル系モノマー40〜0重量%との混合
物90〜99.5重量部、及び、カルボキシル基含有ビ
ニル系モノマー10〜0.5重量部からなり、上記粘着
付与樹脂は、軟化点が125〜160℃であり、かつ酸
価が0を超えて〜30であるものにより構成するところ
にある。
The gist of the present invention is to provide a pressure-sensitive adhesive composition containing 100 parts by weight of an acrylic polymer, 10 to 40 parts by weight of a tackifying resin, and 0.01 to 2 parts by weight of a curing agent excluding an isocyanate type. A pressure-sensitive adhesive composition comprising
The acrylic polymer has an alkyl group with 2 to 2 carbon atoms.
90 to 99.5 parts by weight of a mixture of 60 to 100% by weight of an alkyl ester monomer of (meth) acrylic acid of 18 and 40 to 0% by weight of a vinyl-based monomer copolymerizable with the alkyl ester monomer, and containing a carboxyl group It is composed of 10 to 0.5 parts by weight of a vinyl-based monomer, and the tackifying resin has a softening point of 125 to 160 ° C. and an acid value of more than 0 to -30.

【0010】上記アクリル系ポリマーは、アルキル基の
炭素数が2〜18の(メタ)アクリル酸のアルキルエス
テルモノマーと、上記アルキルエステルモノマーと共重
合可能なビニル系モノマーとの混合物、及び、カルボキ
シル基含有ビニル系モノマーよりなる。
The acrylic polymer is a mixture of an alkyl ester monomer of (meth) acrylic acid having an alkyl group having 2 to 18 carbon atoms and a vinyl monomer copolymerizable with the alkyl ester monomer, and a carboxyl group. Containing vinyl monomer.

【0011】上記アルキル基の炭素数が2〜18の(メ
タ)アクリル酸のアルキルエステルモノマーとしては特
に限定されず、例えば、(メタ)アクリル酸エチル、
(メタ)アクリル酸ブチル、(メタ)アクリル酸2−エ
チルヘキシル、(メタ)アクリル酸ラウリル等が挙げら
れる。
The alkyl ester monomer of (meth) acrylic acid having 2 to 18 carbon atoms in the alkyl group is not particularly limited, and examples thereof include ethyl (meth) acrylate,
Examples thereof include butyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, and lauryl (meth) acrylate.

【0012】上記モノマーと共重合可能なビニル系モノ
マーとしては特に限定されず、例えば、2−ヒドロキシ
エチル(メタ)アクリレート、2−ヒドロキシプロピル
(メタ)アクリレート等の水酸基含有モノマー;(メ
タ)アクリルアミド、アクロニトリル、N−ビニルピロ
リドン、無水マレイン酸等;(メタ)アクリル酸メチ
ル、酢酸ビニル、スチレン、ふっ素アクリレート、イソ
ボニル(メタ)アクリレート等が挙げられる。
The vinyl monomer copolymerizable with the above monomers is not particularly limited, and examples thereof include hydroxyl group-containing monomers such as 2-hydroxyethyl (meth) acrylate and 2-hydroxypropyl (meth) acrylate; (meth) acrylamide, Acrylonitrile, N-vinylpyrrolidone, maleic anhydride and the like; methyl (meth) acrylate, vinyl acetate, styrene, fluorine acrylate, isobornyl (meth) acrylate and the like can be mentioned.

【0013】上記カルボキシル基含有ビニル系モノマー
としては特に限定されず、例えば、(メタ)アクリル
酸、イタコン酸、クロトン酸等のエチレン性2重結合を
もつカルボン酸等が挙げられる。また、上記アルキルエ
ステルモノマーと共重合可能なビニル系モノマーとカル
ボキシル基含有ビニル系モノマーとは同じであってもよ
い。
The carboxyl group-containing vinyl monomer is not particularly limited, and examples thereof include carboxylic acids having an ethylenic double bond such as (meth) acrylic acid, itaconic acid and crotonic acid. Further, the vinyl monomer copolymerizable with the alkyl ester monomer and the carboxyl group-containing vinyl monomer may be the same.

