JP2009036817A - Antireflective coating, and polarizing plate and image display device using the same - Google Patents

Antireflective coating, and polarizing plate and image display device using the same Download PDF

Info

Publication number
JP2009036817A
JP2009036817A JP2007198716A JP2007198716A JP2009036817A JP 2009036817 A JP2009036817 A JP 2009036817A JP 2007198716 A JP2007198716 A JP 2007198716A JP 2007198716 A JP2007198716 A JP 2007198716A JP 2009036817 A JP2009036817 A JP 2009036817A
Authority
JP
Japan
Prior art keywords
acid
film
layer
mass
refractive index
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2007198716A
Other languages
Japanese (ja)
Inventor
Toshiyuki Ikeda
俊之 池田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Konica Minolta Opto Inc
Original Assignee
Konica Minolta Opto Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Konica Minolta Opto Inc filed Critical Konica Minolta Opto Inc
Priority to JP2007198716A priority Critical patent/JP2009036817A/en
Publication of JP2009036817A publication Critical patent/JP2009036817A/en
Pending legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To provide: an antireflective coating improved in antistatic property, transparency, tinting resistance, adhesion, and durability against high temperature and high humidity and excellent also in productivity; and a polarizing plate and a display device using the antireflective coating and excellent in visibility. <P>SOLUTION: The antireflective coating comprises the followings sequentially provided by coating on a transparent film substrate directly or through another layer: a conductive layer; and a low refractive index layer having a lower refractive index than the substrate. The conductive layer comprises a π-conjugated conductive polymer and an ionizing radiation curing resin. <P>COPYRIGHT: (C)2009,JPO&INPIT

Description

本発明は、反射防止フィルム、それを用いた偏光板、及び画像表示装置に関するものである。   The present invention relates to an antireflection film, a polarizing plate using the same, and an image display device.

一般に、反射防止フィルムは、陰極管表示装置(CRT)、プラズマディスプレイ(PDP)、エレクトロルミネッセンスディスプレイ(ELD)や液晶表示装置(LCD)のような画像表示装置において、外光の反射によるコントラスト低下や像の映り込みを防止するために、多層薄膜の光干渉によって、反射率を低減する機能を有しており、ディスプレイの最表面に配置される。   In general, an antireflection film is used in an image display device such as a cathode ray tube display device (CRT), a plasma display (PDP), an electroluminescence display (ELD), or a liquid crystal display device (LCD). In order to prevent the reflection of an image, it has a function of reducing the reflectance by optical interference of the multilayer thin film, and is disposed on the outermost surface of the display.

一般的に、反射防止は、透明基材上に直接、または他の層を介して、下層よりも屈折率の低い低屈折率層を形成することで行われている。また、光学物品の表面に傷が付くと、ひいては表示パネルの視認性を悪くするため、反射防止フィルムにハード性能を付与することが行われている。さらに、プラスチックからなる光学物品は絶縁性であるために、静電気等により帯電し、表面にほこり等が付着することにより、表示パネルの視認性が悪くなることを防ぐために、帯電防止性能を付与することが求められている。   In general, antireflection is performed by forming a low refractive index layer having a refractive index lower than that of the lower layer directly on a transparent substrate or via another layer. In addition, when the surface of the optical article is damaged, in order to deteriorate the visibility of the display panel, hard performance is imparted to the antireflection film. Furthermore, since the optical article made of plastic is insulative, it is charged with static electricity or the like, and anti-static performance is imparted to prevent the visibility of the display panel from being deteriorated due to dust adhering to the surface. It is demanded.

特許文献1及び特許文献2には、これらのハード性能及び帯電防止性能を付与する方法として、透明フィルム基材上にハードコート層を形成し、その上に金属酸化物を含有させた帯電防止層を形成し、さらにその上に下層よりも屈折率の低い低屈折率層を形成して、反射防止フィルムを作製する方法が記載されている。   In Patent Document 1 and Patent Document 2, as a method for imparting these hard performance and antistatic performance, an antistatic layer in which a hard coat layer is formed on a transparent film substrate and a metal oxide is contained thereon. And a method of producing an antireflection film by forming a low refractive index layer having a lower refractive index than that of the lower layer thereon.

しかしながら、導電性を有する金属酸化物によって帯電防止層を形成すると、透明性が損なわれやすくなるという難点があった。また、導電性を有する金属酸化物は屈折率が高いものが多く、反射防止フィルムの層構成によっては反射スペクトルがV字形状になり、可視光領域において短波長域や長波長域の反射率が高くなることで反射防止フィルムに色味が発生しやすくなるという問題点があった。   However, when the antistatic layer is formed of a conductive metal oxide, there is a problem that transparency is easily impaired. In addition, many conductive metal oxides have a high refractive index, and depending on the layer structure of the antireflection film, the reflection spectrum becomes V-shaped, and the reflectance in the short wavelength region and the long wavelength region in the visible light region is high. There was a problem that it becomes easy to generate color in an antireflection film by becoming high.

また、透明性を確保するために帯電防止剤として界面活性剤を用いることも出来るが、この場合にはイオン導電性のために湿度の影響を受けやすく、安定した帯電防止性能を得ることが困難になる。   In order to ensure transparency, a surfactant can be used as an antistatic agent, but in this case, it is easily affected by humidity due to ionic conductivity, and it is difficult to obtain a stable antistatic performance. become.

特許文献3には、上記の問題を解決するために、π共役系導電性ポリマーであるポリチオフェンの誘導体を用いて帯電防止層を形成する方法が示されているが、気相反応によって形成するために大掛かりな設備が必要になることや、処理時間が長くかかるために生産性が悪く、大量生産に適さないと言う欠点があった。また、この方法では帯電防止層にバインダー成分を有さないため、帯電防止層と接する層との密着性が十分でなく、高温高湿といった環境変化に対する耐久性に劣るという問題もあった。
特開2002−267804号公報 特開2006−35624号公報 特開2005−114852号公報
Patent Document 3 discloses a method of forming an antistatic layer using a derivative of polythiophene, which is a π-conjugated conductive polymer, in order to solve the above problem. However, there is a drawback that a large-scale facility is required and the processing time is long, so that productivity is poor and it is not suitable for mass production. Further, in this method, since the antistatic layer does not have a binder component, there is a problem that the adhesion to the layer in contact with the antistatic layer is not sufficient and the durability against environmental changes such as high temperature and high humidity is poor.
JP 2002-267804 A JP 2006-35624 A JP 2005-114852 A

本発明は上記の事情に鑑みてなされたものであり、帯電防止性や透明性、色付き、密着性、及び高温高湿に対する耐久性が改善され、生産性にも優れた反射防止フィルム、該反射防止フィルムを用いた視認性に優れた偏光板、及び表示装置を提供することを目的とする。   The present invention has been made in view of the above circumstances, and an antireflection film having improved antistatic properties, transparency, coloring, adhesion, durability against high temperature and high humidity, and excellent productivity, and the reflection It aims at providing the polarizing plate excellent in visibility using a prevention film, and a display apparatus.

本発明の上記課題は以下の構成により達成される。   The above object of the present invention is achieved by the following configurations.

1.
透明フィルム基材上に、導電層と、基材よりも屈折率の低い低屈折率層が、直接または他の層を介してこの順に塗設された反射防止フィルムであって、前記導電層がπ共役系導電性ポリマーと電離放射線硬化型樹脂を含有することを特徴とする反射防止フィルム。
1.
An antireflection film in which a conductive layer and a low refractive index layer having a refractive index lower than that of the base material are coated on the transparent film base material in this order directly or via another layer, and the conductive layer is An antireflection film comprising a π-conjugated conductive polymer and an ionizing radiation curable resin.

2.
前記π共役系導電性ポリマーが、ポリチオフェン誘導体、ポリピロール誘導体、ポリアニリン誘導体、ポリアセチレン誘導体のうちの、少なくとも1種であることを特徴とする1に記載の反射防止フィルム。
2.
2. The antireflection film according to 1, wherein the π-conjugated conductive polymer is at least one of a polythiophene derivative, a polypyrrole derivative, a polyaniline derivative, and a polyacetylene derivative.

3.
前記電離放射線硬化型樹脂が、分子中に重合可能な不飽和結合を2個以上有するアクリル系化合物を含有することを特徴とする1又は2に記載の反射防止フィルム。
3.
3. The antireflection film according to 1 or 2, wherein the ionizing radiation curable resin contains an acrylic compound having two or more polymerizable unsaturated bonds in the molecule.

4.
前記導電層が、下記一般式(1)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物を含有することを特徴とする1乃至3の何れか1項に記載の反射防止フィルム。
4).
4. The antireflection film as described in any one of 1 to 3, wherein the conductive layer contains an organosilicon compound represented by the following general formula (1), a hydrolyzate thereof, or a polycondensate thereof. .

1 nSiX1 4-n (1)
式中、R1は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X1は水酸基または加水分解可能な置換基であり、nは1〜3の整数である。
R 1 n SiX 1 4-n (1)
In the formula, R 1 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 1 is a hydroxyl group or a hydrolyzable substituent, and n is an integer of 1 to 3.

5.
前記低屈折率層が、コロイダルシリカ、フッ化マグネシウム、及び外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子よりなる群の中から選ばれた少なくとも1種の無機粒子を含有することを特徴とする1乃至4の何れか1項に記載の反射防止フィルム。
5).
At least one inorganic particle selected from the group consisting of hollow silica-based particles in which the low refractive index layer has colloidal silica, magnesium fluoride, and an outer shell layer, and the inside is porous or hollow. 5. The antireflection film according to any one of 1 to 4, which is contained.

6.
外殻層を有しかつ内部が多孔質または空洞である前記中空シリカ系粒子が、導電性金属酸化物被覆層を有することを特徴とする、5に記載の反射防止フィルム。
6).
6. The antireflection film according to 5, wherein the hollow silica-based particles having an outer shell layer and having a porous or hollow interior have a conductive metal oxide coating layer.

7.
前記導電性金属酸化物被覆層が、酸化アンチモン化合物からなることを特徴とする6に記載の反射防止フィルム。
7).
7. The antireflection film according to 6, wherein the conductive metal oxide coating layer is made of an antimony oxide compound.

8.
前記低屈折率層が、下記一般式(2)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物と、外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子とを含有することを特徴とする、1乃至7の何れか1項に記載の反射防止フィルム。
8).
A hollow silica system in which the low refractive index layer has an organosilicon compound represented by the following general formula (2) or a hydrolyzate or polycondensate thereof, and an outer shell layer and is porous or hollow inside The antireflection film according to any one of 1 to 7, wherein the antireflection film comprises particles.

2 mSiX2 4-m (2)
式中、R2は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X2は水酸基または加水分解可能な置換基であり、mは0〜3の整数である。
R 2 m SiX 2 4-m (2)
In the formula, R 2 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 2 is a hydroxyl group or a hydrolyzable substituent, and m is an integer of 0 to 3.

9.
前記低屈折率層が、バインダーとの反応性を有する基を少なくとも1つ含むシリコーン化合物を含有することを特徴とする1乃至8の何れか1項に記載の反射防止フィルム。
9.
9. The antireflection film as described in any one of 1 to 8, wherein the low refractive index layer contains a silicone compound containing at least one group having reactivity with a binder.

10.
1乃至9の何れか1項に記載の反射防止フィルムを一方の面に用いることを特徴とする偏光板。
10.
A polarizing plate comprising the antireflection film according to any one of 1 to 9 on one surface.

11.
1乃至9の何れか1項に記載の反射防止フィルム又は10に記載の偏光板を用いることを特徴とする画像表示装置。
11.
10. An image display device comprising the antireflection film according to any one of 1 to 9 or the polarizing plate according to 10.

本発明によれば、透明フィルム基材上に、導電層と、基材よりも屈折率の低い低屈折率層が、直接または他の層を介してこの順に塗設された反射防止フィルムであって、導電層がπ共役系導電性ポリマーと電離放射線硬化型樹脂を含有するものである。このような構成にすることによって、帯電防止性や透明性、色付き、密着性、及び高温高湿に対する耐久性が改善され、生産性にも優れた反射防止フィルム、及び該反射防止フィルムを用いた偏光板、及び画像形成装置を提供することができる。   According to the present invention, there is provided an antireflection film in which a conductive layer and a low refractive index layer having a refractive index lower than that of the base material are applied in this order directly or via another layer on the transparent film base material. The conductive layer contains a π-conjugated conductive polymer and an ionizing radiation curable resin. By adopting such a configuration, the antistatic property, transparency, coloring, adhesion, and durability against high temperature and high humidity were improved, and the antireflection film excellent in productivity and the antireflection film were used. A polarizing plate and an image forming apparatus can be provided.

つぎに、本発明の実施の形態を説明するが、本発明はこれらに限定されるものではない。   Next, embodiments of the present invention will be described, but the present invention is not limited thereto.

また、本文中、「(メタ)アクリレート」との記載は、「メタクリレートもしくはアクリレート」のことを示す。   Further, in the text, the description “(meth) acrylate” means “methacrylate or acrylate”.

本発明による反射防止フィルムにおいて、導電層と低屈折率層は透明フィルム基材上に塗設されたものであり、導電層はπ共役系導電性ポリマーと電離放射線硬化型樹脂を含有するものである。   In the antireflection film according to the present invention, the conductive layer and the low refractive index layer are coated on a transparent film substrate, and the conductive layer contains a π-conjugated conductive polymer and an ionizing radiation curable resin. is there.

本発明による反射防止フィルムでは、π共役系導電性ポリマーが、ポリチオフェン誘導体、ポリピロール誘導体、ポリアニリン誘導体、ポリアセチレン誘導体のうちの、少なくとも1種であることが好ましい。   In the antireflection film according to the present invention, the π-conjugated conductive polymer is preferably at least one of a polythiophene derivative, a polypyrrole derivative, a polyaniline derivative, and a polyacetylene derivative.

また、本発明による反射防止フィルムでは、電離放射線硬化型樹脂が、分子中に重合可能な不飽和結合を2個以上有するアクリル系化合物を含有することが好ましい。   In the antireflection film according to the present invention, the ionizing radiation curable resin preferably contains an acrylic compound having two or more polymerizable unsaturated bonds in the molecule.

さらに、本発明による反射防止フィルムでは、導電層が、下記一般式(1)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物を含有することが好ましい。   Furthermore, in the antireflection film according to the present invention, the conductive layer preferably contains an organosilicon compound represented by the following general formula (1), a hydrolyzate thereof, or a polycondensate thereof.

1 nSiX1 4-n (1)
式中、R1は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X1は水酸基または加水分解可能な置換基であり、nは1〜3の整数である。
R 1 n SiX 1 4-n (1)
In the formula, R 1 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 1 is a hydroxyl group or a hydrolyzable substituent, and n is an integer of 1 to 3.

本発明による反射防止フィルムでは、低屈折率層が、コロイダルシリカ、フッ化マグネシウム、及び外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子よりなる群の中から選ばれた少なくとも1種の無機粒子を含有することが好ましい。   In the antireflection film according to the present invention, the low refractive index layer is selected from the group consisting of colloidal silica, magnesium fluoride, and hollow silica-based particles having an outer shell layer and porous or hollow inside. It is preferable to contain at least one inorganic particle.

また、本発明による反射防止フィルムでは、外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子が、導電性金属酸化物被覆層を有するものであることが好ましい。   In the antireflection film according to the present invention, it is preferable that the hollow silica-based particles having an outer shell layer and porous or hollow inside have an electroconductive metal oxide coating layer.

さらに、本発明における反射防止フィルムでは、導電性金属酸化物被覆層が、酸化アンチモン化合物からなるものであることが好ましい。   Furthermore, in the antireflection film of the present invention, the conductive metal oxide coating layer is preferably made of an antimony oxide compound.

本発明による反射防止フィルムでは、低屈折率層が、下記一般式(2)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物と、外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子とを含有することが好ましい。   In the antireflection film according to the present invention, the low refractive index layer has an organosilicon compound represented by the following general formula (2) or a hydrolyzate or polycondensate thereof, and an outer shell layer, and the inside is porous. Or it is preferable to contain the hollow silica particle which is a cavity.

2 mSiX2 4-m (2)
式中、R2は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X2は水酸基または加水分解可能な置換基であり、mは0〜3の整数である。
R 2 m SiX 2 4-m (2)
In the formula, R 2 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 2 is a hydroxyl group or a hydrolyzable substituent, and m is an integer of 0 to 3.

また、本発明による反射防止フィルムでは、低屈折率層が、バインダーとの反応性を有する基を少なくとも1つ含むシリコーン化合物を含有することが好ましい。   In the antireflection film according to the present invention, the low refractive index layer preferably contains a silicone compound containing at least one group having reactivity with the binder.

つぎに、導電層について説明する。
(導電層)
本発明の導電層は帯電防止層として機能する。コーティングによって形成される導電層は、導電性ポリマーから形成することが出来る。また、反射防止フィルムの色付きを抑制するために好ましい導電層の屈折率としては、波長550nm測定で、1.45〜1.60の範囲であることが好ましい。
Next, the conductive layer will be described.
(Conductive layer)
The conductive layer of the present invention functions as an antistatic layer. The conductive layer formed by coating can be formed from a conductive polymer. Moreover, as a preferable refractive index of a conductive layer in order to suppress coloring of an antireflection film, it is preferable that it is the range of 1.45-1.60 by wavelength 550nm measurement.

π共役系導電性ポリマーについて説明する。   The π-conjugated conductive polymer will be described.

本発明において使用する導電性ポリマーはπ共役系導電性高分子であり、主鎖がπ共役系で構成されている有機高分子であれば使用することができる。例えば、ポリチオフェン類、ポリピロール類、ポリアニリン類、ポリフェニレン類、ポリアセチレン類、ポリフェニレンビニレン類、ポリアセン類、ポリチオフェンビニレン類、及びこれらの共重合体が挙げられる。重合の容易さや安定性の点からは、ポリチオフェン類、ポリピロール類、ポリアニリン類、ポリアセチレン類が好ましい。   The conductive polymer used in the present invention is a π-conjugated conductive polymer, and any organic polymer whose main chain is composed of a π-conjugated system can be used. Examples thereof include polythiophenes, polypyrroles, polyanilines, polyphenylenes, polyacetylenes, polyphenylene vinylenes, polyacenes, polythiophene vinylenes, and copolymers thereof. From the viewpoint of ease of polymerization and stability, polythiophenes, polypyrroles, polyanilines, and polyacetylenes are preferable.

π共役系導電性ポリマーは、無置換のままでも十分な導電性やバインダ樹脂への溶解性が得られるが、導電性や溶解性をより高めるために、アルキル基、カルボキシ基、スルホ基、アルコキシ基、ヒドロキシ基、シアノ基等の官能基を導入してもよい。   π-conjugated conductive polymer can provide sufficient conductivity and solubility in binder resin even if it is not substituted. However, in order to further improve conductivity and solubility, alkyl group, carboxy group, sulfo group, alkoxy A functional group such as a group, a hydroxy group, or a cyano group may be introduced.

