JP3391982B2 - Leather-like sheet with good air permeability and method for producing the same - Google Patents

Leather-like sheet with good air permeability and method for producing the same

Info

Publication number
JP3391982B2
JP3391982B2 JP16122796A JP16122796A JP3391982B2 JP 3391982 B2 JP3391982 B2 JP 3391982B2 JP 16122796 A JP16122796 A JP 16122796A JP 16122796 A JP16122796 A JP 16122796A JP 3391982 B2 JP3391982 B2 JP 3391982B2
Authority
JP
Japan
Prior art keywords
sheet
leather
polyurethane
fiber
air permeability
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP16122796A
Other languages
Japanese (ja)
Other versions
JPH108382A (en
Inventor
浩一郎 下方
久夫 米田
法生 牧山
浩 上原
豊 高橋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kuraray Co Ltd
Original Assignee
Kuraray Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kuraray Co Ltd filed Critical Kuraray Co Ltd
Priority to JP16122796A priority Critical patent/JP3391982B2/en
Publication of JPH108382A publication Critical patent/JPH108382A/en
Application granted granted Critical
Publication of JP3391982B2 publication Critical patent/JP3391982B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明の属する技術分野】本発明は、表面がポリウレタ
ン繊維の橋架け構造を有する微細孔が形成されている銀
面を有し、その銀面とその下に存在している基体層との
間で一体感のある風合いを有し、特にいらつき感のない
高級な外観を有し、更に透気性、透湿性に優れた銀付皮
革様シート及びその製造方法に関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention has a silver surface on the surface of which fine pores having a polyurethane fiber bridging structure are formed, and between the silver surface and an underlying substrate layer. The present invention relates to a silver-leathered leather-like sheet having a feeling of unity, a high-grade appearance with no particular irritability, and excellent air permeability and moisture permeability, and a method for producing the same.

【0002】[0002]

【従来の技術】従来より銀面を有する皮革様シートの製
造方法に関して多くの提案がなされてきた。それら提案
の多くは、繊維質シートの一面に弾性重合体からなる湿
式凝固層あるいは乾式凝固層を付与し銀面を形成する方
法である。また透気・透湿性を有する銀付皮革様シート
の製造方法についても多くの提案がなされてきた。それ
らの方法は、繊維質表面に、発泡剤、添加剤、凝固調節
剤等を添加して湿式凝固法又は乾式凝固法により形成さ
れた通気性多孔質層を積層する方法、あるいはレーザー
光線等により表面の銀面層に穴をあける方法等である。
2. Description of the Related Art Conventionally, many proposals have been made regarding a method for producing a leather-like sheet having a silver surface. Most of these proposals are methods of forming a silver surface by providing a wet coagulation layer or a dry coagulation layer made of an elastic polymer on one surface of a fibrous sheet. Many proposals have also been made for a method for producing a leather-like sheet with silver having air permeability and moisture permeability. Those methods include a method of laminating a breathable porous layer formed by a wet coagulation method or a dry coagulation method by adding a foaming agent, an additive, a coagulation regulator, etc. to the fibrous surface, or a surface by a laser beam or the like. And the method of making a hole in the silver surface layer.

【0003】天然皮革調の外観を有し、さらに透気透湿
性を有する皮革様シートの製造方法として、弾性重合体
を含有する繊維質シートの表面を熱溶融する方法や、表
面に繊維又は弾性重合体の溶剤を付与して、該シートの
表面を構成する繊維或いは弾性重合体を溶かして表面を
平滑化し銀面を形成する方法が提案されている(例えば
特公昭48ー535号公報、特公昭48ー536号公
報、特公昭48ー537号公報等)。さらに繊維絡合体
の表面に極細繊維立毛面を形成し、繊維の溶剤或いは膨
潤剤を付与し熱プレスで繊維を接合して表面を平滑化
し、さらにその表面に弾性重合体の被覆層を設ける皮革
様シートの製造方法も知られている。
As a method for producing a leather-like sheet having a natural leather-like appearance and further having air permeability and moisture permeability, a method of heat-melting the surface of a fibrous sheet containing an elastic polymer, or a method of forming fibers or elasticity on the surface A method has been proposed in which a solvent for a polymer is applied and the fibers or elastic polymer constituting the surface of the sheet are melted to smooth the surface and form a silver surface (for example, JP-B-48-535, JP-B-48-536, JP-B-48-537, etc.). Further, a leather in which an ultrafine fiber napped surface is formed on the surface of the fiber entangled body, the solvent or swelling agent of the fiber is applied, the fibers are joined by hot pressing to smooth the surface, and the elastic polymer coating layer is further provided on the surface. A method for manufacturing such a sheet is also known.

【0004】[0004]

【発明が解決しようとする課題】しかしながら、従来よ
り提案されている方法のうち、繊維シート表面に弾性重
合体からなる多孔質層を付与する方法の場合には、得ら
れるシートは透気性の点で満足できるものではない。ま
たこの方法の場合には、銀面はゴム反発感が強いことや
表面の折れシワ形態が悪い等の問題もある。表面の被覆
層にレーザー等により穴をあける方法の場合には、透気
性については満足できるものの外観の高級感に欠ける。
また繊維質シートを構成する繊維及び弾性重合体を熱溶
融或いは溶剤等により溶解して平滑化し銀面を形成する
方法の場合には、透気・透湿性に関しては満足できるも
のの、表面が硬くなり、充実感に欠け、かつ、外観のい
らつき感が発生し高級感に欠けるものとなる。本発明
は、基体層と銀面とが天然皮革のように一体感と充実感
を有し、さらに外観においていらつき感がなく高級感を
有し、さらに透気性・透湿性に優れた銀付き皮革様シー
ト及びその製造方法を提供することにある。
However, among the methods proposed hitherto, in the case of a method of providing a porous layer made of an elastic polymer on the surface of a fiber sheet, the obtained sheet has air permeability. I am not satisfied with. Further, in the case of this method, there are problems that the silver surface has a strong rubber repulsion sensation and the surface has a bad wrinkle morphology. In the case of the method of making holes in the coating layer on the surface with a laser or the like, the air permeability is satisfactory, but the appearance is not high-grade.
Further, in the case of a method in which the fibers and elastic polymer constituting the fibrous sheet are melted by heat or melted by a solvent to smooth and form a silver surface, the air permeability and moisture permeability are satisfactory, but the surface becomes hard. However, the product lacks a sense of fulfillment and also has a feeling of frustration in appearance, resulting in a lack of luxury. INDUSTRIAL APPLICABILITY The present invention has a base layer and a silver surface that have a sense of unity and fulfillment like natural leather, and have a high-grade appearance with no irritating appearance, and also have excellent air permeability and moisture permeability. A leather-like sheet and a method for manufacturing the same.