【0014】上記アルキル基の炭素数が2〜18の(メ
タ)アクリル酸のアルキルエステルモノマーと上記アル
キルエステルモノマーと共重合可能なビニル系モノマー
との混合物は、上記アルキル基の炭素数が2〜18の
(メタ)アクリル酸のアルキルエステルモノマー60〜
100重量%、上記アルキルエステルモノマーと共重合
可能なビニル系モノマー40〜0重量%からなる。上記
アルキル基の炭素数が2〜18の(メタ)アクリル酸の
アルキルエステルモノマーが60重量%未満であると、
粘着剤が硬くなり、凝集力は良くなるが粘着力、タック
が悪くなり粘着力と凝集力とのバランスがとれなくなる
ので、上記範囲に限定される。
The mixture of the alkyl ester monomer of (meth) acrylic acid having 2 to 18 carbon atoms in the alkyl group and the vinyl monomer copolymerizable with the alkyl ester monomer has 2 to 8 carbon atoms in the alkyl group. 18- (meth) acrylic acid alkyl ester monomer 60-
100% by weight, 40 to 0% by weight of a vinyl-based monomer copolymerizable with the alkyl ester monomer. When the alkyl ester monomer of (meth) acrylic acid having 2 to 18 carbon atoms in the alkyl group is less than 60% by weight,
The pressure-sensitive adhesive is hardened and the cohesive force is improved, but the adhesive force and tack are deteriorated, and the adhesive force and the cohesive force cannot be balanced, so the range is limited.

【0015】また、上記アクリル系ポリマーは、上記ア
ルキル基の炭素数が2〜18の(メタ)アクリル酸のア
ルキルエステルモノマーと上記アルキルエステルモノマ
ーと共重合可能なビニル系モノマーとの混合物90〜9
9.5重量部、及び、上記カルボキシル基含有ビニル系
モノマー10〜0.5重量部からなる。上記カルボキシ
ル基含有ビニル系モノマーが10重量部を超えると、硬
化剤による架橋反応が多くなり粘着剤が硬くなるので、
保持力は向上するが、粘着力、タックが悪くなる。ま
た、0.5重量部未満であると、架橋構造が少なく凝集
力が向上せず保持力は良くならないので、上記範囲に限
定される。
The acrylic polymer is a mixture 90 to 9 of a mixture of an alkyl ester monomer of (meth) acrylic acid having 2 to 18 carbon atoms in the alkyl group and a vinyl monomer copolymerizable with the alkyl ester monomer.
9.5 parts by weight and 10 to 0.5 parts by weight of the carboxyl group-containing vinyl monomer. If the amount of the carboxyl group-containing vinyl monomer exceeds 10 parts by weight, the crosslinking reaction by the curing agent increases and the pressure-sensitive adhesive becomes hard.
Holding power is improved, but adhesion and tack are poor. If the amount is less than 0.5 parts by weight, the cross-linking structure is small, the cohesive force is not improved, and the holding force is not improved, so the content is limited to the above range.

【0016】本発明の粘着剤組成物は、上記アクリル系
ポリマーのほか、粘着付与樹脂及び硬化剤からなる。本
発明で使用される上記粘着付与樹脂としては、軟化点が
125〜160℃でありかつ酸価が0を超えて〜30で
あるもの、及び、軟化点が60〜125℃でありかつ酸
価が30を超えて〜80であるものが挙げられる。本発
明で使用される粘着付与樹脂は、単独で使用しても良い
し、2種以上を組み合わせて使用しても良い。2種以上
を組み合わせて使用する場合は、使用される粘着付与樹
脂全体で軟化点及び酸価が上記範囲を満足していればよ
い。
The pressure-sensitive adhesive composition of the present invention comprises a tackifying resin and a curing agent in addition to the above acrylic polymer. The tackifying resin used in the present invention has a softening point of 125 to 160 ° C and an acid value of more than 0 to -30, and a softening point of 60 to 125 ° C and an acid value. Of more than 30 to 80. The tackifying resin used in the present invention may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the softening point and the acid value of the entire tackifying resin used may satisfy the above ranges.

【0017】上記酸価とは、試料1g中に含まれる遊離
脂肪酸、樹脂酸を中和するのに要する水酸化カリウムの
mg数をいい、JIS K 0070に準じて測定さ
れ、次式により算出される。 A=(B×f×5.611)/S A:酸価 B:N/10水酸化カリウムエチルアルコール溶液の使
用量(ml) f:N/10水酸化カリウムエチルアルコール溶液のフ
ァクター S:試料(g)
The above-mentioned acid value means the number of mg of potassium hydroxide required to neutralize the free fatty acid and resin acid contained in 1 g of the sample, which is measured according to JIS K 0070 and calculated by the following formula. It A = (B × f × 5.611) / S A: Acid value B: Amount of N / 10 potassium hydroxide ethyl alcohol solution used (ml) f: Factor of N / 10 potassium hydroxide ethyl alcohol solution S: Sample (G)