このようなπ共役系導電性ポリマーの具体例としては、ポリチオフェン、ポリ(3−メチルチオフェン)、ポリ(3−エチルチオフェン)、ポリ(3−プロピルチオフェン)、ポリ(3−ブチルチオフェン)、ポリ(3−ヘキシルチオフェン)、ポリ(3−オクチルチオフェン)、ポリ(3−デシルチオフェン)、ポリ(3−ドデシルチオフェン)、ポリ(3−ブロモチオフェン)、ポリ(3−クロロチオフェン)、ポリ(3−シアノチオフェン)、ポリ(3−フェニルチオフェン)、ポリ(3,4−ジメチルチオフェン)、ポリ(3,4−ジブチルチオフェン)、ポリ(3−ヒドロキシチオフェン)、ポリ(3−メトキシチオフェン)、ポリ(3−エトキシチオフェン)、ポリ(3−ブトキシチオフェン)、ポリ(3−ヘキシルオキシチオフェン)、ポリ(3−オクチルオキシチオフェン)、ポリ(3−デシルオキシチオフェン)、ポリ(3−ドデシルオキシチオフェン)、ポリ(3,4−ジヒドロキシチオフェン)、ポリ(3,4−ジメトキシチオフェン)、ポリ(3,4−ジエトキシチオフェン)、ポリ(3,4−ジプロポキシチオフェン)、ポリ(3,4−ジブトキシチオフェン)、ポリ(3,4−ジヘキシルオキシチオフェン)、ポリ(3,4−ジオクチルオキシチオフェン)、ポリ(3,4−ジデシルオキシチオフェン)、ポリ(3,4−ジドデシルオキシチオフェン)、ポリ(3,4−エチレンジオキシチオフェン)、ポリ(3,4−プロピレンジオキシチオフェン)、ポリ(3,4−ブテンジオキシチオフェン)、ポリ(3−メチル−4−メトキシチオフェン)、ポリ(3−メチル−4−エトキシチオフェン)、ポリ(3−カルボキシチオフェン)、ポリ(3−メチル−4−カルボキシチオフェン)、ポリ(3−メチル−4−カルボキシエチルチオフェン)、ポリ(3−メチル−4−カルボキシブチルチオフェン)、ポリピロール、ポリ(N−メチルピロール)、ポリ(3−メチルピロール)、ポリ(3−エチルピロール)、ポリ(3−N−プロピルピロール)、ポリ(3−ブチルピロール)、ポリ(3−オクチルピロール)、ポリ(3−デシルピロール)、ポリ(3−ドデシルピロール)、ポリ(3,4−ジメチルピロール)、ポリ(3,4−ジブチルピロール)、ポリ(3−カルボキシピロール)、ポリ(3−メチル−4−カルボキシピロール)、ポリ(3−メチル−4−カルボキシエチルピロール)、ポリ(3−メチル−4−カルボキシブチルピロール)、ポリ(3−ヒドロキシピロール)、ポリ(3−メトキシピロール)、ポリ(3−エトキシピロール)、ポリ(3−ブトキシピロール)、ポリ(3−ヘキシルオキシピロール)、ポリ(3−メチル−4−ヘキシルオキシピロール)、ポリアニリン、ポリ(2−メチルアニリン)、ポリ(3−イソブチルアニリン)、ポリ(2−アニリンスルホン酸)、ポリ(3−アニリンスルホン酸)、ポリフェニルアセチレン等が挙げられる。これらはそれぞれ単独でも良いし、2種からなる共重合体でも好適に用いることができる。   Specific examples of such π-conjugated conductive polymers include polythiophene, poly (3-methylthiophene), poly (3-ethylthiophene), poly (3-propylthiophene), poly (3-butylthiophene), poly (3-hexylthiophene), poly (3-octylthiophene), poly (3-decylthiophene), poly (3-dodecylthiophene), poly (3-bromothiophene), poly (3-chlorothiophene), poly (3 -Cyanothiophene), poly (3-phenylthiophene), poly (3,4-dimethylthiophene), poly (3,4-dibutylthiophene), poly (3-hydroxythiophene), poly (3-methoxythiophene), poly (3-ethoxythiophene), poly (3-butoxythiophene), poly (3-hexyloxythio) ), Poly (3-octyloxythiophene), poly (3-decyloxythiophene), poly (3-dodecyloxythiophene), poly (3,4-dihydroxythiophene), poly (3,4-dimethoxythiophene) , Poly (3,4-diethoxythiophene), poly (3,4-dipropoxythiophene), poly (3,4-dibutoxythiophene), poly (3,4-dihexyloxythiophene), poly (3,4 -Dioctyloxythiophene), poly (3,4-didecyloxythiophene), poly (3,4-didodecyloxythiophene), poly (3,4-ethylenedioxythiophene), poly (3,4-propylenedi) Oxythiophene), poly (3,4-butenedioxythiophene), poly (3-methyl-4-methoxythiophene), poly Li (3-methyl-4-ethoxythiophene), poly (3-carboxythiophene), poly (3-methyl-4-carboxythiophene), poly (3-methyl-4-carboxyethylthiophene), poly (3-methyl -4-carboxybutylthiophene), polypyrrole, poly (N-methylpyrrole), poly (3-methylpyrrole), poly (3-ethylpyrrole), poly (3-N-propylpyrrole), poly (3-butylpyrrole) ), Poly (3-octylpyrrole), poly (3-decylpyrrole), poly (3-dodecylpyrrole), poly (3,4-dimethylpyrrole), poly (3,4-dibutylpyrrole), poly (3- Carboxypyrrole), poly (3-methyl-4-carboxypyrrole), poly (3-methyl-4-carboxyethylpyrrole) Poly (3-methyl-4-carboxybutylpyrrole), poly (3-hydroxypyrrole), poly (3-methoxypyrrole), poly (3-ethoxypyrrole), poly (3-butoxypyrrole), poly (3-hexyl) Oxypyrrole), poly (3-methyl-4-hexyloxypyrrole), polyaniline, poly (2-methylaniline), poly (3-isobutylaniline), poly (2-anilinesulfonic acid), poly (3-anilinesulfone) Acid), polyphenylacetylene and the like. Each of these may be used alone or two types of copolymers can be suitably used.

これらのπ共役系導電性ポリマーには、ドーパント成分が添加されていても良い。ドーパント成分としては、例えば、ハロゲン類、ルイス酸、プロトン酸、遷移金属ハライドなどの低分子量ドーパントや、ポリアニオンのようなポリマー等が挙げられる。   A dopant component may be added to these π-conjugated conductive polymers. Examples of the dopant component include low molecular weight dopants such as halogens, Lewis acids, proton acids, transition metal halides, and polymers such as polyanions.

ポリアニオンとは、π共役系導電性ポリマーに対するドーパントとして機能するアニオン基を有する高分子であり、置換もしくは未置換のポリアルキレン、置換もしくは未置換のポリアルケニレン、置換もしくは未置換のポリイミド、置換もしくは未置換のポリアミド、置換もしくは未置換のポリエステル及びこれらの共重合体であって、アニオン基を有する構成単位とアニオン基を有さない構成単位からなるものである。   A polyanion is a polymer having an anionic group that functions as a dopant for a π-conjugated conductive polymer, and is a substituted or unsubstituted polyalkylene, a substituted or unsubstituted polyalkenylene, a substituted or unsubstituted polyimide, a substituted or unsubstituted Substituted polyamides, substituted or unsubstituted polyesters, and copolymers thereof, comprising a structural unit having an anionic group and a structural unit having no anionic group.

ポリアルキレンとは主鎖がメチレンの繰り返しで構成されているポリマーであり、例えば、ポリエチレン、ポリプロピレン、ポリブテン、ポリペンテン、ポリヘキセン、ポリビニルアルコール、ポリビニルフェノール、ポリアクリロニトリル、ポリアクリレート、ポリスチレン等が挙げられる。   Polyalkylene is a polymer whose main chain is composed of repeating methylene, and examples thereof include polyethylene, polypropylene, polybutene, polypentene, polyhexene, polyvinyl alcohol, polyvinylphenol, polyacrylonitrile, polyacrylate, polystyrene, and the like.

ポリアルケニレンとは主鎖に不飽和結合が1個以上含まれる構成単位からなるポリマーであり、例えば、プロペニレン、1−メチルプロペニレン、1−ブチルプロペニレン、1−デシルプロペニレン、1−シアノプロペニレン、1−フェニルプロペニレン、1−ヒドロキシプロペニレン、1−ブテニレン、1−メチル−1−ブテニレン、1−エチル−1−ブテニレン、1−オクチル−1−ブテニレン、2−メチル−1−ブテニレン、2−エチル−1−ブテニレン、2−ブチル−1−ブテニレン、2−ヘキシル−1−ブテニレン、2−オクチル−1−ブテニレン、2−デシル−1−ブテニレン、2−フェニル−1−ブテニレン、2−ブテニレン、1−メチル−2−ブテニレン、1−エチル−2−ブテニレン、1−オクチル−2−ブテニレン、2−メチル−2−ブテニレン、2−エチル−2−ブテニレン、2−ブチル−2−ブテニレン、2−ヘキシル−2−ブテニレン、2−オクチル−2−ブテニレン、2−デシル−2−ブテニレン、2−フェニル−2−ブテニレン、2−プロピレンフェニル−2−ブテニレン、2−ペンテニレン、4−エチル−2−ペンテニレン、4−プロピル−2−ペンテニレン、4−ブチル−2−ペンテニレン、4−ヘキシル−2−ペンテニレン、4−シアノ−2−ペンテニレン、3−メチル−2−ペンテニレン、3−フェニル−2−ペンテニレン、4−ヒドロキシ−2−ペンテニレン、ヘキセニレン等から選ばれる1種以上の構成単位を含む重合体が挙げられる。   Polyalkenylene is a polymer composed of structural units containing one or more unsaturated bonds in the main chain. For example, propenylene, 1-methylpropenylene, 1-butylpropenylene, 1-decylpropenylene, 1-cyanopropene. Nylene, 1-phenylpropenylene, 1-hydroxypropenylene, 1-butenylene, 1-methyl-1-butenylene, 1-ethyl-1-butenylene, 1-octyl-1-butenylene, 2-methyl-1-butenylene, 2-ethyl-1-butenylene, 2-butyl-1-butenylene, 2-hexyl-1-butenylene, 2-octyl-1-butenylene, 2-decyl-1-butenylene, 2-phenyl-1-butenylene, 2- Butenylene, 1-methyl-2-butenylene, 1-ethyl-2-butenylene, 1-octyl-2-butenylene, 2 Methyl-2-butenylene, 2-ethyl-2-butenylene, 2-butyl-2-butenylene, 2-hexyl-2-butenylene, 2-octyl-2-butenylene, 2-decyl-2-butenylene, 2-phenyl- 2-butenylene, 2-propylenephenyl-2-butenylene, 2-pentenylene, 4-ethyl-2-pentenylene, 4-propyl-2-pentenylene, 4-butyl-2-pentenylene, 4-hexyl-2-pentenylene, 4 Examples include polymers containing one or more structural units selected from -cyano-2-pentenylene, 3-methyl-2-pentenylene, 3-phenyl-2-pentenylene, 4-hydroxy-2-pentenylene, hexenylene, and the like.

ポリイミドとしてはピロメリット酸二無水物、ビフェニルテトラカルボン酸二無水物、ベンゾフェノンテトラカルボン酸二無水物、2,2’,3,3’−テトラカルボキシジフェニルエーテル二無水物、2,2’−[4,4’−ジ(ジカルボキシフェニルオキシ)フェニル]プロパン二無水物等の無水物と、オキシジアミン、パラフェニレンジアミン、メタフェニレンジアミン、ベンゾフェノンジアミン等のジアミンとからなるポリイミドが挙げられる。   As polyimide, pyromellitic dianhydride, biphenyltetracarboxylic dianhydride, benzophenonetetracarboxylic dianhydride, 2,2 ′, 3,3′-tetracarboxydiphenyl ether dianhydride, 2,2 ′-[4 , 4′-di (dicarboxyphenyloxy) phenyl] propane dianhydride and the like, and polyimides composed of diamines such as oxydiamine, paraphenylenediamine, metaphenylenediamine, and benzophenonediamine.

ポリアミドとしてはポリアミド6、ポリアミド6,6、ポリアミド6,10等が挙げられる。   Examples of the polyamide include polyamide 6, polyamide 6,6, polyamide 6,10 and the like.

ポリエステルとしてはポリエチレンテレフタレート、ポリブチレンテレフタレート等が挙げられる。   Examples of the polyester include polyethylene terephthalate and polybutylene terephthalate.

ポリアニオンのアニオン基としては、π共役系導電性ポリマーへの化学酸化ドープが起こりうる官能基であれば良いが、製造の容易さや安定性の観点から、一置換硫酸エステル基、一置換リン酸エステル基、リン酸基、カルボキシ基、スルホ基等が好ましい。さらに、官能基のπ共役系導電性ポリマーへのドープ効果の観点から、スルホ基、一置換硫酸エステル基、カルボキシ基がより好ましい。   The anion group of the polyanion may be a functional group that can undergo chemical oxidation doping to the π-conjugated conductive polymer, but from the viewpoint of ease of production and stability, a monosubstituted sulfate group and a monosubstituted phosphate ester Group, phosphoric acid group, carboxy group, sulfo group and the like are preferable. Furthermore, from the viewpoint of the doping effect of the functional group on the π-conjugated conductive polymer, a sulfo group, a monosubstituted sulfate group, and a carboxy group are more preferable.

ポリアニオンの具体例としては、ポリビニルスルホン酸、ポリスチレンスルホン酸、ポリアリルスルホン酸、ポリアクリル酸エチルスルホン酸、ポリアクリル酸ブチルスルホン酸、ポリ(2−アクリルアミド−2−メチルプロパンスルホン酸)、ポリイソプレンスルホン酸、ポリビニルカルボン酸、ポリスチレンカルボン酸、ポリアリルカルボン酸、ポリアクリルカルボン酸、ポリメタクリルカルボン酸、ポリ(2−アクリルアミド−2−メチルプロパンカルボン酸)、ポリイソプレンカルボン酸、ポリアクリル酸等が挙げられる。これらの単独重合体でも良く、2種以上の共重合体でも良い。これらのうち、ポリスチレンスルホン酸、ポリイソプレンスルホン酸、ポリアクリル酸エチルスルホン酸、ポリアクリル酸ブチルスルホン酸が好ましい。これらのポリアニオンは、バインダ樹脂との相溶性が高く、得られる導電層の導電性をより高めることができる。   Specific examples of polyanions include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacrylic acid ethyl sulfonic acid, polyacrylic acid butyl sulfonic acid, poly (2-acrylamido-2-methylpropane sulfonic acid), polyisoprene. Sulfonic acid, polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacryl carboxylic acid, polymethacryl carboxylic acid, poly (2-acrylamido-2-methylpropane carboxylic acid), polyisoprene carboxylic acid, polyacrylic acid, etc. Can be mentioned. These homopolymers may be used, or two or more types of copolymers may be used. Among these, polystyrene sulfonic acid, polyisoprene sulfonic acid, polyacrylic acid ethyl sulfonic acid, and polyacrylic acid butyl sulfonic acid are preferable. These polyanions have high compatibility with the binder resin, and can further increase the conductivity of the obtained conductive layer.

本発明においては、ポリアニオンの他にも、π共役系導電性ポリマーを酸化還元することができれば、以下のようなドナー性あるいはアクセプタ性のドーパントを用いることができる。   In the present invention, in addition to the polyanion, the following donor or acceptor dopant can be used as long as the π-conjugated conductive polymer can be oxidized and reduced.

ドナー性ドーパントとしては、ナトリウム、カリウム等のアルカリ金属、カルシウム、マグネシウム等のアルカリ土類金属、テトラメチルアンモニウム、テトラエチルアンモニウム、テトラプロピルアンモニウム、テトラブチルアンモニウム、メチルトリエチルアンモニウム、ジメチルジエチルアンモニウム等の4級アミン化合物等が挙げられる。   Donor dopants include alkali metals such as sodium and potassium, alkaline earth metals such as calcium and magnesium, quaternary compounds such as tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, methyltriethylammonium and dimethyldiethylammonium. An amine compound etc. are mentioned.

アクセプタ性ドーパントとしては、Cl2、Br2、I2、ICl、IBr、IF等のハロゲン化合物、PF5、AsF5、SbF5、BF5、BCl5、BBr5、SO3等のルイス酸、テトラシアノエチレン、テトラシアノエチレンオキサイド、テトラシアノベンゼン、ジクロロジシアノベンゾキノン、テトラシアノキノジメタン、テトラシアノアザナフタレン等の有機シアノ化合物、プロトン酸、有機金属化合物、フラーレン、水素化フラーレン、水酸化フラーレン、カルボン酸化フラーレン、スルホン酸化フラーレン等を使用できる。 Examples of the acceptor dopant include halogen compounds such as Cl 2 , Br 2 , I 2 , ICl, IBr, and IF, Lewis acids such as PF 5 , AsF 5 , SbF 5 , BF 5 , BCl 5 , BBr 5 , and SO 3 , Organic cyano compounds such as tetracyanoethylene, tetracyanoethylene oxide, tetracyanobenzene, dichlorodicyanobenzoquinone, tetracyanoquinodimethane, tetracyanoazanaphthalene, protonic acid, organometallic compound, fullerene, hydrogenated fullerene, fullerene hydroxide, Carboxy oxide fullerene, sulfonated fullerene and the like can be used.

プロトン酸としては無機酸、有機酸が挙げられる。無機酸としては、例えば塩酸、硫酸、硝酸、リン酸、フッ化水素酸、過塩素酸等が挙げられる。また、有機酸としては、有機カルボン酸、有機スルホン酸等が挙げられる。   Examples of the protonic acid include inorganic acids and organic acids. Examples of the inorganic acid include hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, hydrofluoric acid, perchloric acid and the like. Moreover, organic carboxylic acid, organic sulfonic acid, etc. are mentioned as an organic acid.

有機カルボン酸としては、脂肪族、芳香族、環状脂肪族等にカルボキシ基を1つまたは2つ以上を含むものを使用できる。例えば、ギ酸、酢酸、シュウ酸、安息香酸、フタル酸、マレイン酸、フマル酸、マロン酸、酒石酸、クエン酸、乳酸、コハク酸、モノクロロ酢酸、ジクロロ酢酸、トリクロロ酢酸、トリフルオロ酢酸、ニトロ酢酸、トリフェニル酢酸等が挙げられる。   As organic carboxylic acid, what contains 1 or 2 or more of carboxy groups in aliphatic, aromatic, cycloaliphatic, etc. can be used. For example, formic acid, acetic acid, oxalic acid, benzoic acid, phthalic acid, maleic acid, fumaric acid, malonic acid, tartaric acid, citric acid, lactic acid, succinic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoroacetic acid, nitroacetic acid, And triphenylacetic acid.

有機スルホン酸としては、脂肪族、芳香族、環状脂肪族等にスルホ基を1つまたは2つ以上含むもの、またはスルホ基を含む高分子を使用できる。   As the organic sulfonic acid, aliphatic, aromatic, cycloaliphatic or the like containing one or more sulfo groups or a polymer containing sulfo groups can be used.