【0005】[0005]

【課題を解決するための手段】本発明は、繊維絡合不織
布及びその内部に含有された弾性体からなる基体層と、
その少なくとも一面に形成された厚さ10〜100μm
のウレタン被覆層からなる皮革様シートであって、該ポ
リウレタン被覆層は直径300μm以下の微細孔を10
0個/cm2以上有し、かつ一部の微細孔にはポリウレ
タン繊維の橋架け構造が存在していることを特徴とする
皮革様シートである。
DISCLOSURE OF THE INVENTION The present invention provides a base layer composed of a fiber-entangled nonwoven fabric and an elastic body contained therein,
10-100 μm thick formed on at least one surface
A leather-like sheet consisting of the urethane coating layer, wherein the polyurethane coating layer has fine pores with a diameter of 300 μm or less.
It is a leather-like sheet characterized by having 0 or more / cm 2 and having a polyurethane fiber bridging structure in some of the fine pores.

【0006】本発明に用いる基体層の繊維絡合不織布を
構成する繊維としては、少なくとも2種類のポリマーか
らなる極細繊維発生型繊維からつくられる。例えば、海
成分が溶剤または水酸化ナトリウム等の分解剤により溶
解または分解することで島成分がフィブリル化する、断
面が海島構造を有する抽出型繊維あるいは機械的にまた
は処理剤によって各ポリマーからなる極細繊維にフィブ
リル化する分割型繊維等があげられる。もちろん通常の
太さの繊維からなるものであってもよいし、更に上記極
細繊維発生型繊維と通常繊維とを混合使用したものでも
よい。しかし好ましくは、上記極細繊維発生型繊維から
なる不織布の場合である。
The fibers constituting the fiber-entangled nonwoven fabric of the base layer used in the present invention are made of ultrafine fiber-generating fibers composed of at least two kinds of polymers. For example, when the sea component is dissolved or decomposed by a solvent or a decomposing agent such as sodium hydroxide, the island component is fibrillated. Extractable fibers having a sea-island structure in cross section or ultrafine fibers made of each polymer mechanically or by a treating agent. Examples include split fibers that are fibrillated into fibers. Of course, it may be composed of fibers having an ordinary thickness, or may be a mixture of the above ultrafine fiber-generating fibers and ordinary fibers. However, it is preferably a non-woven fabric made of the above ultrafine fiber-generating fiber.

【0007】極細繊維を構成するポリマーとしては、6
ーナイロン、66ーナイロンをはじめとする溶融紡糸可
能なポリアミド類、ポリエチレンテレフタレート、ポリ
ブチレンテレフタレート、カチオン可染型変性ポリエチ
レンテレフタレートをはじめとする溶融紡糸可能なポリ
エステル類、ポリプロピレンで代表されるポリオレフィ
ン類などから選ばれた少なくとも1種類のポリマーが挙
げられる。また、抽出型繊維で抽出または分解除去され
る成分としては、極細繊維成分と溶剤または分解剤に対
する溶解性または分解性を異にし、極細繊維成分との相
溶性の小さいポリマーであり、かつ紡糸条件下で極細繊
維成分より溶融粘度が小さいかあるいは表面張力が小さ
いポリマーであり、例えば、ポリエチレン、ポリスチレ
ン、ポリエチレンプロピレン共重合体、変性ポリエステ
ルなどのポリマーから選ばれた少なくとも1種類のポリ
マーである。この極細繊維の海成分と島成分の量比は
1:2〜2:1であって、海成分を抽出した後の好適デ
ニールとしては風合いや充実感の点で、0.01〜0.
0001drの範囲が良い。
As the polymer constituting the ultrafine fibers, 6
-Nylon, 66-Nylon and other melt-spinnable polyamides, polyethylene terephthalate, polybutylene terephthalate, melt-spinnable polyesters such as cationic dyeable modified polyethylene terephthalate, and polyolefins represented by polypropylene At least one polymer selected from the group consisting of: Further, as the component extracted or decomposed and removed by the extraction type fiber, a polymer having different solubility or decomposability with respect to the solvent or the decomposing agent with the ultrafine fiber component, and having a small compatibility with the ultrafine fiber component, and the spinning condition It is a polymer having a lower melt viscosity or a lower surface tension than the ultrafine fiber component, and is, for example, at least one polymer selected from polymers such as polyethylene, polystyrene, polyethylene propylene copolymer and modified polyester. The amount ratio of the sea component to the island component of this ultrafine fiber is 1: 2 to 2: 1, and the suitable denier after extracting the sea component is 0.01 to 0.
A range of 0001dr is good.

