JP5442552B2 - Resin material and manufacturing method thereof - Google Patents

Resin material and manufacturing method thereof Download PDF

Info

Publication number
JP5442552B2
JP5442552B2 JP2010163723A JP2010163723A JP5442552B2 JP 5442552 B2 JP5442552 B2 JP 5442552B2 JP 2010163723 A JP2010163723 A JP 2010163723A JP 2010163723 A JP2010163723 A JP 2010163723A JP 5442552 B2 JP5442552 B2 JP 5442552B2
Authority
JP
Japan
Prior art keywords
olefin
synthetic resin
component
gypsum board
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2010163723A
Other languages
Japanese (ja)
Other versions
JP2010229423A (en
JP2010229423A5 (en
Inventor
章彦 古閑
Original Assignee
株式会社プラシンクス
株式会社プラト
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 株式会社プラシンクス, 株式会社プラト filed Critical 株式会社プラシンクス
Priority to JP2010163723A priority Critical patent/JP5442552B2/en
Publication of JP2010229423A publication Critical patent/JP2010229423A/en
Publication of JP2010229423A5 publication Critical patent/JP2010229423A5/ja
Application granted granted Critical
Publication of JP5442552B2 publication Critical patent/JP5442552B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、樹脂素材及びその製造方法に関するものであり、特に詳しくは、使用済みのオレフィン系合成樹脂素材と使用済みの石膏ボードとから完全リサイクル化を達成した新規の樹脂素材及びその製造方法に関するものである。   The present invention relates to a resin material and a method for producing the same, and in particular, relates to a novel resin material that has been completely recycled from a used olefin-based synthetic resin material and a used gypsum board, and a method for producing the same. Is.

従来から、産業用廃棄物としての石膏ボードをリサイクルする必要性がある事は周知である。
然しながら、一般的は、産業廃棄物をリサイクル処理を行う事は環境には良いと分かっていても、実際のリサイクルに要するコストが高いと産業界には受け入れられないのが現状である。
Conventionally, it is well known that there is a need to recycle gypsum board as industrial waste.
However, in general, although it is known that recycling of industrial waste is good for the environment, it is unacceptable to the industry if the cost required for actual recycling is high.

処で、石膏ボードは、主原料の石膏を紙で被覆した板である。
そして、石膏ボードは経済性に優れ、耐久性、断熱性、遮音性が有り、建材用素材として多用されており、生産量は年間500万トンを超えている。
その為、当該石膏ボードの廃棄量は年間170万トンを超える状況にあり、製造時に発生する廃石膏ボードは、ほぼ100%リサイクルされるが、建築時に発生する廃石膏ボードは、約38%がリサイクルされているものの、建物の解体時に発生する廃石膏ボードは、リサイクル率が悪く、最終処分場に埋め立てられているのが現状である。
By the way, the gypsum board is a plate in which gypsum as a main raw material is coated with paper.
Gypsum board is economical, durable, heat-insulating, and sound-insulating, and is widely used as a building material. The production volume exceeds 5 million tons per year.
Therefore, the amount of gypsum board discarded exceeds 1.7 million tons per year. Almost 100% of waste gypsum board generated during production is recycled, but about 38% of waste gypsum board generated during construction Although it is recycled, the waste gypsum board that is generated when the building is demolished has a low recycling rate and is currently landfilled at the final disposal site.

従って、係る石膏ボードの有効なリサイクル処理の開発が必要となっている。
一方、他の産業廃棄物として、使用済み梱包材のポリプロピレン及びポリエチレン又は一般廃棄物のプラスチック容器に使用されているオレフィン系合成樹脂製品が知られており、係る使用済みのオレフィン系合成樹脂製品の再利用に関しても、必要性は認められながら、コストの問題があって、効率的なリサイクル処理方法は未だ実現されていない。
Therefore, it is necessary to develop an effective recycling process for such gypsum board.
On the other hand, as other industrial wastes, polypropylene and polyethylene used as packaging materials and olefin synthetic resin products used in plastic containers for general waste are known, and such used olefin synthetic resin products are known. Regarding the reuse, the necessity is recognized, but there is a problem of cost, and an efficient recycling method has not yet been realized.

処で、当該オレフィン系合成樹脂は、安価であって成形性が良いので、リサイクル用の原材料として流通量も多く、リサイクル材としても入手しやすいという特徴はあるが、成形時に加熱すると、とても柔らかくなり、異形押出加工する際には、硬さを調節して成形する必要がある。又、オレフィン系プラスチックの剛性を上げる目的があり、その為、係る硬さの調整に滑石という鉱石を徴粉砕した粉末のタルク等を配合して成形している。   However, since the olefin synthetic resin is inexpensive and has good moldability, it has a feature that it has a large circulation amount as a raw material for recycling and is easily available as a recycled material, but it is very soft when heated during molding. Therefore, when performing profile extrusion, it is necessary to mold by adjusting the hardness. In addition, there is an object of increasing the rigidity of the olefin plastic, and therefore, the hardness is adjusted by blending powder talc or the like obtained by collecting and grinding an ore called talc.

係るタルクの配合率は、オレフィン系の樹脂の重量に対して通常10%〜60%の配合を行い、かなりのウェイトを占める配合材料となっている。
そこで、当該オレフィン系の樹脂の溶融成形に際して、硬さを調整するためのタルクの代替品として当該建築廃材の石膏ボードを使用しようとする試みが過去に見られたが、成功せずに終っている。
The blending ratio of such talc is usually 10% to 60% with respect to the weight of the olefin resin, and is a blending material occupying a considerable weight.
Therefore, attempts have been made in the past to use the gypsum board of construction waste as a substitute for talc to adjust the hardness during melt molding of the olefin resin, but it ended without success. Yes.

その原因を検討すると、1つは、石膏ボードは耐久性を持たせる為と、もともと石膏に含まれる結晶水として含まれる水分で20%以上の水分が存在する。
一方、通常のプラスチックに混合するタルクの含水率は、ほぼ0%に規定されており、その理由としては、高温に加熱溶融されているオレフィン系の樹脂中に、若し含水率を有するタルクを混合させた場合、当該含水されている水が蒸発して成形時にプラスチックが発泡してしまい、成型された樹脂の強度低下を起す原因となるからである。
Examining the cause, one of the reasons is that the gypsum board has durability, and there is 20% or more of water originally included as crystal water contained in gypsum.
On the other hand, the water content of talc mixed with ordinary plastics is specified to be almost 0%. The reason for this is that talc having a water content is contained in an olefin-based resin heated and melted at a high temperature. This is because, when mixed, the water containing the water evaporates and the plastic foams during molding, causing a decrease in strength of the molded resin.

従って、石膏ボードの石膏には、20%の水を含んでいるので、オレフィン系の樹脂の骨材としては使えるものでは無い事は明らかである。
そして、もう1つの理由としては、石膏ボードは、石膏と紙から構成されており、仮に石膏の含水率を無くせたとしても、石膏と紙との分離が前提となり、この分離工程が容易ではない事から、更に余計なエネルギーの投入が必要となる。
Therefore, the gypsum of the gypsum board contains 20% of water, so it is obvious that it cannot be used as an aggregate of olefin resin.
And as another reason, the gypsum board is composed of gypsum and paper, and even if the moisture content of gypsum can be eliminated, the separation of gypsum and paper is a precondition, and this separation process is not easy. Therefore, it is necessary to input extra energy.