スルホ基を1つ含むものとしては、例えば、メタンスルホン酸、エタンスルホン酸、1−プロパンスルホン酸、1−ブタンスルホン酸、1−ヘキサンスルホン酸、1−ヘプタンスルホン酸、1−オクタンスルホン酸、1−ノナンスルホン酸、1−デカンスルホン酸、1−ペンタデカンスルホン酸、2−ブロモエタンスルホン酸、3−クロロ−2−ヒドロキシプロパンスルホン酸、トリフルオロメタンスルホン酸、トリフルオロエタンスルホン酸、コリスチンメタンスルホン酸、2−アクリルアミド−2−メチルプロパンスルホン酸、アミノメタンスルホン酸、1−アミノ−2−ナフトール−4−スルホン酸、2−アミノ−5−ナフトール−7−スルホン酸、3−アミノプロパンスルホン酸、N−シクロヘキシル−3−アミノプロパンスルホン酸、ベンゼンスルホン酸、アルキルベンゼンスルホン酸、p−トルエンスルホン酸、キシレンスルホン酸、エチルベンゼンスルホン酸、プロピルベンゼンスルホン酸、ブチルベンゼンスルホン酸、ペンチルベンゼンスルホン酸、ヘキシルベンゼンスルホン酸、ヘプチルベンゼンスルホン酸、オクチルベンゼンスルホン酸、ノニルベンゼンスルホン酸、デシルベンゼンスルホン酸、ヘキサデシルベンゼンスルホン酸、2,4−ジメチルベンゼンスルホン酸、ジプロピルベンゼンスルホン酸、4−アミノベンゼンスルホン酸、o−アミノベンゼンスルホン酸、m−アミノベンゼンスルホン酸、4−アミノ−2−クロロトルエン−5−スルホン酸、4−アミノ−3−メチルベンゼン−1−スルホン酸、4−アミノ−5−メトキシ−2−メチルベンゼンスルホン酸、2−アミノ−5−メチルベンゼン−1−スルホン酸、4−アミノ−2−メチルベンゼン−1−スルホン酸、5−アミノ−2−メチルベンゼン−1−スルホン酸、4−アミノ−3−メチルベンゼン−1−スルホン酸、4−アセトアミド−3−クロロベンゼンスルホン酸、4−クロロ−3−ニトロベンゼンスルホン酸、p−クロロベンゼンスルホン酸、ナフタレンスルホン酸、メチルナフタレンスルホン酸、プロピルナフタレンスルホン酸、ブチルナフタレンスルホン酸、ペンチルナフタレンスルホン酸、4−アミノ−1−ナフタレンスルホン酸、8−クロロナフタレン−1−スルホン酸、ナフタレンスルホン酸ホルマリン重縮合物、メラミンスルホン酸ホルマリン重縮合物、アントラキノンスルホン酸、ピレンスルホン酸等が挙げられる。また、これらの金属塩も使用できる。   Examples of those containing one sulfo group include methanesulfonic acid, ethanesulfonic acid, 1-propanesulfonic acid, 1-butanesulfonic acid, 1-hexanesulfonic acid, 1-heptanesulfonic acid, 1-octanesulfonic acid, 1-nonanesulfonic acid, 1-decanesulfonic acid, 1-pentadecanesulfonic acid, 2-bromoethanesulfonic acid, 3-chloro-2-hydroxypropanesulfonic acid, trifluoromethanesulfonic acid, trifluoroethanesulfonic acid, colistin methanesulfone Acid, 2-acrylamido-2-methylpropanesulfonic acid, aminomethanesulfonic acid, 1-amino-2-naphthol-4-sulfonic acid, 2-amino-5-naphthol-7-sulfonic acid, 3-aminopropanesulfonic acid N-cyclohexyl-3-aminopropanesulfone Benzenesulfonic acid, alkylbenzenesulfonic acid, p-toluenesulfonic acid, xylenesulfonic acid, ethylbenzenesulfonic acid, propylbenzenesulfonic acid, butylbenzenesulfonic acid, pentylbenzenesulfonic acid, hexylbenzenesulfonic acid, heptylbenzenesulfonic acid, octylbenzene Sulfonic acid, nonylbenzenesulfonic acid, decylbenzenesulfonic acid, hexadecylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, dipropylbenzenesulfonic acid, 4-aminobenzenesulfonic acid, o-aminobenzenesulfonic acid, m- Aminobenzenesulfonic acid, 4-amino-2-chlorotoluene-5-sulfonic acid, 4-amino-3-methylbenzene-1-sulfonic acid, 4-amino-5-methoxy-2-methylbenze Sulfonic acid, 2-amino-5-methylbenzene-1-sulfonic acid, 4-amino-2-methylbenzene-1-sulfonic acid, 5-amino-2-methylbenzene-1-sulfonic acid, 4-amino-3 -Methylbenzene-1-sulfonic acid, 4-acetamido-3-chlorobenzenesulfonic acid, 4-chloro-3-nitrobenzenesulfonic acid, p-chlorobenzenesulfonic acid, naphthalenesulfonic acid, methylnaphthalenesulfonic acid, propylnaphthalenesulfonic acid, butyl Naphthalenesulfonic acid, pentylnaphthalenesulfonic acid, 4-amino-1-naphthalenesulfonic acid, 8-chloronaphthalene-1-sulfonic acid, naphthalenesulfonic acid formalin polycondensate, melaminesulfonic acid formalin polycondensate, anthraquinonesulfonic acid, pyrene Examples include sulfonic acid It is done. These metal salts can also be used.

スルホ基を2つ以上含むものとしては、例えば、エタンジスルホン酸、ブタンジスルホン酸、ペンタンジスルホン酸、デカンジスルホン酸、o−ベンゼンジスルホン酸、m−ベンゼンジスルホン酸、p−ベンゼンジスルホン酸、トルエンジスルホン酸、キシレンジスルホン酸、クロロベンゼンジスルホン酸、フルオロベンゼンジスルホン酸、ジメチルベンゼンジスルホン酸、ジエチルベンゼンジスルホン酸、アニリン−2,4−ジスルホン酸、アニリン−2,5−ジスルホン酸、3,4−ジヒドロキシ−1,3−ベンゼンジスルホン酸、ナフタレンジスルホン酸、メチルナフタレンジスルホン酸、エチルナフタレンジスルホン酸、ペンタデシルナフタレンジスルホン酸、3−アミノ−5−ヒドロキシ−2,7−ナフタレンジスルホン酸、1−アセトアミド−8−ヒドロキシ−3,6−ナフタレンジスルホン酸、2−アミノ−1,4−ベンゼンジスルホン酸、1−アミノ−3,8−ナフタレンジスルホン酸、3−アミノ−1,5−ナフタレンジスルホン酸、8−アミノ−1−ナフトール−3,6−ジスルホン酸、4−アミノ−5−ナフトール−2,7−ジスルホン酸、4−アセトアミド−4’−イソチオシアノトスチルベン−2,2’−ジスルホン酸、4−アセトアミド−4’−マレイミジルスチルベン−2,2’−ジスルホン酸、ナフタレントリスルホン酸、ジナフチルメタンジスルホン酸、アントラキノンジスルホン酸、アントラセンスルホン酸等が挙げられる。また、これらの金属塩も使用できる。   Examples of those containing two or more sulfo groups include ethanedisulfonic acid, butanedisulfonic acid, pentanedisulfonic acid, decanedisulfonic acid, o-benzenedisulfonic acid, m-benzenedisulfonic acid, p-benzenedisulfonic acid, and toluenedisulfonic acid. Xylene disulfonic acid, chlorobenzene disulfonic acid, fluorobenzene disulfonic acid, dimethylbenzene disulfonic acid, diethylbenzene disulfonic acid, aniline-2,4-disulfonic acid, aniline-2,5-disulfonic acid, 3,4-dihydroxy-1,3 Benzene disulfonic acid, naphthalene disulfonic acid, methyl naphthalene disulfonic acid, ethyl naphthalene disulfonic acid, pentadecyl naphthalene disulfonic acid, 3-amino-5-hydroxy-2,7-naphthalene disulfonic acid, 1- Cetamide-8-hydroxy-3,6-naphthalenedisulfonic acid, 2-amino-1,4-benzenedisulfonic acid, 1-amino-3,8-naphthalenedisulfonic acid, 3-amino-1,5-naphthalenedisulfonic acid, 8-amino-1-naphthol-3,6-disulfonic acid, 4-amino-5-naphthol-2,7-disulfonic acid, 4-acetamido-4′-isothiocyanotostilbene-2,2′-disulfonic acid, Examples include 4-acetamido-4′-maleimidyl stilbene-2,2′-disulfonic acid, naphthalene trisulfonic acid, dinaphthylmethane disulfonic acid, anthraquinone disulfonic acid, and anthracene sulfonic acid. These metal salts can also be used.

次に電離放射線硬化型樹脂について説明する。   Next, the ionizing radiation curable resin will be described.

本発明に係る導電層には、バインダーとして塗膜の製膜性や物理的特性、及び導電層への積層膜との密着性の向上のために電離放射線硬化型樹脂を含有させる。   The conductive layer according to the present invention contains an ionizing radiation curable resin as a binder in order to improve the film formability and physical characteristics of the coating film and the adhesion to the laminated film on the conductive layer.

電離放射線硬化型樹脂としては、紫外線や電子線のような電離放射線の照射により直接、または光重合開始剤の作用を受けて間接的に重合反応を生じる官能基を2個以上有するモノマーまたはオリゴマーを用いることができる。官能基としては(メタ)アクリロイルオキシ基等のような不飽和二重結合を有する基、エポキシ基、シラノール基等が挙げられる。中でも不飽和二重結合を2個以上有するラジカル重合性のモノマーやオリゴマーを好ましく用いることができる。必要に応じて光重合開始剤を組み合わせてもよい。   As the ionizing radiation curable resin, a monomer or oligomer having two or more functional groups that cause polymerization reaction directly by irradiation of ionizing radiation such as ultraviolet rays or electron beams or indirectly by the action of a photopolymerization initiator is used. Can be used. Examples of the functional group include a group having an unsaturated double bond such as a (meth) acryloyloxy group, an epoxy group, and a silanol group. Among these, radically polymerizable monomers and oligomers having two or more unsaturated double bonds can be preferably used. You may combine a photoinitiator as needed.

このような電離放射線硬化型樹脂としては、例えば多官能(メタ)アクリレート化合物等が挙げられ、ペンタエリスリトール多官能(メタ)アクリレート、ジペンタエリスリトール多官能(メタ)アクリレート等が好ましい。   Examples of such ionizing radiation curable resins include polyfunctional (meth) acrylate compounds, and pentaerythritol polyfunctional (meth) acrylate, dipentaerythritol polyfunctional (meth) acrylate, and the like are preferable.

多官能(メタ)アクリレート化合物としては、例えばエチレングリコールジ(メタ)アクリレート、ジエチレングリコールジ(メタ)アクリレート、1,6−ヘキサンジオールジ(メタ)アクリレート、ネオペンチルグリコールジ(メタ)アクリレート、トリメチロールプロパントリ(メタ)アクリレート、トリメチロールエタントリ(メタ)アクリレート、テトラメチロールメタントリ(メタ)アクリレート、テトラメチロールメタンテトラ(メタ)アクリレート、ペンタグリセロールトリ(メタ)アクリレート、ペンタエリスリトールジ(メタ)アクリレート、ペンタエリスリトールトリ(メタ)アクリレート、ペンタエリスリトールテトラ(メタ)アクリレート、グリセリントリ(メタ)アクリレート、ジペンタエリスリトールトリ(メタ)アクリレート、ジペンタエリスリトールテトラ(メタ)アクリレート、ジペンタエリスリトールペンタ(メタ)アクリレート、ジペンタエリスリトールヘキサ(メタ)アクリレート、トリス(アクリロイルオキシエチル)イソシアヌレート等が好ましく挙げられる。   Examples of the polyfunctional (meth) acrylate compound include ethylene glycol di (meth) acrylate, diethylene glycol di (meth) acrylate, 1,6-hexanediol di (meth) acrylate, neopentyl glycol di (meth) acrylate, and trimethylolpropane. Tri (meth) acrylate, trimethylolethane tri (meth) acrylate, tetramethylolmethane tri (meth) acrylate, tetramethylolmethane tetra (meth) acrylate, pentaglycerol tri (meth) acrylate, pentaerythritol di (meth) acrylate, penta Erythritol tri (meth) acrylate, pentaerythritol tetra (meth) acrylate, glycerin tri (meth) acrylate, dipentaerythritol tri ( Data) acrylate, dipentaerythritol tetra (meth) acrylate, dipentaerythritol penta (meth) acrylate, dipentaerythritol hexa (meth) acrylate, tris (acryloyloxyethyl) isocyanurate preferred.

これらの化合物は、それぞれ単独または2種以上を混合して用いられる。また、上記モノマーの2量体、3量体等のオリゴマーであってもよい。   These compounds are used alone or in admixture of two or more. Moreover, oligomers, such as a dimer and a trimer of the said monomer, may be sufficient.

電離放射線硬化型樹脂の硬化促進のために、光重合開始剤と分子中に重合可能な不飽和結合を2個以上有するアクリル系化合物とを、質量比で3:7〜1:9含有することが好ましい。   In order to accelerate curing of the ionizing radiation curable resin, a photopolymerization initiator and an acrylic compound having two or more polymerizable unsaturated bonds in the molecule are contained in a mass ratio of 3: 7 to 1: 9. Is preferred.

光重合開始剤としては、具体的には、アセトフェノン、ベンゾフェノン、ヒドロキシベンゾフェノン、ミヒラーケトン、α−アミロキシムエステル、チオキサントン等及びこれらの誘導体を挙げることができるが、特にこれらに限定されるものではない。   Specific examples of the photopolymerization initiator include acetophenone, benzophenone, hydroxybenzophenone, Michler's ketone, α-amyloxime ester, thioxanthone, and derivatives thereof, but are not particularly limited thereto.

また、本発明に係る導電層には、下記一般式(1)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物を含有することが、高温高湿といった環境変化に対する耐久性の点で好ましい。   In addition, the conductive layer according to the present invention contains an organosilicon compound represented by the following general formula (1), a hydrolyzate thereof, or a polycondensate thereof, which has durability against environmental changes such as high temperature and high humidity. This is preferable.

1 nSiX1 4-n (1)
式中、R1は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X1は水酸基または加水分解可能な置換基であり、nは1〜3の整数である。
R 1 n SiX 1 4-n (1)
In the formula, R 1 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 1 is a hydroxyl group or a hydrolyzable substituent, and n is an integer of 1 to 3.

アルキル基としては、メチル基、エチル基、プロピル基、イソプロピル基、t−ブチル基、s−ブチル基、ヘキシル基、デシル基、ヘキサデシル基等が挙げられる。アリール基としてはフェニル基、ナフチル基等が挙げられる。   Examples of the alkyl group include methyl group, ethyl group, propyl group, isopropyl group, t-butyl group, s-butyl group, hexyl group, decyl group, hexadecyl group and the like. Examples of the aryl group include a phenyl group and a naphthyl group.

1の加水分解可能な置換基としては、アルコキシ基、ハロゲン基、カルボキシル基等が挙げられる。 Examples of the hydrolyzable substituent for X 1 include an alkoxy group, a halogen group, and a carboxyl group.

具体例としては、ビニルトリメトキシシラン、ビニルトリエトキシシラン、ビニルトリアセトキシシラン、ビニルトリメトキシエトキシシラン、3−クロロプロピルトリメトキシシラン、3−クロロプロピルトリエトキシシラン、3−グリシドキシプロピルトリメトキシシラン、3−グリシドキシプロピルトリエトキシシラン、3−グリシドキシプロピルメチルジエトキシシラン、2−(3,4−エポシシシクロヘキシル)エチルトリメトキシシラン、2−(3,4−エポキシシクロヘキシル)エチルトリエトキシシラン、3−アクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルトリエトキシシラン、3−メタクリロキシプロピルメチルジメトキシシラン、3−メタクリロキシプロピルメチルジエトキシシラン、3−アミノプロピルトリメトキシシラン、3−アミノプロピルトリエトキシシラン、N−2−アミノエチル−3−アミノプロピルメチルジメトキシシラン、N−2−アミノエチル−3−アミノプロピルトリメトキシシラン、N−2−アミノエチル−3−アミノプロピルトリエトキシシラン、3−トリエトキシシリル−N−1,3−ジメチルブチリデンプロピルアミン、N−フェニル−3−アミノプロピルトリメトキシシラン、3−メルカプトプロピルトリメトキシシラン、3−メルカプトプロピルメチルジメトキシシラン、3−イソシアネートプロピルトリエトキシシラン、p−スチリルトリメトキシシラン等が挙げられ、これらを単独または2種以上を混合して用いられる。   Specific examples include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, vinyltrimethoxyethoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 3-glycidoxypropyltrimethoxy. Silane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2- (3,4-epoxycyclohexyl) ethyltrimethoxysilane, 2- (3,4-epoxycyclohexyl) ethyl Triethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryl Roxypropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropylmethyldimethoxysilane, N-2-aminoethyl-3-aminopropyltri Methoxysilane, N-2-aminoethyl-3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-1,3-dimethylbutylidenepropylamine, N-phenyl-3-aminopropyltrimethoxysilane, 3- Examples include mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, p-styryltrimethoxysilane, and the like. These may be used alone or in admixture of two or more.