【0008】次に、繊維絡合不織布に弾性樹脂液を含浸
し、加熱乾燥することでゲル化させるか或いは弾性樹脂
の非溶剤を含む液に浸漬して湿式凝固することで緻密な
発泡スポンジを形成する。ここで含浸する弾性樹脂とし
ては、例えば、平均分子量500〜3000のポリエス
テルジオール、ポリエーテルジオール、ポリカーボネー
トジオールあるいはポリエステルポリエーテルジオール
等から選ばれた少なくとも1種類のポリマージオール
と、4,4’−ジフェニルメタンジイソシアネート、イ
ソホロンジイソシアネート、ヘキサメチレンジイソシア
ネートなどの芳香族系、脂環族系或いは脂肪族系のジイ
ソシアネートなどから選ばれた少なくとも1種類のジイ
ソシアネート化合物と、2個以上の活性水素原子を有す
る少なくとも1種類の低分子化合物で分子量300以下
の化合物、例えば、エチレングリコール、プロピレング
リコール、1.4ーブタンジオール、ヘキサンジオー
ル、3ーメチル−1,5―ペンタンジオール、1,4ー
シクロヘキサンジオール、キシレングリコール等のジオ
ール類、エチレンジアミン、プロピレンジアミン、キシ
リレンジアミン、イソホロンジアミン、ピペラジン、フ
ェニレンジアミン、トリレンジアミン等のジアミン化合
物、アジピン酸ヒドラジド、イソフタル酸ジヒドラジド
等のヒドラジン或いはヒドラジド類等から選ばれた少な
くとも1種類とを反応させて得たポリウレタンである。
Next, the fiber entangled non-woven fabric is impregnated with an elastic resin liquid, and is gelled by heating and drying, or is immersed in a liquid containing a non-solvent of the elastic resin and wet-solidified to form a dense foam sponge. Form. Examples of the elastic resin to be impregnated here include at least one polymer diol selected from polyester diols, polyether diols, polycarbonate diols, polyester polyether diols and the like having an average molecular weight of 500 to 3000, and 4,4′-diphenylmethane. At least one diisocyanate compound selected from aromatic, alicyclic or aliphatic diisocyanates such as diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate, and at least one kind having at least two active hydrogen atoms molecular weight 300 the following compounds of low molecular compounds, such as ethylene glycol, propylene glycol, 1.4 over butanediol, hexanediol, 3 Mechiru 1,5 Pentanjio le, 1 Diols such as 4-cyclohexanediol and xylene glycol, diamine compounds such as ethylenediamine, propylenediamine, xylylenediamine, isophoronediamine, piperazine, phenylenediamine and tolylenediamine; hydrazines and hydrazides such as adipic acid hydrazide and isophthalic acid dihydrazide. It is a polyurethane obtained by reacting with at least one selected from the above.

【0009】特に好ましくは、1,4ーブタンジオール
または3ーメチル−1,5−ペンタンジオールを主体と
した鎖伸長剤を所定のモル比で反応させて得たポリウレ
タンである。ポリウレタンの他に、ポリエステルエラス
トマー等の他の弾性樹脂およびアクリル系等の樹脂であ
ってもよい。また、これらを混合した重合体組成物でも
よい。しかし、柔軟性、弾性回復性、スポンジ形成性等
より上記のポリウレタンが好ましく用いられる。なお弾
性樹脂液中の弾性樹脂濃度は10〜50重量%、ヤング
率は1〜15kg/mmの範囲が好ましい。また上記
ポリウレタンとしてポリマージオールと上記低分子化合
物のモル比が1:1〜1:7の範囲が好ましい。
[0009] Particularly preferred is polyurethane obtained by reacting a chain extender consisting mainly of 1,4-butanediol or 3 Mechiru 1,5 Pentanjio Le at a predetermined molar ratio. In addition to polyurethane, other elastic resin such as polyester elastomer and acrylic resin may be used. Also, a polymer composition obtained by mixing these may be used. However, the above-mentioned polyurethane is preferably used because of its flexibility, elastic recovery property, sponge forming property and the like. The elastic resin concentration in the elastic resin liquid is preferably 10 to 50% by weight, and the Young's modulus is preferably 1 to 15 kg / mm 2 . As the polyurethane, the molar ratio of the polymer diol and the low molecular weight compound is preferably in the range of 1: 1 to 1: 7.

【0010】本発明において、銀面を構成する樹脂はポ
リウレタンであり、さらにその銀面層は、ポリウレタン
不織布を加熱加圧することによりフィルム化したもので
あり、このようなポリウレタン不織布から構成されたも
のであることにより、前記した本発明の優れた性能が得
られる。
In the present invention, the resin constituting the silver surface is polyurethane, and the silver surface layer is formed by heating and pressing a polyurethane non-woven fabric to form a film, which is composed of such a polyurethane non-woven fabric. As a result, the excellent performance of the present invention described above can be obtained.