上記の理由から、従来では、石膏ボードをオレフィン系の樹脂のリサイクルに於ける骨材として使用する方法は実現されていない。
一方、オレフィン系の樹脂に未乾燥のフィラーを混合して発泡剤を形成し、金属基板等の表面に貼り付ける成形体の製造方法に関しては、例えば、特開2008−81648号公報(特許文献1)等で知られているが、石膏ボードそのものをフィラーとしてオレフィン系の樹脂の中に混在させる技術に関しては、公知例が見当たらない。
For the above reasons, a method of using gypsum board as an aggregate in recycling of olefin-based resin has not been realized.
On the other hand, regarding a method for producing a molded body in which an undried filler is mixed with an olefin-based resin to form a foaming agent and is attached to the surface of a metal substrate or the like, for example, JP 2008-81648 A (Patent Document 1). However, there is no known example regarding the technology of mixing the gypsum board itself into the olefin resin as a filler.

特開2008−81648号公報JP 2008-81648 A

従って、本発明の目的は、現在大量に産業廃棄物として排出される建築廃材としての使用済み石膏ボードと、同じく大量に産業廃棄物として排出されるペットボトルに代表される使用済みオレフィン系樹脂成形物とから、新規な特性を有する樹脂素材をリサイクル製品として製造し、産業廃棄物の減少に寄与させると共に、完全リサイクル処理の達成により当該新規リサイクル製品のコストを大幅に低減する事が可能な、樹脂素材及びその製造方法を提供するものである。   Accordingly, an object of the present invention is to provide a used gypsum board as a building waste material that is currently discharged in large quantities as industrial waste, and a used olefin resin molding represented by PET bottles that are also discharged in large quantities as industrial waste. It is possible to manufacture resin materials with new properties from recycled materials as recycled products, contribute to the reduction of industrial waste, and to achieve a complete recycling process, it is possible to greatly reduce the cost of the new recycled products. A resin material and a manufacturing method thereof are provided.

本発明に係る当該樹脂素材及びその製造方法は、上記目的を達成するために、以下に示す様な基本的技術構成を採用するものである。   In order to achieve the above object, the resin material and the method for producing the same according to the present invention employ a basic technical configuration as shown below.

即ち、本発明に係る第1の態様は、使用済みのオレフィン系合成樹脂成形物と使用済みの繊維状のセルロース成分を含む骨材とを攪拌機能を有する混合装置内に供給し、当該混合装置内で攪拌操作を行いつつ、当該使用済みのオレフィン系合成樹脂を粉砕溶融すると共に、当該使用済みのオレフィン系合成樹脂成分に当該骨材成分と当該繊維状のセルロース成分とを混合処理して再生合成樹脂素材を製造する方法に於いて、当該骨材として予め含水率が5%以上の骨材を使用すると共に、当該使用済みのオレフィン系合成樹脂を攪拌粉砕する際に、摩擦による発熱により溶融された当該溶融オレフィン系合成樹脂の溶融温度を、当該骨材に含有された水の蒸発作用によって、セルロース成分の炭化温度以下に抑制しながら攪拌混合処理を行うに際し、当該繊維状のセルロース成分を含む骨材として、使用済みの石膏ボード及び使用済みのダンボールとが使用される事を特徴とする再生合成樹脂素材の製造方法である。


That is, in the first aspect of the present invention, a used olefin-based synthetic resin molded product and a used aggregate containing a fibrous cellulose component are supplied into a mixing apparatus having a stirring function, and the mixing apparatus while performing stirring operation at an internal, with grinding melt the spent olefin synthetic resin, mixing processes and cellulose component of the aggregate component and the fibrous olefin synthetic resin component of the spent reproduced In the method of producing a synthetic resin material, an aggregate having a moisture content of 5% or more is used as the aggregate in advance, and when the used olefin synthetic resin is agitated and pulverized, it melts due to heat generated by friction. the melting temperature of been the molten olefinic synthetic resin, by evaporation action of water contained in the said aggregate, perform the stirring and mixing process while suppressing below carbonization temperature of the cellulose component Saishi, as aggregate comprising a cellulose component of the fiber, a manufacturing method of reproducing a synthetic resin material, characterized in that the used gypsum board and spent cardboard is used.


本発明に於ける当該樹脂素材の製造方法によって製造された当該樹脂素材は、その原材料は全てリサイクル用に準備されている材料を利用するものであるから、入手が容易で有る他、原材料の価格も低く、然も単に混合装置中で、スクリュー等によって攪拌する操作を実行するのみであるから、当該リサイクル処理に要するエネルギー及びコストは低く抑えられるので、リサイクル製品の価格は安価となり、理想的な完全リサイクル工程と完全リサイクル商品が得られるという作用効果を発揮するものである。   The resin material manufactured by the method of manufacturing the resin material according to the present invention uses materials that are prepared for recycling. However, since only the operation of stirring with a screw or the like is performed in the mixing apparatus, the energy and cost required for the recycling process can be kept low, so the price of the recycled product is low and ideal. It has the effect of being able to obtain fully recycled processes and fully recycled products.

更に、当該使用済みオレフィン系合成樹脂成形物と使用済み石膏ボードの混合体に少量のステアリン酸ナトリウムを混合することによって、短時間でかつ紙成分であるセルロース繊維成分を炭化させることなく、オレフィン系合成樹脂と石膏ボードとを混合させることが可能となる。   Furthermore, by mixing a small amount of sodium stearate into the mixture of the used olefin-based synthetic resin molded product and the used gypsum board, the olefin-based material can be obtained in a short time without carbonizing the cellulose fiber component, which is a paper component. It becomes possible to mix the synthetic resin and the gypsum board.

図1は、本発明に於ける樹脂素材の構造を示す断面図である。FIG. 1 is a cross-sectional view showing the structure of a resin material in the present invention. 図2は、本発明に於ける樹脂素材の製造装置の概略を示す図である。FIG. 2 is a diagram showing an outline of a resin material manufacturing apparatus in the present invention. 図3は、本発明に於ける樹脂素材の製造方法の一具体例を説明するフローチャートである。FIG. 3 is a flowchart for explaining a specific example of the method for producing a resin material in the present invention.

以下に、本発明にかかる樹脂素材及び当該樹脂素材の製造方法の具体的な構成を、図面を参照しながら以下に詳細に説明する。   Below, the specific structure of the resin raw material concerning this invention and the manufacturing method of the said resin raw material is demonstrated in detail, referring drawings.

即ち、図1は、本発明に係る樹脂素材1の一具体例の構成を示す図であって、図中、オレフィン系合成樹脂成分2の中に、粉体状の石膏成分3及び繊維状セルロース成分4と、が略均一に分散されて混在している樹脂素材が示されている。   That is, FIG. 1 is a diagram showing the configuration of a specific example of the resin material 1 according to the present invention. In the figure, the olefin-based synthetic resin component 2 includes a powdery gypsum component 3 and fibrous cellulose. A resin material in which component 4 is dispersed in a substantially uniform manner is shown.

係る構成の結果、当該繊維状セルロース成分4の一部が適宜の割合で当該成型された樹脂体の表面に顕出しているので、当該樹脂素材の表面が木質調の風合いを呈するものである。   As a result of such a configuration, a part of the fibrous cellulose component 4 is exposed on the surface of the molded resin body at an appropriate ratio, so that the surface of the resin material exhibits a woody texture.