【0018】上記軟化点が125〜160℃でありかつ
酸価が0を超えて〜30である粘着付与樹脂としては、
例えば、ペンセルD−125(軟化点125℃、酸価1
3、荒川化学工業社製)、ペンセルD−135(軟化点
135℃、酸価13、荒川化学工業社製)、ペンセルD
−160(軟化点160℃、酸価13、荒川化学工業社
製)等が挙げられる。このような粘着付与樹脂は、単独
で使用しても良いし、2種以上を組み合わせて使用して
も良い。また、粘着付与樹脂を組み合わせて使用する場
合には、軟化点が125〜160℃の範囲外にある粘着
付与樹脂(調節用粘着付与樹脂)、又は、酸価が0を超
えて〜30の範囲外にある粘着付与樹脂(調節用粘着付
与樹脂)を混合して、使用される粘着付与樹脂全体で軟
化点及び酸価が上記範囲を満足していればよい。
The tackifying resin having a softening point of 125 to 160 ° C. and an acid value of more than 0 to -30 includes:
For example, Pencel D-125 (softening point 125 ° C, acid value 1
3, Arakawa Chemical Industry Co., Ltd.), Pencel D-135 (softening point 135 ° C., acid value 13, Arakawa Chemical Industry Co., Ltd.), Pencel D
-160 (softening point 160 ° C., acid value 13, Arakawa Chemical Industry Co., Ltd.) and the like. Such tackifying resins may be used alone or in combination of two or more kinds. When a tackifying resin is used in combination, the tackifying resin having a softening point outside the range of 125 to 160 ° C. (controlling tackifying resin) or the acid value exceeding 0 to the range of -30. It suffices that an external tackifying resin (controlling tackifying resin) is mixed and the softening point and acid value of the entire tackifying resin used satisfy the above ranges.

【0019】上記軟化点が60〜125℃でありかつ酸
価が30を超えて〜80である粘着付与樹脂としては、
例えば、ハリタックAQ−60(軟化点60℃、酸価6
5、ハリマ化成社製)、ハリタックAQ−110(軟化
点110℃、酸価65〜75、ハリマ化成社製)、ペン
タリン830(軟化点110℃、酸価75、理化ハーキ
ュリス社製)等が挙げられる。このような粘着付与樹脂
は、単独で使用しても良いし、2種以上を組み合わせて
使用しても良い。また、粘着付与樹脂を組み合わせて使
用する場合には、軟化点が60〜125℃の範囲外にあ
る粘着付与樹脂(調節用粘着付与樹脂)、又は、酸価が
30を超えて〜80の範囲外にある粘着付与樹脂(調節
用粘着付与樹脂)を混合して、使用される粘着付与樹脂
全体で軟化点及び酸価が上記範囲を満足していればよ
い。
The tackifying resin having a softening point of 60 to 125 ° C. and an acid value of more than 30 and -80 is as follows:
For example, Haritac AQ-60 (softening point 60 ° C, acid value 6
5, Harima Kasei Co., Ltd., Haritac AQ-110 (softening point 110 ° C., acid value 65-75, Harima Chemicals Co., Ltd.), pentaline 830 (softening point 110 ° C., acid value 75, manufactured by Rika Herculis Co., Ltd.) and the like. To be Such tackifying resins may be used alone or in combination of two or more kinds. When the tackifying resins are used in combination, the tackifying resin having a softening point outside the range of 60 to 125 ° C. (tackifying resin for adjustment) or the acid value of more than 30 to the range of 80 is used. It suffices that an external tackifying resin (controlling tackifying resin) is mixed and the softening point and acid value of the entire tackifying resin used satisfy the above ranges.

【0020】上記調節用粘着付与樹脂としては、例え
ば、ハリタックF−90(軟化点90℃、酸価145以
上、ハリマ化成社製)、FTR6125(軟化点125
℃、酸価0、三井石油化学社製)、FTR7125(軟
化点125℃、酸価0、三井石油化学社製)、FTR6
110(軟化点110℃、酸価0、三井石油化学社
製)、ハリスターAD−130(軟化点130℃、酸価
45、荒川化学工業社製)、ハリスターDS−110S
(軟化点110℃、酸価20以下、荒川化学工業社
製)、FMG−21(軟化点125℃、荒川化学工業社
製)、アルコンP−140(軟化点140℃、酸価0、
荒川化学工業社製)、タマノル803(軟化点145〜
160℃、酸価45〜60、荒川化学工業社製)等が挙
げられる。
Examples of the above-mentioned adjusting tackifying resin include Haritac F-90 (softening point 90 ° C., acid value 145 or more, manufactured by Harima Kasei Co., Ltd.), FTR6125 (softening point 125.
C, acid value 0, Mitsui Petrochemical Co., Ltd.), FTR7125 (softening point 125 ° C., acid value 0, Mitsui Petrochemical Co., Ltd.), FTR6
110 (softening point 110 ° C., acid value 0, manufactured by Mitsui Petrochemical Co., Ltd.), Halister AD-130 (softening point 130 ° C., acid value 45, manufactured by Arakawa Chemical Industry Co., Ltd.), Halister DS-110S.
(Softening point 110 ° C., acid value 20 or less, Arakawa Chemical Industry Co., Ltd.), FMG-21 (softening point 125 ° C., Arakawa Chemical Industry Co., Ltd.), Alcon P-140 (softening point 140 ° C., acid value 0,
Arakawa Chemical Industry Co., Ltd., Tamanoru 803 (softening point 145-
160 ° C., acid value 45 to 60, manufactured by Arakawa Chemical Industries, Ltd.) and the like.