【0011】本発明の、銀面を構成するポリウレタンと
しては、低分子ジオール、例えば、エチレングリコー
ル、プロピレングリコール、1,4−ブタンジオール、
1,5−ペンタンジオール、1,6−ヘキサンジオー
ル、3−メチル−1,5−ペンタンジオール等から選ば
れた少なくとも1種類とジカルボン酸、例えばアジピン
酸、ピメリン酸、スベリン酸、アゼライン酸、セバシン
酸、イソフタル酸、テレフタル酸等から選ばれた少なく
とも1種類との縮合重合によって得たポリエステルジオ
ール、ポリエチレンエーテルグリコール、ポリプロピレ
ンエーテルグリコール、ポリテトラメチレンエーテルグ
リコール、ポリヘキサメチレンエーテルグリコール等の
ポリエーテルグリコール、ポリカプロラクトングリコー
ル、ポリバレロラクトングリコール等のポリラクトング
リコールから選ばれた少なくとも1種類のポリマージオ
ールであって、平均分子量が500〜3000のポリマ
ージオールをソフトセグメントとするポリウレタンであ
る。とりわけ3ーメチルペンタンジオール−1,5を主
体としたジオールとジカルボン酸との縮合重合によって
得た平均分子量700〜3000のポリエステルジオー
ルを用いることがポリウレタンの溶融成形性、溶剤安定
性、耐加水分解性、耐候性、耐熱性、柔軟性、耐屈曲性
などの点で、特に直径300μm以下の微細孔を100
個/cm以上有し、かつ少なくとも一部の微細孔には
ポリウレタン繊維の橋架け構造が存在しているような銀
面層を形成させやすい点で好ましい。
As the polyurethane constituting the silver surface of the present invention, low molecular diols such as ethylene glycol, propylene glycol, 1,4-butanediol,
1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-Pentanjio least one dicarboxylic acid selected from the Le like, such as adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic Polyester glycol such as polyester diol, polyethylene ether glycol, polypropylene ether glycol, polytetramethylene ether glycol and polyhexamethylene ether glycol obtained by condensation polymerization with at least one selected from acids, isophthalic acid, terephthalic acid, etc. At least one type of polymer diol selected from polylactone glycols such as polycaprolactone glycol and polyvalerolactone glycol, wherein the polymer diol having an average molecular weight of 500 to 3000 is soft. It is a polyurethane to a segment. In particular, it is preferable to use a polyester diol having an average molecular weight of 700 to 3000 obtained by condensation polymerization of a diol mainly composed of 3-methylpentanediol-1,5 and a dicarboxylic acid, the melt moldability of polyurethane, solvent stability, and hydrolysis resistance. From the viewpoint of heat resistance, weather resistance, heat resistance, flexibility, bending resistance, etc., 100 micropores with a diameter of 300 μm or less are used.
The number of holes / cm 2 or more is preferable, and at least a part of the fine pores is preferable in that a silver surface layer having a bridging structure of polyurethane fibers can be easily formed.

【0012】またポリマージオールと反応させる有機ジ
イソシアネートとしては、例えば4,4’ージフェニル
メタンジイソシアネート、トリレンジイソシアネート、
フェニレンジイソシアネート、キシリレンジイソシアネ
ート等の芳香族ジイソシアネート、ヘキサメチレンジイ
ソシアネート、イソホロンジイソシアネート、4.4'
ージシクロヘキシルメタンジイソシアネート、水添トリ
レンジイソシアネート、水添キシレンジイソシアネート
等の脂肪族又は脂環族ジイソシアネート等から選ばれた
少なくとも1種類、又は溶融紡糸性或いは溶融成形性を
阻害しない範囲内で有機トリイソシアネート等のイソシ
アネート基を3個以上有する有機ポリイソシアネートを
併用してもよい。
Examples of the organic diisocyanate to be reacted with the polymer diol include 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate,
Aromatic diisocyanates such as phenylene diisocyanate and xylylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4.4 '
-At least one selected from aliphatic or alicyclic diisocyanates such as dicyclohexylmethane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, etc., or organic triisocyanate within the range that does not impair melt spinnability or melt moldability An organic polyisocyanate having 3 or more isocyanate groups may be used in combination.

【0013】そして鎖伸長剤としては、活性水素原子2
個有する分子量300以下の化合物、例えば、エチレン
グリコール、プロピレングリコール、1,4−ブタンジ
オール、ヘキサンジオール、3−メチル−1,5−ペン
タンジオール、1,4−シクロヘキサンジオール、キシ
レングリコール等のジオール類、エチレンジアミン、プ
ロピレンジアミン、キシリレンジアミン、イソホロンジ
アミン、ピペラジン、フェニレンジアミン、トリレンジ
アミン等のジアミン類、アジピン酸ヒドラジド、イソフ
タル酸ジヒドラジド等のヒドラジン或いはヒドラジド類
等から選ばれた少なくとも1種類が挙げられる。特に好
ましくは、1,4−ブタンジオールまたは3−メチル
1,5−ペンタンジオールを主体とした鎖伸長剤をもち
いたポリウレタンである。なお、該ポリマージオールと
鎖伸長剤とのモル比は不織布の物性によって自由に変え
ることができるが、好ましくは1:2〜7程度である。
As a chain extender, active hydrogen atom 2
Molecular weight of 300 or less of the compound having pieces, such as ethylene glycol, propylene glycol, 1,4-butanediol, hexanediol, 3-methyl-1,5 Pentanjio Le, 1,4-cyclohexanediol, diols such as xylene glycol At least one selected from diamines such as ethylenediamine, propylenediamine, xylylenediamine, isophoronediamine, piperazine, phenylenediamine, and tolylenediamine, hydrazine such as adipic acid hydrazide, and isophthalic acid dihydrazide, and hydrazides. . Particularly preferably, 1,4-butanediol or 3-methyl -
A polyurethane using a chain extender consisting mainly of 1,5 Pentanjio Le. The molar ratio of the polymer diol to the chain extender can be freely changed depending on the physical properties of the nonwoven fabric, but it is preferably about 1: 2 to 7.