又、本発明にかかる樹脂素材の製造方法は、図2に示す様に、オレフィン系合成樹脂成形物2‘と適宜の大きさに破砕された石膏ボード片5とを、適宜の駆動手段、例えば、モータ8により回転せしめられるスクリュー等からなる攪拌手段9を有する混合装置10内に順次に供給し、当該混合装置10内で攪拌操作を行いつつ、当該オレフィン系合成樹脂2’を粉砕溶融すると共に、その後に当該石膏ボード片5を供給してこれを粉砕して粉体状の石膏成分と繊維状のセルロース成分とに分離しながら、溶融されたオレフィン系合成樹脂2と上記2成分を混合する事を特徴とする石膏成分及びセルロース成分を含む樹脂素材の製造方法である。   In addition, as shown in FIG. 2, the method for producing a resin material according to the present invention comprises an olefin-based synthetic resin molded product 2 ′ and a gypsum board piece 5 crushed to an appropriate size. The olefin-based synthetic resin 2 ′ is crushed and melted while being sequentially supplied into a mixing device 10 having a stirring means 9 made of a screw or the like rotated by a motor 8 and performing the stirring operation in the mixing device 10. Then, the molten olefin-based synthetic resin 2 and the above two components are mixed while supplying the gypsum board piece 5 and crushing it to separate it into a powdery gypsum component and a fibrous cellulose component. This is a method for producing a resin material containing a gypsum component and a cellulose component.

つまり、本発明に於いては、従来合成樹脂に骨材を混入する場合には、当該骨材には水分を含まないものを使用する必要があるという常識を覆し、積極的に含水率の高い石膏を使用して石膏成分と繊維状セルロース成分とオレフィン系合成樹脂成分とが均一に混合された木質系の質感を有する新規な樹脂素材が得られるのである。   In other words, in the present invention, when the aggregate is mixed in the conventional synthetic resin, the common sense that it is necessary to use an aggregate that does not contain moisture, and the water content is positively high. By using gypsum, a novel resin material having a woody texture in which a gypsum component, a fibrous cellulose component, and an olefin synthetic resin component are uniformly mixed can be obtained.

此処で、本発明に於ける当該樹脂素材の製造方法の基本的な技術思想について以下に説明する。
即ち、本発明に於いて使用される主体となる樹脂は、容器リサイクルから出た使用済みのオレフィン系(主にPP)樹脂成形物を使用する。
又、石膏ボードも使用済みのもの、つまり廃材となった石膏ボードを使用する。
Here, the basic technical idea of the method for producing the resin material in the present invention will be described below.
That is, as the main resin used in the present invention, a used olefin-based (mainly PP) resin molded product from container recycling is used.
In addition, a gypsum board that has already been used, that is, a gypsum board that has become waste, is used.

そして、本発明では、かかるオレフィン系樹脂成形物を適宜のミキサーによって溶融して、これに当該使用済みの石膏ボードを混合して行く。
混合処理が完了したものは、成形処理後、ある程度の大きさに粉砕し、プラスチックの原料となる。
つまり、再生樹脂を製造する際、工程的には、最初にオレフィン系樹脂成形物の溶融が行わる。
そして、係る溶融時に当該使用済みの石膏ボードを混合する。
In the present invention, the olefin-based resin molded product is melted by an appropriate mixer, and the used gypsum board is mixed therewith.
After the mixing process is completed, the mixture is pulverized to a certain size and becomes a plastic raw material.
That is, when the recycled resin is produced, the olefin resin molded product is first melted in a process.
And the said used gypsum board is mixed at the time of the said fusion | melting.

その結果、当該オレフィン系樹脂は溶融時に温度が170℃を超えているので、当該石膏ボードに含まれている水分は、この熱により、一気に放出される事になる。
次に問題となる石膏ボードの紙について説明するならば、石膏ボードと紙の割合は、廃石膏ボードが処分された方法によって差異があるが、一般的に石膏が8乃至9.58に対して、紙が2乃至0.5の割合となっている。
As a result, since the temperature of the olefin-based resin exceeds 170 ° C. when melted, the moisture contained in the gypsum board is released at once by this heat.
Next, to explain the gypsum board paper in question, the ratio of gypsum board to paper varies depending on how the gypsum board was disposed of, but generally the gypsum is 8 to 9.58. The ratio of paper is 2 to 0.5.

然しながら、一般に、石膏ボードには、平均して20%の含水率を含んでいるので、計算上の当該石膏ボードの混合割合を55%とした場合、仮に、石膏ボードを使って配合を行った場合、樹脂が50%、石膏が45%、紙が5%となり、好ましい混合比率を有する樹脂素材となる。   However, in general, the gypsum board contains a water content of 20% on average. Therefore, when the mixing ratio of the gypsum board in the calculation is 55%, the gypsum board was used for blending. In this case, resin is 50%, gypsum is 45%, and paper is 5%, which is a resin material having a preferable mixing ratio.

本発明に於ける当該樹脂素材は、比較的長い繊維状のセルロース成分が含まれていることから、従来公知のペーパースラッジ入り樹脂と同様に、石膏に含まれていた紙成分から抽出されたセルロース繊維が他の成分と混じり合い、強度を向上させると同時に、成形物の質感が木質系となるというメリットが生まれる。
更に、本発明の樹脂素材の製造方法に付いてより具体的に説明するならば、従来では、一般的に樹脂の溶融は当該樹脂を外部加熱して溶融する。
Since the resin material in the present invention contains a relatively long fibrous cellulose component, the cellulose extracted from the paper component contained in the gypsum as well as the conventionally known resin containing paper sludge. The fiber mixes with other ingredients to improve the strength, and at the same time, a merit that the texture of the molding becomes a woody system is born.
Furthermore, if it demonstrates more concretely about the manufacturing method of the resin raw material of this invention, conventionally, melting of resin is generally melted by heating the said resin externally.

然しながら、本発明に於いては、当該オレフィン系樹脂成形物を混合機(ミキシング機)10に樹脂を投入して、当該スクリュー9を回転させ、その結果、当該オレフィン系樹脂成形物は高回転するプロペラ或はスクリュー等に当り、又、樹脂同士がぶつかり合い、摩擦熱が生じ、これを繰り返す事で、当該オレフィン系樹脂成形物は溶融を始める。   However, in the present invention, the olefin resin molded product is charged into a mixer (mixing machine) 10 and the screw 9 is rotated. As a result, the olefin resin molded product rotates at a high speed. The resin hits a propeller or a screw, and the resins collide with each other to generate frictional heat. By repeating this, the olefin resin molded product starts to melt.

即ち、当該ミキサーで回転せしめられた当該使用済みのオレフィン系樹脂成形物は摩擦熱により溶融し、当該使用済みのオレフィン系樹脂成形物のこの時の温度は170℃を超えている。
係る時点で、仮に当該溶融中の使用済みのオレフィン系樹脂成形物の中に、紙成分を入れたとすれば、数分で紙は炭化してしまうので、紙に期待する繊維や木質系の質感は無くなる。
That is, the used olefin resin molded product rotated by the mixer is melted by frictional heat, and the temperature of the used olefin resin molded product at this time exceeds 170 ° C.
At that time, if the paper component is put in the used olefin resin molding being melted, the paper will carbonize in a few minutes. Will disappear.

