JP2651684B2 - Packaging cement mortar and its manufacturing method - Google Patents

Packaging cement mortar and its manufacturing method

Info

Publication number
JP2651684B2
JP2651684B2 JP62312585A JP31258587A JP2651684B2 JP 2651684 B2 JP2651684 B2 JP 2651684B2 JP 62312585 A JP62312585 A JP 62312585A JP 31258587 A JP31258587 A JP 31258587A JP 2651684 B2 JP2651684 B2 JP 2651684B2
Authority
JP
Japan
Prior art keywords
cement mortar
air
cement
packaging
mixture
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP62312585A
Other languages
Japanese (ja)
Other versions
JPH01152011A (en
Inventor
明光 相上
孝 下境
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
AIGAMI SANGYO JUGEN
Original Assignee
AIGAMI SANGYO JUGEN
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by AIGAMI SANGYO JUGEN filed Critical AIGAMI SANGYO JUGEN
Priority to JP62312585A priority Critical patent/JP2651684B2/en
Publication of JPH01152011A publication Critical patent/JPH01152011A/en
Application granted granted Critical
Publication of JP2651684B2 publication Critical patent/JP2651684B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】 (産業上の利用分野) この発明は、新規なセメントモルタルであって、特に
長期間に亘って硬化せずに保存することが出来るように
した包装セメントモルタル及びその製造法に関する。
Description: TECHNICAL FIELD The present invention relates to a novel cement mortar, and more particularly to a packaging cement mortar capable of being stored without hardening for a long period of time and its production. About the law.

(従来の技術) 従来、モルタルは石灰に砂と水を混ぜることにより構
成されており、また、該モルタルの強度を強くするため
に、該モルタルにセメントを混ぜることによりセメント
モルタルとして一般的に使用されている。
(Prior Art) Conventionally, mortar is generally formed by mixing sand and water with lime, and is generally used as cement mortar by mixing cement with the mortar in order to increase the strength of the mortar. Have been.

これらセメントモルタルは、建築現場等において使用
される場合には、施工後早急に硬化することが要求され
るため、従来、特開昭60−166249号に開示されるように
硬化促進剤をセメントモルタルに添加混合する技術が提
案されていた。
When these cement mortars are used at construction sites, etc., they are required to be hardened immediately after construction. Therefore, conventionally, a hardening accelerator is used as disclosed in JP-A-60-166249. A technique of adding and mixing the same has been proposed.

また、前述の如く、従来、セメントモルタルは施工後
早急に硬化することが常識と考えられていたため、長期
間に亘って未硬化状態を保つことは予想外の事項であっ
た。例えば工業用石膏プラスターに硬化遅延剤を含有さ
せた発明(特開昭52−40527号)が知られているが、そ
の遅延時間は1時間乃至3時間程度にすぎなかった。
Further, as described above, it has conventionally been considered that cement mortar hardens promptly after construction, and it is an unexpected matter to maintain an uncured state for a long period of time. For example, an invention in which a setting retarder is added to industrial gypsum plaster (Japanese Patent Application Laid-Open No. 5240527) is known, but the delay time is only about 1 to 3 hours.

(発明が解決しようとする課題) 前記従来のセメントモルタルは、建築現場等において
モルタルミキサー等により混練りしなければ使用するこ
とが出来ないので、現場作業による各種問題点があるの
みならず、そのために労力、時間を要し、作業効率が低
下するとともに、人件費も余分にかかるなどの問題点が
あった。
(Problems to be Solved by the Invention) The above-mentioned conventional cement mortar cannot be used unless kneaded with a mortar mixer or the like at a building site or the like. Labor and time are required, work efficiency is reduced, and labor costs are increased.

また、建築現場等においてモルタルミキサー等により
混練生成したセメントモルタルは、短時間の間に使用し
ないと硬化するため、必要量宛混練しなければならない
し、余分なものは廃棄しなければならないので、不経済
になる問題点があった。
Also, cement mortar produced by kneading with a mortar mixer etc. at a building site hardens if not used in a short time, so it has to be kneaded to the required amount, and excess must be discarded, There was a problem that became uneconomical.