【0014】次にポリウレタン繊維を主体とした繊維の
集合体によって構成された銀面の製造方法としては、例
えば、ポリウレタンを溶融状態からメルトブロ−ン方式
でつくられた不織布を用いる方法が挙げられ、この方法
の場合には特に透気性と処理効率性向上の点で優れた皮
革様シートが得られる。この方法において用いられる不
織布の厚みは50〜500μm、特に100〜400μ
mが好ましく、繊維直径としては2〜20μm、特に4
〜10μmの範囲が好ましい。また基体層に含浸された
ポリウレタンがポリエステル系のポリウレタンであれ
ば、銀面形成不織布もポリエステル系ポリウレタンとい
ったように、基体層に用いられたポリウレタンと同系統
のポリウレタンからなる不織布を用いるのが接着性を考
慮すると好ましい。また、このポリウレタン不織布の目
付は5〜125g/m2、特に面の状態と透気性を考慮
すると25〜100g/m2の範囲が好ましい。この加
熱溶融接着させる方法としては、エンボスによる加熱プ
レスによって該ポリウレタン繊維の軟化点から20℃〜
80℃高い温度でかつ圧力0.5〜7.0kg/cm2
で積層一体化することが好ましい。しかしながら、軟化
点に対して20℃以上高い温度より低い温度で接着する
と接着性不良が起こり、また、80℃以上高い温度では
微細孔がつぶれすぎて、透気性不良を起こす。よって張
り合わせ温度は該ポリウレタンの軟化点に対し20〜8
0℃高い温度の範囲が好ましい。
Next, as a method for producing a silver surface composed of an aggregate of fibers mainly composed of polyurethane fibers, for example, there is a method of using a non-woven fabric made from a melted state of polyurethane by a melt blown method, In the case of this method, a leather-like sheet having excellent air permeability and improved processing efficiency can be obtained. The thickness of the non-woven fabric used in this method is 50 to 500 μm, especially 100 to 400 μm.
m is preferable, and the fiber diameter is 2 to 20 μm, especially 4
The range of 10 μm is preferable. If the polyurethane impregnated in the base layer is a polyester-based polyurethane, it is advisable to use a non-woven fabric made of the same type of polyurethane as the base layer, such as a polyester surface polyurethane for the silver surface forming non-woven fabric. Is preferable in consideration. The basis weight of the polyurethane nonwoven fabric is preferably 5 to 125 g / m 2 , and particularly preferably 25 to 100 g / m 2 in consideration of the surface condition and air permeability. As a method of heat-melting and bonding, a heating press by embossing is performed at a temperature of 20 ° C to 20 ° C from the softening point of the polyurethane fiber.
80 ° C. high temperature and pressure 0.5-7.0 kg / cm 2
It is preferable to laminate and integrate. However, if the adhesive is adhered at a temperature lower than the softening point by 20 ° C. or higher, the adhesiveness will be poor, and if the temperature is 80 ° C. or higher, the fine pores will be excessively crushed to cause poor air permeability. Therefore, the bonding temperature is 20 to 8 with respect to the softening point of the polyurethane.
A temperature range of 0 ° C. higher is preferred.

【0015】ポリウレタンの軟化点は微量融点測定装置
(YANAGIMOTO XTZ−OL−22)により
求められる。次に張り合わせ圧力としては、0.5kg
/cm2より低い圧力で積層すると接着性不良となり、
7.0kg/cm2より高い圧力では風合いが硬くなっ
てしまう。よって張り合わせ圧力は0.5〜7.0kg
/cm2の範囲が好ましい。こうして得られたコート層
はコート厚さ10〜100μmである。ここでいうコー
ト厚さとは電子顕微鏡写真により求められる厚さの平均
である。
The softening point of polyurethane is determined by a trace melting point measuring device (YANAGIMOTO XTZ-OL-22). Next, the bonding pressure is 0.5 kg
Laminating at a pressure lower than / cm 2 results in poor adhesion,
At a pressure higher than 7.0 kg / cm 2 , the texture becomes hard. Therefore, the laminating pressure is 0.5 to 7.0 kg.
The range of / cm 2 is preferable. The coat layer thus obtained has a coat thickness of 10 to 100 μm. The coat thickness referred to here is the average of the thicknesses obtained from electron micrographs.

【0016】ポリウレタン不織布は、加熱加圧によりフ
ィルム化するがフィルムには微細孔が存在している。微
細孔の直径が300μmを越えるといらつき感不良を起
こし外観が悪化するため、300μ以下である必要があ
り、好ましくは100μ以下である。また、微細孔の存
在個数は100個/cm、好ましくは300個/cm
2以上であり、この個数を満足するすることにより透気
性が向上する。しかしながら、5000個/cmを越
えると若干いらつき感が発生するため好ましくない。よ
り好ましくは300個以上3000個以である。
The polyurethane nonwoven fabric is formed into a film by heating and pressing, but the film has fine pores. If the diameter of the fine pores exceeds 300 μm, the feeling of irritability becomes poor and the appearance deteriorates. Therefore, it is necessary to be 300 μm or less, preferably 100 μm or less. The number of micropores present is 100 / cm 2 , preferably 300 / cm.
It is 2 or more, and the air permeability is improved by satisfying this number. However, if it exceeds 5000 pieces / cm 2 , some irritating feeling is generated, which is not preferable. More preferably 3,000 or less under 300 or more.

【0017】本発明において微細孔の少なくとも一部
に、ポリウレタン繊維の橋架け構造を有していることが
いらつき感を解消する上で極めて重要である。橋架け構
造となっているものの割合としては、全微細孔の1割以
上であればいらつき感を解消し、好ましくは3割以上で
ある。本発明でいう橋架け構造を持った微細孔とは、シ
ートの表面を任意に選び出し電子顕微鏡写真から観察
し、微細孔間平均距離が30μ以上あり、かつ、微細孔
内部に繊維直径3μ以上の繊維が1本以上橋架け状態
(図1)で存在しているものである。ポリウレタン繊維
の橋架け構造を有していることがいらつき感を解消する
上で、なぜ効果的であるのかについては必ずしも明確で
はないが、微細孔に侵入した光が橋架け繊維により遮ら
れて、孔から出ることができないことによるものと予測
される。
In the present invention, it is extremely important that at least a part of the fine pores has a bridging structure of polyurethane fibers in order to eliminate the feeling of irritability. The proportion of those having a bridging structure eliminates the irritating feeling if it is 10% or more of all the fine pores, and is preferably 30% or more. The term "micropores having a bridging structure" as used in the present invention means that the surface of the sheet is arbitrarily selected and observed from an electron micrograph, and the average distance between the micropores is 30 µ or more, and the fiber diameter inside the micropores is 3 µ or more. One or more fibers are present in a bridged state (Fig. 1). It is not always clear why having a polyurethane fiber bridging structure is effective in eliminating the irritating feeling, but the light that has entered the micropores is blocked by the bridging fiber. It is predicted that this is due to the inability to get out of the hole.

