JP2946830B2 - Simple writing adhesive sheet - Google Patents

Simple writing adhesive sheet

Info

Publication number
JP2946830B2
JP2946830B2 JP12894091A JP12894091A JP2946830B2 JP 2946830 B2 JP2946830 B2 JP 2946830B2 JP 12894091 A JP12894091 A JP 12894091A JP 12894091 A JP12894091 A JP 12894091A JP 2946830 B2 JP2946830 B2 JP 2946830B2
Authority
JP
Japan
Prior art keywords
sheet
writing
adhesive
resin
paper
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP12894091A
Other languages
Japanese (ja)
Other versions
JPH04353585A (en
Inventor
栄治 湯浅
亮 三宅
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
OJI SEISHI KK
Original Assignee
OJI SEISHI KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by OJI SEISHI KK filed Critical OJI SEISHI KK
Priority to JP12894091A priority Critical patent/JP2946830B2/en
Publication of JPH04353585A publication Critical patent/JPH04353585A/en
Application granted granted Critical
Publication of JP2946830B2 publication Critical patent/JP2946830B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【産業上の利用分野】本発明は簡易筆記粘着シートに関
し、特にマーキングペンによる筆記性,消去性が良く、
任意の場所に貼り付け,剥離再使用が可能な簡易筆記粘
着シートに関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a simple writing pressure-sensitive adhesive sheet, and more particularly to a writing pen with good writing and erasing properties.
The present invention relates to a simple writing pressure-sensitive adhesive sheet that can be attached to an arbitrary location and can be peeled and reused.

【0002】[0002]

【従来の技術】従来のチョークを用いる黒板に代り、マ
ーキングペンで筆記し、その筆跡を布等で消去できるホ
ワイトボードが使用されるようになっている。一般に、
ホワイトボードは剛性の基板上に、セラミックや合成樹
脂で表面を形成し、マーキングペンのインキが付着し易
くして筆記性を持たせ、一方インキが浸透しないように
加工して消去性を持たせている。
2. Description of the Related Art Instead of a conventional blackboard using chalk, a whiteboard which can be written with a marking pen and erased with a cloth or the like has been used. In general,
The whiteboard is made of a rigid substrate with a ceramic or synthetic resin surface to make it easier for the marking pen ink to adhere to it and to provide writability. ing.

【0003】しかし、セラミックは製造が容易でなく、
合成樹脂を基板表面に塗装焼き付けする方法も生産性が
劣るため、いずれも非常に高価である。また、プラスチ
ックシートに硬化樹脂加工して筆記層を設け、基板表面
に貼り合わせたものが使用されているが、これもやはり
高価である。さらに、消去可能な筆記性シートに磁石を
取り付けたマグネットシート等も知られているが、これ
らは貼り付ける場所が磁石作用のあるところに限定され
る。
However, ceramics are not easy to manufacture,
The method of painting and baking a synthetic resin on the substrate surface is also very expensive because of low productivity. In addition, a plastic sheet is provided with a writing layer by processing with a cured resin and bonded to the substrate surface, but this is also expensive. Further, a magnet sheet or the like in which a magnet is attached to an erasable writable sheet is also known, but these are limited to a place where the magnet is attached.

【0004】このような黒板と同じような構成では、全
体の据え置き面積が広く、重量が大きくなるため、生産
や搬送が容易でない。そして、これらはいずれも材料と
生産性および物流取り扱い等から高価なものになってい
る。
[0004] In a structure similar to such a blackboard, the entire stationary area is large and the weight is large, so that production and transport are not easy. All of these are expensive due to materials, productivity, distribution handling, and the like.

【0005】ホワイトボードの筆記層を形成する合成樹
脂としては、メラミン樹脂や不飽和エステル樹脂等の熱
硬化性樹脂や紫外線硬化性樹脂が使用されているが、熱
硬化樹脂は形成された表面の耐汚染性や硬度が不充分
で、繰り返し使用すると消去性が悪化してしまう。そし
て、紫外線硬化樹脂は耐汚染性や硬度は充分であるが、
塗料中に含まれる光重合開始剤や光増感剤が分解し、筆
記層表面が黄変する欠点がある。
As a synthetic resin for forming a writing layer of a whiteboard, a thermosetting resin such as a melamine resin or an unsaturated ester resin or an ultraviolet curable resin is used. The stain resistance and hardness are insufficient, and the erasability deteriorates when used repeatedly. And UV curing resin has sufficient stain resistance and hardness,
There is a disadvantage that the photopolymerization initiator and the photosensitizer contained in the coating material are decomposed and the surface of the writing layer is yellowed.

