JPH0121782B2 - - Google Patents

Info

Publication number
JPH0121782B2
JPH0121782B2 JP17096282A JP17096282A JPH0121782B2 JP H0121782 B2 JPH0121782 B2 JP H0121782B2 JP 17096282 A JP17096282 A JP 17096282A JP 17096282 A JP17096282 A JP 17096282A JP H0121782 B2 JPH0121782 B2 JP H0121782B2
Authority
JP
Japan
Prior art keywords
opening
tape
plastic film
piece
metal lid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP17096282A
Other languages
Japanese (ja)
Other versions
JPS5962108A (en
Inventor
Hideo Ootsuka
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toyo Seikan Group Holdings Ltd
Original Assignee
Toyo Seikan Kaisha Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyo Seikan Kaisha Ltd filed Critical Toyo Seikan Kaisha Ltd
Priority to JP17096282A priority Critical patent/JPS5962108A/en
Publication of JPS5962108A publication Critical patent/JPS5962108A/en
Publication of JPH0121782B2 publication Critical patent/JPH0121782B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】 本発明は開口容易な金属蓋の製造方法に関し、
さらに詳しくは開口部を覆つてテープ片が接着さ
れ、このテープ片を剥離することによつて開口が
行なわれるタイプの開口容易な金属蓋の製造方法
に関する。
DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for manufacturing an easy-to-open metal lid;
More specifically, the present invention relates to a method of manufacturing an easy-to-open metal lid of the type in which a piece of tape is adhered to cover the opening, and the opening is made by peeling off the tape piece.

第1図、第2図に示す開口容易な金属蓋1(以
下金属蓋とよぶ)は、パネル部2に、内容液3の
注ぎ出し口、飲み口、もしくはストローの差込口
となる涙滴形の開口部4が形成されており、開口
部4を覆つてパネル部2の外面にテープ片5が剥
離可能に接着されている。なお5xがテープ片5
の接着された部分であり、5yが摘み部である。
接着は熱接着(テープ片5の内面層を形成する熱
可塑性プラスチツクフイルムの熱融着、もしくは
ホツトメルト接着剤による接着)、又は粘着等に
よつて行なわれる。6は開口部4の金属が露出し
た端面4aを、内容液3に対し遮断して保護する
ための内面テープである。
The easy-to-open metal lid 1 (hereinafter referred to as the metal lid) shown in FIGS. 1 and 2 has a teardrop opening on the panel portion 2 that serves as a spout for pouring out the liquid content 3, a drinking spout, or a slot for inserting a straw. A shaped opening 4 is formed, and a piece of tape 5 is releasably adhered to the outer surface of the panel portion 2 so as to cover the opening 4. Note that 5x is tape piece 5
This is the glued part, and 5y is the knob.
The adhesion is performed by thermal adhesion (thermal adhesion of a thermoplastic film forming the inner surface layer of the tape piece 5 or adhesion using a hot melt adhesive), adhesive, or the like. Reference numeral 6 denotes an inner surface tape for protecting the end surface 4a of the opening 4 where the metal is exposed by blocking it from the liquid content 3.

次に開口部4の近傍を拡大して示した図面であ
る第3図によつて、具体的な例を説明する。パネ
ル部2は錫めつき鋼板やテインフリースチール等
の金属板よりなり、内面は保護塗膜7によつて被
覆されており、外面も必要に応じプライマー層、
焼付塗膜又は印刷膜等(図示されない)によつて
被覆されている。テープ片5は内面側より、粘着
剤層5a、プラスチツクフイルム層5b(例えば
ポリエチレンテレフタレートよりなる)、蒸着ア
ルミニウム層5cおよび塗膜5dよりなつてい
る。
Next, a specific example will be explained with reference to FIG. 3, which is an enlarged view of the vicinity of the opening 4. The panel part 2 is made of a metal plate such as a tin-plated steel plate or stain-free steel, and the inner surface is coated with a protective coating 7, and the outer surface is also coated with a primer layer as required.
It is covered with a baked paint film, a printed film, etc. (not shown). The tape piece 5 is composed of, from the inner side, an adhesive layer 5a, a plastic film layer 5b (for example, made of polyethylene terephthalate), a vapor-deposited aluminum layer 5c, and a coating film 5d.