【0021】本発明の粘着剤組成物は、上記アクリル系
ポリマー100重量部に対して、上記粘着付与樹脂10
〜40重量部からなる。上記粘着付与樹脂が10重量部
未満であると、オレフィンへの粘着力が悪くなりテープ
材料や被着体への適性が悪くなり、40重量部を超える
と、凝集力が悪くなり、保持力が発現しにくくなるの
で、上記範囲に限定される。
The pressure-sensitive adhesive composition of the present invention contains 10 parts of the tackifying resin based on 100 parts by weight of the acrylic polymer.
-40 parts by weight. When the amount of the tackifying resin is less than 10 parts by weight, the adhesive force to olefins is poor and the suitability for tape materials and adherends is poor. When it is more than 40 parts by weight, the cohesive force is poor and the holding power is poor. Since it is difficult to express, it is limited to the above range.

【0022】本発明の粘着剤組成物を構成する上記硬化
剤としては、アジリジン系化合物、金属キレート、アミ
ン基含有エポキシ硬化剤等の1種類又は2種類以上の組
み合わせから選択される。
The above-mentioned curing agent constituting the pressure-sensitive adhesive composition of the present invention is selected from one kind or a combination of two or more kinds such as an aziridine compound, a metal chelate and an amine group-containing epoxy hardening agent.

【0023】上記硬化剤としてはイソシアネート系を除
けば特に限定されず、例えば、トリス−2,4,6−
(1−アジリジニル)−1,3,5−トリアジン、トリ
ス〔1−(2−メチル)アジリジニル〕ホスフィンオキ
シド、ヘキサ〔1−(2−メチル)−アジリジニル〕ト
リホスファトリアジン等のアジリジン系化合物;エチル
アセトアセテートアルミニウムジイソプロピレート、ア
ルミニウムトリス(エチルアセトアセテート)、ジルコ
ニウムテトラアセチルアセトナート、ジイソプロポキシ
ビス(アセチルアセトン)チタネート、ジ−n−ブトキ
シビス(トリエタノールアミン)チタネート、ジヒドロ
キシビス(ラクティクアシド)チタネート、テトラオク
チレングリコールチタネート、ジイソプロポキシビス
(アセト酢酸エチル)チタネート等の金属キレート;T
EDRAD−X、TEDRAD−C(三菱瓦斯化学社
製)等のアミン基含有エポキシ硬化剤等が挙げられる。
The above-mentioned curing agent is not particularly limited except isocyanate type, and for example, Tris-2,4,6-
Aziridine compounds such as (1-aziridinyl) -1,3,5-triazine, tris [1- (2-methyl) aziridinyl] phosphine oxide, hexa [1- (2-methyl) -aziridinyl] triphosphatriazine; ethyl Acetoacetate aluminum diisopropylate, aluminum tris (ethylacetoacetate), zirconium tetraacetylacetonate, diisopropoxybis (acetylacetone) titanate, di-n-butoxybis (triethanolamine) titanate, dihydroxybis (lacticaside) titanate , Tetraoctylene glycol titanate, diisopropoxybis (ethyl acetoacetate) titanate and other metal chelates; T
Examples thereof include amine group-containing epoxy curing agents such as EDRAD-X and TEDRAD-C (manufactured by Mitsubishi Gas Chemical Co., Inc.).