【0006】また、筆記層の表面が平滑性に優れている
ことが必要で、充分な平滑面を形成していないと消去性
が悪くなる。特に、筆記後長時間放置した筆跡を消去し
ようとする場合には、筆記面の凹部に入って乾燥したマ
ーキングインキの染料や顔料が簡単には拭き取れず、水
や溶剤で手入れしないと消すことができなくなってしま
う。
Further, the surface of the writing layer needs to have excellent smoothness, and if the surface is not sufficiently smooth, the erasability will be poor. In particular, when trying to erase a handwriting that has been left for a long time after writing, the dye or pigment of the marking ink that has entered the concave portion of the writing surface and cannot be easily wiped off can be erased without cleaning with water or a solvent. I can no longer do it.

【0007】さらに、任意の場所に貼り付けて使用する
安価で手軽なものとして、紙等の裏面に粘着剤を塗布し
た各種のタック紙が利用できる。しかし筆記面が普通の
紙では1回使用すると文字を消すことが困難であり、ま
た一般のタック紙は使用後剥離した時に紙が破れたり粘
着剤が貼り付け面に残るなど、使用取扱が厄介で失敗す
ると後の掃除が大変である。
Further, as an inexpensive and easy-to-use device that is attached to an arbitrary place and used, various tack papers having a back surface such as paper coated with an adhesive can be used. However, it is difficult to erase characters when the writing surface is used once with ordinary paper, and the handling of ordinary tack paper is troublesome, for example, when the paper is peeled off after use, the paper breaks or the adhesive remains on the sticking surface. If it fails, cleaning afterwards is difficult.

【0008】[0008]

【発明が解決しようとする課題】マーキングペンの筆記
性が良くしかも筆跡が布等で簡単に拭き消すことが可能
で、どこでも場所を限定することなく貼り付けて使用で
きて、さらに剥離して再使用することも可能な、安価で
手軽な簡易筆記粘着シートを提供する。
The marking pen has good writability and the handwriting can be easily wiped off with a cloth or the like, and it can be used by sticking it anywhere without limiting the place, and it can be peeled off and re-used. An inexpensive and easy-to-use simple writing adhesive sheet that can be used is provided.

【0009】[0009]

【課題を解決するための手段】本発明は、表面のスムー
スター平滑度が20cmHg以下である基材シート面に
電子線硬化性樹脂を塗工硬化してなるシートの、裏面に
JIS−Z−0237に規定する180度剥離法ステン
レス板接着力が30〜500gの接着力を有する粘着層
を設けたことを特徴とする簡易筆記粘着シートである。
According to the present invention, there is provided a sheet obtained by coating and curing an electron beam-curable resin on the surface of a substrate sheet having a smoother smoothness of 20 cmHg or less on the surface, and JIS-Z- on the back surface. A simple writing pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer having a 180-degree peeling method stainless steel plate having an adhesive force of 30 to 500 g as specified in [0237].

【0010】[0010]

【作用】本発明者等は、上記のような要望に応えるため
鋭意研究した結果、特定の平滑性に優れた基材シートの
表面に電子線硬化樹脂の筆記層を設け、このシートの裏
面に特定の粘着層を設けることにより本発明を完成し
た。
The present inventors have conducted intensive studies to meet the above-mentioned demands. As a result, a writing layer of an electron beam-curable resin is provided on the surface of a specific base sheet having excellent smoothness, and the back surface of this sheet is provided. The present invention has been completed by providing a specific adhesive layer.