導電層を塗布する際には、有機溶媒が用いられることが好ましい。有機溶媒としては、例えば、アルコール類(例えば、メタノール、エタノール、プロパノール、イソプロパノール、ブタノール、イソブタノール、セカンダリーブタノール、ターシャリーブタノール、ペンタノール、ヘキサノール、シクロヘキサノール、ベンジルアルコール等)、多価アルコール類(例えば、エチレングリコール、ジエチレングリコール、トリエチレングリコール、ポリエチレングリコール、プロピレングリコール、ジプロピレングリコール、ポリプロピレングリコール、ブチレングリコール、ヘキサンジオール、ペンタンジオール、グリセリン、ヘキサントリオール、チオジグリコール等)、多価アルコールエーテル類(例えば、エチレングリコールモノメチルエーテル、エチレングリコールモノエチルエーテル、エチレングリコールモノブチルエーテル、ジエチレングリコールモノメチルエーテル、ジエチレングリコールモノメチルエーテル、ジエチレングリコールモノブチルエーテル、プロピレングリコールモノメチルエーテル、プロピレングリコールモノブチルエーテル、エチレングリコールモノメチルエーテルアセテート、トリエチレングリコールモノメチルエーテル、トリエチレングリコールモノエチルエーテル、エチレングリコールモノフェニルエーテル、プロピレングリコールモノフェニルエーテル等)、アミン類(例えば、エタノールアミン、ジエタノールアミン、トリエタノールアミン、N−メチルジエタノールアミン、N−エチルジエタノールアミン、モルホリン、N−エチルモルホリン、エチレンジアミン、ジエチレンジアミン、トリエチレンテトラミン、テトラエチレンペンタミン、ポリエチレンイミン、ペンタメチルジエチレントリアミン、テトラメチルプロピレンジアミン等)、アミド類(例えば、ホルムアミド、N,N−ジメチルホルムアミド、N,N−ジメチルアセトアミド等)、複素環類(例えば、2−ピロリドン、N−メチル−2−ピロリドン、シクロヘキシルピロリドン、2−オキサゾリドン、1,3−ジメチル−2−イミダゾリジノン等)、スルホキシド類(例えば、ジメチルスルホキシド等)、スルホン類(例えば、スルホラン等)、尿素、アセトニトリル、アセトン等が挙げられるが、特に、アルコール類、多価アルコール類、多価アルコールエーテル類が好ましい。   When applying the conductive layer, an organic solvent is preferably used. Examples of the organic solvent include alcohols (eg, methanol, ethanol, propanol, isopropanol, butanol, isobutanol, secondary butanol, tertiary butanol, pentanol, hexanol, cyclohexanol, benzyl alcohol, etc.), polyhydric alcohols ( For example, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, butylene glycol, hexanediol, pentanediol, glycerin, hexanetriol, thiodiglycol, etc.), polyhydric alcohol ethers ( For example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene Glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, ethylene glycol monophenyl ether , Propylene glycol monophenyl ether, etc.), amines (for example, ethanolamine, diethanolamine, triethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, morpholine, N-ethylmorpholine, ethylenediamine, diethylenediamine, trie Lentetramine, tetraethylenepentamine, polyethyleneimine, pentamethyldiethylenetriamine, tetramethylpropylenediamine, etc.), amides (eg, formamide, N, N-dimethylformamide, N, N-dimethylacetamide, etc.), heterocyclics (eg, 2-pyrrolidone, N-methyl-2-pyrrolidone, cyclohexyl pyrrolidone, 2-oxazolidone, 1,3-dimethyl-2-imidazolidinone, etc.), sulfoxides (eg dimethyl sulfoxide etc.), sulfones (eg sulfolane) Etc.), urea, acetonitrile, acetone and the like, and alcohols, polyhydric alcohols, and polyhydric alcohol ethers are particularly preferable.

導電層は上記組成物をグラビアコーター、ディップコーター、リバースコーター、ワイヤーバーコーター、ダイコーター、またはスプレー塗布、インクジェット塗布等を用いて透明樹脂フィルム、あるいはハードコート層表面にウェット膜厚0.1〜100μmで塗布し、塗布後、加熱乾燥し、必要に応じて硬化して形成される。硬化工程は、後述する低屈折率層で記載した内容を用いることができる。
(低屈折率層)
つぎに、本発明による反射防止フィルムの低屈折率層について説明する。
The conductive layer is a gravure coater, dip coater, reverse coater, wire bar coater, die coater, or a transparent resin film using spray coating, ink jet coating or the like. It is formed by coating at 100 μm, followed by heating and drying after coating, and curing as necessary. The content described in the low refractive index layer described later can be used in the curing step.
(Low refractive index layer)
Next, the low refractive index layer of the antireflection film according to the present invention will be described.

本発明による反射防止フィルムの低屈折率層とは、透明フィルム基材の屈折率より低い層をいう。具体的な屈折率としては、23℃、波長550nmで1.20〜1.45の範囲のものが好ましい。また、低屈折率層の膜厚は、光学干渉層としての特性から、5nm〜0.5μmが好ましく、10nm〜0.3μmがより好ましく、30nm〜0.2μmであることがさらに好ましい。   The low refractive index layer of the antireflection film according to the present invention refers to a layer lower than the refractive index of the transparent film substrate. A specific refractive index is preferably in the range of 1.20 to 1.45 at 23 ° C. and a wavelength of 550 nm. Further, the film thickness of the low refractive index layer is preferably 5 nm to 0.5 μm, more preferably 10 nm to 0.3 μm, and further preferably 30 nm to 0.2 μm, from the characteristics as the optical interference layer.

コーティングによって形成される低屈折率層は、有機珪素化合物もしくはその加水分解物あるいはその重縮合物、ポリビニルアルコール、ポリオキシエチレン、ポリメチルメタクリレート、ポリメチルアクリレート、ジアセチルセルロース、トリアセチルセルロース、ニトロセルロース、ポリエステル、アルキド樹脂、フルオロアクリレート、含フッ素ポリマー等から形成される。フッ素ポリマーとしては、例えばフルオロオレフィン類(例えばフルオロエチレン、ビニリデンフルオライド、テトラフルオロエチレン、パーフルオロオクチルエチレン、ヘキサフルオロプロピレン、パーフルオロ−2,2−ジメチル−1,3−ジオキソール等)、(メタ)アクリル酸の部分または完全フッ素化アルキルエステル誘導体類(例えばビスコート6FM(大阪有機化学製)やM−2020(ダイキン製)等)、完全または部分フッ素化ビニルエーテル類等が挙げられる。これらの中で好ましくは、炭素数が1〜4の有機珪素化合物もしくはその加水分解物あるいはその重縮合物であり、具体的には、テトラメトキシシラン、テトラエトキシシラン、テトラブトキシシラン等もしくはこれらの加水分解物あるいは重縮合物が挙げられる。   The low refractive index layer formed by the coating is composed of an organic silicon compound or a hydrolyzate thereof or a polycondensate thereof, polyvinyl alcohol, polyoxyethylene, polymethyl methacrylate, polymethyl acrylate, diacetyl cellulose, triacetyl cellulose, nitrocellulose, It is formed from polyester, alkyd resin, fluoroacrylate, fluorine-containing polymer or the like. Examples of the fluoropolymer include fluoroolefins (eg, fluoroethylene, vinylidene fluoride, tetrafluoroethylene, perfluorooctylethylene, hexafluoropropylene, perfluoro-2,2-dimethyl-1,3-dioxole, etc.) (meta ) A part of acrylic acid or a fully fluorinated alkyl ester derivative (for example, Biscoat 6FM (manufactured by Osaka Organic Chemical) or M-2020 (manufactured by Daikin)), a fully or partially fluorinated vinyl ether or the like. Among these, an organic silicon compound having 1 to 4 carbon atoms, a hydrolyzate thereof, or a polycondensate thereof is preferable. Specifically, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, etc. Examples include hydrolysates and polycondensates.

本発明に係る低屈折率層には、コロイダルシリカ、フッ化マグネシウム、及び外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子よりなる群の中から選ばれた少なくとも1種の無機粒子を含有することが好ましい。   The low refractive index layer according to the present invention includes at least one selected from the group consisting of colloidal silica, magnesium fluoride, and hollow silica-based particles having an outer shell layer and porous or hollow inside. It is preferable to contain the inorganic particles.

コロイダルシリカの具体例としては、二酸化ケイ素をコロイド状に水または有機溶媒に分散させたものであり、特に限定はされないが球状、針状または数珠状である。   Specific examples of colloidal silica are those in which silicon dioxide is dispersed in water or an organic solvent in a colloidal form, and are not particularly limited, but are spherical, acicular or beaded.

コロイダルシリカの平均粒径は50〜300nmの範囲が好ましく、変動係数が1〜40%の単分散であることが好ましい。平均粒径は、走査電子顕微鏡(SEM)等による電子顕微鏡写真から計測することができる。動的光散乱法や静的光散乱法等を利用する粒度分布計等によって計測してもよい。   The average particle size of the colloidal silica is preferably in the range of 50 to 300 nm, and is preferably monodispersed with a coefficient of variation of 1 to 40%. The average particle diameter can be measured from an electron micrograph taken with a scanning electron microscope (SEM) or the like. You may measure by the particle size distribution meter etc. which utilize a dynamic light scattering method, a static light scattering method, etc.

コロイダルシリカは、市販されており、例えば日産化学工業社のスノーテックスシリーズ、触媒化成工業社のカタロイド−Sシリーズ、バイエル社のレバシルシリーズ等が挙げられる。また、アルミナゾルや水酸化アルミニウムでカチオン変性したコロイダルシリカやシリカの一次粒子を2価以上の金属イオンで粒子間を結合し、数珠状に連結した数珠状コロイダルシリカも好ましく用いられる。数珠状コロイダルシリカは日産化学工業社のスノーテックス−AKシリーズ、スノーテックス−PSシリーズ、スノーテックス−UPシリーズ等があり、具体的にはIPS−ST−L(イソプロパノール分散、粒子径40〜50nm、固形分30%)、MEK−ST−MS(メチルエチルケトン分散、粒子径17〜23nm、固形分35)等が挙げられる。   Colloidal silica is commercially available, and examples thereof include the Snowtex series of Nissan Chemical Industries, the Cataloid-S series of Catalytic Chemical Industry, and the Lebasil series of Bayer. Further, bead-like colloidal silica in which primary particles of colloidal silica or silica cation-modified with alumina sol or aluminum hydroxide are bonded to each other with metal ions having a valence of 2 or more and connected in a bead shape is also preferably used. There are beaded colloidal silicas such as SNOWTEX-AK series, SNOWTEX-PS series, SNOWTEX-UP series of NISSAN CHEMICAL INDUSTRIES, and specifically IPS-ST-L (isopropanol dispersion, particle size 40-50 nm, Solid content 30%), MEK-ST-MS (methyl ethyl ketone dispersion, particle diameter 17-23 nm, solid content 35) and the like.

フッ化マグネシウムとしては、例えば日産化学工業社のイソプロパノール分散フッ化マグネシウムゾルや、シーアイ化成社のナノテックシリーズ等が挙げられる。   Examples of magnesium fluoride include isopropanol-dispersed magnesium fluoride sol manufactured by Nissan Chemical Industries, Nanotech series manufactured by CI Kasei.

外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子の具体例としては、(1)多孔質粒子と該多孔質粒子表面に設けられた被覆層からなる複合粒子、または(2)内部に空洞を有し、かつ内容物が溶媒、気体または多孔質物質で充填された空洞粒子である。   Specific examples of hollow silica-based particles having an outer shell layer and having a porous or hollow interior include (1) composite particles comprising porous particles and a coating layer provided on the surface of the porous particles, or ( 2) Cavity particles having a cavity inside and filled with a solvent, gas or porous substance.

なお、空洞粒子は、内部に空洞を有する粒子であり、空洞は粒子壁で囲まれている。空洞内には、調製時に使用した溶媒、気体または多孔質物質等の内容物で充填されている。このような中空シリカ系粒子の平均粒径は5〜200nm、好ましくは10〜70nmが望ましい。中空シリカ系粒子の粒径は変動係数が1〜40%の単分散であることが好ましい。   Note that the cavity particles are particles having a cavity inside, and the cavity is surrounded by a particle wall. The cavity is filled with contents such as a solvent, a gas, or a porous material used at the time of preparation. The average particle size of such hollow silica-based particles is 5 to 200 nm, preferably 10 to 70 nm. The particle size of the hollow silica particles is preferably monodispersed with a coefficient of variation of 1 to 40%.

本発明で用いられる中空シリカ系粒子の平均粒径は、走査電子顕微鏡(SEM)等による電子顕微鏡写真から計測することができる。動的光散乱法や静的光散乱法等を利用する粒度分布計等によって計測してもよい。   The average particle diameter of the hollow silica particles used in the present invention can be measured from an electron micrograph taken with a scanning electron microscope (SEM) or the like. You may measure by the particle size distribution meter etc. which utilize a dynamic light scattering method, a static light scattering method, etc.

本発明で使用する中空シリカ系粒子の平均粒径は、形成される低屈折率層の透明被膜の厚さに応じて適宜選択され、透明被膜の膜厚の3/2〜1/10、好ましくは2/3〜1/10が望ましい。これらの中空シリカ系粒子は、低屈折率層の形成のため、適当な媒体に分散した状態で使用することが好ましい。   The average particle size of the hollow silica-based particles used in the present invention is appropriately selected according to the thickness of the transparent coating of the low refractive index layer to be formed, and is preferably 3/2 to 1/10 of the thickness of the transparent coating. Is preferably 2/3 to 1/10. These hollow silica particles are preferably used in a state of being dispersed in an appropriate medium in order to form a low refractive index layer.

分散媒としては、水、アルコール(例えばメタノール、エタノール、イソプロピルアルコール)、及びケトン(例えばメチルエチルケトン、メチルイソブチルケトン)、ケトンアルコール(例えばジアセトンアルコール)、プロピレンモノメチルエーテル、プロピレングリコールモノメチルエーテルアセテート等が好ましい。   As the dispersion medium, water, alcohol (for example, methanol, ethanol, isopropyl alcohol), ketone (for example, methyl ethyl ketone, methyl isobutyl ketone), ketone alcohol (for example, diacetone alcohol), propylene monomethyl ether, propylene glycol monomethyl ether acetate and the like are preferable. .

複合粒子の被覆層の厚さまたは空洞粒子の粒子壁の厚さは、1〜40nm、好ましくは1〜20nm、さらに好ましくは2〜15nmが望ましい。複合粒子の場合、被覆層の厚さが1nm未満の場合は、粒子を完全に被覆することができないことがあり、塗布液成分が容易に複合粒子の内部に進入して内部の多孔性が減少し、低屈折率化の効果が十分得られないことがある。また、被覆層の厚さが20nmを越えると、塗布液成分が内部に進入することはないが、複合粒子の多孔性(細孔容積)が低下し低屈折率化の効果が十分得られなくなることがある。   The thickness of the coating layer of the composite particles or the thickness of the particle walls of the hollow particles is 1 to 40 nm, preferably 1 to 20 nm, more preferably 2 to 15 nm. In the case of composite particles, if the thickness of the coating layer is less than 1 nm, the particles may not be completely covered, and the coating liquid component can easily enter the composite particles to reduce the internal porosity. However, the effect of lowering the refractive index may not be obtained sufficiently. In addition, when the thickness of the coating layer exceeds 20 nm, the coating liquid component does not enter the inside, but the porosity (pore volume) of the composite particles is lowered and the effect of lowering the refractive index cannot be sufficiently obtained. Sometimes.

また空洞粒子の場合、粒子壁の厚さが1nm未満の場合は、粒子形状を維持できないことがあり、また厚さが20nmを越えても、低屈折率化の効果が十分に現れないことがある。   In the case of hollow particles, when the particle wall thickness is less than 1 nm, the particle shape may not be maintained, and even when the thickness exceeds 20 nm, the effect of lowering the refractive index may not be sufficiently exhibited. is there.

複合粒子の被覆層または空洞粒子の粒子壁は、シリカを主成分とすることが好ましい。また、シリカ以外の成分が含まれていてもよく、具体的にはAl23、B23、TiO2、ZrO2、SnO2、CeO2、P23、Sb23、Sb25、SbO2、MoO3、ZnO2、WO3等が挙げられる。複合粒子を構成する多孔質粒子としては、シリカからなるもの、シリカとシリカ以外の無機化合物とからなるもの、CaF2、NaF、NaAlF6、MgF等からなるものが挙げられる。このうち特にシリカとシリカ以外の無機化合物との複合酸化物からなる多孔質粒子が好適である。 The coating layer of the composite particles or the particle wall of the hollow particles is preferably composed mainly of silica. In addition, components other than silica may be included. Specifically, Al 2 O 3 , B 2 O 3 , TiO 2 , ZrO 2 , SnO 2 , CeO 2 , P 2 O 3 , Sb 2 O 3 , sb 2 O 5, SbO 2, MoO 3, ZnO 2, WO 3 and the like. Examples of the porous particles constituting the composite particles include those made of silica, those made of silica and an inorganic compound other than silica, and those made of CaF 2 , NaF, NaAlF 6 , MgF, and the like. Of these, porous particles made of a composite oxide of silica and an inorganic compound other than silica are particularly suitable.

シリカ以外の無機化合物としては、Al23、B23、TiO2、ZrO2、SnO2、CeO2、P23、Sb23、Sb25、SbO2、MoO3、ZnO2、WO3との1種または2種以上を挙げることができる。このような多孔質粒子では、シリカをSiO2で表し、シリカ以外の無機化合物を酸化物換算(MOx)で表わしたときのモル比:MOx/SiO2が、0.0001〜1.0、好ましくは0.001〜0.3の範囲にあることが望ましい。 Examples of inorganic compounds other than silica include Al 2 O 3 , B 2 O 3 , TiO 2 , ZrO 2 , SnO 2 , CeO 2 , P 2 O 3 , Sb 2 O 3 , Sb 2 O 5 , SbO 2 , MoO 3. , ZnO 2 , WO 3 , or two or more of them. In such porous particles, the molar ratio when the silica is represented by SiO 2 and the inorganic compound other than silica is represented by oxide (MOx): MOx / SiO 2 is 0.0001 to 1.0, preferably Is preferably in the range of 0.001 to 0.3.

多孔質粒子のモル比:MOx/SiO2が、0.0001未満のものは、得ることが困難であり、得られたとしても細孔容積が小さく、屈折率の低い粒子が得られない。また多孔質粒子のモル比:MOx/SiO2が1.0を越えると、シリカの比率が少なくなるので、細孔容積が大きくなり、さらに屈折率が低いものを得ることが難しいことがある。 A porous particle having a molar ratio of MOx / SiO 2 of less than 0.0001 is difficult to obtain, and even if obtained, a pore volume is small and particles having a low refractive index cannot be obtained. Further, when the molar ratio of the porous particles: MOx / SiO 2 exceeds 1.0, the ratio of silica decreases, so that the pore volume increases and it may be difficult to obtain a low refractive index.

このような多孔質粒子の細孔容積は、0.1〜1.5ml/g、好ましくは0.2〜1.5ml/gの範囲であることが望ましい。細孔容積が0.1ml/g未満では、十分に屈折率の低下した粒子が得られず、1.5ml/gを越えると粒子の強度が低下し、得られる被膜の強度が低下することがある。   The pore volume of such porous particles is desirably in the range of 0.1 to 1.5 ml / g, preferably 0.2 to 1.5 ml / g. When the pore volume is less than 0.1 ml / g, particles having a sufficiently reduced refractive index cannot be obtained, and when the pore volume exceeds 1.5 ml / g, the strength of the particles is lowered and the strength of the resulting coating may be lowered. is there.

なお、このような多孔質粒子の細孔容積は水銀圧入法によって求めることができる。また、空洞粒子の内容物としては、粒子調製時に使用した溶媒、気体、多孔質物質等が挙げられる。溶媒中には空洞粒子調製する際に使用される粒子前駆体の未反応物、使用した触媒等が含まれていてもよい。   In addition, the pore volume of such porous particles can be determined by a mercury intrusion method. Examples of the contents of the hollow particles include a solvent, a gas, and a porous substance used at the time of preparing the particles. The solvent may contain an unreacted particle precursor used when preparing the hollow particles, the catalyst used, and the like.

また多孔質物質としては、多孔質粒子で例示した化合物からなるものが挙げられる。これらの内容物は、単一の成分からなるものであってもよいが、複数成分の混合物であってもよい。   Moreover, what consists of the compound illustrated by the porous particle as a porous substance is mentioned. These contents may be composed of a single component or may be a mixture of a plurality of components.