さらに、屋根工事等において、屋根にセメントモルタ
ルを上げて使用する場合には、従来のようにモルタルミ
キサー等を現場に置き、セメントモルタルを混練したも
のを、使用の度に屋根の上まで上げなければならず、使
用上不便であり、合理性を欠くという問題点があった。
In addition, when using cement mortar on the roof in roof construction, etc., place a mortar mixer etc. on the site as before and knead the cement mortar and raise it to the top of the roof each time it is used. This is inconvenient to use and lacks rationality.

(課題を解決するための手段) この発明は、セメントモルタル組成物に空気に触れて
硬化遅延の効果が減衰する硬化遅延剤と水を添加混練し
て得たセメントモルタルの適量を袋内に密封することに
より、前記従来の問題点を悉く解決したのである。
(Means for Solving the Problems) The present invention seals an appropriate amount of a cement mortar obtained by adding and kneading a cement mortar composition with water and a curing retarder whose curing retarding effect is attenuated by exposure to air. By doing so, all of the above-mentioned conventional problems have been solved.

即ちこの発明は石灰、砂、セメントを混合したセメン
トモルタル組成物と、空気に接触すると硬化遅延の硬化
が減衰するようなポリオール複合体を主成分とする硬化
遅延剤と水との混練物を、不通気性袋で密封したことを
特徴とする包装セメントモルタルである。また他の発明
は石灰、砂、セメントを混合してなるセメントモルタル
組成物に、空気と接触することにより硬化遅延の硬化が
減衰するようなポリオール複合体を主成分とする硬化遅
延剤と水とを混合し、均一に混練した後、不通気性袋に
入れて密封することを特徴とした包装セメントモルタル
の製造法である。
That is, the present invention provides a kneaded product of water and a cement mortar composition obtained by mixing lime, sand, and cement, and a curing retarder containing a polyol complex as a main component such that the curing of the curing retardation is attenuated when contacted with air. This is a packaging cement mortar sealed with an air-impermeable bag. Another invention is a lime, sand, cement mortar composition obtained by mixing cement, a curing retarder containing a polyol complex as a main component such that the curing of the curing retardation is attenuated by contact with air, and water. Is mixed, uniformly kneaded, and then put in an air-impermeable bag and sealed, thereby producing a packaging cement mortar.

前記におけるセメントモルタルの各成分の量は通常使
用されているものと同一である。
The amounts of the respective components of the cement mortar in the above are the same as those usually used.

(作用) この発明においては、セメントモルタル組成物に硬化
遅延剤と水とを添加混練し、該セメントモルタルを不通
気性袋内に密封しているため、長期間保存しても混練時
の状態を保っている。また、使用時に開封すると、混練
直後の状態と同一であるため、一定時間後硬化し、普通
のセメントモルタルと同一の作用がある。
(Action) In the present invention, the cement mortar composition is kneaded with a setting retarder and water, and the cement mortar is sealed in an air-impermeable bag. Is kept. Further, when opened at the time of use, since it is the same as the state immediately after kneading, it is hardened after a certain period of time, and has the same action as ordinary cement mortar.

(実 施 例) 以下、この発明の実施例を詳細に説明する。(Examples) Hereinafter, examples of the present invention will be described in detail.

まず、モルタルミキサーの中で石灰500Kg、砂4000K
g、セメント40Kgを混合してなるセメントモルタル組成
物に、後記する硬化遅延剤12.5リットルと水350リット
ルを混入し、所定時間混練して、セメントモルタル490
2.5Kgを得た。
First, 500Kg lime and 4000K sand in a mortar mixer
g, a cement mortar composition obtained by mixing 40 kg of cement, 12.5 liters of a hardening retarder described later and 350 liters of water are mixed and kneaded for a predetermined time, and cement mortar 490
2.5 kg was obtained.