【0018】この銀付表面の穴の数および穴の大きさ
は、着色の際に溶剤組成がジメチルホルムアミド濃度が
10重量%未満の溶剤にて希釈した樹脂及び着色剤にて
着色することによって表面の微細孔をつぶさずに着色す
ることができる。それに対し、10重量%以上にすると
表面の微細孔がつぶれ透気性が損なわれてしまう。次い
で必要に応じて公知の方法によってエンボス型押し、染
色、柔軟処理、モミ処理等の仕上げ処理を行って、銀付
皮革様シートに仕上げる。なお、本発明において、ごく
少量ならば直径300μmを越える気孔が存在していて
も良い。微細孔直径とは、穴の表面の面積と同一の面積
を有する円の直径と定義する。
The number of holes and the size of the holes on the surface with silver are determined by coloring with a resin and a colorant diluted with a solvent having a solvent composition of less than 10% by weight of dimethylformamide during coloring. It is possible to color the micropores without crushing. On the other hand, when it is 10% by weight or more, the fine pores on the surface are crushed and the air permeability is impaired. Then, if necessary, finish treatment such as embossing, dyeing, softening treatment, and fir treatment is carried out by a known method to finish the leather-like sheet with silver. In the present invention, pores having a diameter of more than 300 μm may be present if the amount is very small. The micropore diameter is defined as the diameter of a circle having the same area as the surface area of the hole.

【0019】本発明で得られる銀付皮革様シートは、表
面がポリウレタン繊維の橋架け構造を有する微細孔を持
った銀面からなり、銀面とその下の基体層との間で一体
感のある風合いを有し、更に透気性、透湿性に優れ特に
いらつき感のない極めて優れた外観を有する銀付皮革様
シートである。従って、本発明の銀付皮革用シートは紳
士靴、スポーツシューズ、一般靴等に使用するのに適し
ている。
The silver-like leather-like sheet obtained by the present invention is composed of a silver surface having fine pores having a polyurethane fiber bridging structure on the surface, and the silver surface and the underlying base layer provide a sense of unity. A silver-like leather-like sheet having a certain texture, and also having excellent air permeability and moisture permeability and an extremely excellent appearance with no particular irritability. Therefore, the silver leather sheet of the present invention is suitable for use in men's shoes, sports shoes, general shoes and the like.

【0020】[0020]

【実施例】次に、本発明の実施態様を具体的な実施例で
説明するが、本発明はこれらの実施例に限定される物で
はない。なお、実施例中の部及び%は断りのない限り、
重量に関するものである。
EXAMPLES The embodiments of the present invention will now be described with reference to specific examples, but the present invention is not limited to these examples. The parts and% in the examples are unless otherwise specified.
It is about weight.

【0021】実施例1 基体層として、高流動性ポリエチレン(海成分)、6ー
ナイロン(微細繊維束繊維島成分)からなる繊維6デニ
ールの海島型繊維を繊維長51mmにカットして得たス
テープル繊維を用い、乾式繊維ウエブを作り、クロスラ
ップ法で積層ウエブとし、ニードルパンチ法で繊維絡合
し熱処理して目付300g/m2の不織布とした。この
不織布にポリエステル型ポリウレタン(鎖伸長剤は1,
4−ブタンジオールでポリマージオールと鎖伸長剤のモ
ル比は1:4)の20%ジメチルホルムアミド溶液を含
浸し表面に付着したウレタンをナイフで切った後、ジメ
チルホルムアミド水溶液中で凝固した。次いで温水洗浄
にて溶剤のジメチルホルムアミドを除去した後、熱トル
エンにて繊維中のポリエチレンを溶解除去して極細繊維
束の平均本数1000本/束、平均繊度0.001デニ
ールの6ーナイロン極細繊維の絡合不織布と多孔質ポリ
ウレタンからなる繊維シートを得た。
Example 1 A staple fiber obtained by cutting a 6-denier sea-island type fiber having a fiber length of 51 mm, which is made of high-fluidity polyethylene (sea component) and 6-nylon (fine fiber bundle fiber island component), as a base layer. Was used to prepare a dry fiber web, which was used as a laminated web by the cross lap method, and the fibers were entangled by the needle punching method and heat-treated to give a nonwoven fabric having a basis weight of 300 g / m 2 . Polyester polyurethane (chain extender is 1,
4-butanediol was impregnated with a 20% dimethylformamide solution in which the molar ratio of the polymer diol and the chain extender was 1: 4, the urethane adhering to the surface was cut with a knife, and then solidified in an aqueous dimethylformamide solution. Then, the solvent dimethylformamide was removed by washing with warm water, and polyethylene in the fiber was dissolved and removed with hot toluene to obtain an average number of ultrafine fiber bundles of 1000 / bundle and an average fineness of 0.001 deniers of 6-nylon ultrafine fibers. A fiber sheet made of entangled nonwoven fabric and porous polyurethane was obtained.