然しながら、当該170℃に加熱させたオレフィン系樹脂成形物は、ミキサーの中でゲル化している。
そして、係る加熱溶融状態のオレフィン系樹脂成形物の中に含水率20%の石膏ボードを投入すると、激しい水分蒸発が開始される。
However, the olefin resin molded product heated to 170 ° C. is gelled in the mixer.
When a gypsum board having a water content of 20% is put into the heat-melted olefin resin molded product, intense water evaporation is started.

係る時点では、まだ石膏ボードは石膏と紙とが分離していない状態で、内部の水分が蒸発をしている状態にある。
そして、係る状況を詳細に観察するならば、当該水分蒸発がされている間は水分が熱せられて高温になると考えられるが、逆にステアリン酸ナトリウムが有効に作用している場合には、100℃以上の水蒸気で紙を冷やしていると考えられる。
At that time, the gypsum board is still in a state where the gypsum and the paper are not separated, and the internal moisture is evaporated.
If the situation is observed in detail, it is considered that the water is heated to a high temperature while the water is evaporated, but conversely, when sodium stearate is acting effectively, 100 It is thought that the paper is cooled with water vapor at or above.

つまり、水分が蒸発している間は、紙は水蒸気によって170℃のゲル化している樹脂の熱から灰化するのを防いでいるのである。
換言するならば、本発明に於いては、上記した構成を採用することによって、紙或いはセルロース繊維の灰化のタイミングを外して、樹脂との混合を遂行していく。
当該混合が終了したら、当該混合体を一気に冷却する。
In other words, while the water is evaporating, the paper is prevented from ashing from the heat of the gelled resin at 170 ° C. by water vapor.
In other words, in the present invention, by adopting the above-described configuration, the timing of ashing of paper or cellulose fiber is removed and mixing with the resin is performed.
When the mixing is completed, the mixture is cooled at once.

この時、さらに炭化を防ぐのに材料の0.5乃至3重量%、好ましくは1%ほどのステアリン酸ナトリウムを同時に添加する事も好ましい具体例であり、これによって当該セルロース繊維が炭化する時間を更に遅くする事が可能である。 At this time, an additional 0.5 to 3% by weight of the material to prevent carbonization, preferably also preferred embodiment the addition of sodium stearate as 1% at the same time, whereby the time which the cellulose fibers are carbonized It can be made even slower.

ステアリン酸ナトリウムを入れることにより、おそらくステアリン酸ナトリウムが石膏ボードに付着して塗膜を作り、摩擦力を低下させた結果、紙の温度上昇を防ぎ、炭化のスピードを遅らせるものと推定される。   By adding sodium stearate, it is presumed that sodium stearate will probably adhere to the gypsum board to create a coating film and reduce the frictional force, thereby preventing an increase in the temperature of the paper and slowing the carbonization speed.

これは、本発明の別の応用としてダンボールを樹脂に混合する際、ダンボールを炭化させずに混合する時も同じ手段を使用する事が可能である。
つまり、本発明に於いては、あらかじめ混合機の中に使用済みのオレフィン系樹脂成形物を入れて高速回転混合させ、そのプラスチック同士の摩擦熱により石膏の含水率を下げると言う、従来にない技術思想を導入したもので、この時、当該使用済みのオレフィン系樹脂成形物は溶融を始めているので170℃前後の温度になっている。ここに合水率の高い使用済みの石膏ボードをそのまま或は適度に破砕してから投入すると、使用済みの石膏ボードは粉体化して、石膏の粉粒体となり、紙は剪断され、比較的長い繊維状のセルロース成分となる。その時、使用済みの石膏ボードの持っていた水分が一気に蒸発、放熱を行い、紙の温度を、紙が炭化する温度に上昇する事を防ぐ事が可能となる。
As another application of the present invention, when the cardboard is mixed with the resin, the same means can be used when the cardboard is mixed without being carbonized .
In other words, in the present invention, a used olefin resin molded product is put in a mixer in advance and mixed at high speed, and the moisture content of the gypsum is lowered by frictional heat between the plastics. At this time, the used olefin-based resin molded product has started to melt, and thus has a temperature of around 170 ° C. If a used gypsum board with a high water content is put here as it is or after being appropriately crushed, the used gypsum board is pulverized into a gypsum powder, the paper is sheared, It becomes a long fibrous cellulose component. At that time, the moisture of the used gypsum board evaporates and dissipates heat at once, and it is possible to prevent the temperature of the paper from rising to a temperature at which the paper is carbonized.

水蒸気が出ている間は、全く紙は炭化しない事から、水蒸気が紙を冷やしてくれているものと推測できる。
その後、色々実験を繰り返した結果、当該石膏ボードの水が当該オレフィン系樹脂成形物と石膏ボードとの混合を促進している事が判明した。
Since the paper is not carbonized at all while the water vapor is emitted, it can be assumed that the water vapor has cooled the paper.
Then, as a result of repeating various experiments, it was found that the water of the gypsum board promoted the mixing of the olefin resin molded product and the gypsum board.

尚、本発明に於いて使用される石膏ボードは、その成分は特に限定されるものではないが、一般的に使用されている、半水石膏、二水石膏或いは無水石膏等を主成分とする石膏ボード使用する事が出来る。   In addition, although the component is not specifically limited, the gypsum board used in this invention has hemihydrate gypsum, dihydrate gypsum, or anhydrous gypsum as a main component. You can use plasterboard.

また、この方法でオレフィン系樹脂成形物中に紙を混合すると、従来の方法の様に、粉砕した紙を混合するのに比べて、強度が増す事が判明した。これは混合機の中で、紙は引っ張られ、引きちぎられる所謂剪断処理を受けることとなり、粉砕物と比べて圧倒的に繊維長が長くなるから強度が増す事になると考えられる。   Further, it has been found that when paper is mixed into the olefin resin molded product by this method, the strength is increased as compared with the case of mixing pulverized paper as in the conventional method. This is because the paper is subjected to a so-called shearing process in which the paper is pulled and torn in the mixer, and the fiber length is overwhelmingly longer than that of the pulverized product.

更に、本発明では、従来プラスチックの中に繊維長の長いセルロース分は混合で出来ないとされていたのに対し、例えば、ステアリン酸ナトリウムを1%乃至3%程度混合する事により、繊維が鳥の羽根状になっている所に油脂成分が付着して濡れ性能が上がり、プラスチックが受け入れやすくなることと、繊維質が摩擦によって崩壊又は炭化しないようにコントロールされ、その結果、異物間の混合が均一化される事が判明した。   Furthermore, according to the present invention, cellulose having a long fiber length cannot be mixed in a conventional plastic, whereas, for example, by mixing about 1% to 3% of sodium stearate, the fiber can be removed. The oil and fat component adheres to the wing-shaped part of the material to improve the wetting performance, making the plastic easier to accept, and controlling that the fiber does not collapse or carbonize due to friction. It turned out to be uniform.

更に、本発明に於いては、プラスチックに石膏ボードをそのまま混合させるに際しては、石膏と紙とを分離せずにそのまま含水率も下げずにオレフィン系樹脂成形物と混合するという点も特徴となる。   Furthermore, in the present invention, when gypsum board is mixed with plastic as it is, it is also characterized in that gypsum and paper are mixed with an olefin resin molded product without decreasing the water content without separating the gypsum and paper. .