そこで、厚手の塩化ビニール袋に前記セメントモルタ
ルを50Kg宛充填し、口部を熱シールすれば、本発明の包
装セメントモルタルができる。
Then, a thick vinyl chloride bag is filled with the cement mortar in an amount of 50 kg, and the mouth portion is heat-sealed to obtain the packaging cement mortar of the present invention.

前記において使用する硬化遅延剤としては、ポリオー
ル複合体を主成分としたポゾリスNo.100(日曹マスター
ビルダーズ株式会社製造)を使用する。
As the curing retarder used in the above, Pozoris No. 100 (manufactured by Nisso Master Builders Co., Ltd.) containing a polyol complex as a main component is used.

前記硬化遅延剤の混入割合としては、セメントモルタ
ル100Kg当り200〜330ccの混入割合とする。
The mixing ratio of the hardening retardant is set to 200 to 330 cc per 100 kg of cement mortar.

尚、上記のように構成された包装セメントモルタルを
使用する場合には、該セメントモルタルが充填された不
通気性袋を開封するので、セメントモルタルは、外気と
接触することにより硬化遅延剤の効果が減衰し、通常の
セメントモルタルと同様になる。
Incidentally, when using the packaging cement mortar configured as described above, since the air-impermeable bag filled with the cement mortar is opened, the cement mortar is brought into contact with the outside air, and the effect of the setting retarder is obtained. Is attenuated and becomes similar to ordinary cement mortar.

この発明の包装セメントモルタルは、約1ヵ月間、そ
の品質を維持することが認められる。即ち、製造後1ヶ
月経過した本実施例にかかわる包装セメントモルタルを
開封し、屋根工事に使用したところ、通常のセメントモ
ルタルと同等の効果が認められた。
It is recognized that the packaging cement mortar of the present invention maintains its quality for about one month. That is, when the packaging cement mortar according to the present example, which had been manufactured for one month, was opened and used for roofing work, the same effect as that of ordinary cement mortar was recognized.

上記実施例において、硬化遅延剤として、ポリオール
複合体を主成分としたポゾリスNo.100(日曹マスタービ
ルダーズ株式会社製造)を使用しているが、要は空気と
接触することにより硬化遅延の効果が減衰する性質を有
する薬剤ならば、使用できるので、前記ポリオール複合
体を主成分とする薬剤に類似のものは使用することがで
きる。
In the above example, Pozoris No. 100 (manufactured by Nisso Master Builders Co., Ltd.) containing a polyol complex as a main component is used as a curing retarder. Any drug having a property of attenuating can be used, and therefore, a drug similar to the drug containing the polyol complex as a main component can be used.

また、前記実施例においては、モルタルミキサーの中
で石灰、砂、セメントを混合してなるセメントモルタル
組成物に、前記硬化遅延剤と水を混入し、所定時間練り
上げた後、厚手のビニール袋に充填したが、この発明の
包装袋は厚手のビニール袋に限定されるものでなく、強
靱な不通気性袋ならば使用することができる。
Further, in the above embodiment, in a mortar mixer, lime, sand, a cement mortar composition obtained by mixing cement, the curing retarder and water were mixed, kneaded for a predetermined time, and then put in a thick plastic bag. Although filled, the packaging bag of the present invention is not limited to a thick plastic bag, and any tough, impermeable bag can be used.

(発明の効果) この発明はあらかじめ製造したセメントモルタルが不
通気性袋に充填されているため、建築現場等においてセ
メントモルタルを練る作業を行う必要がなくなり、この
分、手間を省くことができるので、人件費を削減するこ
とができるとともに、作業効率を高めることができる。
従って、工期を短縮するとともに、建築コストを低減す
ることができる効果がある。
(Effect of the Invention) In the present invention, since the cement mortar manufactured in advance is filled in the air-impermeable bag, it is not necessary to perform the work of kneading the cement mortar at a building site or the like, and the labor can be saved by that much. In addition, labor costs can be reduced and work efficiency can be increased.
Therefore, there is an effect that the construction period can be shortened and the construction cost can be reduced.