内面テープ6は、プラスチツクフイルム層6a
(例えばポリエチレンよりなる)、および粘着剤層
6bよりなり、開口部4の周辺のパネル部2の内
面2aに接着(粘着され)ており、また開口部4
内に凹入して、開口部4上のテープ片5の部分の
周縁部を除くほぼ全面に接着(粘着)されてい
る。そして僅かな間隙8(第3図では誇張して大
き目に書かれているが、実際はごく小さい)を残
して、端面4aは内面テープ6とテープ片5によ
つて覆われている(本明細書においては、このよ
うに間隙8が残る場合も、覆われているとよぶ)。
開口のさいは摘み部5yを引上げると、内面テー
プ6の開口部4の内側周縁部が引裂かれて、開口
部4内の内面テープ部分はテープ片5と共に除去
されて、開口が行なわれる。
The inner surface tape 6 has a plastic film layer 6a.
(made of polyethylene, for example) and an adhesive layer 6b, and is adhered (adhesive) to the inner surface 2a of the panel section 2 around the opening 4, and the opening 4
It is recessed inward and is adhered (adhesive) to almost the entire surface of the tape piece 5 above the opening 4 except for the peripheral edge. The end surface 4a is covered with the inner surface tape 6 and the tape piece 5, leaving a slight gap 8 (exaggeratedly drawn in FIG. 3, but actually very small). , even when the gap 8 remains like this, it is called covered).
When opening the opening, when the knob 5y is pulled up, the inner peripheral edge of the opening 4 of the inner surface tape 6 is torn, and the inner surface tape portion within the opening 4 is removed together with the tape piece 5, thereby completing the opening.

ところが従来は、これらの接着は空気中で行な
つているため、間隙8内には空気、すなわち酸素
や湿分が残り、そのためパネル部2が特に鋼をベ
ースとする金属板よりなる場合、端面4aの露出
した鋼が、容器9(すなわち内容液3を充填さ
れ、金属蓋1によつて2重巻締部10を形成して
密封された)の長期保存(例えば1年間の)中に
発錆し、開口した時テープ片5や内面テープ6に
赤褐色の錆が附着したり、また端面4aが錆色を
呈して、商品価値を低下させるという問題を生ず
る。
However, in the past, these adhesives were bonded in air, so air, that is, oxygen and moisture, remained in the gap 8. Therefore, when the panel part 2 is made of a metal plate based on steel, the edge surface The exposed steel of 4a is generated during long-term storage (for example, one year) of the container 9 (that is, filled with the liquid content 3 and sealed with the metal lid 1 forming a double seam 10). When the tape is opened, reddish-brown rust adheres to the tape piece 5 and the inner tape 6, and the end surface 4a becomes rust-colored, resulting in problems such as lowering the product value.

本発明は以上に述べた従来技術の問題点の解消
を図ることを目的とする。
It is an object of the present invention to solve the problems of the prior art described above.

上記目的を達成するため本発明は、パネル部に
開口部が形成され、該開口部を覆つて該パネル部
の外面に、剥離可能にテープ片が接着され、かつ
該開口部の周辺の該パネル部の内面にプラスチツ
クフイルムが接着され、該開口部の端面が該テー
プ片および/または該プラスチツクフイルムによ
つて覆われてなる開口容易な金属蓋の製造方法に
おいて、該端面を覆うさいの該テープ片又は該プ
ラスチツクフイルムの接着を窒素ガス雰囲気中で
行なうことを特徴とする開口容易な金属蓋の製造
方法を提供するものである。
In order to achieve the above object, the present invention includes an opening formed in a panel part, a piece of tape removably adhered to the outer surface of the panel part covering the opening, and a tape piece around the opening part of the panel part. In the method for producing an easy-to-open metal lid in which a plastic film is adhered to the inner surface of the opening, and the end face of the opening is covered with the tape piece and/or the plastic film, the tape covers the end face. The present invention provides a method for manufacturing an easy-to-open metal lid, characterized in that the adhesive piece or the plastic film is bonded in a nitrogen gas atmosphere.

以下本発明について説明する。 The present invention will be explained below.