【0024】上記硬化剤は、上記アクリル系ポリマー1
00重量部に対して0.01〜2重量部である。0.0
1重量部未満であると、最適な架橋構造体を作れないの
で保持力、定荷重剥離力が犠牲となり、2重量部を超え
ると、架橋構造が多くなりすぎ、粘着力、タックが悪く
なるので、上記範囲に限定される。
The curing agent is the acrylic polymer 1 described above.
It is 0.01 to 2 parts by weight with respect to 00 parts by weight. 0.0
If it is less than 1 part by weight, an optimum crosslinked structure cannot be produced, so the holding force and constant force peeling force are sacrificed, and if it exceeds 2 parts by weight, the crosslinked structure becomes too much and the adhesive strength and tack deteriorate. Is limited to the above range.

【0025】本発明の粘着剤組成物には、必要に応じて
増粘剤、チクソ性付与剤、増量剤、充填剤、顔料、防錆
剤等を配合してもよい。
If desired, the pressure-sensitive adhesive composition of the present invention may contain a thickener, a thixotropic agent, a bulking agent, a filler, a pigment, a rust preventive and the like.

【0026】本発明の上記粘着剤組成物を、テープ又は
シートに塗工することにより、粘着テープ、特に両面テ
ープ又は粘着シート等の粘着加工品を製造することがで
きる。このようなテープ又はシートの基材としては特に
限定されず、例えば、レーヨン系、セルロース系等の各
種不織布;ポリエチレン、ポリエステル等の各種フィル
ム;セロハン、ポリエチレン、ポリプロピレン、ポリス
チレン、ポリエステル等を基材とする各種フィルム;発
砲ポリエチレン、ウレタンフォーム、ネオプレン等各種
ゴム発砲体等が挙げられる。
By applying the above-mentioned pressure-sensitive adhesive composition of the present invention to a tape or a sheet, a pressure-sensitive adhesive product such as a pressure-sensitive adhesive tape, particularly a double-sided tape or a pressure-sensitive adhesive sheet can be produced. The base material of such a tape or sheet is not particularly limited, and for example, various non-woven fabrics such as rayon-based or cellulose-based; various films such as polyethylene and polyester; cellophane, polyethylene, polypropylene, polystyrene, polyester, etc. Examples of various films include foamed polyethylene, urethane foam, various rubber foams such as neoprene, and the like.

【0027】[0027]

【作用】本発明の粘着剤組成物は、粘着剤組成物中のア
クリル系ポリマーと粘着付与樹脂が硬化剤によって適度
な架橋構造体を生成することにより、幅広い粘着物性を
発現することにより効果を発揮する。上記アクリル系ポ
リマーと配合される粘着付与樹脂は、とくにポリプロピ
レン(PP)等のポリオレフィンへの粘着力を向上する
作用を発揮する。これにより、さまざまなテープ材料や
被着体への応力が可能となる。アクリル系ポリマーと粘
着付与樹脂が硬化剤により架橋することにより、粘着付
与樹脂の熱軟化による流動を押さえることができ、保持
力等の凝集力を発現することができる。また粘着付与樹
脂の軟化点の低いものでも保持力が発現できるので、低
温の難被着体への粘着力も満足することができる。ま
た、同時に定荷重剥離力の最適範囲も広がる。本発明の
粘着剤組成物は、粘着付与樹脂を限定することにより、
アクリル系ポリマーへの架橋を最適化することで幅広い
粘着物性を発現して本発明の目的を達成する。
The pressure-sensitive adhesive composition of the present invention exerts an effect by expressing a wide range of pressure-sensitive adhesive properties by the acrylic polymer and the tackifying resin in the pressure-sensitive adhesive composition forming an appropriate crosslinked structure by the curing agent. Demonstrate. The tackifying resin blended with the acrylic polymer exhibits an action of improving the adhesive force to polyolefin such as polypropylene (PP). This allows stress on various tape materials and adherends. By cross-linking the acrylic polymer and the tackifying resin with the curing agent, the flow of the tackifying resin due to thermal softening can be suppressed, and cohesive force such as holding force can be exhibited. Further, even if the tackifying resin has a low softening point, the holding force can be exhibited, so that the adhesive force to a low-temperature adherend can be satisfied. At the same time, the optimum range of the constant load peeling force is expanded. The pressure-sensitive adhesive composition of the present invention, by limiting the tackifying resin,
By optimizing the cross-linking to the acrylic polymer, a wide range of adhesive physical properties are expressed and the object of the present invention is achieved.