【0011】本発明で使用する基材シートの筆記層が形
成される側の表面平滑性は、スムースター平滑度が20
cmHg以下の、平滑性に優れていることが重要であ
る。20cmHgを越えて平滑性が悪い場合は、筆記層
の塗工量を増加しなければならず、筆記性,消去性の品
質面、と操業面および経済面で好ましくない。
The surface smoothness of the base sheet used in the present invention on the side on which the writing layer is formed has a smoother smoothness of 20%.
It is important that the smoothness is not more than cmHg. If the smoothness exceeds 20 cmHg and the smoothness is poor, the coating amount of the writing layer must be increased, which is not preferable in terms of the quality of writing and erasability, and the operation and economy.

【0012】基材シートは、スムースター平滑度が20
cmHg以下であれば一般の基材シートで良く、例えば
ポリエステル,ポリプロピレン,ポリエチレン,ポリ塩
化ビニル,ポリ塩化ビニリデン,ポリカーボネート,ポ
リアミド,ポリスチレン等のフィルムシートまたはこれ
らの複合シートあるいはラミネート紙,コーテッド紙,
アンダーコート紙,片面平滑性の良い片艶晒クラフト紙
等が使用される。そして特に、安価で手軽なことが要望
される用途には、加工性や価格の面からキャストコーテ
ッド紙,アートコート紙のようなコーテッド紙が好まし
い。
The base sheet has a smoother smoothness of 20.
If it is not more than cmHg, a general substrate sheet may be used. For example, a film sheet of polyester, polypropylene, polyethylene, polyvinyl chloride, polyvinylidene chloride, polycarbonate, polyamide, polystyrene or the like, a composite sheet thereof, a laminated paper, a coated paper,
Undercoat paper, single-side bleached kraft paper having good one-sided smoothness, and the like are used. In particular, for applications requiring low cost and ease, coated paper such as cast coated paper and art-coated paper is preferable from the viewpoint of processability and price.

【0013】本発明において、筆記層の形成に用いられ
る電子線硬化性樹脂塗料は、塗膜形成性成分と反応性希
釈剤を主成分とし、必要に応じて溶剤,染顔料,充填剤
等を含有し、塗工面を電子線照射することにより数秒で
架橋硬化する。
In the present invention, the electron beam-curable resin paint used for forming the writing layer contains a film-forming component and a reactive diluent as main components, and may contain a solvent, a dye, a pigment, a filler and the like as necessary. It is cross-linked and cured in a few seconds by irradiating the coated surface with an electron beam.

【0014】塗膜形成性成分には通常アクリロイル基や
メタクリロイル基、あるいはその他の付加重合性二重結
合を分子内に有する高分子重合体,オリゴマー,モノマ
ー等があり、例えばポリエステル(メタ)アクリレー
ト,ウレタン(メタ)アクリレート,エポキシ(メタ)
アクリレート等が好ましく用いられる。そして、特にマ
ーキングペンによる筆記性と耐汚染性、および硬化塗膜
の表面硬化に優れる点からポリエステル(メタ)アクリ
レートがより好ましい。
The coating film-forming component usually includes an acryloyl group, a methacryloyl group, or another polymer having a polymerizable double bond in the molecule, an oligomer, a monomer, and the like. For example, polyester (meth) acrylate, Urethane (meth) acrylate, epoxy (meth)
Acrylates and the like are preferably used. In particular, polyester (meth) acrylate is more preferable in terms of excellent writing properties and stain resistance with a marking pen, and excellent surface curing of the cured coating film.

【0015】反応性希釈剤は上記塗膜形成性成分の粘度
を低下させて、塗布作業を容易にすると共に、電子線照
射を受けて塗膜形成性成分を架橋網状化させるために配
合されるもので、通常、多官能性のオリゴマー,モノマ
ーである。本発明の反応性希釈剤としては、分子内に2
個以上のアクリレート基及び/又はメタクリレート基を
有するモノマーが好ましく用いられ、これらの具体例と
しては、例えばトリメチロールプロパントリ(メタ)ア
クリレート,ペンタエリスリトールトリ(メタ)アクリ
レート,ブタジンオールジ(メタ)アクリレート,ネオ
ペンチルグリコールジ(メタ)アクリレート,1,6−
ヘキサンジオールジ(メタ)アクリレート,ジエチレン
グリコールジ(メタ)アクリレート等を挙げることがで
きる。
The reactive diluent is compounded to lower the viscosity of the above-mentioned film-forming component to facilitate the coating operation and to crosslink the film-forming component by irradiation with electron beams. These are usually polyfunctional oligomers and monomers. As the reactive diluent of the present invention, 2
Monomers having at least two acrylate groups and / or methacrylate groups are preferably used. Specific examples thereof include, for example, trimethylolpropane tri (meth) acrylate, pentaerythritol tri (meth) acrylate, butazinol di (meth) acrylate, Pentyl glycol di (meth) acrylate, 1,6-
Examples include hexanediol di (meth) acrylate and diethylene glycol di (meth) acrylate.