本発明に於いて使用されるオレフィン系合成樹脂としては、使用済みのポリプロピレン樹脂やポリエチレン樹脂が使用できる。
そして、本発明に於いては、当該オレフィン系合成樹脂成分としては、使用済みのプラスチック容器類、或いはポリプロピレン樹脂で構成された樹脂製品の様な、産業廃棄物として取り扱われる製品を原材料として、そのリサイクル製品を製造するものである。
As the olefin-based synthetic resin used in the present invention, used polypropylene resin and polyethylene resin can be used.
In the present invention, as the olefin-based synthetic resin component, as a raw material, a product handled as industrial waste, such as a used plastic container or a resin product made of polypropylene resin, It manufactures recycled products.

そして、これ等のオレフィン系合成樹脂を一旦溶融されて、適宜の大きさのペレットの形状に加工されるが、本発明では、主に係るペレット状又は粉砕されたオレフィン系合成樹脂を使用する事が望ましい。   These olefin-based synthetic resins are once melted and processed into pellets of an appropriate size. In the present invention, mainly the pellet-shaped or pulverized olefin-based synthetic resins are used. Is desirable.

一方、本発明に於いて使用される石膏ボードも使用済みで産業廃棄物として取り扱われる石膏ボードを原材料として使用するものである。
従って、本発明に於いては、何れもかなり大量に産業廃棄物市場に存在しているものを原材料として使用するものであるから、原材料の調達に係るコストは低額に抑えられる利点がある。
On the other hand, the gypsum board used in the present invention is also used as a raw material, which is already used and handled as industrial waste.
Accordingly, in the present invention, since a large amount of materials existing in the industrial waste market are used as raw materials, there is an advantage that the cost for procurement of raw materials can be suppressed to a low cost.

本発明に於いては、上記した通り、当該オレフィン系合成樹脂成分としての、使用済みオレフィン系合成樹脂成型物を、適当なサイズに破砕して、それを適宜の混合機に入れて攪拌処理する事により、当該樹脂同士の摩擦熱により発熱が起こり、当該オレフィン系合成樹脂成型物は溶融状態になる。   In the present invention, as described above, the used olefin-based synthetic resin molded product as the olefin-based synthetic resin component is crushed into an appropriate size, and is put into an appropriate mixer and stirred. As a result, heat is generated by the frictional heat between the resins, and the olefin-based synthetic resin molding is in a molten state.

その状態で、当該溶融状態の使用済みのオレフィン系合成樹脂内に、適度のサイズに破砕した使用済みの石膏ボードを混入して、使用済みのオレフィン系合成樹脂と共に攪拌操作を継続させると、当該石膏が含水している水がその間に蒸発し、それにより、当該使用済みのオレフィン系合成樹脂の溶融温度が当該石膏に含まれている紙の炭化温度以下となる様に調整が行われ、使用済みの石膏ボードから分離された石膏粒体と紙とが分離されるが、当該紙成分は化温度以下の温度条件下に存在しえるので炭化することなく、当該混合機の攪拌操作によって、剪断操作を受けて、比較的長い長さを有する繊維状のセルロースが分離されてくる。 In this state, in the olefin-based synthetic resin used in the molten state, by mixing a gypsum board spent crushing to moderate size, and to continue the stirring operation along with the spent olefin synthetic resin, the gypsum evaporates during which water is water, whereby the melting temperature of the spent olefin synthetic resin is adjusted so that the following carbonization temperature of the paper contained in the gypsum performed, using The gypsum granules and paper separated from the finished gypsum board are separated, but the paper components can exist under temperature conditions below the conversion temperature, so that they are not carbonized and are sheared by stirring the mixer. In response to the operation, fibrous cellulose having a relatively long length is separated.

係る3種類の成分が略均一に混合され当該石膏成分とセルロース成分当該オレフィン系合成樹脂をマトリクスとして、その中に分散されている状態の樹脂素材が得られる。
係る樹脂素材を一旦細かく細片化して、適宜の押し出し成型機或いは射出成型機等を使用して所望の形に成型した樹脂製品を得る事が出来る。
The three kinds of components are mixed substantially uniformly, and the resin material in a state in which the gypsum component and the cellulose component are dispersed in the olefin-based synthetic resin as a matrix is obtained.
It is possible to obtain a resin product in which the resin material is finely divided into pieces and molded into a desired shape using an appropriate extrusion molding machine or injection molding machine.

次に、本発明に於ける当該樹脂素材或いはそれを用いた樹脂成型品に於ける、オレフィン系合成樹脂成分、粉体状の石膏成分及び当該繊維状セルロース成分のそれぞれの混合割合について、種々実験した結果、先ず当該オレフィン系合成樹脂成分と当該石膏ボードとの混合比率は、20:80から60:40の範囲である事が望ましい事が判明し、且つ、上記した様に、当該石膏ボードと紙(当該セルロース系繊維成分)の割合が一般的に使用される廃石膏ボードでは、石膏が8〜9.5に対して、紙が0.5から2の割合となっていることから、当該オレフィン系合成樹脂成分、当該石膏成分及び繊維状セルロース系成分との相互混合比率、オレフィン系合成樹脂成分:石膏成分:繊維状セルロース系成分は、20:64〜76:4〜16、乃至は、60:32〜38:2〜8である事が望ましい事が判明した。   Next, various experiments were conducted on the mixing ratios of the olefin-based synthetic resin component, the powdery gypsum component, and the fibrous cellulose component in the resin material or the resin molded product using the resin material in the present invention. As a result, first, it was found that the mixing ratio of the olefin-based synthetic resin component and the gypsum board is preferably in the range of 20:80 to 60:40, and as described above, In the waste gypsum board in which the ratio of paper (the cellulosic fiber component) is generally used, since the gypsum is 8 to 9.5 and the ratio of paper is 0.5 to 2, Olefin synthetic resin component, mutual mixing ratio of gypsum component and fibrous cellulose component, olefin synthetic resin component: gypsum component: fibrous cellulose component, 20:64 to 76: 4 to 16 Or it is, 60: 32-38: It has been found that it is desirable 2-8.

従って、本発明に於ける当該樹脂素材或いはそれを用いた樹脂成型品における、
オレフィン系合成樹脂成分の混入比率が30〜50%、
粉体状の石膏成分の混入比率が63〜40%及び、
繊維状セルロース成分の混入比率が14〜5%
である組成比を有している事が望ましい。
Therefore, in the resin material in the present invention or a resin molded product using the resin material,
The mixing ratio of the olefin synthetic resin component is 30 to 50%,
The mixing ratio of the powdery gypsum component is 63 to 40%, and
Mixing ratio of fibrous cellulose component is 14-5%
It is desirable to have a composition ratio of

本発明に於いては、当該オレフィン系合成樹脂成分と当該石膏成分との混合比率によって、得られる新規な樹脂素材の特性が変化するものであって、当該オレフィン系合成樹脂成分が当該石膏成分よりも多ければ、石膏入り樹脂素材となり、反対に当該石膏成分が当該オレフィン系合成樹脂成分よりも多ければ、樹脂入り石膏ボードとなる。   In the present invention, the characteristics of the resulting new resin material change depending on the mixing ratio of the olefin-based synthetic resin component and the gypsum component, and the olefin-based synthetic resin component is different from the gypsum component. If it is more, it becomes a resin material containing gypsum, and conversely if it is more than the olefin-based synthetic resin component, it becomes a resin-containing gypsum board.