【0028】[0028]

【実施例】以下に実施例を掲げて本発明を更に詳しく説
明するが、本発明はこれら実施例のみに限定されるもの
ではない。
The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

【0029】実施例1〜6、比較例1〜6 冷却管を備えた4つ口フラスコ内に表1に示した割合
で、モノマーを仕込み、次に酢酸エチル81.8重量部
を仕込み、昇温して30分間還流させた後、ベンゾール
パーオキサイド0.1重量部を滴下し、7時間反応させ
た。この後、更に、ベンゾールパーオキサイド0.1重
量部を滴下し、3時間反応させた。ついで、これにトル
エン40.4重量部を加え、冷却して透明で粘凋なアク
リル系ポリマー溶液を得た。表1に示した割合で、上記
アクリル系ポリマー溶液と粘着付与樹脂を混合し混合物
を得た。次に硬化剤を混合し、粘着剤組成物を得た。上
記で得た粘着剤組成物を離型紙にドクターブレードで4
5μm(DRY)塗工した。次に80℃の乾燥機で5分
間乾燥させた。次に、厚さ40μm、秤量50g/m2
の不織布に両面から粘着剤を圧着ローラーで張り合わ
せ、両面テープを作成した。この両面テープを温度20
℃、湿度65%の恒温恒湿内で7日間養生した。
Examples 1 to 6 and Comparative Examples 1 to 6 In a four-necked flask equipped with a cooling tube, the monomer was charged at the ratio shown in Table 1, and then 81.8 parts by weight of ethyl acetate was charged and the mixture was heated. After warming and refluxing for 30 minutes, 0.1 part by weight of benzol peroxide was added dropwise and reacted for 7 hours. Thereafter, 0.1 part by weight of benzol peroxide was further added dropwise and the reaction was carried out for 3 hours. Then, 40.4 parts by weight of toluene was added thereto and cooled to obtain a transparent and viscous acrylic polymer solution. The acrylic polymer solution and the tackifying resin were mixed in the proportions shown in Table 1 to obtain a mixture. Next, a curing agent was mixed to obtain an adhesive composition. The pressure-sensitive adhesive composition obtained above was applied to a release paper with a doctor blade.
5 μm (DRY) coating was applied. Next, it was dried for 5 minutes in a dryer at 80 ° C. Next, the thickness is 40 μm and the weight is 50 g / m 2.
A double-sided tape was prepared by sticking an adhesive on both sides of the non-woven fabric with a pressure roller. This double-sided tape is at temperature 20
It was aged for 7 days in a constant temperature and humidity of ℃ and 65% humidity.

【0030】実施例7〜12、比較例7〜12 アクリル系ポリマーのモノマー組成及び粘着付与樹脂
を、表2に示した割合に変えた以外は、実施例1〜6、
比較例1〜6と同様にして粘着剤組成物を得、両面テー
プを作成した。
Examples 7-12, Comparative Examples 7-12 Examples 1-6, except that the monomer composition of the acrylic polymer and the tackifying resin were changed to the proportions shown in Table 2.
A pressure-sensitive adhesive composition was obtained in the same manner as in Comparative Examples 1 to 6 to prepare a double-sided tape.

【0031】表1及び表2中、BAは、ブチルアクリレ
ート、2EHAは、2−エチルヘキシルアクリレート、
AACは、アクリル酸、2HEMAは、2−ヒドロキシ
エチルメタクリレートを、それぞれ表す。表1中、D−
135は、荒川化学工業社製、ペンセルD−135(軟
化点135℃、酸価13)を、D−160は、荒川化学
工業社製、ペンセルD−160(軟化点160℃、酸価
13)を、P−140は、荒川化学工業社製、アルコン
P−140(軟化点140℃、酸価0)を、AD−13
0は、ハリマ化成社製、ハリエスターAD−130(軟
化点130℃、酸価45)を、それぞれ表す。
In Tables 1 and 2, BA is butyl acrylate, 2EHA is 2-ethylhexyl acrylate,
AAC represents acrylic acid and 2HEMA represents 2-hydroxyethyl methacrylate, respectively. In Table 1, D-
135 is Pencel D-135 (softening point 135 ° C, acid value 13) manufactured by Arakawa Chemical Industry Co., Ltd., and D-160 is Pencel D-160 (softening point 160 ° C, acid value 13) manufactured by Arakawa Chemical Industry Co., Ltd. P-140 is Arakawa Chemical Industry Co., Ltd., Alcon P-140 (softening point 140 ℃, acid value 0), AD-13
0 represents Harrier Star AD-130 (softening point 130 ° C., acid value 45) manufactured by Harima Chemicals, Inc., respectively.

