JP2666654B2 - How to apply water-soluble rust preventive oil to steel - Google Patents
How to apply water-soluble rust preventive oil to steelInfo
- Publication number
- JP2666654B2 JP2666654B2 JP4079446A JP7944692A JP2666654B2 JP 2666654 B2 JP2666654 B2 JP 2666654B2 JP 4079446 A JP4079446 A JP 4079446A JP 7944692 A JP7944692 A JP 7944692A JP 2666654 B2 JP2666654 B2 JP 2666654B2
- Authority
- JP
- Japan
- Prior art keywords
- rust
- oil
- preventive oil
- steel
- water
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION
【0001】[0001]
【産業上の利用分野】この発明は、一時防錆を施すため
に、鉄鋼製品(鋼板,鋼管,形鋼等)である鋼材の表面
へ、水溶性防錆油を塗付する時の塗付方法に関するもの
である。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to the application of a water-soluble rust preventive oil to the surface of a steel product (steel plate, steel pipe, shaped steel, etc.) for temporary rust prevention. It is about the method.
【0002】従来、この種の鋼材表面へ、例えば塗料,
エアー等を吹付ける方法としては、次に述べるものが一
般に知られている。[0002] Conventionally, for example, paint,
As a method of blowing air or the like, the following method is generally known.
【0003】即ち、(1) 内部に塗装用スプレー装置を設
けた吹付室内で、鋼材表面へ塗料を吹付けると共に、吹
付室の内壁全面にライニングを施して、余剰塗料を回収
できるようにした、水溶性塗料を塗布する吹付室(実公
昭52-16732号公報参照)。[0003] (1) In a spraying chamber provided with a spraying device for painting, a paint is sprayed on the surface of a steel material, and lining is applied to the entire inner wall of the spraying chamber so that excess paint can be collected. A spray chamber for applying a water-soluble paint (see Japanese Utility Model Publication No. 52-16732).
【0004】また(2) ベルトコンベアー上で鋼材表面へ
スプレー塗装することとし、余剰塗料をナイフ状の刃で
かきとると共に、かきとった余剰塗料を回収して再使用
できるようにしたスプレー式自動塗装装置(実公昭61-9
27号公報参照)。[0004] (2) Spray coating on steel surface by means of spray coating on a belt conveyor, scraping off excess paint with a knife-like blade, and recovering the scraped excess paint so that it can be reused. Coating equipment (61-9
No. 27).
【0005】さらに(3) 内側にノズル孔を分散配置させ
たスリーブと、このスリーブ外周部の円形ケースとの間
に、エアーを送入することにより、スリーブ内を貫通す
る鋼材(管体)へエアーを吹付ける。そしてこのエアー
によって、鋼材への付着オイルを除去するオイル用エア
ーワイパー(実開昭 58-9202号公報参照)。[0005] (3) Air is fed between a sleeve in which nozzle holes are dispersedly arranged on the inside and a circular case on the outer periphery of the sleeve, so that a steel material (tube) penetrating through the inside of the sleeve is formed. Blow air. An air wiper for oil that removes oil adhering to steel by this air (see Japanese Utility Model Laid-Open No. 58-9202).
【0006】なお形鋼への防錆油の塗付は、油槽の中
に、そのまま製品を浸けて塗付するドブ漬方式が一般的
である。[0006] The application of rust-preventive oil to a shaped steel is generally carried out by dip pickling in which the product is immersed in an oil bath and applied.
【0007】[0007]
【この発明が解決しようとする課題】しかし、この発明
が問題とする防錆油の塗付時には、例えば、H形鋼等の
形鋼では輸送効率向上のため各形鋼を組み会わせる、所
謂パイリングを行うので、防錆油の付着量が多いとフラ
ンジとフランジの間に油が溜まる(特に水溶性防錆油で
は、水分の蒸発が遅く、ノリ状に固まって脱脂不良を起
こす。)ことがあり、油膜を薄く均一に短時間で形成さ
せる必要がある。However, at the time of applying the rust-preventive oil, which is a problem of the present invention, for example, in the case of a section steel such as an H-section steel, each section steel is combined to improve the transport efficiency. Due to the piling, if the amount of rust-preventive oil is large, oil accumulates between the flanges (especially, with water-soluble rust-preventive oil, the evaporation of water is slow and the paste hardens to cause poor degreasing). Therefore, it is necessary to form an oil film thinly and uniformly in a short time.