このような中空粒子の製造方法としては、例えば特開平7−133105号公報の段落番号[0010]〜[0033]に開示された複合酸化物コロイド粒子の調製方法が好適に採用される。具体的に、複合粒子が、シリカ、シリカ以外の無機化合物とからなる場合、以下の第1工程〜第3工程を実施するこれによって中空粒子を製造することができる。
(第1工程:多孔質粒子前駆体の調製)
第1工程では、予め、シリカ原料とシリカ以外の無機化合物原料のアルカリ水溶液を個別に調製するか、または、シリカ原料とシリカ以外の無機化合物原料との混合水溶液を調製しておき、この水溶液を目的とする複合酸化物の複合割合に応じて、pH10以上のアルカリ水溶液中に攪拌しながら徐々に添加して多孔質粒子前駆体を調製する。
As a method for producing such hollow particles, for example, the method for preparing composite oxide colloidal particles disclosed in paragraphs [0010] to [0033] of JP-A-7-133105 is preferably employed. Specifically, when the composite particles are composed of silica and an inorganic compound other than silica, hollow particles can be produced by carrying out the following first to third steps.
(First step: Preparation of porous particle precursor)
In the first step, an alkaline aqueous solution of a silica raw material and an inorganic compound raw material other than silica is separately prepared in advance, or a mixed aqueous solution of a silica raw material and an inorganic compound raw material other than silica is prepared in advance, According to the composite ratio of the target composite oxide, a porous particle precursor is prepared by gradually adding it to an alkaline aqueous solution having a pH of 10 or more while stirring.

シリカ原料としては、アルカリ金属、アンモニウムまたは有機塩基のケイ酸塩を用いる。アルカリ金属のケイ酸塩としては、ケイ酸ナトリウム(水ガラス)やケイ酸カリウムが用いられる。有機塩基としては、テトラエチルアンモニウム塩等の第4級アンモニウム塩、モノエタノールアミン、ジエタノールアミン、トリエタノールアミン等のアミン類を挙げることができる。なお、アンモニウムのケイ酸塩または有機塩基のケイ酸塩には、ケイ酸液にアンモニア、第4級アンモニウム水酸化物、アミン化合物等を添加したアルカリ性溶液も含まれる。   As the silica raw material, alkali metal, ammonium or organic base silicate is used. Sodium silicate (water glass) or potassium silicate is used as the alkali metal silicate. Examples of the organic base include quaternary ammonium salts such as tetraethylammonium salt, and amines such as monoethanolamine, diethanolamine, and triethanolamine. The ammonium silicate or the organic base silicate includes an alkaline solution obtained by adding ammonia, a quaternary ammonium hydroxide, an amine compound or the like to a silicic acid solution.

また、シリカ以外の無機化合物の原料としては、アルカリ可溶の無機化合物が用いられる。具体的には、Al、B、Ti、Zr、Sn、Ce、P、Sb、Mo、Zn、W等から選ばれる元素のオキソ酸、該オキソ酸のアルカリ金属塩またはアルカリ土類金属塩、アンモニウム塩、第4級アンモニウム塩を挙げることができる。より具体的には、アルミン酸ナトリウム、四硼酸ナトリウム、炭酸ジルコニルアンモニウム、アンチモン酸カリウム、錫酸カリウム、アルミノケイ酸ナトリウム、モリブデン酸ナトリウム、硝酸セリウムアンモニウム、燐酸ナトリウムが適当である。   In addition, alkali-soluble inorganic compounds are used as raw materials for inorganic compounds other than silica. Specifically, an oxo acid of an element selected from Al, B, Ti, Zr, Sn, Ce, P, Sb, Mo, Zn, W, etc., an alkali metal salt or alkaline earth metal salt of the oxo acid, ammonium And salts and quaternary ammonium salts. More specifically, sodium aluminate, sodium tetraborate, zirconyl ammonium carbonate, potassium antimonate, potassium stannate, sodium aluminosilicate, sodium molybdate, cerium ammonium nitrate, and sodium phosphate are suitable.

これら水溶液の添加と同時に混合水溶液のpH値は変化するが、このpH値を所定の範囲に制御するような操作は特に必要ない。水溶液は、最終的に、無機酸化物の種類、及びその混合割合によって定まるpH値となる。このときの水溶液の添加速度には特に制限はない。また、複合酸化物粒子の製造に際して、シード粒子の分散液を出発原料と使用することも可能である。   Although the pH value of the mixed aqueous solution changes simultaneously with the addition of these aqueous solutions, an operation for controlling the pH value within a predetermined range is not particularly required. The aqueous solution finally has a pH value determined by the type of inorganic oxide and the mixing ratio thereof. There is no restriction | limiting in particular in the addition rate of the aqueous solution at this time. Further, in the production of composite oxide particles, a dispersion of seed particles can be used as a starting material.

当該シード粒子としては、特に制限はないが、SiO2、Al23、TiO2、またはZrO2等の無機酸化物またはこれらの複合酸化物の微粒子が用いられ、通常、これらのゾルを用いることができる。さらに上記の製造方法によって得られた多孔質粒子前駆体分散液をシード粒子分散液としてもよい。 The seed particles are not particularly limited, but inorganic oxides such as SiO 2 , Al 2 O 3 , TiO 2 , or ZrO 2 or fine particles of these composite oxides are used, and usually these sols are used. be able to. Furthermore, the porous particle precursor dispersion obtained by the above production method may be used as a seed particle dispersion.

シード粒子分散液を使用する場合、シード粒子分散液のpHを10以上に調整した後、該シード粒子分散液中に上記化合物の水溶液を、アルカリ水溶液中に攪拌しながら添加する。この場合も、必ずしも分散液のpH制御を行う必要はない。このようにしてシード粒子を用いると、調製する多孔質粒子の粒径コントロールが容易であり、粒度の揃ったものを得ることができる。   When the seed particle dispersion is used, the pH of the seed particle dispersion is adjusted to 10 or more, and then an aqueous solution of the above compound is added to the alkaline aqueous solution while stirring. Also in this case, it is not always necessary to control the pH of the dispersion. When seed particles are used in this way, it is easy to control the particle size of the porous particles to be prepared, and particles with uniform particle sizes can be obtained.

上記したシリカ原料、及び無機化合物原料は、アルカリ側で高い溶解度を有する。しかしながら、この溶解度の大きいpH領域で両者を混合すると、ケイ酸イオン、及びアルミン酸イオン等のオキソ酸イオンの溶解度が低下し、これらの複合物が析出して粒子に成長したり、またはシード粒子上に析出して粒子成長が起る。従って、粒子の析出、成長に際して、従来法のようなpH制御は必ずしも行う必要がない。   The silica raw material and the inorganic compound raw material described above have high solubility on the alkali side. However, when both are mixed in this highly soluble pH region, the solubility of oxo acid ions such as silicate ions and aluminate ions decreases, and these composites precipitate and grow into particles, or seed particles. It grows on the top and particle growth occurs. Therefore, it is not always necessary to perform pH control as in the conventional method for precipitation and growth of particles.

第1工程におけるシリカとシリカ以外の無機化合物との複合割合は、シリカに対する無機化合物を酸化物(MOx)に換算し、MOx/SiO2のモル比が、0.05〜2.0、好ましくは0.2〜2.0の範囲内にあることが望ましい。この範囲内において、シリカの割合が少なくなる程、多孔質粒子の細孔容積が増大する。しかしながら、モル比が2.0を越えても、多孔質粒子の細孔の容積はほとんど増加しない。他方、モル比が0.05未満の場合は、細孔容積が小さくなる。 The composite ratio of silica and inorganic compound other than silica in the first step is that the inorganic compound relative to silica is converted to oxide (MOx), and the molar ratio of MOx / SiO 2 is 0.05 to 2.0, preferably It is desirable to be within the range of 0.2 to 2.0. Within this range, the pore volume of the porous particles increases as the proportion of silica decreases. However, even when the molar ratio exceeds 2.0, the pore volume of the porous particles hardly increases. On the other hand, when the molar ratio is less than 0.05, the pore volume becomes small.

空洞粒子を調製する場合、MOx/SiO2のモル比は、0.25〜2.0の範囲内にあることが望ましい。
(第2工程:多孔質粒子からのシリカ以外の無機化合物の除去)
第2工程では、第1工程で得られた多孔質粒子前駆体から、シリカ以外の無機化合物(珪素と酸素以外の元素)の少なくとも一部を選択的に除去する。具体的な除去方法としては、多孔質粒子前駆体中の無機化合物を鉱酸や有機酸を用いて溶解除去したり、または、陽イオン交換樹脂と接触させてイオン交換除去する。
When preparing hollow particles, the molar ratio of MOx / SiO 2 is preferably in the range of 0.25 to 2.0.
(Second step: removal of inorganic compounds other than silica from porous particles)
In the second step, at least a part of inorganic compounds other than silica (elements other than silicon and oxygen) is selectively removed from the porous particle precursor obtained in the first step. As a specific removal method, the inorganic compound in the porous particle precursor is dissolved and removed using a mineral acid or an organic acid, or is contacted with a cation exchange resin for ion exchange removal.

なお、第1工程で得られる多孔質粒子前駆体は、珪素と無機化合物構成元素が酸素を介して結合した網目構造の粒子である。このように多孔質粒子前駆体から無機化合物(珪素と酸素以外の元素)を除去することにより、一層多孔質で細孔容積の大きい多孔質粒子が得られる。また、多孔質粒子前駆体から無機酸化物(珪素と酸素以外の元素)を除去する量を多くすれば、空洞粒子を調製することができる。   The porous particle precursor obtained in the first step is a particle having a network structure in which silicon and an inorganic compound constituent element are bonded through oxygen. By removing the inorganic compound (elements other than silicon and oxygen) from the porous particle precursor in this way, porous particles having a larger porosity and a larger pore volume can be obtained. Further, if the amount of removing the inorganic oxide (elements other than silicon and oxygen) from the porous particle precursor is increased, the hollow particles can be prepared.

また、多孔質粒子前駆体からシリカ以外の無機化合物を除去するに先立って、第1工程で得られる多孔質粒子前駆体分散液に、シリカのアルカリ金属塩を脱アルカリして得られる、フッ素置換アルキル基含有シラン化合物を含有するケイ酸液または加水分解性の有機珪素化合物を添加して、シリカ保護膜を形成することが好ましい。シリカ保護膜の厚さは0.5〜40nm、好ましくは0.5〜15nmの厚さであればよい。なお、シリカ保護膜を形成しても、この工程での保護膜は多孔質であり、厚さが薄いので、上記したシリカ以外の無機化合物を、多孔質粒子前駆体から除去することは可能である。   In addition, prior to removing inorganic compounds other than silica from the porous particle precursor, fluorine-substituted, obtained by dealkalizing an alkali metal salt of silica into the porous particle precursor dispersion obtained in the first step. It is preferable to add a silicic acid solution containing an alkyl group-containing silane compound or a hydrolyzable organosilicon compound to form a silica protective film. The thickness of the silica protective film may be 0.5 to 40 nm, preferably 0.5 to 15 nm. Even if a silica protective film is formed, the protective film in this step is porous and thin, so that it is possible to remove inorganic compounds other than silica from the porous particle precursor. is there.

このようなシリカ保護膜を形成することによって、粒子形状を保持したまま、上記したシリカ以外の無機化合物を、多孔質粒子前駆体から除去することができる。また、後述するシリカ被覆層を形成する際に、多孔質粒子の細孔が被覆層によって閉塞されてしまうことがなく、このため細孔容積を低下させることなく、後述するシリカ被覆層を形成することができる。なお、除去する無機化合物の量が少ない場合は、粒子が壊れることがないので、必ずしも保護膜を形成する必要はない。   By forming such a silica protective film, inorganic compounds other than silica described above can be removed from the porous particle precursor while maintaining the particle shape. Further, when forming the silica coating layer described later, the pores of the porous particles are not blocked by the coating layer, and therefore the silica coating layer described later is formed without reducing the pore volume. be able to. Note that when the amount of the inorganic compound to be removed is small, the particles are not broken, and thus it is not always necessary to form a protective film.

また、空洞粒子を調製する場合は、このシリカ保護膜を形成しておくことが望ましい。空洞粒子を調製する際には、無機化合物を除去すると、シリカ保護膜と、シリカ保護膜内の溶媒、未溶解の多孔質固形分とからなる空洞粒子の前駆体が得られ、空洞粒子の前駆体に後述の被覆層を形成すると、形成された被覆層が、粒子壁となり空洞粒子が形成される。   Further, when preparing hollow particles, it is desirable to form this silica protective film. When preparing the hollow particles, the inorganic compound is removed to obtain a hollow particle precursor composed of a silica protective film, a solvent in the silica protective film, and an undissolved porous solid content. When a coating layer to be described later is formed on the body, the formed coating layer becomes a particle wall to form hollow particles.

上記シリカ保護膜形成のために添加するシリカ源の量は、粒子形状を保持できる範囲で少ないことが好ましい。シリカ源の量が多すぎると、シリカ保護膜が厚くなりすぎるので、多孔質粒子前駆体からシリカ以外の無機化合物を除去することが困難となることがある。   The amount of the silica source added for forming the silica protective film is preferably small as long as the particle shape can be maintained. If the amount of the silica source is too large, the silica protective film becomes too thick, and it may be difficult to remove inorganic compounds other than silica from the porous particle precursor.

シリカ保護膜形成用に使用される加水分解性の有機珪素化合物としては、下記の一般式(3)
R”mSi(OR′)4-m ・・・(3)
(式中、R”とR′は、アルキル基、アリール基、ビニル基、アクリル基等の炭化水素基、mは0、1、2または3を表わす。)
で表されるアルコキシシランを用いることができる。特に、フッ素置換したテトラメトキシシラン、テトラエトキシシラン、テトライソプロポキシシラン等のテトラアルコキシシランが好ましく用いられる。
As a hydrolyzable organosilicon compound used for forming a silica protective film, the following general formula (3)
R "mSi (OR ') 4-m ... (3)
(In the formula, R ″ and R ′ represent a hydrocarbon group such as an alkyl group, an aryl group, a vinyl group, an acrylic group, and m represents 0, 1, 2, or 3.)
The alkoxysilane represented by these can be used. In particular, tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, and tetraisopropoxysilane substituted with fluorine are preferably used.

添加方法としては、これらのアルコキシシラン、純水、及びアルコールの混合溶液に触媒としての少量のアルカリまたは酸を添加した溶液を、多孔質粒子の分散液に加え、アルコキシシラン、純水、及びアルコールの混合溶液に触媒としての少量のアルカリまたは酸を添加した溶液を、多孔質粒子の分散液に加え、アルコキシシランを加水分解して生成したケイ酸重合物を無機酸化物粒子の表面に沈着させる。   As a method of addition, a solution obtained by adding a small amount of alkali or acid as a catalyst to a mixed solution of these alkoxysilane, pure water, and alcohol is added to the dispersion of porous particles, and then alkoxysilane, pure water, and alcohol are added. A solution obtained by adding a small amount of alkali or acid as a catalyst to a mixed solution of the above is added to a dispersion of porous particles, and a silicic acid polymer produced by hydrolyzing alkoxysilane is deposited on the surface of inorganic oxide particles. .

このとき、アルコキシシラン、アルコール、触媒を同時に分散液中に添加してもよい。アルカリ触媒としては、アンモニア、アルカリ金属の水酸化物、アミン類を用いることができる。また、酸触媒としては、各種の無機酸と有機酸を用いることができる。   At this time, alkoxysilane, alcohol, and catalyst may be simultaneously added to the dispersion. As the alkali catalyst, ammonia, an alkali metal hydroxide, or an amine can be used. As the acid catalyst, various inorganic acids and organic acids can be used.

多孔質粒子前駆体の分散媒が、水単独、または有機溶媒に対する水の比率が高い場合には、ケイ酸液を用いてシリカ保護膜を形成することも可能である。ケイ酸液を用いる場合には、分散液中にケイ酸液を所定量添加し、同時にアルカリを加えてケイ酸液を多孔質粒子表面に沈着させる。なお、ケイ酸液と上記アルコキシシランを併用してシリカ保護膜を作製してもよい。
(第3工程:シリカ被覆層の形成)
第3工程では、第2工程で調製した多孔質粒子分散液(空洞粒子の場合は空洞粒子前駆体分散液)に、フッ素置換アルキル基含有シラン化合物を含有する加水分解性の有機珪素化合物またはケイ酸液等を加えることにより、粒子の表面を加水分解性有機珪素化合物またはケイ酸液等の重合物で被覆してシリカ被覆層を形成する。
When the dispersion medium of the porous particle precursor is water alone or when the ratio of water to the organic solvent is high, a silica protective film can be formed using a silicic acid solution. When a silicic acid solution is used, a predetermined amount of the silicic acid solution is added to the dispersion, and at the same time an alkali is added to deposit the silicic acid solution on the surface of the porous particles. In addition, you may produce a silica protective film together using a silicic acid liquid and the said alkoxysilane.
(3rd process: Formation of a silica coating layer)
In the third step, a hydrolyzable organosilicon compound or silica containing a fluorine-substituted alkyl group-containing silane compound is added to the porous particle dispersion (in the case of hollow particles, a hollow particle precursor dispersion) prepared in the second step. By adding an acid solution or the like, the surface of the particles is coated with a hydrolyzable organosilicon compound or a polymer such as a silicic acid solution to form a silica coating layer.

なお、ケイ酸液とは、水ガラス等のアルカリ金属ケイ酸塩の水溶液をイオン交換処理して脱アルカリしたケイ酸の低重合物の水溶液である。   The silicic acid solution is an aqueous solution of a low silicic acid polymer obtained by dealkalizing an aqueous solution of an alkali metal silicate such as water glass by ion exchange treatment.

被覆層形成用に使用される有機珪素化合物またはケイ酸液の添加量は、コロイド粒子の表面を十分被覆できる程度であればよく、最終的に得られるシリカ被覆層の厚さが1〜40nm、好ましくは1〜20nmとなるように量で、多孔質粒子(空洞粒子の場合は空洞粒子前駆体)分散液中で添加される。またシリカ保護膜を形成した場合はシリカ保護膜とシリカ被覆層の合計の厚さが1〜40nm、好ましくは1〜20nmの範囲となるような量で、有機珪素化合物またはケイ酸液は添加される。   The addition amount of the organosilicon compound or silicic acid solution used for forming the coating layer only needs to be sufficient to cover the surface of the colloidal particles, and the finally obtained silica coating layer has a thickness of 1 to 40 nm, Preferably, it is added in an amount of 1 to 20 nm in a dispersion of porous particles (in the case of hollow particles, hollow particle precursor). When the silica protective film is formed, the organosilicon compound or the silicate solution is added in such an amount that the total thickness of the silica protective film and the silica coating layer is in the range of 1 to 40 nm, preferably 1 to 20 nm. The

ついで、被覆層が形成された粒子の分散液を加熱処理する。加熱処理によって、多孔質粒子の場合は、多孔質粒子表面を被覆したシリカ被覆層が緻密化し、多孔質粒子がシリカ被覆層によって被覆された複合粒子の分散液が得られる。また空洞粒子前駆体の場合、形成された被覆層が緻密化して空洞粒子壁となり、内部が溶媒、気体または多孔質固形分で充填された空洞を有する空洞粒子の分散液が得られる。   Next, the dispersion liquid of the particles on which the coating layer is formed is heat-treated. By the heat treatment, in the case of porous particles, the silica coating layer covering the surface of the porous particles is densified, and a dispersion of composite particles in which the porous particles are coated with the silica coating layer is obtained. In the case of a hollow particle precursor, the formed coating layer is densified to form hollow particle walls, and a dispersion of hollow particles having cavities filled with a solvent, gas, or porous solid content is obtained.