【0016】さらに、これらに2−エチルヘキシル(メ
タ)アクリレート,2−ヒドロキシエチル(メタ)アク
リレート,グリシジル(メタ)アクリレート,N−ビニ
ル−2−ピロリドン,テトラヒドロフルフリル(メタ)
アクリレート等の単官能性モノマーを併用することがで
きる。
Furthermore, 2-ethylhexyl (meth) acrylate, 2-hydroxyethyl (meth) acrylate, glycidyl (meth) acrylate, N-vinyl-2-pyrrolidone, tetrahydrofurfuryl (meth)
Monofunctional monomers such as acrylates can be used in combination.

【0017】硬化性塗料の塗布量は少なすぎると充分な
耐汚染性と硬度が得られず、また多すぎると硬化時基材
シートに歪みを生じカール等が起こるため0.5〜50
μmが好ましく、特に1〜10μm程度がより好まし
い。電子線照射はエレクトロカーテン型電子線照射装置
が好ましく用いられるが、これに限らず、一般に使用さ
れている各種の型式や方式の照射装置を用いても良い。
If the coating amount of the curable paint is too small, sufficient stain resistance and hardness cannot be obtained.
μm is preferable, and particularly preferably about 1 to 10 μm. Electron beam irradiation is preferably performed using an electron curtain type electron beam irradiation apparatus, but is not limited thereto, and irradiation apparatuses of various types and systems generally used may be used.

【0018】本発明の筆記層は、マーキングぺンの筆記
性に優れ、筆記文字を訂正したり筆跡等が不要になった
場合には、いつでも布等で容易に拭き消し可能であり、
繰り返して使用できる。
The writing layer of the present invention is excellent in the writing property of the marking pen, and can be easily wiped off with a cloth or the like at any time when the written characters are corrected or the handwriting becomes unnecessary.
Can be used repeatedly.

【0019】本発明においては、筆記層シートの裏面に
JIS−Z−0237に規定された180度剥離法によ
るステンレス板に対する接着力が30〜500gの接着
力を有する粘着層を設ける。この接着力が30g未満で
は貼り付けてもすぐ剥がれ落ちたり、均一に付かずふく
れが出たりするおそれがある。また一方500gを越え
るような高い接着力では、再剥離が思うようにできない
ため、接着力の規定は重要である。
In the present invention, an adhesive layer having an adhesive strength of 30 to 500 g to a stainless steel plate by a 180-degree peeling method specified in JIS-Z-0237 is provided on the back surface of the writing layer sheet. If the adhesive strength is less than 30 g, there is a risk that the adhesive will peel off immediately after application, or that it will not adhere evenly and blisters will appear. On the other hand, if the adhesive strength is as high as 500 g or more, re-peeling cannot be performed as expected, so the regulation of the adhesive strength is important.

【0020】なお、接着力の調節は接着剤と粘着付与剤
および助剤の選択と配合の調節により、用途に適した範
囲に設定できる。また各種の粒子等の充填剤を混入させ
て接着力を調節する方法も採用できる。粘着層の塗工量
は5〜30g/m2 、より好ましくは10〜25g/m
2 の範囲で調節される。そして、塗工量は接着力に関係
があるため上記材料の選択と配合調節に合わせて設定す
る必要がある。
The adjustment of the adhesive force can be set in a range suitable for the application by selecting the adhesive, the tackifier and the auxiliary and adjusting the compounding. Further, a method of adjusting the adhesive force by mixing various fillers such as particles can also be adopted. The coating amount of the adhesive layer is 5 to 30 g / m 2, more preferably 10 to 25 g / m
Adjusted in 2 ranges. Since the coating amount is related to the adhesive strength, it is necessary to set the amount in accordance with the selection of the above materials and the adjustment of the mixture.