【0032】表2中、P−830は、理化ハーキュレス
社製、ペンタリン830(軟化点110℃、酸価75)
を、AQ−60は、ハリマ化成社製、ハリタックAQ−
60(軟化点60℃、酸価65)を、F−90は、ハリ
マ化成社製、ハリタックF−90(軟化点90℃、酸価
145以上)を、DS−110Sは、ハリマ化成社製、
ハリエスターDS−110S(軟化点110℃、酸価2
0以下)を、FTR6110は、三井石油化学工業社
製、FTR6110(軟化点110℃、酸価0.1以
下)を、それぞれ表す。また、表1及び表2中、硬化剤
は、アジリジン系HDU(三光化学工業社製)を表す。
In Table 2, P-830 is pentaline 830 manufactured by Rika Hercules Co., Ltd. (softening point 110 ° C., acid value 75).
AQ-60 is a product of Harima Kasei Co., Ltd., Haritac AQ-
60 (softening point 60 ° C., acid value 65), F-90 manufactured by Harima Chemicals, Haritac F-90 (softening point 90 ° C., acid value 145 or more), DS-110S manufactured by Harima Chemicals,
Harrier Star DS-110S (softening point 110 ° C, acid value 2
0 or less), and FTR6110 represents Mitsui Petrochemical Co., Ltd., FTR6110 (softening point 110 ° C., acid value 0.1 or less), respectively. Further, in Tables 1 and 2, the curing agent represents an aziridine-based HDU (manufactured by Sanko Chemical Industry Co., Ltd.).

【0033】物性の測定 (1)PP粘着力 PP板に両面テープ(25μmPETフィルム裏打ち付
き)を貼りつけ、90°剥離強度を測定した。 (2)保持力 両面テープ(25μmPETフィルム裏打ち付き)を2
5mm×25mmでステンレス板に貼合わせた。これを
80℃に30分養生してから1Kg荷重を24時間か
け、24時間後のずれまたは、落下時間を測定した。 (3)定荷重剥離力 PP板に幅25mm、長さ50mm巾の面積に両面テー
プ(25μmPETフィルム裏打ち付き)を貼付け、2
Kgロールを1往復させて、接着した。60℃ギヤーオ
ーブン中に30分間放置した後、テープ面が下になるよ
うにして100gの静荷重をかけた(角度はPP板に対
して90°)。3時間放置し、テープが、PP板から剥
離した距離を測定した。
Measurement of Physical Properties (1) PP Adhesive Strength A double-sided tape (with a 25 μm PET film backing) was attached to a PP plate, and 90 ° peel strength was measured. (2) Holding power 2 pieces of double-sided tape (with 25 μm PET film backing)
It was stuck on a stainless plate with a size of 5 mm × 25 mm. After this was cured at 80 ° C. for 30 minutes, a load of 1 Kg was applied for 24 hours, and the deviation or dropping time after 24 hours was measured. (3) Peeling force under constant load A double-sided tape (with a 25 μm PET film backing) is pasted on a PP plate with an area of width 25 mm and length 50 mm, 2
The Kg roll was reciprocated once and adhered. After leaving it in a gear oven at 60 ° C. for 30 minutes, a static load of 100 g was applied with the tape surface facing downward (angle is 90 ° with respect to the PP plate). After standing for 3 hours, the distance that the tape peeled from the PP plate was measured.

【0034】(4)曲面接着性 両面テープを厚さ0.05mm、幅15mm、長さ15
0mmのアルミ板に貼り付けた。これを、厚さ2mm、
幅250mmのPP板に幅方向に圧着ローラーで貼合わ
せた。30分後に、このPP板を200mmの治具に治
まるように曲げて収め曲面をつけた。これに冷却サイク
ルを10回与えて、アルミ板のはがれた高さを測定し
た。 (5)低温接着性 5℃雰囲気下で厚さ10mmのウレタンフォーム(あら
かじめステンレス板に貼り付けておく)に両面テープ
(25μmPETフィルム裏打ち付き)を幅25mmで
貼付けし、ロールで1往復させて接着した。同条件で2
4時間放置後、引っ張り試験機で180℃剥離強度を測
定した。引っ張り速度は300mm/分であった。上記
各試験結果を表1及び表2に示した。
(4) Adhesiveness on curved surface A double-sided tape having a thickness of 0.05 mm, a width of 15 mm and a length of 15 is used.
It was attached to a 0 mm aluminum plate. 2mm thick,
A PP plate having a width of 250 mm was laminated in the width direction with a pressure roller. After 30 minutes, this PP plate was bent so as to be settled by a jig of 200 mm and a curved surface was formed. A cooling cycle was applied to this 10 times, and the peeling height of the aluminum plate was measured. (5) Low-temperature adhesion In a 5 ° C atmosphere, a double-sided tape (with a 25 μm PET film backing) with a width of 25 mm was applied to a 10-mm-thick urethane foam (previously adhered to a stainless steel plate) and adhered by rolling back and forth once with a roll. did. 2 under the same conditions
After standing for 4 hours, the peeling strength at 180 ° C. was measured with a tensile tester. The pulling speed was 300 mm / min. The test results are shown in Tables 1 and 2.