【0008】従って、これらのことを考慮すると、前述
した従来の吹付ける方法の(1) では、付着した塗料の被
膜形成促進や被膜を均一に塗布する技術的思想はない。
そのため、被膜が均一になるように塗付しないと、製品
の接触部に防錆油がたまり、コストが高いばかりでな
く、輸送中に油が落下する等の問題が生じる。[0008] Therefore, in view of these facts, in the above-mentioned conventional spraying method (1), there is no technical idea of accelerating the formation of the film of the adhered paint or uniformly applying the film.
Therefore, if the coating is not applied so that the coating is uniform, rust-preventive oil accumulates at the contacting parts of the product, which not only increases the cost, but also causes problems such as oil dropping during transportation.
【0009】また(2) では、余剰塗料をナイフでかきと
っているために、余剰塗料の回収効率が悪い。しかも、
かきとった後の残塗料の均一性が悪い。In (2), the excess paint is scraped off with a knife, so that the excess paint recovery efficiency is poor. Moreover,
Poor uniformity of residual paint after scraping.
【0010】さらに(3) では、余剰付着オイルをエアー
で除去する時に、管の径に応じて装置を交換しなければ
ならない。しかもノズル孔が円形孔であるため、余剰付
着オイルを均一に除去するのがむずかしい。Further, in the method (3), when the surplus oil is removed by air, the apparatus must be replaced according to the diameter of the pipe. In addition, since the nozzle hole is a circular hole, it is difficult to uniformly remove the surplus adhered oil.
【0011】この発明は前述した事情に鑑みて創案され
たもので、その目的は鋼材表面への水溶性防錆油の塗付
時において、油性被膜の形成時間を短縮できると共に、
油性被膜を均一に塗付でき、しかも鋼材表面に付着した
余剰油を除去して均一な塗付状態にすることができると
共に、余剰油を回収して再使用することができる鋼材へ
の水溶性防錆油の塗付方法を提供することにある。The present invention has been made in view of the above-mentioned circumstances, and has as its object to reduce the time required for forming an oily film when applying a water-soluble rust-preventive oil to the surface of steel.
The oily coating can be applied uniformly, and the excess oil adhering to the surface of the steel material can be removed to achieve a uniform application state, and the excess oil can be collected and reused. An object of the present invention is to provide a method for applying rust preventive oil.
【0012】[0012]
【課題を解決するための手段】この発明の塗付方法によ
れば、まず鋼材の温度を30〜50℃に予熱すると共に、こ
の鋼材表面に前記水溶性防錆油を15〜70kg/cm2の高圧下
で塗付し、この水溶性防錆油が塗付された鋼材の表面
に、種々の鋼材サイズに適応できる吹付け部により3kg
/cm2以上の圧空を吹付けて、余分に塗付した防錆油を除
去すると共に、鋼材表面への防錆油塗布量を均一にす
る。また、前記圧空で除去した余剰防錆油を回収して再
使用する。According to the coating method of the present invention, first, the temperature of the steel material is preheated to 30 to 50 ° C, and the surface of the steel material is coated with the water-soluble rust preventive oil at 15 to 70 kg / cm 2. 3kg by spraying part which can be applied to various steel sizes on the surface of steel coated with this water-soluble rust-preventive oil.
By spraying compressed air of / cm 2 or more, excess rust preventive oil is removed and the amount of rust preventive oil applied to the steel surface is made uniform. The surplus rust-preventive oil removed by the compressed air is collected and reused.
【0013】そして、例えばスプレー式ではスプレー時
の膨張により油温度が下がるので、鋼材を30〜50℃に予
熱することにより、水溶性防錆油の水分の蒸発を促し、
油性被膜形成時間を短縮する。[0013] For example, in the spray type, the oil temperature is lowered by expansion during spraying. Therefore, by preheating the steel material to 30 to 50 ° C, the water-soluble rust-preventive oil is promoted to evaporate,
Shortens the time for forming an oily film.
【0014】また、高圧下の塗付により防錆油を凝集さ
せ、油性被膜を形成させてから、鋼材表面へ均一に塗付
する。さらに鋼材表面に付着した余剰油を除去して、均
一な塗布状態にすると共に、余剰油を回収して再使用す
るようにしたものである。Further, the rust-preventive oil is agglomerated by application under high pressure to form an oily film, and then uniformly applied to the surface of the steel material. Further, the excess oil adhering to the surface of the steel material is removed to make a uniform coating state, and the excess oil is collected and reused.