【0021】粘着剤は接着剤と粘着付与剤および助剤か
らなり、接着剤としては、例えばポリイソプレンゴム,
ポリイソブチルゴム,スチレンブタジエンゴム,ブタジ
エンアクリロニトリルゴム等のゴム系樹脂や(メタ)ア
クリル酸エステル系樹脂,ポリビニルエーテル系樹脂,
ポリ酢酸ビニル系樹脂,塩化ビニル酢酸ビニル共重合体
系樹脂,ポリスチレン系樹脂,ポリエステル系樹脂,ポ
リアミド系樹脂,ポリ塩素化オレフィン系樹脂,ポリビ
ニルブチラール系樹脂等が挙げられる。
The pressure-sensitive adhesive comprises an adhesive, a tackifier, and an auxiliary. Examples of the adhesive include polyisoprene rubber,
Rubber resins such as polyisobutyl rubber, styrene butadiene rubber, butadiene acrylonitrile rubber, (meth) acrylate resin, polyvinyl ether resin,
Examples thereof include polyvinyl acetate resin, vinyl chloride vinyl acetate copolymer resin, polystyrene resin, polyester resin, polyamide resin, polychlorinated olefin resin, polyvinyl butyral resin, and the like.

【0022】そして、これらの接着剤に適当量添加され
る粘着付与剤としては、例えばロジン,ダンマル,重合
ロジン,部分水添ロジン,エステルロジン,ポリテルペ
ン系樹脂,テルベン変性体,石油系樹脂,シクロペンタ
ジエン系樹脂,フェノール系樹脂,スチレン系樹脂,キ
シレン系樹脂,クマロン−インデン系樹脂等が挙げられ
る。なお、必要に応じて、軟化剤,充填剤,老化防止剤
等を添加する。
Examples of tackifiers added to these adhesives in appropriate amounts include, for example, rosin, dammar, polymerized rosin, partially hydrogenated rosin, ester rosin, polyterpene-based resin, modified terpene, petroleum-based resin, and cyclohexane. Examples include pentadiene-based resins, phenol-based resins, styrene-based resins, xylene-based resins, and cumarone-indene-based resins. If necessary, a softening agent, a filler, an antioxidant and the like are added.

【0023】また、粘着剤層の表面に剥離シートを貼着
しておくことで簡易筆記粘着シートの使用時や保存時の
取扱が良好となる。さらに、粘着剤層塗工時に剥離シー
トを工程紙として使用し、それを筆記消去性基材シート
と貼り合わせて製造することもできる。
Further, by sticking a release sheet on the surface of the pressure-sensitive adhesive layer, handling of the simplified writing pressure-sensitive adhesive sheet at the time of use and storage is improved. Further, a release sheet can be used as a process paper at the time of applying the pressure-sensitive adhesive layer, and the release sheet can be bonded to a writing-erasable base material sheet.

【0024】[0024]

【実施例】以下に本発明の実施例を挙げて具体的に説明
するが、勿論これらに限定するものではない。なお、特
にことわらない限り実施例中の部および%はそれぞれ重
量部および重量%である。
EXAMPLES The present invention will now be described specifically with reference to examples of the present invention, but it is needless to say that the present invention is not limited thereto. Unless otherwise specified, parts and% in Examples are parts by weight and% by weight, respectively.