このときの加熱処理温度は、シリカ被覆層の微細孔を閉塞できる程度であれば特に制限はなく、80〜300℃の範囲が好ましい。加熱処理温度が80℃未満ではシリカ被覆層の微細孔を完全に閉塞して緻密化できないことがあり、また処理時間に長時間を要してしまうことがある。また加熱処理温度が300℃を越えて長時間処理すると緻密な粒子となることがあり、低屈折率化の効果が得られないことがある。   The heat treatment temperature at this time is not particularly limited as long as it can close the fine pores of the silica coating layer, and is preferably in the range of 80 to 300 ° C. When the heat treatment temperature is less than 80 ° C., the fine pores of the silica coating layer may not be completely closed and densified, and the treatment time may take a long time. Further, when the heat treatment temperature exceeds 300 ° C. for a long time, fine particles may be formed, and the effect of lowering the refractive index may not be obtained.

このようにして得られた中空シリカ系粒子の屈折率は、1.42未満と低い。このような中空シリカ系粒子は、多孔質粒子内部の多孔性が保持されているか、内部が空洞であるので、屈折率が低くなるものと推察される。   The refractive index of the hollow silica particles thus obtained is as low as less than 1.42. Such hollow silica-based particles are presumed to have a low refractive index because the porosity inside the porous particles is maintained or the inside is hollow.

また、塗布組成物に添加したときの安定性の点から中空粒子としては、表面に炭化水素主鎖を有するポリマーが共有結合している中空粒子が好ましい。   From the viewpoint of stability when added to the coating composition, the hollow particles are preferably hollow particles in which a polymer having a hydrocarbon main chain is covalently bonded to the surface.

つぎに、炭化水素主鎖を有するポリマーが共有結合している中空粒子について説明する。炭化水素主鎖を有するポリマーとは、直接共有結合、または中空シリカ系粒子の表面のシリカと炭化水素主鎖を有するポリマーとの間に結合剤を介在させ、シリカと結合剤とを共有結合し、結合剤とポリマーとが共有結合しているものも言う。結合剤としては、カップリング剤が好ましく用いられる。   Next, hollow particles in which a polymer having a hydrocarbon main chain is covalently bonded will be described. The polymer having a hydrocarbon main chain is a direct covalent bond, or a binder is interposed between the silica on the surface of the hollow silica-based particle and the polymer having the hydrocarbon main chain, and the silica and the binder are covalently bonded. It also refers to those in which the binder and the polymer are covalently bonded. As the binder, a coupling agent is preferably used.

炭化水素主鎖を有するポリマーが共有結合している中空粒子は、(1)中空シリカ系粒子表面を未処理、もしくはカップリング剤などで処理した状態で、中空シリカ系粒子表面と共有結合を形成可能な官能基を有するポリマーを反応させ、中空シリカ系粒子表面にポリマーをグラフトさせる方法、あるいは(2)中空シリカ系粒子表面を未処理、もしくはカップリング剤などで処理した状態で、中空シリカ系粒子表面から単量体を重合することでポリマー鎖を生長させ、表面グラフトさせる方法等により製造することができる。具体的な製造方法としては、特開2006−257308号公報に記載の方法を用いることができる。   Hollow particles to which a polymer having a hydrocarbon main chain is covalently bonded (1) Forms a covalent bond with the surface of the hollow silica particle in the state where the surface of the hollow silica particle is untreated or treated with a coupling agent or the like. A method in which a polymer having a functional group is reacted and the polymer is grafted on the surface of the hollow silica particle; or (2) the hollow silica system in a state where the surface of the hollow silica particle is untreated or treated with a coupling agent or the like. It can be produced by a method of polymerizing a monomer from the particle surface to grow a polymer chain and surface grafting. As a specific manufacturing method, the method described in JP-A-2006-257308 can be used.

上記製造方法では、表面修飾率向上の観点から、中空シリカ系粒子表面から単量体を重合することでポリマー鎖を生長させ、表面グラフトさせる方法が好ましい。重合開始能、もしくは連鎖移動能を有する官能基を含むカップリング剤で中空シリカ系粒子を表面処理し、そこから単量体を重合し、ポリマー鎖を生長させて表面グラフトさせる方法がさらに好ましい。重合開始能もしくは連鎖移動能を有する官能基を、中空シリカ系粒子に導入するための表面処理剤(カップリング剤)としては、アルコキシ金属化合物(例えばチタンカップリング剤、アルコキシシラン化合物(シランカップリング剤))が好ましく用いられる。   In the above production method, from the viewpoint of improving the surface modification rate, a method of polymerizing a monomer from the surface of the hollow silica-based particle to grow a polymer chain and grafting the surface is preferable. More preferred is a method in which a hollow silica-based particle is surface-treated with a coupling agent containing a functional group having a polymerization initiating ability or a chain transfer ability, a monomer is polymerized therefrom, a polymer chain is grown, and the surface is grafted. As a surface treatment agent (coupling agent) for introducing a functional group having a polymerization initiating ability or a chain transfer ability into hollow silica particles, an alkoxy metal compound (for example, a titanium coupling agent, an alkoxysilane compound (silane coupling) Agent)) is preferably used.

中空シリカ系粒子は平均粒径の異なる2種以上の中空シリカ系粒子を含有していてもよい。   The hollow silica particles may contain two or more kinds of hollow silica particles having different average particle diameters.

本発明に係る低屈折率層には、導電性金属酸化物被覆層を有する中空シリカ系粒子を用いることも、導電性をさらに高めることができ好ましい。導電性金属酸化物被覆層を形成する金属酸化物としては特に制限はないが、例えば、酸化スズ、アンチモンスズ酸化物、インジウムスズ酸化物、酸化アンチモン、アルミニウム亜鉛酸化物、ガリウム亜鉛酸化物およびこれらの混合物から選ばれるものが挙げられる。この中でも、酸化アンチモンにより被覆されている中空シリカ系粒子が特に好ましい。   For the low refractive index layer according to the present invention, it is preferable to use hollow silica-based particles having a conductive metal oxide coating layer because the conductivity can be further increased. The metal oxide for forming the conductive metal oxide coating layer is not particularly limited. For example, tin oxide, antimony tin oxide, indium tin oxide, antimony oxide, aluminum zinc oxide, gallium zinc oxide, and these The thing chosen from the mixture of these is mentioned. Among these, hollow silica particles coated with antimony oxide are particularly preferable.

導電性金属酸化物被覆層の平均厚さとしては、1〜40nm、より好ましくは1〜20nmの範囲であり、中空シリカ系粒子を十分に被覆でき、得られる導電性金属酸化物被覆中空シリカ系粒子の導電性が十分となる点で、被覆層の厚さは1nm以上が好ましい。導電性の向上効果が十分で、導電性金属酸化物被覆中空シリカ系粒子の平均粒子径が小さい場合にも屈折率が十分である点で、被覆層の厚さは40nm以下が好ましい。   The average thickness of the conductive metal oxide coating layer is in the range of 1 to 40 nm, more preferably 1 to 20 nm, the hollow silica-based particles can be sufficiently coated, and the resulting conductive metal oxide-coated hollow silica system The thickness of the coating layer is preferably 1 nm or more in that the conductivity of the particles is sufficient. The thickness of the coating layer is preferably 40 nm or less in that the effect of improving the conductivity is sufficient and the refractive index is sufficient even when the average particle size of the conductive metal oxide-coated hollow silica-based particles is small.

本発明の特に好ましい態様である酸化アンチモン被覆層を有する中空シリカ系粒子について説明する。   A hollow silica-based particle having an antimony oxide coating layer, which is a particularly preferred embodiment of the present invention, will be described.

酸化アンチモンは、Sb23、Sb25、SbO2等いずれでも良く、酸化アンチモン被覆層中には酸化スズなどを含有していても良い。酸化アンチモン被覆層中のこれらの酸化アンチモンの合計含有率は10%以上が好ましい。また、酸化アンチモン被覆層は、さらにシリカ等で被覆されていても良い。 The antimony oxide may be any of Sb 2 O 3 , Sb 2 O 5 , SbO 2 and the like, and the antimony oxide coating layer may contain tin oxide or the like. The total content of these antimony oxides in the antimony oxide coating layer is preferably 10% or more. The antimony oxide coating layer may be further coated with silica or the like.

酸化アンチモン被覆中空シリカ粒子の体積抵抗値は、10〜5000Ω/cmが好ましく、10〜2000Ω/cmの範囲にあることがより好ましい。体積抵抗値をこの範囲にすることで、粒子の屈折率を低く保ちつつ、低屈折率塗膜の表面抵抗を低下せしめることが可能となる。体積抵抗値は、核粒子の粒子サイズ、表面被覆金属酸化物層の膜厚、組成を調整することにより制御できる。   The volume resistance value of the antimony oxide-coated hollow silica particles is preferably 10 to 5000 Ω / cm, and more preferably 10 to 2000 Ω / cm. By setting the volume resistance value within this range, the surface resistance of the low refractive index coating film can be lowered while keeping the refractive index of the particles low. The volume resistance value can be controlled by adjusting the particle size of the core particles, the film thickness of the surface-coated metal oxide layer, and the composition.

体積抵抗値については、以下の方法で測定した。   The volume resistance value was measured by the following method.

内部に円柱状のくりぬき(断面積0.5cm2)を有するセラミック製セルを用い、架台電極上にセルを置き、内部に試料粉体0.6gを充填し、円柱状突起を有する上部電極の突起を挿入し、油圧機にて上下電極を加圧し、100kg/cm2加圧時の抵抗値(Ω)と試料の高さ(cm)を測定し、抵抗値に高さを乗することによって求めた。 Using a ceramic cell with a cylindrical hollow (cross-sectional area of 0.5 cm 2 ) inside, place the cell on the gantry electrode, fill with 0.6 g of sample powder inside, and By inserting protrusions, pressing the upper and lower electrodes with a hydraulic machine, measuring the resistance value (Ω) and the sample height (cm) when 100 kg / cm 2 is applied, and multiplying the resistance value by the height Asked.

酸化アンチモン被覆中空シリカ系粒子の製造方法について説明する。   A method for producing antimony oxide-coated hollow silica particles will be described.

まず、多孔質シリカ系粒子、または内部に空洞を有するシリカ系粒子の分散液を前述の方法等により調製する。分散液の固形分濃度として0.1〜40質量%、さらには0.5〜20質量%の範囲にあることが好ましい。固形分濃度が0.1質量%未満の場合は、生産効率が低く、固形分濃度が40質量%を超えると、得られる酸化アンチモン被覆中空シリカ系粒子が凝集することがあり、被膜の透明性が低下したり、ヘイズが悪化することがある。   First, a dispersion of porous silica-based particles or silica-based particles having cavities inside is prepared by the method described above. The solid content concentration of the dispersion is preferably in the range of 0.1 to 40% by mass, more preferably 0.5 to 20% by mass. When the solid content concentration is less than 0.1% by mass, the production efficiency is low, and when the solid content concentration exceeds 40% by mass, the resulting antimony oxide-coated hollow silica-based particles may agglomerate, and the transparency of the film May decrease or haze may deteriorate.

また、アンチモン酸の分散液(水溶液)を調製する。アンチモン酸の調製方法としては、多孔質シリカ系粒子または内部に空洞を有するシリカ系粒子の細孔や空洞を埋めることなく、粒子表面に酸化アンチモンの被覆層を形成することができれば特に制限はないが、以下に示す方法は均一で薄い酸化アンチモン被覆層を形成することができるので好ましい。   Also, an antimonic acid dispersion (aqueous solution) is prepared. The antimonic acid preparation method is not particularly limited as long as the antimony oxide coating layer can be formed on the particle surface without filling the pores and cavities of the porous silica particles or the silica particles having cavities inside. However, the following method is preferable because a uniform and thin antimony oxide coating layer can be formed.

具体的には、アンチモン酸アルカリ水溶液を陽イオン交換樹脂で処理してアンチモン酸(ゲル)分散液を調製し、次いで陰イオン交換樹脂で処理する。アンチモン酸アルカリ水溶液としては、例えば特開平2−180717号公報に記載されている、酸化アンチモンゾルの製造方法に用いるアンチモン酸アルカリ水溶液は好適である。   Specifically, an alkali antimonate aqueous solution is treated with a cation exchange resin to prepare an antimonic acid (gel) dispersion, and then treated with an anion exchange resin. As the alkali antimonate aqueous solution, for example, an alkali antimonate aqueous solution used in a method for producing an antimony oxide sol described in JP-A-2-180717 is suitable.

アンチモン酸アルカリ水溶液は、三酸化アンチモン(Sb23)、アルカリ物質及び過酸化水素を反応させて得たものであることが好ましく、酸化アンチモンとアルカリ物質と過酸化水素のモル比を1:2.0〜2.5:0.8〜1.5、好ましくは1:2.1〜2.3:0.9〜1.2とし、三酸化アンチモンとアルカリ物質を含む系に、過酸化水素を三酸化アンチモン1モルあたり、0.2モル/hr以下の速度で添加して得られる。 The alkali antimonate aqueous solution is preferably obtained by reacting antimony trioxide (Sb 2 O 3 ), an alkali substance and hydrogen peroxide, and the molar ratio of antimony oxide, alkali substance and hydrogen peroxide is 1: 2.0 to 2.5: 0.8 to 1.5, preferably 1: 2.1 to 2.3: 0.9 to 1.2, and the system containing antimony trioxide and an alkaline substance is peroxidized. It is obtained by adding hydrogen at a rate of 0.2 mol / hr or less per mol of antimony trioxide.

この時使用される三酸化アンチモンは、粉末、特に平均粒子径が10μm以下の微粉末のものが好ましく、また、アルカリ物質としては、LiOH、KOH、NaOH、Mg(OH)2、Ca(OH)2等を挙げることができ、中でもKOH、NaOHなどのアルカリ金属水酸化物が好ましい。これらのアルカリ物質は、得られるアンチモン酸溶液を安定化させる効果を有する。 The antimony trioxide used at this time is preferably a powder, particularly a fine powder having an average particle size of 10 μm or less, and examples of the alkaline substance include LiOH, KOH, NaOH, Mg (OH) 2 , and Ca (OH). 2, etc. Among them, alkali metal hydroxides such as KOH and NaOH are preferable. These alkaline substances have the effect of stabilizing the resulting antimonic acid solution.

まず、水に所定量のアルカリ物質と三酸化アンチモンを加えて三酸化アンチモン懸濁液を調製する。この三酸化アンチモン懸濁液の三酸化アンチモン濃度は、Sb23として3〜15質量%の範囲とすることが望ましい。次いで、この懸濁液を50℃以上、好ましくは80℃以上に加温し、これに濃度が5〜35質量%の過酸化水素水を三酸化アンチモン1モルあたり0.2モル/hr以下の速度で添加する。過酸化水素水の添加速度が0.2モル/hrより速い場合は、得られる酸化アンチモン粒子の粒子径が大きくなり、粒子径分布が広がるので好ましくない。また、過酸化水素水の添加速度が非常に遅い場合は生産性が悪いので、好ましい添加速度範囲としては、0.04〜0.2モル/hrの範囲である。 First, a predetermined amount of an alkaline substance and antimony trioxide are added to water to prepare an antimony trioxide suspension. The antimony trioxide concentration of the antimony trioxide suspension is preferably in the range of 3 to 15% by mass as Sb 2 O 3 . Next, the suspension is heated to 50 ° C. or higher, preferably 80 ° C. or higher, and hydrogen peroxide solution having a concentration of 5 to 35% by mass is added to 0.2 mol / hr or less of antimony trioxide. Add at a rate. When the hydrogen peroxide solution is added at a rate higher than 0.2 mol / hr, the particle size of the obtained antimony oxide particles is increased, and the particle size distribution is widened, which is not preferable. Moreover, since productivity is bad when the addition rate of hydrogen peroxide water is very slow, a preferable addition rate range is 0.04 to 0.2 mol / hr.

上記反応で得られたアンチモン酸アルカリ(MHSbO3:Mがアルカリ金属の場合)水溶液を、必要に応じて未溶解の残渣を分離した後、さらに必要に応じて希釈し、陽イオン交換樹脂で処理し、アルカリイオンを除去することによってアンチモン酸ゲル(HSbO3 -n分散液を調製する。 Alkali antimonate obtained by the above reaction (MHSbO 3: If M is an alkali metal) of an aqueous solution, after separation of the undissolved residues optionally, diluted if necessary, treated with a cation exchange resin Then, an antimonic acid gel (HSbO 3 ) n dispersion is prepared by removing alkali ions.

また、アンチモン酸アルカリ水溶液には、スズ酸アルカリ水溶液、リン酸ナトリウム水溶液等のドーピング剤を含む水溶液が含まれていても良い。このようなドーピング剤が含まれているとさらに導電性の高い酸化アンチモン被覆中空シリカ系粒子が得られる。   Further, the alkali antimonate aqueous solution may contain an aqueous solution containing a doping agent such as an alkali stannate aqueous solution and a sodium phosphate aqueous solution. When such a doping agent is contained, antimony oxide-coated hollow silica-based particles having higher conductivity can be obtained.

ここで、アンチモン酸は、(HSbO3 -n(n=2以上の重合体)で表すことができ、粒子径が1〜5nm程度のアンチモン酸(HSbO3 -)の重合物からなり、微粒子が凝集し、ゲル状態を呈している。 Here, antimonic acid can be represented by (HSbO 3 ) n (a polymer having n = 2 or more), and is composed of a polymer of antimonic acid (HSbO 3 ) having a particle diameter of about 1 to 5 nm. Are aggregated to form a gel state.

陽イオン交換樹脂で処理する際のアンチモン酸アルカリ水溶液の濃度は、固形分Sb25として0.01〜5質量%、さらには0.1〜3質量%の範囲にあることが好ましい。固形分として0.01質量%未満の場合は生産効率が低く、5質量%を超えるとアンチモン酸の大きな凝集体が生成することがあり、アンチモン酸による中空シリカ系粒子の被覆ができにくく、できたとしても不均一になることがある。 The concentration of the alkali antimonate aqueous solution used in the treatment with the cation exchange resin is preferably in the range of 0.01 to 5% by mass, more preferably 0.1 to 3% by mass as the solid content Sb 2 O 5 . When the solid content is less than 0.01% by mass, the production efficiency is low. In some cases, it may become non-uniform.