また、使用する予定のセメントモルタルの分量だけ使
用の都度開封すればよいため、経済的にセメントモルタ
ルを使用することができるとともに、残留分は、前記不
通気性袋に入れて密封すれば、次の日に使用出来るなど
の効果がある。
In addition, since it is only necessary to open each time the amount of cement mortar to be used is opened, the cement mortar can be used economically, and the remaining portion can be put in the air-impermeable bag and sealed. It has the effect that it can be used on a day.

また、セメントモルタルを混練した状態で長期間保存
することが出来るため(例えば30日以上)、事務所等に
包装セメントモルタルを常時保管しておき、必要に応じ
て建築現場に持っていくことができるので、準備作業効
率を高めることができるなどの効果がある。
In addition, since cement mortar can be stored for a long period of time in a kneaded state (for example, 30 days or more), it is always possible to keep the packing cement mortar in an office or the like and take it to a construction site as needed. Since it is possible, the preparatory work efficiency can be improved.

また、屋根工事等において、屋根にセメントモルタル
を上げて使用する場合、包装セメントモルタルをそのま
ま屋根の上に上げることにより、その場で必要な量だけ
使用し残余は密封して後に使用することができるので、
取扱い及び使い勝手を向上させることができる効果もあ
る。
In addition, when using cement mortar on the roof in roof construction, etc., raise the packaging mortar on the roof as it is, so that only the necessary amount can be used on the spot and the remainder can be sealed and used later. So you can
There is also an effect that handling and usability can be improved.

───────────────────────────────────────────────────── フロントページの続き (56)参考文献 特開 昭59−223261(JP,A) 特開 昭53−81517(JP,A) 特開 昭61−1793(JP,A) 特開 昭57−187044(JP,A) 特開 昭56−81779(JP,A) 「材料」第16巻第167号P.615〜619、 昭和42年8月15日、社団法人日本材料学 会発行 ──────────────────────────────────────────────────続 き Continuation of the front page (56) References JP-A-59-223261 (JP, A) JP-A-53-81517 (JP, A) JP-A-61-1793 (JP, A) JP-A-57-223 187044 (JP, A) JP-A-56-81779 (JP, A) "Materials", Vol. 16, No. 167, p. 615-619, issued by Japan Society of Materials Science on August 15, 1967

Claims (2)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】石灰、砂、セメントを混合したセメントモ
ルタル組成物と、空気に接触すると硬化遅延の効果が減
衰するようなポリオール複合体を主成分とする硬化遅延
剤と水との混練物を、不通気性袋で密封したことを特徴
とする包装セメントモルタル。
1. A kneaded product of a cement mortar composition containing a mixture of lime, sand, and cement, a setting retarder containing a polyol complex as a main component such that the effect of setting delay is attenuated by contact with air, and water. A packaging cement mortar, which is sealed with an air-impermeable bag.
【請求項2】石灰、砂、セメントを混合してなるセメン
トモルタル組成物に、空気と接触することにより硬化遅
延の効果が減衰するようなポリオール複合体を主成分と
する硬化遅延剤と水とを混合し、均一に混練した後、不
通気性袋に入れて密封することを特徴とした包装セメン
トモルタルの製造法。
2. A cement mortar composition comprising a mixture of lime, sand and cement, a curing retarder mainly composed of a polyol complex whose contact retarding effect is reduced by contact with air, and water. A method for producing a packaging cement mortar, comprising mixing, uniformly kneading, and then placing the mixture in an air-impermeable bag and sealing the mixture.
JP62312585A 1987-12-10 1987-12-10 Packaging cement mortar and its manufacturing method Expired - Fee Related JP2651684B2 (en)