【0025】実施例1 基材シートとして、表面のスムースター平滑度が3cm
Hgで、坪量85g/m2 のキャストコーテッド紙を使
用して、キャスト仕上げ面にポリエステルポリアクリレ
ートとポリウレタンポリアクリレートの各プレポリマー
混合物(商品名:78E204,モービル石油社製)を
1.5μm(硬化後)となるようにバーコーターで塗布
し、エレクトロカーテン型電子線照射装置(CB:15
0型,ESI社製)で1.5Mradの照射線量で処理
して樹脂成分を硬化させ筆記層シートを得た。
Example 1 As a substrate sheet, the smoother smoothness of the surface was 3 cm.
Using a cast coated paper having a basis weight of 85 g / m 2 in Hg, a prepolymer mixture of polyester polyacrylate and polyurethane polyacrylate (trade name: 78E204, manufactured by Mobil Sekiyu KK) was 1.5 μm on the cast finished surface ( (After curing) by a bar coater, and an electro-curtain type electron beam irradiation device (CB: 15
(Type 0, manufactured by ESI) with an irradiation dose of 1.5 Mrad to cure the resin component to obtain a writing layer sheet.

【0026】次にアクリル酸共重合体エマルジョン(サ
イデン化学(株)製:商品名「サイビノールX−389
−446E」)100部にポリエポキサイド化合物(サ
イデン化学(株)製:商品名「A−3」)1部を添加混
合した粘着剤を、市販のポリエチレンラミネート剥離紙
の剥離面上にリバースロールコーターで固形分として2
5g/m2 となるよう塗布し、熱風乾燥機で乾燥した。
この粘着剤塗布面に筆記層シートの裏面を貼り合せて簡
易筆記粘着シートを得た。
Next, an acrylic acid copolymer emulsion (manufactured by Seiden Chemical Co., Ltd., trade name: Cybinol X-389)
-446E ") and 100 parts of a polyepoxide compound (manufactured by Seiden Chemical Co., Ltd .: trade name" A-3 "), and then mixing and adding a pressure-sensitive adhesive to the release surface of a commercially available polyethylene laminate release paper. 2 as solids
It was applied so as to have a concentration of 5 g / m 2 and dried with a hot air drier.
The back surface of the writing layer sheet was stuck to the pressure-sensitive adhesive applied surface to obtain a simple writing pressure-sensitive adhesive sheet.

【0027】このシートはマーキングペンによる筆記
性,消去性は良好で、筆記後15日を経た筆跡も布で容
易に拭き消すことができた。また、このシートのJIS
−Z−0237,180度剥離法ステンレス板に対する
接着力は100gで、剥離紙を剥がし粘着面をガラス
面,金属面に貼り付け、剥離と貼り付けを繰り返したが
紙破れや貼り付け面への糊残りによる汚れは生じなかっ
た。
This sheet had good writing and erasing properties with a marking pen, and handwriting 15 days after writing could be easily wiped off with a cloth. The JIS of this sheet
-Z-0237, 180-degree peeling method Adhesive strength to a stainless steel plate is 100 g. Peeling off the release paper, sticking the adhesive surface to the glass surface or metal surface, and repeating peeling and sticking. No stain was caused by the adhesive residue.

【0028】実施例2 基材シートとして、表面のスムースター平滑度が15c
mHgで、坪量157g/m2 のコート紙を使用し、ま
た粘着剤としてアクリル酸共重合体エマルジョン(東洋
インキ製:商品名「オリバインBPW−5222」)を
使用した以外は、実施例1と同様にして簡易筆記粘着シ
ートを得た。
Example 2 As a substrate sheet, the smoother smoothness of the surface was 15c.
Example 1 was the same as Example 1 except that a coated paper having a mHg of 157 g / m 2 and a basis weight of 157 g / m 2 was used, and an acrylic acid copolymer emulsion (trade name “Olivine BPW-5222” manufactured by Toyo Ink) was used as an adhesive. Similarly, a simple writing adhesive sheet was obtained.

【0029】このシートはマーキングペンによる筆記
性,消去性は良好で、筆記後15日を経た筆跡も布で容
易に拭き消すことができた。また、このシートのJIS
−Z−0237,180度剥離法ステンレス板に対する
接着力は450gで、剥離紙を剥がし粘着面をガラス
面,金属面に貼り付け、剥離と貼り付けを繰り返したが
紙破れや貼り付け面への糊の残りによる汚れは生じなか
った。
This sheet had good writing and erasing properties with a marking pen, and handwriting 15 days after writing could be easily wiped off with a cloth. The JIS of this sheet
-Z-0237, 180-degree peeling method Adhesive strength to a stainless steel plate is 450 g. Peeling off the release paper, sticking the adhesive surface to the glass surface and metal surface, and repeating peeling and sticking, No stain was caused by the remaining glue.