【0015】[0015]
【実施例】以下、この発明の鋼材への水溶性防錆油の塗
付方法を、図示する実施例によって説明する。DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A method for applying a water-soluble rust preventive oil to steel according to the present invention will be described below with reference to the illustrated embodiments.
【0016】まず、この発明の塗付方法を実施する塗付
装置について述べると、塗付装置1(図1〜図5参照)
は、製造設備2からの鋼材3を予熱する予熱炉4と、こ
の予熱炉4によって予熱された鋼材3に、水溶性防錆油
を吹付けると共に、余分に塗付した防錆油を除去すべく
圧空を吹付ける吹付け室5と、この吹付け室5で除去し
た余剰防錆油を回収して再使用する回収部6とを備えて
なる。First, a coating apparatus for carrying out the coating method of the present invention will be described. The coating apparatus 1 (see FIGS. 1 to 5)
In the preheating furnace 4 for preheating the steel material 3 from the manufacturing equipment 2, the water-soluble rust preventive oil is sprayed on the steel material 3 preheated by the preheat furnace 4, and the excess rust preventive oil is removed. A blowing chamber 5 for blowing compressed air is provided, and a collecting section 6 for collecting and reusing excess rust preventive oil removed in the blowing chamber 5 is provided.
【0017】そして、この実施例での吹付け室5は、防
錆油をポンプ圧縮して吹き出すスプレーガン7のノズル
7aが、鋼材4の周囲位置に複数設置されている塗付ブー
ス8と、圧空を吹き出す油切りノズル9が、鋼材3の周
囲位置に複数設置されている油切りブース10とからなっ
ている。The spray chamber 5 in this embodiment is provided with a nozzle of a spray gun 7 for spraying rust preventive oil by pump compression.
7a is composed of a plurality of coating booths 8 installed around the steel material 4 and an oil drain booth 10 provided with a plurality of oil drain nozzles 9 for blowing compressed air around the steel material 3.
【0018】回収部6は、吹付け室5の底部に形成され
ている集油ブース11と、この集油ブース11に接続されて
おり、集めた余剰防錆油を防錆油供給タンク13へ送る回
収ポンプ12(図6参照)とからなっている。The collecting section 6 is connected to the oil collecting booth 11 formed at the bottom of the spray chamber 5 and is connected to the oil collecting booth 11. It comprises a recovery pump 12 for feeding (see FIG. 6).
【0019】塗付ブース8のスプレーガン7は、図6に
示すように、供給タンク13から供給ポンプ14を介して高
圧状態の防錆油が送られ、塗付時には圧空供給部15から
圧空が送られることにより、スプレーガン7が開いて水
溶性防錆油をノズル7aから鋼材3へ吹付けられるよう
に、また塗付を止める時には同様にしてスプレーガン7
を閉じることで止められるように構成されている。As shown in FIG. 6, the spray gun 7 of the coating booth 8 is supplied with high-pressure rust-preventive oil from a supply tank 13 via a supply pump 14, and pressurized air is supplied from a compressed air supply unit 15 during coating. By being sent, the spray gun 7 is opened so that the water-soluble rust-preventive oil can be sprayed from the nozzle 7a onto the steel material 3 and, similarly, when the application is stopped, the spray gun 7 is sprayed.
It is configured to be stopped by closing.
【0020】油切りブース10の各油切りノズル9は、図
7および図8に示すように、傾動自在な略U字状の支持
部16に設けられており、全体を傾動させることにより、
製品高さに応じてノズル位置を調節できるようになって
いる。そして圧空供給部15から送られてきた圧空(図6
参照)を、種々の高さの製品(鋼材)へ吹付けることが
できるように構成されている。As shown in FIGS. 7 and 8, each of the oil drain nozzles 9 of the oil drain booth 10 is provided on a substantially U-shaped support portion 16 which can be freely tilted.
The nozzle position can be adjusted according to the product height. The compressed air sent from the compressed air supply unit 15 (FIG. 6)
) Can be sprayed on products (steel materials) of various heights.