陽イオン交換樹脂の使用量は、得られるアンチモン酸分散液のpHが1〜4、さらには1.5〜3.5の範囲とすることが好ましい。pH1未満の場合は鎖状粒子にならず凝集粒子が生成する傾向にあり、pH4を超えると単分散粒子が生成する傾向がある。また、pH1未満の場合は、酸化アンチモンの溶解度が高いために所定量の酸化アンチモンの被覆が困難になり、pH4を超えると、得られる酸化アンチモン被覆中空シリカ系粒子が凝集体となることがあり、被膜中での分散性が低下したり、帯電防止効果が不十分となることがある。   The amount of the cation exchange resin used is preferably such that the pH of the resulting antimonic acid dispersion is in the range of 1 to 4, more preferably in the range of 1.5 to 3.5. When the pH is less than 1, there is a tendency that aggregated particles are generated instead of chain particles, and when the pH exceeds 4, monodispersed particles tend to be generated. In addition, when the pH is less than 1, the solubility of antimony oxide is high, so that it is difficult to coat a predetermined amount of antimony oxide. When the pH exceeds 4, the obtained antimony oxide-coated hollow silica-based particles may be aggregated. In some cases, the dispersibility in the film may be reduced, and the antistatic effect may be insufficient.

次いで、アンチモン酸分散液と多孔質シリカ系粒子、または内部に空洞を有するシリカ系粒子の分散液とを混合し、50〜250℃、好ましくは70〜120℃で、通常1〜24時間熟成を行うことによって酸化アンチモン被覆中空シリカ系粒子分散液を得ることができる。   Next, the antimonic acid dispersion and porous silica-based particles or a dispersion of silica-based particles having cavities inside are mixed and aged at 50 to 250 ° C., preferably 70 to 120 ° C., usually for 1 to 24 hours. By performing this, an antimony oxide-coated hollow silica-based particle dispersion can be obtained.

アンチモン酸分散液とシリカ系粒子分散液との混合比率は、シリカ系粒子を固形分として100質量部に、アンチモン酸をSb25として1〜200質量部、好ましくは5〜100質量部となるように添加する。アンチモン酸の混合比率が1質量部未満の場合は、被覆が不均一であったり被覆層の厚さが不十分となり、酸化アンチモンで被覆する効果、即ち、導電性を付与、向上する効果が十分に得られないことがある。アンチモン酸の混合比率が200質量部を超えても、被覆に寄与しない酸化アンチモンが増加したり、得られる酸化アンチモン被覆中空シリカ系粒子の導電性がさらに向上することも無く、屈折率が1.60を超えて高くなることがある。 The mixing ratio of the antimonic acid dispersion and the silica-based particle dispersion is 100 parts by mass with silica-based particles as a solid content, and 1 to 200 parts by mass, preferably 5 to 100 parts by mass with antimonic acid as Sb 2 O 5. Add as follows. When the mixing ratio of antimonic acid is less than 1 part by mass, the coating is uneven or the thickness of the coating layer becomes insufficient, and the effect of coating with antimony oxide, that is, the effect of imparting and improving conductivity is sufficient. May not be obtained. Even when the mixing ratio of antimonic acid exceeds 200 parts by mass, the antimony oxide that does not contribute to the coating does not increase, and the conductivity of the resulting antimony oxide-coated hollow silica-based particles is not further improved. May be higher than 60.

混合した分散液の濃度は固形分として1〜40質量%、さらには2〜30質量%の範囲にあることが好ましい。混合分散液の濃度が1質量%未満の場合は、酸化アンチモンの被覆効率が不十分であったり、生産効率が低下する。一方40質量%を超えるとアンチモン酸の使用量が多い場合に、得られる酸化アンチモン被覆中空シリカ系粒子が凝集することがある。   It is preferable that the density | concentration of the mixed dispersion exists in the range of 1-40 mass% as solid content, and also 2-30 mass%. When the concentration of the mixed dispersion is less than 1% by mass, the coating efficiency of antimony oxide is insufficient or the production efficiency is lowered. On the other hand, when it exceeds 40 mass%, when the amount of antimonic acid used is large, the resulting antimony oxide-coated hollow silica-based particles may aggregate.

本発明に係る低屈折率層には、触媒を含有することが好ましい。触媒としては、塩酸、硫酸、硝酸等の無機酸類、シュウ酸、酢酸、ギ酸、メタンスルホン酸等の有機酸類、水酸化ナトリウム、水酸化カリウム、アンモニア等の無機塩基類、トリエチルアミン、ピリジン等の有機塩基類、トリイソプロポキシアルミニウム、テトラブトキシジルコニウム等の金属アルコキシド類、後述する金属キレート化合物等が挙げられるが、中でも酸触媒および金属キレート化合物が好ましく用いられる。   The low refractive index layer according to the present invention preferably contains a catalyst. Catalysts include inorganic acids such as hydrochloric acid, sulfuric acid and nitric acid, organic acids such as oxalic acid, acetic acid, formic acid and methanesulfonic acid, inorganic bases such as sodium hydroxide, potassium hydroxide and ammonia, and organic acids such as triethylamine and pyridine. Examples include bases, metal alkoxides such as triisopropoxyaluminum and tetrabutoxyzirconium, metal chelate compounds described later, and the like. Among them, acid catalysts and metal chelate compounds are preferably used.

酸触媒では塩酸、硫酸、シュウ酸、酢酸、フタル酸等が好ましく用いられる。金属キレート化合物としては、Zr、Ti、Alから選ばれる金属を中心金属とするキレート化合物が、特に制限なく好適に用いることができる。   As the acid catalyst, hydrochloric acid, sulfuric acid, oxalic acid, acetic acid, phthalic acid and the like are preferably used. As the metal chelate compound, a chelate compound having a metal selected from Zr, Ti, and Al as a central metal can be suitably used without particular limitation.

具体例としては、トリ−n−ブトキシエチルアセトアセテートジルコニウム、ジ−n−ブトキシビス(エチルアセトアセテート)ジルコニウム、n−ブトキシトリス(エチルアセトアセテート)ジルコニウム、テトラキス(n−プロピルアセトアセテート)ジルコニウム、テトラキス(アセチルアセトアセテート)ジルコニウム、テトラキス(エチルアセトアセテート)ジルコニウムなどのジルコニウムキレート化合物、ジイソプロポキシビス(エチルアセトアセテート)チタニウム、ジイソプロポキシビス(アセチルアセテート)チタニウム、ジイソプロポキシビス(アセチルアセトン)チタニウムなどのチタニウムキレート化合物、ジイソプロポキシエチルアセトアセテートアルミニウム、ジイソプロポキシアセチルアセトナートアルミニウム、イソプロポキシビス(エチルアセトアセテート)アルミニウム、イソプロポキシビス(アセチルアセトナート)アルミニウム、トリス(エチルアセトアセテート)アルミニウム、トリス(アセチルアセトナート)アルミニウム、モノアセチルアセトナートビス(エチルアセトアセテート)アルミニウムなどのアルミニウムキレート化合物などが挙げられる。   Specific examples include tri-n-butoxyethyl acetoacetate zirconium, di-n-butoxybis (ethyl acetoacetate) zirconium, n-butoxy tris (ethyl acetoacetate) zirconium, tetrakis (n-propyl acetoacetate) zirconium, tetrakis ( Zirconium chelate compounds such as acetylacetoacetate) zirconium, tetrakis (ethylacetoacetate) zirconium, diisopropoxybis (ethylacetoacetate) titanium, diisopropoxybis (acetylacetate) titanium, diisopropoxybis (acetylacetone) titanium, etc. Titanium chelate compound, diisopropoxyethyl acetoacetate aluminum, diisopropoxyacetylacetonate aluminum , Isopropoxybis (ethylacetoacetate) aluminum, isopropoxybis (acetylacetonate) aluminum, tris (ethylacetoacetate) aluminum, tris (acetylacetonato) aluminum, monoacetylacetonatobis (ethylacetoacetate) aluminum, etc. Examples of the aluminum chelate compound.

これらの金属キレート化合物のうち、トリ−n−ブトキシエチルアセトアセテートジルコニウム、ジイソプロポキシエチルアセトアセテートアルミニウム、トリス(エチルアセトアセテート)アルミニウムが特に好ましく用いられる。また、これらの金属キレート化合物は、単独でも併用でも使用することができる。   Of these metal chelate compounds, tri-n-butoxyethyl acetoacetate zirconium, diisopropoxyethyl acetoacetate aluminum, and tris (ethyl acetoacetate) aluminum are particularly preferably used. These metal chelate compounds can be used either alone or in combination.

また、本発明に係る低屈折率層には、下記一般式(2)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物を含有することが好ましい。   The low refractive index layer according to the present invention preferably contains an organosilicon compound represented by the following general formula (2), a hydrolyzate thereof or a polycondensate thereof.

2 mSiX2 4-m (2)
式中、R2は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X2は水酸基または加水分解可能な置換基であり、mは0〜3の整数である。
R 2 m SiX 2 4-m (2)
In the formula, R 2 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 2 is a hydroxyl group or a hydrolyzable substituent, and m is an integer of 0 to 3.

アルキル基としては、メチル基、エチル基、プロピル基、イソプロピル基、t−ブチル基、s−ブチル基、ヘキシル基、デシル基、ヘキサデシル基等が挙げられる。アリール基としてはフェニル基、ナフチル基等が挙げられる。   Examples of the alkyl group include methyl group, ethyl group, propyl group, isopropyl group, t-butyl group, s-butyl group, hexyl group, decyl group, hexadecyl group and the like. Examples of the aryl group include a phenyl group and a naphthyl group.

2の加水分解可能な置換基としては、アルコキシ基、ハロゲン基、カルボキシル基等が挙げられる。 Examples of the hydrolyzable substituent for X 2 include an alkoxy group, a halogen group, and a carboxyl group.

具体例としては、テトラメトキシシラン、テトラエトキシシラン、メチルトリメトキシシラン、メチルトリエトキシシラン、ジメチルジメトキシシラン、ジメチルジエトキシシラン、フェニルトリメトキシシラン、フェニルトリエトキシシラン、ジフェニルジメトキシシラン、ジフェニルジエトキシシラン、ヘキシルトリメトキシシラン、ヘキシルトリエトキシシラン、デシルトリメトキシシラン、デシルトリエトキシシラン、イソブチルトリメトキシシラン、トリフルオロプロピルトリメトキシシラン、ビニルトリメトキシシラン、ビニルトリエトキシシラン、ビニルトリアセトキシシラン、ビニルトリメトキシエトキシシラン、3−クロロプロピルトリメトキシシラン、3−クロロプロピルトリエトキシシラン、3−グリシドキシプロピルトリメトキシシラン、3−グリシドキシプロピルトリエトキシシラン、3−グリシドキシプロピルメチルジエトキシシラン、2−(3,4−エポシシシクロヘキシル)エチルトリメトキシシラン、2−(3,4−エポキシシクロヘキシル)エチルトリエトキシシラン、3−アクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルトリメトキシシラン、3−メタクリロキシプロピルトリエトキシシラン、3−メタクリロキシプロピルメチルジメトキシシラン、3−メタクリロキシプロピルメチルジエトキシシラン、3−アミノプロピルトリメトキシシラン、3−アミノプロピルトリエトキシシラン、N−2−アミノエチル−3−アミノプロピルメチルジメトキシシラン、N−2−アミノエチル−3−アミノプロピルトリメトキシシラン、N−2−アミノエチル−3−アミノプロピルトリエトキシシラン、3−トリエトキシシリル−N−1,3−ジメチルブチリデンプロピルアミン、N−フェニル−3−アミノプロピルトリメトキシシラン、3−メルカプトプロピルトリメトキシシラン、3−メルカプトプロピルメチルジメトキシシラン、3−イソシアネートプロピルトリエトキシシラン、p−スチリルトリメトキシシラン、ジエチルシラン等が挙げられ、これらを単独または2種以上を混合して用いられる。   Specific examples include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane. , Hexyltrimethoxysilane, hexyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, isobutyltrimethoxysilane, trifluoropropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, vinyltri Methoxyethoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 3-glycidoxypropi Trimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2- (3,4-epoxycyclohexyl) ethyltrimethoxysilane, 2- (3,4-epoxycyclohexyl) ) Ethyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxy Silane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropylmethyldimethoxysilane, N-2-aminoethyl-3-aminopropyltrimeth Sisilane, N-2-aminoethyl-3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-1,3-dimethylbutylidenepropylamine, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercapto Examples thereof include propyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, p-styryltrimethoxysilane, diethylsilane and the like, and these are used alone or in admixture of two or more.

低屈折率層を形成する塗布組成物には、有機溶媒を含有することが好ましい。具体的な有機溶媒の例としては、アルコール(例、メタノール、エタノール、イソプロパノール、ブタノール、ベンジルアルコール)、ケトン(例、アセトン、メチルエチルケトン、メチルイソブチルケトン、シクロヘキサノン)、エステル(例、酢酸メチル、酢酸エチル、酢酸プロピル、酢酸ブチル、蟻酸メチル、蟻酸エチル、蟻酸プロピル、蟻酸ブチル)、脂肪族炭化水素(例、ヘキサン、シクロヘキサン)、ハロゲン化炭化水素(例、メチレンクロライド、クロロホルム、四塩化炭素)、芳香族炭化水素(例、ベンゼン、トルエン、キシレン)、アミド(例、ジメチルホルムアミド、ジメチルアセトアミド、n−メチルピロリドン)、エーテル(例、ジエチルエーテル、ジオキサン、テトラハイドロフラン)、エーテルアルコール(例、1−メトキシ−2−プロパノール)、プロピレングリコールモノメチルエーテル、プロピレングリコールモノメチルエーテルアセテートが挙げられる。中でも、トルエン、メチルエチルケトン、メチルイソブチルケトン、シクロヘキサノン、エタノール、イソプロパノール及びプロピレングリコールモノメチルエーテルが特に好ましい。   The coating composition for forming the low refractive index layer preferably contains an organic solvent. Specific examples of organic solvents include alcohols (eg, methanol, ethanol, isopropanol, butanol, benzyl alcohol), ketones (eg, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone), esters (eg, methyl acetate, ethyl acetate). , Propyl acetate, butyl acetate, methyl formate, ethyl formate, propyl formate, butyl formate), aliphatic hydrocarbons (eg, hexane, cyclohexane), halogenated hydrocarbons (eg, methylene chloride, chloroform, carbon tetrachloride), aromatic Group hydrocarbon (eg, benzene, toluene, xylene), amide (eg, dimethylformamide, dimethylacetamide, n-methylpyrrolidone), ether (eg, diethyl ether, dioxane, tetrahydrofuran), ether alcohol (eg, 1-methoxy-2-propanol), propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate. Of these, toluene, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, ethanol, isopropanol, and propylene glycol monomethyl ether are particularly preferable.

低屈折率層を形成する塗布組成物中の固形分濃度は、1〜4質量%であることが好ましく、固形分濃度を4質量%以下とすることによって、塗布ムラが生じにくくなり、1質量%以上とすることによって、乾燥負荷が軽減される。   The solid content concentration in the coating composition for forming the low refractive index layer is preferably 1 to 4% by mass. By setting the solid content concentration to 4% by mass or less, coating unevenness is less likely to occur, and 1% by mass. By setting it as% or more, the drying load is reduced.

低屈折率層を形成する塗布組成物には、フッ素系またはシリコーン系の界面活性剤を含有することが好ましい。上記界面活性剤を含有させることで、塗布ムラを低減したり膜表面の防汚性を向上させるのに有効である。   The coating composition for forming the low refractive index layer preferably contains a fluorine-based or silicone-based surfactant. Inclusion of the surfactant is effective for reducing coating unevenness and improving the antifouling property of the film surface.

フッ素系界面活性剤としては、パーフルオロアルキル基を含有するモノマー、オリゴマー、ポリマーを母核としたもので、ポリオキシエチレンアルキルエーテル、ポリオキシエチレンアルキルアリルエーテル、ポリオキシエチレン等の誘導体等が挙げられる。   Fluorosurfactants include perfluoroalkyl group-containing monomers, oligomers, and polymers as the core, and include derivatives such as polyoxyethylene alkyl ether, polyoxyethylene alkyl allyl ether, and polyoxyethylene. It is done.

フッ素系界面活性剤は市販品を用いることもでき、例えばサーフロン「S−381」、「S−382」、「SC−101」、「SC−102」、「SC−103」、「SC−104」(何れも旭硝子株式会社製)、フロラード「FC−430」、「FC−431」、「FC−173」(何れもフロロケミカル−住友スリーエム製)、エフトップ「EF352」、「EF301」、「EF303」(何れも新秋田化成株式会社製)、シュベゴーフルアー「8035」、「8036」(何れもシュベグマン社製)、「BM1000」、「BM1100」(いずれもビーエム・ヒミー社製)、メガファック「F−171」、「F−470」(いずれも大日本インキ化学工業株式会社製)、等を挙げることができる。   Commercially available products may be used as the fluorosurfactant, for example, Surflon “S-381”, “S-382”, “SC-101”, “SC-102”, “SC-103”, “SC-104”. (All manufactured by Asahi Glass Co., Ltd.), FLORARD “FC-430”, “FC-431”, “FC-173” (all manufactured by Fluorochemical-Sumitomo 3M), F-top “EF352”, “EF301”, “ EF303 "(both manufactured by Shin-Akita Kasei Co., Ltd.), Schwego Fureer" 8035 "," 8036 "(both manufactured by Schwegman)," BM1000 "," BM1100 "(all manufactured by BM Himmy), Mega Fucks “F-171”, “F-470” (both manufactured by Dainippon Ink & Chemicals, Inc.) and the like can be mentioned.

フッ素系界面活性剤のフッ素含有割合は、0.05〜2質量%、好ましくは0.1〜1質量%である。上記のフッ素系界面活性剤は、1種または2種以上を併用することができる。   The fluorine content of the fluorosurfactant is 0.05 to 2% by mass, preferably 0.1 to 1% by mass. One or two or more of the above fluorosurfactants can be used in combination.

つぎに、シリコーン界面活性剤について説明する。   Next, the silicone surfactant will be described.

シリコーン界面活性剤は、ケイ素原子に結合した有機基の種類により、ストレートシリコーンオイルと変性シリコーンオイルに大別できる。   Silicone surfactants can be broadly classified into straight silicone oils and modified silicone oils depending on the type of organic group bonded to the silicon atom.

ここで、ストレートシリコーンオイルとは、メチル基、フェニル基、水素原子を置換基として結合したものをいう。変性シリコーンオイルとは、ストレートシリコーンオイルから二次的に誘導された構成部分をもつものである。一方、シリコーンオイルの反応性からも分類することができる。これらをまとめると、以下のようになる。
(シリコーンオイル)
1.ストレートシリコーンオイル
1−1.非反応性シリコーンオイル:ジメチル、メチルフェニル置換等。
Here, the straight silicone oil refers to one in which a methyl group, a phenyl group, or a hydrogen atom is bonded as a substituent. A modified silicone oil is one having components derived secondarily from straight silicone oil. On the other hand, it can be classified from the reactivity of silicone oil. These are summarized as follows.
(Silicone oil)
1. Straight silicone oil 1-1. Non-reactive silicone oil: dimethyl, methylphenyl substitution, etc.