更に、本発明に於いては、上記した当該オレフィン系合成樹脂素材の各成分以外に、ステアリン酸ナトリウムが更に含まれているものであっても良い。
本発明に於ける当該ステアリン酸ナトリウムの混入割合は、特に限定されないが、ステアリン酸ナトリウムの混入量は、0.5乃至3重量%である事が好ましく、特には、1重量%である事が望ましい。
Furthermore, in the present invention, sodium stearate may be further included in addition to the above components of the olefin synthetic resin material.
The mixing ratio of sodium stearate in the present invention is not particularly limited, but the mixing amount of sodium stearate is preferably 0.5 to 3% by weight, particularly 1% by weight. desirable.

次に、本発明により得られた当該新規な樹脂素材は、比較的長い繊維長を持ったセルロース成分がオレフィン系合成樹脂と石膏成分と間に介在している事から樹脂素材としての強度が向上すると共に、当該長い繊維長を持つセルロースが適度に当該樹脂素材の表面に出現しているので、木質調の質感が得られる。   Next, the new resin material obtained by the present invention is improved in strength as a resin material because the cellulose component having a relatively long fiber length is interposed between the olefin synthetic resin and the gypsum component. In addition, since the cellulose having the long fiber length appears moderately on the surface of the resin material, a woody texture can be obtained.

又、本発明に於ける当該樹脂素材は、耐水性に強く従って屋外のデッキ材として使用いることが可能であり、更には、当該樹脂素材の表面の滑り抵抗があるので、水にぬれた状態で人がその上を歩いても滑る可能性は低いという特徴を持っている。
以下の表1は、従来の屋外のデッキ材として代表的な木材である杉材と本発明の樹脂素材の表面滑り抵抗値を測定して比較したものである。
In addition, the resin material in the present invention is strong in water resistance and therefore can be used as an outdoor deck material, and further has a slip resistance on the surface of the resin material, so that it is wet with water. Therefore, it has a feature that a person is unlikely to slide even if he / she walks on it.
Table 1 below compares and compares the surface slip resistance values of cedar, which is a typical wood as a conventional outdoor deck material, and the resin material of the present invention.

Figure 0005442552
Figure 0005442552

上記の比較データから、本発明に於ける当該樹脂素材は、杉材と略同等の滑り抵抗値を有するものである事が理解される。
尚、参考データとして、条例施設整備マニュアルに規定されている滑り抵抗値を示す。
下足で歩行する部分 0.4 〜0.9
上足で歩行する部分 0.35〜0.9
素足で歩行する部分 0.45〜0.9
傾斜路部分 0.5 〜0.9
From the above comparison data, it is understood that the resin material in the present invention has a slip resistance value substantially equal to that of cedar.
For reference data, the slip resistance value specified in the Ordinance Facility Maintenance Manual is shown.
The part which walks with lower leg 0.4-0.9
Part walking with upper leg 0.35-0.9
Part walking with bare feet 0.45-0.9
Ramp part 0.5-0.9

尚、上記した滑り抵抗値の測定方法は、人の歩行を前提とした測定方法であり、錘を付けたゴム片を床上に置き、斜め上から引張った時に当該ゴム片が動き出す荷重から求めたものであり、JIS A1454(高分子系張り床材試験法)によるものである。   The above-mentioned measuring method of the slip resistance value is a measuring method on the premise of human walking, and is obtained from the load at which the rubber piece moves when the rubber piece with a weight is placed on the floor and pulled diagonally from above. It is based on JIS A1454 (polymer type tension flooring test method).

又、本発明に係る当該樹脂素材に於いて、使用済み石膏ボードの混合割合を重量比で55%とした新石膏ボードの物性値を杉材の物性値と対比したものを表2に示す   In addition, in the resin material according to the present invention, the physical properties of the new gypsum board in which the mixing ratio of the used gypsum board is 55% by weight are compared with the physical properties of cedar.

Figure 0005442552
Figure 0005442552

上記データは成形断面及び成形条件によって変化する。
上記した物性表から見ると、本発明に係る当該樹脂素材は、木材の杉より若干強度的に劣るものの、耐候性、耐蟻性、耐朽性に富んでいる部材である事が判る。
The above data varies depending on the molding section and molding conditions.
From the above physical property table, it can be seen that the resin material according to the present invention is a member having excellent weather resistance, ant resistance, and decay resistance, although it is slightly inferior in strength to wood cedar.

これらから判断すると、本発明に係る当該樹脂素材は、屋外のエクステリア及び、水周りの建材に適していると思われる。
つまり、本発明に係る樹脂素材としては、滑り抵抗値(C.S.R.)が0.74乃至0.81である事が特徴である。
Judging from these, it seems that the resin material according to the present invention is suitable for outdoor exteriors and building materials around water.
That is, the resin material according to the present invention is characterized in that the slip resistance value (CSR) is 0.74 to 0.81.

次に、本発明に於ける当該樹脂素材を製造する方法に付いて説明する。
本発明の当該樹脂素材の製造方法は、基本的には、図2に示す様に、オレフィン系合成樹脂2‘と石膏ボード5とを攪拌機能9を有する混合装置10内に順次に供給し、当該混合装置10内で攪拌操作を行いつつ、当該オレフィン系合成樹脂2’を粉砕溶融すると共に、当該石膏ボード5を粉砕して粉体状の石膏成分3と繊維状のセルロース成分4とに分離しながら、上記3成分を混合する事を特徴とする石膏成分及びセルロース成分を含む樹脂素材の製造方法である。
Next, the method for producing the resin material in the present invention will be described.
The method for producing the resin material of the present invention basically supplies the olefin-based synthetic resin 2 ′ and the gypsum board 5 sequentially into a mixing apparatus 10 having a stirring function 9, as shown in FIG. While performing the stirring operation in the mixing apparatus 10, the olefin synthetic resin 2 ′ is pulverized and melted, and the gypsum board 5 is pulverized to be separated into a powdery gypsum component 3 and a fibrous cellulose component 4. However, it is a method for producing a resin material containing a gypsum component and a cellulose component, characterized by mixing the above three components.

そして、本発明の特に技術上の特徴点は、当該オレフィン系合成樹脂2‘を攪拌粉砕する際に、摩擦熱による発熱により溶融された当該溶融オレフィン系合成樹脂2の溶融温度を、当該石膏ボード5を混入する際に、当該石膏ボード5がもともと含水している水を蒸発させることにより、セルロース成分4の化温度以下に抑制しながら、攪拌処理する事にある。   In particular, the technical feature of the present invention is that when the olefin synthetic resin 2 ′ is stirred and pulverized, the melting temperature of the molten olefin synthetic resin 2 melted by heat generated by frictional heat is determined by the gypsum board. When 5 is mixed, the water that the gypsum board 5 originally contains water is evaporated, whereby the stirring treatment is performed while suppressing the temperature below the conversion temperature of the cellulose component 4.