【0035】[0035]

【表1】 [Table 1]

【0036】[0036]

【表2】 [Table 2]

【0037】[0037]

【発明の効果】本発明は、粘着付与樹脂に含まれるカル
ボキシル基とアクリルポリマーに含まれるカルボキシル
基を硬化剤により架橋させることにより、粘着剤に最適
な架橋構造を発現させ、曲面接着性、定荷重剥離力、低
温でのウレタンフォーム等の難被着体への接着性とその
他の粘着物性とのバランスを満足することができる。
INDUSTRIAL APPLICABILITY The present invention develops an optimum cross-linking structure for a pressure-sensitive adhesive by crosslinking a carboxyl group contained in a tackifying resin and a carboxyl group contained in an acrylic polymer with a curing agent, thereby obtaining a curved surface adhesiveness, It is possible to satisfy the balance between the peeling force under load, the adhesiveness to a difficult-to-be-adhered body such as urethane foam at a low temperature, and other adhesive properties.

Claims (3)

【特許請求の範囲】[Claims] 【請求項1】 アクリル系ポリマー100重量部、粘着
付与樹脂10〜40重量部及びイソシアネート系を除く
硬化剤0.01〜2重量部からなる粘着剤組成物であっ
て、前記アクリル系ポリマーは、アルキル基の炭素数が
2〜18の(メタ)アクリル酸のアルキルエステルモノ
マー60〜100重量%と前記アルキルエステルモノマ
ーと共重合可能なビニル系モノマー40〜0重量%との
混合物90〜99.5重量部、及び、カルボキシル基含
有ビニル系モノマー10〜0.5重量部からなり、前記
粘着付与樹脂は、軟化点が125〜160℃であり、か
つ酸価が0を超えて〜30であることを特徴とする粘着
剤組成物。
1. A pressure-sensitive adhesive composition comprising 100 parts by weight of an acrylic polymer, 10 to 40 parts by weight of a tackifying resin, and 0.01 to 2 parts by weight of a curing agent excluding an isocyanate type, wherein the acrylic polymer comprises: A mixture of 60 to 100% by weight of an alkyl ester monomer of (meth) acrylic acid having an alkyl group having 2 to 18 carbon atoms and 40 to 0% by weight of a vinyl-based monomer copolymerizable with the alkyl ester monomer 90 to 99.5. The tackifying resin has a softening point of 125 to 160 ° C. and an acid value of more than 0 to 30. A pressure-sensitive adhesive composition comprising:
【請求項2】 アクリル系ポリマー100重量部、粘着
付与樹脂10〜40重量部及びイソシアネート系を除く
硬化剤0.01〜2重量部からなる粘着剤組成物であっ
て、前記アクリル系ポリマーは、アルキル基の炭素数が
2〜18の(メタ)アクリル酸のアルキルエステルモノ
マー60〜100重量%と前記アルキルエステルモノマ
ーと共重合可能なビニル系モノマー40〜0重量%との
混合物90〜99.5重量部、及び、カルボキシル基含
有ビニル系モノマー10〜0.5重量部からなり、前記
粘着付与樹脂は、軟化点が60〜125℃であり、かつ
酸価が30を超えて〜80であることを特徴とする粘着
剤組成物。
2. A pressure-sensitive adhesive composition comprising 100 parts by weight of an acrylic polymer, 10 to 40 parts by weight of a tackifying resin, and 0.01 to 2 parts by weight of a curing agent excluding an isocyanate type, wherein the acrylic polymer is A mixture of 60 to 100% by weight of an alkyl ester monomer of (meth) acrylic acid having an alkyl group having 2 to 18 carbon atoms and 40 to 0% by weight of a vinyl-based monomer copolymerizable with the alkyl ester monomer 90 to 99.5. The tackifying resin has a softening point of 60 to 125 ° C. and an acid value of more than 30 to 80. A pressure-sensitive adhesive composition comprising:
【請求項3】 請求項1又は2記載の粘着剤組成物を塗
工してなることを特徴とする粘着加工品。
3. An adhesive processed product obtained by applying the adhesive composition according to claim 1 or 2.
JP6170949A 1994-07-22 1994-07-22 Tacky agent composition and tacky processed article Pending JPH0834962A (en)