【0021】なお、回収ポンプ12および供給ポンプ14
は、圧空を駆動源として作動するものである。また、図
6において、符号17は圧空供給部15から送られてきた圧
空を供給,停止させる電磁弁で、18はレベルセンサー
で、19は制御部で、20は圧空を駆動源として作動する攪
拌機である。The recovery pump 12 and the supply pump 14
Operates using compressed air as a drive source. In FIG. 6, reference numeral 17 denotes an electromagnetic valve for supplying and stopping compressed air sent from the compressed air supply unit 15, reference numeral 18 denotes a level sensor, reference numeral 19 denotes a control unit, and reference numeral 20 denotes a stirrer operated by using the compressed air as a driving source. It is.
【0022】このような構成からなる塗付装置1を使用
して、本発明の水溶性防錆油の塗付方法を実施するに
は、次に述べるようにして行う。The method of applying the water-soluble rust-preventive oil of the present invention using the coating apparatus 1 having such a configuration is performed as follows.
【0023】まず、水溶性防錆油スプレー前に、塗付し
ようとする鋼材3の温度を、予熱炉4で30〜50℃に昇温
させる。この昇温時の温度は、30℃以下では水溶性防錆
油の水分を蒸発させる効果が小さい。また、50℃を越え
ると防錆油剤の損傷の恐れがあり防錆性能を悪化させる
ことから、設定されている。First, the temperature of the steel material 3 to be applied is raised to 30 to 50 ° C. in the preheating furnace 4 before spraying the water-soluble rust-preventive oil. When the temperature at the time of this temperature rise is 30 ° C. or less, the effect of evaporating the water content of the water-soluble rust preventive oil is small. Also, if the temperature exceeds 50 ° C., the rust preventive oil may be damaged, and the rust preventive performance is deteriorated.
【0024】次に、この予熱した鋼材3を吹付け室5へ
送り、図示しないセンサーで鋼材3を検出したら、この
鋼材3へ、塗付ブース8におけるスプレーガン7のノズ
ル7aから、水溶性防錆油を15〜70kg/cm2の圧力にて噴射
し塗付する。この防錆油噴射圧力は、圧力が低いとミス
ト径が大きくなり防錆油剤が鋼材に衝突する際発生する
凝集効果が小さく油膜を形成されずに流れる。また、圧
力が高いとミスト径が小さくなりすぎミストの飛散が大
きくなって回収効率が悪いことから、設定されている。Next, the preheated steel material 3 is sent to the spraying chamber 5, and when the steel material 3 is detected by a sensor (not shown), the steel material 3 is supplied to the steel material 3 from the nozzle 7 a of the spray gun 7 in the coating booth 8. Rust oil is sprayed at a pressure of 15 to 70 kg / cm 2 and applied. When the rust-preventive oil injection pressure is low, the mist diameter increases, and the cohesive effect generated when the rust-preventive oil collides with the steel material is small, and the rust-preventive oil flows without forming an oil film. Further, if the pressure is high, the mist diameter becomes too small, the scattering of the mist becomes large, and the collection efficiency is poor.
【0025】次に、油切りブース12の各油切りノズル9
によって、3kg/cm2以上の圧力空気で、鋼材3の表面に
余分に付着した防錆油を除去し、鋼材表面への防錆油の
塗布状態を均一にさせる。この時の圧空の圧力は、低い
と余剰防錆油を均一に除去できないことから、設定され
ている。Next, each oil drain nozzle 9 of the oil drain booth 12
By using a pressure air of 3 kg / cm 2 or more, extra rust-preventive oil adhering to the surface of the steel material 3 is removed, and the state of application of the rust-preventive oil to the steel material surface is made uniform. The pressure of the compressed air at this time is set because if it is low, excess rust preventive oil cannot be uniformly removed.
【0026】なお、ここでの各油切りノズル9は、余剰
防錆油を均一に除去できるように、圧力空気を扇状に広
げることができるように形成されている。また、各油切
りノズル9の支持部16を傾動させることにより、鋼材3
のサイズに応じてノズル位置を調整できるようになって
いる。Each of the oil draining nozzles 9 is formed so that the pressurized air can be spread in a fan shape so that excess rust preventive oil can be uniformly removed. Further, by tilting the support portion 16 of each oil drain nozzle 9, the steel material 3
The nozzle position can be adjusted according to the size of the nozzle.
【0027】次いで、図示しないセンサーで鋼材3の通
過を検出して、各スプレーガン7および油切りノズル9
を停止させて、一動作を完了する。Next, the passage of the steel material 3 is detected by a sensor (not shown), and the spray gun 7 and the oil drain nozzle 9 are detected.