【0022】次に、平均分子量1150のポリ3ーメチ
ルー1.5ーペンチルアジペートグリコールと4.4ー
ジフェニルメタンジイソシアネートおよび1.4ーブタ
ンジオールを1:4:3のモル比(イソシアネート基に
もとづく理論窒素量4.63%)で仕込みスクリユー式
混練型重合機を用い溶融重合法でポリウレタンを重合し
た。このポリウレタンの軟化点は125℃であった。得
られたポリウレタンは溶融状態のままメルトブロー法
で、温度260℃に加熱したダイオリフイスの両側にあ
るスロットから温度260℃に加熱した高速空気流で繊
維状溶融ポリウレタンを微細繊維状に搬送し、2m/分
で移動する金網上に捕集距離40cmの位置で捕集し
た。捕集したウエブは微細繊維のランダムウエブであ
り、平均目付74g/m2、平均厚み0.3mm、見掛
け密度0.25g/cm3であった。
Then, poly-3-methyl-1.5-pentyl adipate glycol having an average molecular weight of 1150, 4.4-diphenylmethane diisocyanate and 1.4-butanediol are mixed in a molar ratio of 1: 4: 3 (theoretical nitrogen amount based on the isocyanate group is 4 .63%), and polyurethane was polymerized by a melt polymerization method using a screw type kneading type polymerization machine. The softening point of this polyurethane was 125 ° C. The obtained polyurethane was melt-blown in a molten state, and the fibrous molten polyurethane was conveyed into fine fibrous form by a high-speed air stream heated to a temperature of 260 ° C. from slots on both sides of a die orifice heated to a temperature of 260 ° C. It was collected at a position of a collection distance of 40 cm on a wire net moving at a speed of 1 / min. The collected web was a fine fiber random web having an average basis weight of 74 g / m 2 , an average thickness of 0.3 mm, and an apparent density of 0.25 g / cm 3 .

【0023】この不織布を上記繊維シ−トにのせ、17
0℃に昇温したエンボスロールでプレス圧4kg/cm
の圧力にて溶融接着を行い銀付皮革様シートを得た。
この銀付皮革様シートは、透気性が2.5cc/cm
/秒で、いらつき感のない高級な皮革様外観を有してい
た。そして表面には平均70μの微細孔が約800個/
存在しており、そして微細孔の橋架けが見られ
た。また被覆層の厚みは50μであった。さらにこの銀
付シートに黒インクMTー6701(大日精化
(株)):イソプロピルアルコール:エチルセソルブ
=2:1:1にて希釈したものを150メッシュグラビ
アロールにて2段塗布し130℃2分間乾燥後165℃
の鏡面ロールにてプレス圧2.5kg/c で面出し
を行い皮革様シートを得た。この表面層には微細孔が約
500個/c 有りそのうち4割が橋架け構造を有し
ており透気性が0.7cc/cm /秒で、かつ、いら
つき感のない高級感を有するものであった。
This non-woven fabric is placed on the above fiber sheet,
Pressing pressure 4kg / cm with embossing roll heated to 0 ℃
Melt adhesion was performed under a pressure of 2 to obtain a leather-like sheet with silver.
This silver-like leather-like sheet has an air permeability of 2.5 cc / cm 2.
/ Sec, it had a high-class leather-like appearance with no irritability. And on the surface there are about 800 micropores with an average of 70μ /
cm 2 was present and micropore bridging was seen. The thickness of the coating layer was 50μ. Furthermore, the grain-sheet black ink MT over 6701 (Dainichi Seika Co.): isopropyl alcohol: Echiruse B cellosolve = 2: 1: 2-stage coated 130 ° C. those diluted with 150 mesh gravure roll at 1 165 ° C after drying for 2 minutes
The mirror-like roll was used to perform surfacing at a pressing pressure of 2.5 kg / cm 2 to obtain a leather-like sheet. In this surface layer has pores of about 500 / c m 2 there them 40% of crosslinked structure permeable is 0.7 cc / cm 2 / sec, and irritability without feeling luxury It had a feeling.

【0024】比較例1 実施例1の基体層に、加熱発泡樹脂ハイムレンXー30
40(大日精化(株))100部に顔料Xー2070
(大日精化(株))を30部添加し、さらにメチルエチ
ルケトン:水=1:1を50部にて希釈したインクを5
5Mグラビアロール1段塗布した後、この銀付シートに
さらに黒インクMTー6701(大日精化):イソプロ
ピルアルコール:エチルセソルブ=2:1:1にて希
釈したものを150Mグラビアロールにて2段塗布し1
30℃2分間乾燥した。そして165℃の鏡面ロールに
てプレス圧2.5kg/cmで面出しを行い、皮革様
シートを得た。この皮革様シートは透気性はあるものの
黒度不足およびいらつき感が強くなり、高級感に乏しい
物であった。この表面層には微細孔が約600個/cm
有りそのうち橋架け構造を有するものは全く存在して
いなかった。
Comparative Example 1 Heat-foaming resin Heimlen X-30 was added to the base layer of Example 1.
40 (Dainichiseika Co., Ltd.) 100 parts pigment X-2070
30 parts of (Dainichi Seika Co., Ltd.) was added, and further 5 parts of ink prepared by diluting 50 parts of methyl ethyl ketone: water = 1: 1.
After applying one stage 5M gravure roll, the silver sheet with more black ink MT over 6701 (Dainichiseika): isopropyl alcohol: Echiruse B cellosolve = 2: 1: 2 at 150M gravure roll those diluted with 1 Step application 1
It was dried at 30 ° C. for 2 minutes. Chamfering was then performed with a mirror pressure roll at 165 ° C. under a pressing pressure of 2.5 kg / cm 2 to obtain a leather-like sheet. Although this leather-like sheet had air permeability, it lacked in blackness and became more irritating, and was poor in luxury. This surface layer has about 600 pores / cm
2 Yes There was no bridge structure at all.