即ち、溶融状態にある使用済みのオレフィン系合成樹脂2に使用済みの石膏ボード5を混入させて両者を粉砕し、当該使用済みの石膏ボード5を石膏成分3と紙成分に分離し、更に当該紙成分を剪断処理して繊維状セルロース成分4を発生させる際に、当該使用済みのオレフィン系合成樹脂2の溶融温度をセルロース4の炭化温度以下に維持しながら混合処理するものである。



That is, by mixing the used gypsum board 5 to olefin synthetic resin 2 used in a molten state was ground both to separate the gypsum board 5 of the spent to gypsum component 3 and the paper component, further the When the fibrous cellulose component 4 is generated by shearing the paper component, mixing treatment is performed while maintaining the melting temperature of the used olefin-based synthetic resin 2 below the carbonization temperature of the cellulose 4.



そして、本発明では、上記混合処理により当該石膏ボード5の各成分の分離が完了した時点で当該混合体を急速に冷却するものである。
更に、本発明に於いては、上記した様に、オレフィン系合成樹脂2‘と石膏ボード5とを攪拌機能を有する混合装置内に順次に供給する際に、ステアリン酸ナトリウムを添加する事が好ましい。
And in this invention, the said mixture is rapidly cooled at the time of completion | finish of isolation | separation of each component of the said gypsum board 5 by the said mixing process.
Furthermore, in the present invention, as described above, it is preferable to add sodium stearate when sequentially supplying the olefin-based synthetic resin 2 ′ and the gypsum board 5 into the mixing apparatus having a stirring function. .

本発明に於いては、当該ステアリン酸ナトリウムの混入量は、0.5乃至3重量%であって、更に望ましくは、1重量%である。
又、本発明に於いて、当該混合機に投入される当該オレフィン系合成樹脂2‘と当該石膏ボード5との混合割合は、オレフィン系合成樹脂が20乃至60重量%、好ましくは30乃至45重量%であり、又当該石膏ボードが、40乃至80重量%、好ましくは55%乃至70重量%である事が望ましい。
In the present invention, the amount of sodium stearate mixed is 0.5 to 3% by weight, more preferably 1% by weight.
In the present invention, the mixing ratio of the olefin synthetic resin 2 ′ and the gypsum board 5 charged into the mixer is 20 to 60% by weight of olefin synthetic resin, preferably 30 to 45% by weight. It is desirable that the gypsum board is 40 to 80% by weight, preferably 55% to 70% by weight.

本発明に於いては、上記の方法によって混合され製造されたオレフィン系合成樹脂素材を例えば、異形押出成形装置或は射出成形装置を使用して成形加工する事が出来る。
上記した通り、本発明は、完全リサイクルを実現するものであって、具体的には、使用済みオレフィン系合成樹脂成形物と使用済み石膏ボードとを攪拌機能を有する混合装置内に順次に供給し、当該混合装置内で攪拌操作を行いつつ、当該オレフィン系合成樹脂を粉砕溶融すると共に、当該石膏ボードを粉砕して粉体状の石膏成分と繊維状のセルロース成分とに分離しながら、当該溶融されたオレフィン系合成樹脂に当該粉体状の石膏成分と当該繊維状のセルロース成分とを混合し、成型加工処理して木質調の完全リサイクル樹脂素材を製造する方法であるから、原材料のコストは低価格に抑えられると共に、その後の加工工程も外部加熱による余分なエネルギーの消耗がないので、加工コストも低く抑える事が可能である。
In the present invention, the olefinic synthetic resin material mixed and produced by the above method can be molded using, for example, a profile extrusion molding apparatus or an injection molding apparatus.
As described above, the present invention realizes complete recycling. Specifically, the used olefin-based synthetic resin molded product and the used gypsum board are sequentially supplied into a mixing apparatus having a stirring function. The olefin synthetic resin is pulverized and melted while stirring in the mixing apparatus, and the gypsum board is pulverized and separated into a powdery gypsum component and a fibrous cellulose component. This is a method of mixing the powdered gypsum component and the fibrous cellulose component to the olefin-based synthetic resin, and molding and processing it to produce a completely recycled resin material with a wood tone. In addition to being kept at a low price, since the subsequent processing steps do not consume extra energy due to external heating, the processing costs can be kept low.

又、本発明に於いて使用される添加剤としては、ステアリン酸ナトリウムも使用済みが好ましいが、産業廃棄物の一つである廃油を少量添加することも可能である。
以下に、本発明に於ける当該樹脂素材の製造方法の手順を図3に示すフローチャートを参照しながら説明する。
As an additive used in the present invention, sodium stearate is preferably used, but it is also possible to add a small amount of waste oil which is one of industrial wastes.
Below, the procedure of the manufacturing method of the said resin raw material in this invention is demonstrated, referring the flowchart shown in FIG.

即ち、ステップS−1に於いて、使用済みのオレフィン系樹脂成形物を選択し、ステップS−2で適宜の大きさのペレット状に粉砕する。
この段階では、例えば、株式会社ホーライ製のVシリーズ粉砕機を使用する事が可能である。
That is, in step S-1, a used olefin resin molded product is selected, and in step S-2, it is pulverized into pellets of an appropriate size.
At this stage, for example, a V series grinder manufactured by Horai Co., Ltd. can be used.

当該ペレット状粉砕物の成分は、一般的に、PPが60%、PEが30%、PSが10%の割合と成っている。
その後、ステップS−3に進み、当該ペレットを、回転羽根9を有する混合装置10、例えば、株式会社三井三池製のFM500F型の混合装置(ミキサー)を使用する事が可能である。
The components of the pelletized pulverized product generally comprise 60% PP, 30% PE, and 10% PS.
Then, it progresses to step S-3 and it is possible to use the said pellet for the mixing apparatus 10 which has the rotary blade 9, for example, the mixing apparatus (mixer) of the Mitsui Miike Co., Ltd. make.

ステップS−4では、当該混合装置で当該回転羽根9の回転によって、ペレット状のオレフィン系樹脂成形物に摩擦熱が発生し、当該熱によって当該ペレット状のオレフィン系樹脂成形物は溶融を開始する。   In step S-4, friction heat is generated in the pellet-shaped olefin resin molding by the rotation of the rotary blade 9 in the mixing device, and the pellet-shaped olefin resin molding starts to be melted by the heat. .

係る状態になった時に、ステップS−6で選択されている使用済みの石膏ボードを、必要に応じてステップS−7で適宜の大きさに破砕し、当該破砕された当該石膏ボード5をステップS−8で当該混合機内に投入して、少なくとも一部が溶融状態にある溶融オレフィン系樹脂成形物と混合し、ミキシング操作を継続させる。   When it becomes such a state, the used gypsum board selected in step S-6 is crushed to an appropriate size in step S-7 as necessary, and the crushed gypsum board 5 is stepped. In S-8, the mixture is introduced into the mixer and mixed with a molten olefin resin molded product in which at least a part is in a molten state, and the mixing operation is continued.

使用済みの石膏ボードは、通常、900mm×1800mmの大きさを有しているが、建築物の解体現場である程度の大きさに破砕され、解体時には、約300mm×300mm程度の大きさに破砕さえている。   The used gypsum board usually has a size of 900 mm x 1800 mm, but it is crushed to a certain size at the site of building demolition, and even at the time of demolition, it is crushed to a size of about 300 mm x 300 mm. ing.