Is stopped and one operation is completed.
【0028】また、オーバースプレーした余剰油は、回
収部7で回収して再使用する。なお、この余剰油の回収
は、塗付ブース8と油切りブース10との集油ブース11を
連結して、1ケ所で行なっている。The excess oil that has been oversprayed is recovered by the recovery unit 7 and reused. The collection of the surplus oil is performed in one place by connecting the oil collection booth 11 including the application booth 8 and the oil removal booth 10.
【0029】そして、このことから、この発明の塗付方
法による、水溶性防錆油の鋼材表面への均一な塗付が行
われる。From this, the water-soluble rust-preventive oil is uniformly applied to the steel surface by the application method of the present invention.
【0030】なお、この発明の塗付方法は、水溶性塗料
の塗装装置にもそのまま適用することができる。また、
前述した実施例の予熱炉は、製造設備の乾燥炉等によっ
て兼ねることもできる。The coating method of the present invention can be applied to a water-soluble paint coating apparatus as it is. Also,
The preheating furnace of the above-described embodiment can also be used as a drying furnace of a manufacturing facility.
【0031】さらに、スプレーでの塗装,塗油は、高圧
に圧縮してスプレーチップ先端で膨張する際に温度が急
降下するために水分の蒸発が遅くなるが、鋼材の温度を
上げることによって、前記塗料,防錆油の温度降下の分
を補い、かつさらに水分の蒸発を促進できるために塗装
被膜,防錆被膜の形成が速い。Further, in the case of spray coating and oil coating, when the pressure is increased to a high pressure and expanded at the tip of the spray tip, the temperature rapidly drops, so that the evaporation of moisture is slowed down. The formation of the paint film and the rust-preventive film is fast because the temperature drop of the paint and the rust-preventive oil is compensated and the evaporation of the moisture can be further promoted.
【0032】また、余剰防錆油を除去する油切りについ
ては、塗料,防錆油等の防錆剤のみでなく、製造工程で
必要な冷却水の除去にもそのまま適用することができ
る。The oil drainer for removing excess rust preventive oil can be applied to not only rust preventives such as paints and rust preventive oils but also cooling water required in the manufacturing process.
【0033】[0033]
【発明の効果】水溶性防錆油の技術的ポイントは、水溶
性防錆油の半分以上(通常は70〜95%)を占める水分の
蒸発を、いかに短縮できるかであるが、この発明の塗付
方法によれば、防錆油の油性被膜の形成を速くすること
ができる。The technical point of the water-soluble rust-preventive oil is how to reduce the evaporation of water which accounts for more than half (usually 70 to 95%) of the water-soluble rust-preventive oil. According to the coating method, the formation of the oily film of the rust preventive oil can be accelerated.
【0034】即ち、常温であれば油性被膜の形成に2〜
5日かかるが、本方法によれば2〜3時間に短縮するこ
とができる。そのため、防錆性能を発揮するまでの時間
が短縮でき、油ダレが少ない。また、これらのことか
ら、製品(鋼材)を即出荷することができる。That is, at room temperature, formation of an oily film is 2 to
Although it takes 5 days, this method can reduce the time to 2-3 hours. Therefore, the time until the rust prevention performance is exhibited can be reduced, and the oil dripping is small. From these facts, the product (steel material) can be shipped immediately.
【0035】さらに、鋼材への防錆油塗付を薄く均一に
行うことができ、しかも余剰油を回収して再使用するこ
とができるために、従来の1/2 〜1/3 の原単位となって
コストが安く、かつ油だまり,油ダレがなくなるので製
品の保管,輸送に伴う汚れや環境汚染がなく、排物処理
も不要である。Furthermore, it is possible to perform with rust-preventive oil coating to the steel uniformly and thinly, yet in order that can be recovered and reused surplus oil, raw conventional 1/2 to 1/3 As a unit , the cost is low, and since there is no oil pool or oil dripping, there is no dirt or environmental pollution associated with product storage and transportation, and no waste disposal is required.
【0036】また、鋼材を加工後、付着している余剰防
錆油を除去する(脱脂)際にも、均一に除去できるの
で、脱脂時間を短縮することができ、脱脂後の塗装工程
においても、塗装品質を向上させることができる。In addition, even after removing the excess rust-preventive oil adhering to the steel material after working (degreasing), it can be uniformly removed, so that the degreasing time can be shortened and the coating process after the degreasing can be performed. , Can improve the coating quality.