【0025】比較例2 実施例1の基体層に、一液型エーテル・エステル型組成
のCUTー7450NL(大日精化(株))100部、
顔料セイカセブンBSー1710ブラック(大日精化
(株))15部、溶剤ジメチルホルムアミド40部から
なるインクをウエットで100g/m塗布し、30℃
の温水にて脱洗乾燥した。この銀付シートに、黒インク
MTー6701(大日精化):IPA:エチルセロソル
=2:1:1にて希釈したものを150Mグラビアロ
ールにて2段塗布し、130℃2分間乾燥し、さらに1
65℃の鏡面ロールにてプレス圧2.5kg/cm
面出しを行い、皮革様シートを得た。この皮革様シート
は、黒度およびいらつき感等の高級感は満足できるもの
の、表面には微細孔は存在せず透気性に乏しいものであ
った。
Comparative Example 2 100 parts of CUT-7450NL (Dainichiseika Chemicals Co., Ltd.) of one-pack type ether / ester type composition was added to the base layer of Example 1.
Pigment Seika Seven BS-1710 Black (Dainichiseika Co., Ltd.) 15 parts, solvent dimethylformamide 40 parts ink 100 g / m 2 by wet coating, 30 ° C
Was washed with warm water and dried. On this silver- coated sheet, black ink MT-6701 (Dainichi Seika): IPA: ethyl cellosol
The product diluted with 2: 1: 1 is applied in two steps with a 150M gravure roll, dried at 130 ° C for 2 minutes, and further 1
Chamfering was performed at a pressing pressure of 2.5 kg / cm 2 with a mirror surface roll at 65 ° C. to obtain a leather-like sheet. This leather-like sheet was satisfactory in terms of blackness and high-grade feeling such as irritability, but did not have fine pores on the surface and was poor in air permeability.

【0026】[0026]

【表1】 [Table 1]

【0027】表1の結果から明らかなように、実施例の
皮革様シートはいらつき感、ツヤ感、折れシワ感等の外
観および風合いの良好で高級感を持ち、かつ透気性に優
れていることが解る。
As is clear from the results shown in Table 1, the leather-like sheets of the examples have good appearance such as irritability, luster, creases and wrinkles, a good texture, and a high air permeability. Understand.

【0028】[0028]

【発明の効果】本発明の皮革様シートは、銀面層に直径
300μm以下の微細孔を100個/cm2以上有し、
かつ少なくとも一部の微細孔にはポリウレタン繊維の橋
架け構造が存在しているため、風合い、ツヤ感、折れシ
ワ感に優れ、いらつき感の良好な透気性に優れた皮革様
シートである。
Leather-like sheet of the present invention according to the present invention has the following fine pore diameter 300 [mu] m 100 / cm 2 or more to the silver surface layer,
Moreover, since a polyurethane fiber bridging structure is present in at least some of the fine pores, it is a leather-like sheet excellent in texture, gloss and creases, and good in irritability and air permeability.

【図面の簡単な説明】[Brief description of drawings]

【図1】本発明の皮革様シートの代表的な断面の模式図
である。
FIG. 1 is a schematic view of a representative cross section of a leather-like sheet of the present invention.

【図2】本発明の皮革様シートの代表的な表面の模式図
である。
FIG. 2 is a schematic view of a representative surface of the leather-like sheet of the present invention.

【符号の説明】[Explanation of symbols]

1:橋架けとなっているポリウレタン繊維 2:微細孔 3:ポリウレタン被覆層 4:基体層 1: Polyurethane fiber bridging 2: Micropore 3: Polyurethane coating layer 4: Base layer

フロントページの続き (72)発明者 高橋 豊 岐阜県不破郡垂井町表佐4330 クラレプ ラスチックス株式会社内 (56)参考文献 特開 平5−93372(JP,A) 特開 平4−300368(JP,A) 特開 平1−246480(JP,A) 特開 昭64−85379(JP,A) 特開 昭47−5042(JP,A) (58)調査した分野(Int.Cl.7,DB名) D06N 3/00 - 3/18 Front Page Continuation (72) Inventor Toyohashi Toyohashi, Furu-gun, Gifu 4330 Omotesa, Kuraray Plastics Co., Ltd. (56) References JP-A-5-93372 (JP, A) JP-A-4-300368 (JP, A) JP-A 1-246480 (JP, A) JP-A 64-85379 (JP, A) JP-A 47-5042 (JP, A) (58) Fields investigated (Int.Cl. 7 , DB name) ) D06N 3/00-3/18

Claims (2)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 繊維絡合不織布及びその内部に含有され
た弾性体からなる基体層と、その少なくとも一面に形成
された厚さ10〜100μmのウレタン被覆層からなる
皮革様シートであって、該ポリウレタン被覆層は直径3
00μm以下の微細孔を100個/cm2以上有し、か
つ少なくとも一部の微細孔にはポリウレタン繊維の橋架
け構造が存在していることを特徴とする皮革様シート。
1. A leather-like sheet comprising a base layer composed of a fiber-entangled nonwoven fabric and an elastic body contained therein, and a urethane coating layer having a thickness of 10 to 100 μm formed on at least one surface thereof. The diameter of the polyurethane coating is 3
A leather-like sheet characterized in that it has 100 or less fine pores of 00 μm or less per cm 2 , and that at least some of the fine pores have a bridge structure of polyurethane fibers.
【請求項2】 繊維絡合不織布及びその内部に含有され
た弾性重合体からなる基体層の少なくとも一面に、目付
5〜125g/m2のポリウレタン繊維からなる不織布
を重ね合わせ、加熱加圧して該ポリウレタン繊維を融着
させると共に基体層と積層一体化することを特徴とする
皮革様シートの製造方法。
2. A non-woven fabric made of polyurethane fibers having a basis weight of 5 to 125 g / m 2 is superposed on at least one surface of a fiber-entangled non-woven fabric and a base layer made of an elastic polymer contained therein, and the mixture is heated and pressed. A method for producing a leather-like sheet, which comprises fusing polyurethane fibers and laminating and integrating them with a base layer.
JP16122796A 1996-06-21 1996-06-21 Leather-like sheet with good air permeability and method for producing the same Expired - Fee Related JP3391982B2 (en)