当該混合装置10の被破砕材料の投入口は、かなり大きく設計されており、上記した破砕後の石膏ボード5はそのままでも投入は可能である。
然しながら、実際上では、当該石膏ボードには、金属製のビス等が付いていることが多く、当該金属部品は、当該混合装置10や成形時に成形金型或は成形機を破壊する恐れがあるため、除去しておく事が望ましい。
The input port of the material to be crushed in the mixing apparatus 10 is designed to be quite large, and the above-described gypsum board 5 after crushing can be charged as it is.
However, in practice, the gypsum board is often provided with a metal screw or the like, and the metal component may destroy the mixing device 10 or the molding die or the molding machine during molding. Therefore, it is desirable to remove it.

その為、当該石膏ボードは、更に細かく破砕することが望ましく、具体的には、当該石膏ボードを少なくとも一辺の長さ、或は、直径に相当する部分の長さが約30mm程度になる様に、荒粉砕し、それに付着している金属材料等は磁気分別手段等によって除去する様になっている。   For this reason, it is desirable that the gypsum board be further finely crushed. Specifically, the gypsum board is at least one side long or about 30 mm in length corresponding to the diameter. The metal material or the like that is roughly crushed and adhered thereto is removed by a magnetic separation means or the like.

勿論、本発明に於いては、当該石膏ボードの破砕時の大きさに関しては、特に限定しているものではない。
本発明に於いては、必要によっては、ステップS−15に示す様に、当該石膏ボードを当該混合装置10内に投入するタイミングと略同時期に、当該混合装置内にステアリン酸ナトリウムを上記した重量比の範囲内で投入するものである。
Of course, in the present invention, the size of the gypsum board at the time of crushing is not particularly limited.
In the present invention, if necessary, as shown in step S-15, sodium stearate is added to the mixing device at the same time as the gypsum board is put into the mixing device 10. It is added within the range of the weight ratio.

その後、ステップS−9に於いて、上記した混合操作が継続され、ステップS−10に於いて、石膏ボードから石膏成分と紙との分離が完了し、更に当該紙を構成しているセルロース成分が剪断力を受けて、繊維状に伸張せしめられる。   Thereafter, in step S-9, the above mixing operation is continued. In step S-10, the separation of the gypsum component and the paper from the gypsum board is completed, and the cellulose component constituting the paper. Is subjected to a shearing force and stretched into a fibrous form.

その後、ステップS−11に進んで、当該混合体を急冷する操作が行われる。
係るステップでは、当該混合装置10内にある混合された材料は、200℃前後で過熱されており、係る混合体を例えば、株式会社三井三池製のクーリングミキサーDF300等の装置が使用可能である。
Then, it progresses to step S-11 and operation which quenches the said mixture rapidly is performed.
In this step, the mixed material in the mixing apparatus 10 is heated at around 200 ° C., and an apparatus such as a cooling mixer DF300 manufactured by Mitsui Miike Co., Ltd. can be used as the mixture.

当該クーリングミキサーの構成は、上記した混合装置の構成と略同じで、当該ミキサー内に回転するスクリューが配置され、係るスクリューを回転させながら、平均約15℃の冷却水を注入する。
尚、当該クーリングミキサーの内壁は2重構造になっており、外部との断熱性を確保している。
The configuration of the cooling mixer is substantially the same as that of the mixing device described above, and a rotating screw is disposed in the mixer, and cooling water having an average of about 15 ° C. is injected while rotating the screw.
In addition, the inner wall of the cooling mixer has a double structure, ensuring heat insulation from the outside.

当該ステップに於いては、当該混合体の温度は、約20分後には、常温にまで冷却される。
その後、当該冷却された混合体は、ステップS−12の成形加工工程に送られ、一旦溶融加熱した後、所定の金型内に注入され、所定の形状に成形した後、ステップS−13再度上記した冷却水を使用して冷却することによって新石膏ボードが完成する。
In this step, the temperature of the mixture is cooled to room temperature after about 20 minutes.
Thereafter, the cooled mixture is sent to the molding process of step S-12, and once melted and heated, injected into a predetermined mold and molded into a predetermined shape, and then step S-13 again. A new gypsum board is completed by cooling using the cooling water described above.

又、本発明に於いては、当該オレフィン系合成樹脂成形物と石膏ボードとを混合する際に、当該石膏ボードに含まれるセルロース繊維成分の外に、別途紙等のセルロース系成分を追加混入する事も可能である。   In the present invention, when the olefin synthetic resin molded product and the gypsum board are mixed, a cellulose-based component such as paper is additionally mixed in addition to the cellulose fiber component contained in the gypsum board. Things are also possible.

本発明は、オレフィン系合成樹脂成分と石膏材料とから構成された完全リサイクルシステムによる樹脂素材であって、土木建築材料、家具、雑貨等の分野で木質調を持った素材として有効に利用する事が出来る。   The present invention is a resin material by a complete recycling system composed of an olefinic synthetic resin component and a gypsum material, and is effectively used as a material having a woody tone in the fields of civil engineering and building materials, furniture, sundries, etc. I can do it.

Claims (2)

使用済みのオレフィン系合成樹脂成形物と使用済みの繊維状のセルロース成分を含む骨材とを攪拌機能を有する混合装置内に供給し、当該混合装置内で攪拌操作を行いつつ、当該使用済みのオレフィン系合成樹脂を粉砕溶融すると共に、当該使用済みのオレフィン系合成樹脂成分に当該骨材成分と当該繊維状のセルロース成分とを混合処理して再生合成樹脂素材を製造する方法に於いて、当該骨材として予め含水率が5%以上の骨材を使用すると共に、当該使用済みのオレフィン系合成樹脂を攪拌粉砕する際に、摩擦による発熱により溶融された当該溶融オレフィン系合成樹脂の溶融温度を、当該骨材に含有された水の蒸発作用によって、セルロース成分の炭化温度以下に抑制しながら攪拌混合処理を行うに際し、当該繊維状のセルロース成分を含む骨材として、使用済みの石膏ボード及び使用済みのダンボールとが使用される事を特徴とする再生合成樹脂素材の製造方法。 Supply the used olefin-based synthetic resin molding and the aggregate containing the used fibrous cellulose component into a mixing device having a stirring function, and perform the stirring operation in the mixing device while using the used while pulverizing melt the olefinic synthetic resin, in the method for manufacturing recycled synthetic resin material by mixing processes the cellulose component of the spent olefin synthetic resin component to the aggregate component and the fibrous, the When using an aggregate having a moisture content of 5% or more in advance as an aggregate, and stirring and grinding the used olefin synthetic resin, the melting temperature of the molten olefin synthetic resin melted by heat generated by friction is set. , by evaporation action of water contained in the said aggregate, when performing the stirring and mixing process while suppressing below carbonization temperature of the cellulose component, the cellulose formed in the fibrous Manufacturing method of reproducing a synthetic resin material which as an aggregate, characterized in that the used gypsum board and spent cardboard is used containing. 当該使用済みのオレフィン系合成樹脂と当該使用済みの石膏ボードと使用済みのダンボールとを攪拌機能を有する混合装置内に供給すると共に、更に、ステアリン酸ナトリウムを添加する事を特徴とする請求項1に記載の再生合成樹脂素材の製造方法。2. The used olefin-based synthetic resin, the used gypsum board, and used cardboard are fed into a mixing apparatus having a stirring function, and sodium stearate is further added. A method for producing a recycled synthetic resin material as described in 1.
JP2010163723A 2010-07-21 2010-07-21 Resin material and manufacturing method thereof Active JP5442552B2 (en)