【図1】この発明の鋼材への水溶性防錆油の塗付方法を
実施する塗付装置を示す概略図である。FIG. 1 is a schematic view showing a coating apparatus for performing a method for coating a steel material with a water-soluble rust-preventive oil according to the present invention.
【図2】この発明の塗付方法を実施する塗付装置におけ
る吹付け室を示す概略平面図である。FIG. 2 is a schematic plan view showing a spray chamber in a coating apparatus for performing the coating method of the present invention.
【図3】図2のB−B線概略断面図である。FIG. 3 is a schematic sectional view taken along line BB of FIG. 2;
【図4】図2のC−C線概略断面図である。FIG. 4 is a schematic sectional view taken along line CC of FIG. 2;
【図5】図2のD−D線概略断面図である。FIG. 5 is a schematic sectional view taken along line DD of FIG. 2;
【図6】この発明の塗付方法を実施する塗付装置の作動
制御状況を示すブロック図である。FIG. 6 is a block diagram showing an operation control state of a coating device that implements the coating method of the present invention.
【図7】この発明の塗付方法を実施する塗付装置におけ
る油切りノズルの支持部を示す概略図である。FIG. 7 is a schematic view showing a support portion of an oil draining nozzle in an application device for performing the application method of the present invention.
【図8】図7のE−E線矢視図である。8 is a view taken in the direction of the arrows EE in FIG. 7;
1…塗付装置、2…製造設備、3…鋼材、4…予熱炉、
5…吹付け室、6…回収部、7…スプレーガン、7a…ノ
ズル、8…塗付ブース、9…油切りノズル、10…油切り
ブース、11…集油ブース、12…回収ポンプ、13…供給タ
ンク、14…供給ポンプ、15…圧空供給部、16…支持部、
17…電磁弁、18…レベルセンサー、19…制御部、20…攪
拌機。DESCRIPTION OF SYMBOLS 1 ... Coating apparatus, 2 ... Manufacturing equipment, 3 ... Steel materials, 4 ... Preheating furnace,
5 spraying chamber, 6 collecting section, 7 spray gun, 7a nozzle, 8 coating booth, 9 oil drain nozzle, 10 oil drain booth, 11 oil collecting booth, 12 recovery pump, 13 ... supply tank, 14 ... supply pump, 15 ... compressed air supply part, 16 ... support part,
17 ... solenoid valve, 18 ... level sensor, 19 ... control unit, 20 ... stirrer.
───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.6 識別記号 庁内整理番号 FI 技術表示箇所 B05D 7/24 302 B05D 7/24 302Q ──────────────────────────────────────────────────続 き Continued on the front page (51) Int.Cl. 6 Identification code Agency reference number FI Technical display location B05D 7/24 302 B05D 7/24 302Q
Claims (1)
鋼等)の表面に、一時防錆を施すべく、水溶性防錆油を
塗付する時の塗付方法であり、 まず、鋼材の温度を30〜50℃に予熱すると共に、この鋼
材の表面に前記水溶性防錆油を15〜70kg/cm2の高圧下で
塗付し、 次に、この水溶性防錆油が塗付された鋼材の表面に、種
々の鋼材サイズに適応できる吹付け部により3kg/cm2以
上の圧空を吹付けて、余分に塗付した防錆油を除去する
と共に、鋼材表面への防錆油塗布量を均一にし、 また、前記圧空で除去した余剰防錆油を回収して再使用
することを特徴とする鋼材への水溶性防錆油の塗付方
法。1. A coating method for applying a water-soluble rust-preventive oil to a surface of a steel material (steel plate, steel pipe, shaped steel, etc.) immediately after manufacturing to temporarily provide rust prevention. While preheating the temperature to 30 to 50 ° C., the water-soluble rust-preventive oil is applied to the surface of the steel material under a high pressure of 15 to 70 kg / cm 2 , and then the water-soluble rust-preventive oil is applied. Compressed air of 3 kg / cm 2 or more is sprayed onto the surface of the steel material by a spraying part that can be adapted to various steel sizes to remove excess rust-preventive oil and apply rust-preventive oil to the steel surface A method for applying a water-soluble rust preventive oil to a steel material, wherein the amount is made uniform, and the excess rust preventive oil removed by the compressed air is collected and reused.