【0030】比較例1 基材シートとして、表面のスムースター平滑度が35c
mHgで、坪量84gの軽量コート紙を使用し、また粘
着剤としてアクリル酸共重合体エマルジョン(日本カー
バイト製:商品名「ニカゾールTS−662」)を使用
した以外は、実施例1と同様にした。
Comparative Example 1 As a substrate sheet, the surface smoother smoothness was 35c.
Same as Example 1 except that a light-weight coated paper having a mHg of 84 g and a basis weight of 84 g was used, and an acrylic acid copolymer emulsion (manufactured by Nippon Carbide Co., Ltd .: trade name "Nicazole TS-662") was used as an adhesive. I made it.

【0031】このシートはマーキングペンによる筆記性
と筆記直後の消去性は良かったが、15日を経た筆跡は
布で完全には拭き消せなかった。またこのシートの接着
力は1000gであり、剥離紙をはがし粘着面をガラス
面,金属面に貼り付け、使用後剥がした時に紙破れを生
じた。
This sheet had good writing properties with a marking pen and good erasing properties immediately after writing, but handwriting after 15 days could not be completely wiped off with a cloth. The adhesive strength of this sheet was 1000 g. When the release paper was peeled off, the adhesive surface was stuck to the glass surface or the metal surface, and the sheet was torn when peeled after use.

【0032】[0032]

【発明の効果】実施例の結果から明らかなように、本発
明の簡易筆記粘着シートは、マーキングンペンによる筆
記性が良く、布で拭き消す消去性に優れていた。特に筆
記後長時間を経過した筆跡も布で容易に拭き消すことが
できた。そして、任意の場所に貼り付け使用ができ、使
用後剥がした時、紙破れや粘着剤が貼付け面に残るよう
なことがなく、繰り返し使用可能であった。
As is clear from the results of the examples, the simple writing pressure-sensitive adhesive sheet of the present invention was excellent in writability by a marking pen and excellent in erasability to wipe off with a cloth. In particular, handwriting that had passed a long time after writing could be easily wiped off with a cloth. And it could be stuck and used at any place, and when peeled off after use, it could be repeatedly used without tearing the paper or leaving the adhesive on the stuck surface.

───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.6 識別記号 FI D21H 19/24 D21H 27/00 27/00 1/34 J 5/00 B (58)調査した分野(Int.Cl.6,DB名) C09J 7/02 - 7/04 C09D 5/00 C09D 133/08 B32B 7/10 D21H 19/24 D21H 27/00 WPI/L(QUESTEL)──────────────────────────────────────────────────続 き Continuation of front page (51) Int.Cl. 6 identification code FI D21H 19/24 D21H 27/00 27/00 1/34 J 5/00 B (58) Fields studied (Int. Cl. 6 , DB name) C09J 7/02-7/04 C09D 5/00 C09D 133/08 B32B 7/10 D21H 19/24 D21H 27/00 WPI / L (QUESTEL)

Claims (2)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】表面のスムースター平滑度が20cmHg
以下である基材シート面に電子線硬化性樹脂を塗工硬化
してなるシートの、裏面にJIS−Z−0237に規定
する180度剥離法ステンレス板接着力が30〜500
gの接着力を有する粘着層を設けたことを特徴とする簡
易筆記粘着シート。
1. The smoother smoothness of the surface is 20 cmHg.
A sheet obtained by coating and curing an electron beam-curable resin on the surface of a base material sheet described below has a 180-degree peeling stainless steel plate adhesive force specified by JIS-Z-0237 of 30 to 500 on the back surface.
g. An adhesive sheet having an adhesive force of g.
【請求項2】基材シートがコーテッド紙である請求項1
記載の簡易筆記粘着シート。
2. The method according to claim 1, wherein the base sheet is coated paper.
Simple writing adhesive sheet as described.
JP12894091A 1991-05-31 1991-05-31 Simple writing adhesive sheet Expired - Fee Related JP2946830B2 (en)