第4図において、パネル部2にテープ片5が接
着された金属蓋は、開口部4を上方にしてアンビ
ル11上に載置されている。12は内面テープ6
の貼着具であつて、下端部は弾性ゴム層12aよ
りなり、軸線方向に延びる複数の真空吸引孔13
が設けられており、底面12bに粘着剤層6bを
下面にして内面テープ6が吸着されている。
In FIG. 4, the metal lid with the tape piece 5 adhered to the panel portion 2 is placed on the anvil 11 with the opening 4 facing upward. 12 is inner tape 6
The lower end is made of an elastic rubber layer 12a, and has a plurality of vacuum suction holes 13 extending in the axial direction.
is provided, and the inner surface tape 6 is adsorbed to the bottom surface 12b with the adhesive layer 6b facing downward.

開口部4に窒素ガス14を吹付けて、開口部4
近傍を窒素ガス雰囲気に保つた状態で、貼着具1
2を矢印A方向に、粘着剤層6bがテープ片5の
粘着剤層5aおよびパネル部2の開口部4周辺の
内面となるべき部分2aに接触するまで押下げる
ことによつて、第3図に示す内面テープ6が接着
された金属蓋1が得られる。このようにして製造
された金属蓋1は、間隙8が窒素ガスで充満され
ているので、密封後の長期保存によつても端面4
aが発錆し難い。
By blowing nitrogen gas 14 into the opening 4,
While maintaining the vicinity in a nitrogen gas atmosphere, attach the adhesive tool 1.
FIG. A metal lid 1 having an inner surface tape 6 adhered thereto as shown in FIG. In the metal lid 1 manufactured in this way, since the gap 8 is filled with nitrogen gas, the end surface 4 can be stored even after long-term storage after sealing.
a is hard to rust.

第5図は、開口部24の端面24aを保護する
ために、プラスチツクフイルム26(例えばナイ
ロン12よりなる)が開口部24の周辺のパネル
部22の内面22aおよび外面22bに、端面2
4aを覆うようにして熱融着されている。また内
層25aがプラスチツクフイルム(例えばナイロ
ン12よりなる)、中間層25bが蒸着アルミニ
ウム層、外層25cが塗膜よりなるテープ片25
が、パネル部22の外面およびプラスチツクフイ
ルム26の外側部26aに熱融着されている。な
お27はプライマー層(例えばフエノール・エポ
キシ系塗料よりなる)である。
In FIG. 5, a plastic film 26 (made of nylon 12, for example) is placed on the inner surface 22a and outer surface 22b of the panel section 22 around the opening 24 in order to protect the end surface 24a of the opening 24.
It is heat-sealed so as to cover 4a. Further, the tape piece 25 has an inner layer 25a made of a plastic film (for example, made of nylon 12), an intermediate layer 25b made of a vapor-deposited aluminum layer, and an outer layer 25c made of a paint film.
is heat-sealed to the outer surface of the panel portion 22 and the outer portion 26a of the plastic film 26. Note that 27 is a primer layer (for example, made of phenol-epoxy paint).

この場合は、プラスチツクフイルム26は概ね
間隙を残すことなく端面24aを覆うことができ
るが、所により皺発生にもとづく僅かな間隙28
が生じる。従つてこの場合も窒素ガス雰囲気中で
プラスチツクフイルム26の接着を行なうことに
よつて、間隙28が窒素ガスによつて充満される
ので、間隙28における端面24aが発錆し難く
なる。
In this case, the plastic film 26 can cover the end surface 24a without leaving any gaps, but in some places there may be slight gaps 28 due to wrinkles.
occurs. Therefore, in this case as well, by bonding the plastic film 26 in a nitrogen gas atmosphere, the gap 28 is filled with nitrogen gas, making it difficult for the end surface 24a in the gap 28 to rust.

第6図は、テープ片35が凹入して、パネル部
32の開口部34内において内面テープ36と接
着されてなる金属蓋の開口部34近傍を示したも
のであつて、図示は省略したが、テープ片35お
よび内面テープ36の層構成は、夫々第3図のテ
ープ片5および内面テープ6の夫と同様である。
この場合も、窒素ガス雰囲気中でテープ片35の
接着を行なうことによつて、間隙38が窒素ガス
によつて充満されるので、間隙38における端面
34aが発錆し難くなる。
FIG. 6 shows the vicinity of the opening 34 of the metal lid, where the tape piece 35 is recessed and adhered to the inner surface tape 36 within the opening 34 of the panel section 32, and is not shown. However, the layer configurations of the tape piece 35 and the inner surface tape 36 are similar to those of the tape piece 5 and the inner surface tape 6 shown in FIG. 3, respectively.
Also in this case, by adhering the tape pieces 35 in a nitrogen gas atmosphere, the gap 38 is filled with nitrogen gas, so that the end face 34a in the gap 38 is less likely to rust.

本発明によれば、開口部の端面を覆うさいのテ
ープ片又はプラスチツクフイルムの接着を窒素ガ
ス雰囲気中で行なうので、金属蓋が鋼をベースと
する金属板よりなる場合であつても、開口部の端
面が発錆し難いという効果を奏することができ
る。
According to the present invention, since the tape piece or plastic film is bonded in a nitrogen gas atmosphere when covering the end face of the opening, even if the metal lid is made of a steel-based metal plate, the opening It is possible to achieve the effect that the end face of the steel is less likely to rust.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本発明の適用される第1の例の金属蓋
によつて密封された容器の面図、第2図は第1図
の―線に沿う要部縦断面図、第3図は第2図
のA部の拡大縦断面図、第4図は第1図に示す金
属蓋を製造するため内面テープを貼着する工程を
示す縦断面図、第5図および第6図は夫々、本発
明の適用される第2および第3の例の金属蓋の要
部縦断面図である。 1……開口容易な金属蓋、2……パネル部、2
a……開口部周辺のパネル部の内面、4……開口
部、4a……端面、5……テープ片、6……内面
テープ(プラスチツクフイルム)、14……窒素
ガス、22,32……パネル部、24,34……
開口部、24a,34a……端面、25,35…
…テープ片、26……プラスチツクフイルム、3
6……内面テープ(プラスチツクフイルム)。
FIG. 1 is a plan view of a container sealed with a metal lid according to the first example to which the present invention is applied, FIG. FIG. 4 is an enlarged vertical cross-sectional view of part A in FIG. 2, FIG. 4 is a vertical cross-sectional view showing the process of attaching the inner surface tape to manufacture the metal lid shown in FIG. 1, and FIGS. 5 and 6 are respectively, FIG. 6 is a vertical sectional view of a main part of metal lids of second and third examples to which the present invention is applied. 1...Easy-to-open metal lid, 2...Panel part, 2
a...Inner surface of the panel around the opening, 4...Opening, 4a...End face, 5...Tape piece, 6...Inner surface tape (plastic film), 14...Nitrogen gas, 22, 32... Panel part, 24, 34...
Opening, 24a, 34a... End surface, 25, 35...
... Tape piece, 26 ... Plastic film, 3
6...Inner tape (plastic film).

Claims (1)

【特許請求の範囲】[Claims] 1 パネル部に開口部が形成され、該開口部を覆
つて該パネル部の外面に、剥離可能にテープ片が
接着され、かつ該開口部の周辺の該パネル部の内
面にプラスチツクフイルムが接着され、該開口部
の端面が該テープ片および/または該プラスチツ
クフイルムによつて覆われてなる開口容易な金属
蓋の製造方法において、該端面を覆うさいの該テ
ープ片又は該プラスチツクフイルムの接着を、窒
素ガス雰囲気中で行なうことを特徴とする開口容
易な金属蓋の製造方法。
1. An opening is formed in the panel, a piece of tape is removably adhered to the outer surface of the panel covering the opening, and a plastic film is adhered to the inner surface of the panel around the opening. , a method for manufacturing an easy-to-open metal lid in which the end face of the opening is covered with the tape piece and/or the plastic film, which includes adhering the tape piece or the plastic film when covering the end face; A method for manufacturing an easy-to-open metal lid, characterized in that the manufacturing method is carried out in a nitrogen gas atmosphere.
JP17096282A 1982-10-01 1982-10-01 Preparation of easily openable metal lid Granted JPS5962108A (en)