1−2.反応性シリコーンオイル:メチル水素置換等。
2.変性シリコーンオイル
ジメチルシリコーンオイルに、さまざまな有機基を導入することで生まれたものが変性シリコーンオイルである。
1-2. Reactive silicone oil: methyl hydrogen substitution and the like.
2. Modified silicone oil Modified silicone oil is born by introducing various organic groups into dimethyl silicone oil.

2−1.非反応性変性シリコーンオイル:アルキル、アルキル/アラルキル、アルキル/ポリエーテル、ポリエーテル、高級脂肪酸エステル置換等。   2-1. Non-reactive modified silicone oil: alkyl, alkyl / aralkyl, alkyl / polyether, polyether, higher fatty acid ester substitution, etc.

アルキル/アラルキル変性シリコーンオイルは、ジメチルシリコーンオイルのメチル基の一部を長鎖アルキル基あるいはフェニルアルキル基が置換したシリコーンオイルである。   The alkyl / aralkyl-modified silicone oil is a silicone oil in which a part of the methyl group of dimethyl silicone oil is substituted with a long-chain alkyl group or a phenylalkyl group.

ポリエーテル変性シリコーンオイルは、親水性のポリオキシアルキレンを疎水性のジメチルシリコーンを導入した界面活性剤である。   The polyether-modified silicone oil is a surfactant in which hydrophobic dimethyl silicone is introduced into hydrophilic polyoxyalkylene.

高級脂肪酸変性シリコーンオイルは、ジメチルシリコーンオイルのメチル基の一部を高級脂肪酸エステルに置換えたシリコーンオイルである。   The higher fatty acid-modified silicone oil is a silicone oil in which a part of the methyl group of dimethyl silicone oil is replaced with a higher fatty acid ester.

アミノ変性シリコーンオイルは、シリコーンオイルのメチル基の一部をアミノアルキル基に置換えた構造をもつシリコーンオイルである。   The amino-modified silicone oil is a silicone oil having a structure in which a part of the methyl group of the silicone oil is substituted with an aminoalkyl group.

エポキシ変性シリコーンオイルは、シリコーンオイルのメチル基の一部をエポキシ基含有アルキル基に置換えた構造をもつシリコーンオイルである。   The epoxy-modified silicone oil is a silicone oil having a structure in which a part of the methyl group of the silicone oil is substituted with an epoxy group-containing alkyl group.

カルボキシル変性あるいはアルコール変性シリコーンオイルは、シリコーンオイルのメチル基の一部をカルボキシル基あるいは水酸基含有アルキル基に置換えた構造をもつシリコーンオイルである。   The carboxyl-modified or alcohol-modified silicone oil is a silicone oil having a structure in which a part of the methyl group of the silicone oil is substituted with a carboxyl group or a hydroxyl group-containing alkyl group.

これらのうち、ポリエーテル変性シリコーンオイルが好ましく添加される。ポリエーテル変性シリコーンオイルの数平均分子量は、例えば1,000〜100,000、好ましくは2,000〜50,000が適当であり、数平均分子量が1,000未満では、塗膜の乾燥性が低下し、逆に、数平均分子量が100,000を越えると、塗膜表面にブリードアウトしにくくなる。   Of these, polyether-modified silicone oil is preferably added. The number average molecular weight of the polyether-modified silicone oil is, for example, 1,000 to 100,000, preferably 2,000 to 50,000. When the number average molecular weight is less than 1,000, the drying property of the coating film is low. Conversely, if the number average molecular weight exceeds 100,000, bleeding out to the coating surface becomes difficult.

具体的な商品としては、東レダウコーニング社のL−45、L−9300、FZ−3704、FZ−3703、FZ−3720、FZ−3786、FZ−3501、FZ−3504、FZ−3508、FZ−3705、FZ−3707、FZ−3710、FZ−3750、FZ−3760、FZ−3785、FZ−3785、Y−7499、信越化学社のKF96L、KF96、KF96H、KF99、KF54、KF965、KF968、KF56、KF995、KF351、KF351A、KF352、KF353、KF354、KF355、KF615、KF618、KF945、KF6004、FL100、ビックケミージャパン社製の界面活性剤BYKシリーズ、BYK−300/302、BYK−306、BYK−307、BYK−310、BYK−315、BYK−320、BYK−322、BYK−323、BYK−325、BYK−330、BYK−331、BYK−333、BYK−337、BYK−340、BYK−344、BYK−370、BYK−375、BYK−377、BYK−352、BYK−354、BYK−355/356、BYK−358N/361N、BYK−357、BYK−390、BYK−392、BYK−UV3500、BYK−UV3510、BYK−UV3570、BYK−Silclean3700、GE東芝シリコーン社製のジメチルシリコーンシリーズ、XC96−723、YF3800、XF3905、YF3057、YF3807、YF3802、YF3897等が挙げられる。   Specific products include L-45, L-9300, FZ-3704, FZ-3703, FZ-3720, FZ-3786, FZ-3501, FZ-3504, FZ-3508, FZ- from Toray Dow Corning. 3705, FZ-3707, FZ-3710, FZ-3750, FZ-3760, FZ-3785, FZ-3785, Y-7499, Shin-Etsu Chemical KF96L, KF96, KF96H, KF99, KF54, KF965, KF968, KF56, KF995, KF351, KF351A, KF352, KF353, KF354, KF355, KF615, KF618, KF945, KF6004, FL100, surfactants BYK series manufactured by BYK Japan, BYK-300 / 302, BYK-306, BYK-307, BY -310, BYK-315, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-340, BYK-344, BYK-370 BYK-375, BYK-377, BYK-352, BYK-354, BYK-355 / 356, BYK-358N / 361N, BYK-357, BYK-390, BYK-392, BYK-UV3500, BYK-UV3510, BYK -UV3570, BYK-Silklean 3700, dimethyl silicone series manufactured by GE Toshiba Silicone, XC96-723, YF3800, XF3905, YF3057, YF3807, YF3802, YF3897 and the like.

また、シリコーン界面活性剤は、シリコーンオイルのメチル基の一部を親水性基に置換した界面活性剤である。置換の位置は、シリコーンオイルの側鎖、両末端、片末端、両末端側鎖等がある。親水性基としては、ポリエーテル、ポリグリセリン、ピロリドン、ベタイン、硫酸塩、リン酸塩、4級塩等がある。   The silicone surfactant is a surfactant obtained by substituting a part of the methyl group of the silicone oil with a hydrophilic group. The position of substitution includes a side chain of silicone oil, both ends, one end, both end side chains, and the like. Examples of the hydrophilic group include polyether, polyglycerin, pyrrolidone, betaine, sulfate, phosphate, and quaternary salt.

シリコーン界面活性剤としては、疎水基がジメチルポリシロキサン、親水基がポリオキシアルキレンから構成される非イオン界面活性剤が好ましい。   As the silicone surfactant, a nonionic surfactant having a hydrophobic group composed of dimethylpolysiloxane and a hydrophilic group composed of polyoxyalkylene is preferable.

非イオン界面活性剤は、水溶液中でイオンに解離する基を有しない界面活性剤を総称していうが、疎水基のほか親水性基として多価アルコール類の水酸基、また、ポリオキシアルキレン鎖(ポリオキシエチレン)等を親水基として有するものである。親水性はアルコール性水酸基の数が多くなるに従って、またポリオキシアルキレン鎖(ポリオキシエチレン鎖)が長くなるに従って強くなる。疎水基がジメチルポリシロキサン、親水基がポリオキシアルキレンから構成される非イオン界面活性剤を用いると、低屈折率層のムラや膜表面の防汚性が向上する。ポリメチルシロキサンからなる疎水基が表面に配向し汚れにくい膜表面を形成するものと考えられる。   A nonionic surfactant is a generic term for surfactants that do not have a group capable of dissociating into ions in an aqueous solution. Oxyethylene) or the like as a hydrophilic group. Hydrophilicity increases as the number of alcoholic hydroxyl groups increases and as the polyoxyalkylene chain (polyoxyethylene chain) becomes longer. When a nonionic surfactant composed of dimethylpolysiloxane as a hydrophobic group and polyoxyalkylene as a hydrophilic group is used, unevenness of the low refractive index layer and antifouling property of the film surface are improved. It is thought that the hydrophobic group made of polymethylsiloxane is oriented on the surface and forms a film surface that is not easily soiled.

非イオン界面活性剤の具体例としては、例えば東レダウコーニング社のシリコーン界面活性剤SILWET L−77、L−720、L−7001、L−7002、L−7604、Y−7006、FZ−2101、FZ−2104、FZ−2105、FZ−2110、FZ−2118、FZ−2120、FZ−2122、FZ−2123、FZ−2130、FZ−2154、FZ−2161、FZ−2162、FZ−2163、FZ−2164、FZ−2166、FZ−2191、SUPERSILWET SS−2801、SS−2802、SS−2803、SS−2804、SS−2805等が挙げられる。   Specific examples of the nonionic surfactant include silicone surfactants SILWET L-77, L-720, L-7001, L-7002, L-7604, Y-7006, FZ-2101 from Toray Dow Corning, FZ-2104, FZ-2105, FZ-2110, FZ-2118, FZ-2120, FZ-2122, FZ-2123, FZ-2130, FZ-2154, FZ-2161, FZ-2162, FZ-2163, FZ- 2164, FZ-2166, FZ-2191, SUPERSILWET SS-2801, SS-2802, SS-2803, SS-2804, SS-2805, and the like.

これら、疎水基がジメチルポリシロキサン、親水基がポリオキシアルキレンから構成される非イオン界面活性剤の好ましい構造としては、ジメチルポリシロキサン構造部分とポリオキシアルキレン鎖が交互に繰り返し結合した直鎖状のブロックコポリマーであることが好ましい。低屈折率層を形成する塗布組成物を塗布した際のムラ抑制やレベリング性から好ましい。これらの具体例としては、例えば東レダウコーニング社のシリコーン界面活性剤ABN SILWET FZ−2203、FZ−2207、FZ−2208、FZ−2222等が挙げられる。   Preferred structures of these nonionic surfactants comprising a hydrophobic group of dimethylpolysiloxane and a hydrophilic group of polyoxyalkylene include linear structures in which dimethylpolysiloxane structural portions and polyoxyalkylene chains are alternately and repeatedly bonded. A block copolymer is preferred. It is preferable from unevenness suppression and leveling properties when a coating composition for forming a low refractive index layer is applied. Specific examples thereof include silicone surfactants ABN SILWET FZ-2203, FZ-2207, FZ-2208, and FZ-2222 manufactured by Toray Dow Corning.

低屈折率層を形成する塗布組成物には、より過酷な条件下での耐久試験後に本発明の目的効果を発揮しやすい点から、以下に説明する反応性変性シリコーン樹脂(反応性変性シリコーンオイルともいう)を含有することが好ましい。   The coating composition for forming the low refractive index layer has a reactive modified silicone resin (reactive modified silicone oil) to be described below from the viewpoint of easily exerting the object effect of the present invention after a durability test under more severe conditions. (Also referred to as).

2−2.反応性変性シリコーンオイル:アミノ、エポキシ、カルボキシル、アルコール置換等。   2-2. Reactive modified silicone oil: amino, epoxy, carboxyl, alcohol substitution, etc.

反応性変性シリコーン樹脂としては、ポリシロキサンの側鎖、片末端または両末端にアミノ、エポキシ、カルボキシル、水酸基、メタクリル、メルカプト、フェノール等で置換された反応性タイプの変性シリコーン樹脂である。アミノ変性シリコーン樹脂として、具体的にはKF−860,KF−861,X−22−161A、X−22−161B(以上、信越化学工業株式会社製)、FM−3311,FM−3325(以上、チッソ株式会社製)、エポキシ変性シリコーン樹脂としては、KF−105、X−22−163A、X−22−163B、KF−101、KF−1001(以上、信越化学工業株式会社製)、ポリエーテル変性シリコーン樹脂としてはX−22−4272、X−22−4952、カルボキシル変性シリコーン樹脂としてはX−22−3701E、X−22−3710(以上、信越化学工業株式会社製)、カルビノール変性シリコーン樹脂としてはKF−6001、KF−6003(以上、信越化学工業株式会社製)、メタクリル変性シリコーン樹脂としてはX−22−164C(以上、信越化学工業株式会社製)、メルカプト変性シリコーン樹脂としてはKF−2001(以上、信越化学工業株式会社製)、フェノール変性シリコーン樹脂としてはX−22−1821(以上、信越化学工業株式会社製)等が挙げられる。水酸基変性シリコーン樹脂としては、FM−4411、FM−4421、FM−DA21,FM−DA26(以上、チッソ株式会社製)等が挙げられる。その他、片末端反応性シリコーン樹脂のX−22−170DX、X−22−2426、X−22−176F(信越化学工業株式会社製)等も含まれる。   The reactive modified silicone resin is a reactive type modified silicone resin in which the side chain, one end or both ends of polysiloxane is substituted with amino, epoxy, carboxyl, hydroxyl group, methacryl, mercapto, phenol or the like. As amino-modified silicone resins, specifically, KF-860, KF-861, X-22-161A, X-22-161B (above, manufactured by Shin-Etsu Chemical Co., Ltd.), FM-3311, FM-3325 (above, Chisso Corporation), epoxy-modified silicone resins such as KF-105, X-22-163A, X-22-163B, KF-101, KF-1001 (above, Shin-Etsu Chemical Co., Ltd.), polyether-modified X-22-4272, X-22-4952 as silicone resins, X-22-3701E, X-22-3710 (above, manufactured by Shin-Etsu Chemical Co., Ltd.) as carboxyl-modified silicone resins, and carbinol-modified silicone resins KF-6001, KF-6003 (Shin-Etsu Chemical Co., Ltd.), methacryl-modified silicone X-22-164C (made by Shin-Etsu Chemical Co., Ltd.) as the resin, KF-2001 (made by Shin-Etsu Chemical Co., Ltd.) as the mercapto-modified silicone resin, and X-22-1821 as the phenol-modified silicone resin (The above is manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of the hydroxyl group-modified silicone resin include FM-4411, FM-4421, FM-DA21, FM-DA26 (manufactured by Chisso Corporation). In addition, X-22-170DX, X-22-2426, X-22-176F (manufactured by Shin-Etsu Chemical Co., Ltd.) and the like are also included.

上記した界面活性剤は他の界面活性剤と併用して用いてもよく、また、適宜、例えばスルホン酸塩系、硫酸エステル塩系、リン酸エステル塩系等のアニオン界面活性剤、また、ポリオキシエチレン鎖親水基として有するエーテル型、エーテルエステル型等の非イオン界面活性剤等と併用しても良い。上記した界面活性剤の添加量は、低屈折率層塗布組成物中、0.05〜3.0質量%であることが、塗膜の撥水、撥油性、防汚性を高めるばかりでなく、表面の耐擦り傷性にも効果を発揮する点から好ましい。   The above-described surfactants may be used in combination with other surfactants. Also, for example, anionic surfactants such as sulfonate, sulfate, phosphate, etc. You may use together with nonionic surfactants, such as an ether type | mold and ether ester type | mold etc. which have oxyethylene chain hydrophilic group. The addition amount of the surfactant described above is 0.05 to 3.0% by mass in the low refractive index layer coating composition, not only to improve the water repellency, oil repellency and antifouling property of the coating film. From the viewpoint of exerting an effect also on the scratch resistance of the surface.

また、上記した界面活性剤は、塗布ムラを低減させる目的で、導電層にも含有させることができる。   The surfactant described above can also be contained in the conductive layer for the purpose of reducing coating unevenness.

低屈折率層は、グラビアコーター、ディップコーター、リバースコーター、ワイヤーバーコーター、ダイコーター、インクジェット法等公知の方法を用いて、低屈折率層を形成する上記塗布組成物を塗布し、塗布後、加熱乾燥し、必要に応じて硬化処理することで形成される。   The low refractive index layer is a gravure coater, a dip coater, a reverse coater, a wire bar coater, a die coater, a known method such as an inkjet method, and the above coating composition for forming the low refractive index layer is applied, and after coating, It is formed by heat drying and curing treatment as necessary.

塗布量は、ウェット膜厚として0.05〜100μmが適当で、好ましくは、0.1〜50μmである。また、ドライ膜厚が上記膜厚となるように塗布組成物の固形分濃度は調整される。   The coating amount is suitably 0.05 to 100 μm, preferably 0.1 to 50 μm, as the wet film thickness. Further, the solid content concentration of the coating composition is adjusted so that the dry film thickness becomes the above film thickness.

硬化方法としては、加熱することによって熱硬化させる方法、紫外線等の光照射によって硬化させる方法などが挙げられる。熱硬化させる場合は、加熱温度は50〜300℃が好ましく、好ましくは60〜250℃、さらに好ましくは80〜150℃である。光照射によって硬化させる場合は、照射光の露光量は10mJ/cm2〜10J/cm2であることが好ましく、100mJ/cm2〜500mJ/cm2がより好ましい。 Examples of the curing method include a method of thermosetting by heating, a method of curing by irradiation with light such as ultraviolet rays, and the like. In the case of thermosetting, the heating temperature is preferably 50 to 300 ° C, preferably 60 to 250 ° C, more preferably 80 to 150 ° C. When curing by light irradiation, exposure of the irradiation light is preferably, 100mJ / cm 2 ~500mJ / cm 2 and more preferably 10mJ / cm 2 ~10J / cm 2 .

ここで、照射される光の波長域としては特に限定されないが、紫外線領域の波長を有する光が好ましく用いられる。具体的には、低圧水銀灯、中圧水銀灯、高圧水銀灯、超高圧水銀灯、カーボンアーク灯、メタルハライドランプ、キセノンランプ等を用いることができる。照射条件はそれぞれのランプによって異なるが、活性線の照射量は、通常5〜500mJ/cm2、好ましくは5〜150mJ/cm2であるが、特に好ましくは20〜100mJ/cm2である。 Here, the wavelength range of the irradiated light is not particularly limited, but light having a wavelength in the ultraviolet region is preferably used. Specifically, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultrahigh pressure mercury lamp, a carbon arc lamp, a metal halide lamp, a xenon lamp, or the like can be used. Irradiation conditions vary depending on each lamp, but the irradiation amount of active rays is usually 5 to 500 mJ / cm 2 , preferably 5 to 150 mJ / cm 2 , and particularly preferably 20 to 100 mJ / cm 2 .

また、低屈折率層を形成後、温度50〜160℃で加熱処理を行う工程を含んでも良い。加熱処理の期間は、設定される温度によって適宜決定すればよく、例えば50℃であれば、好ましくは3日間以上30日未満の期間、160℃であれば10分以上1日以下の範囲が好ましい。
(ハードコート層:活性線硬化樹脂層)
本発明の反射防止フィルムには、透明樹脂フィルムと反射防止層との間に、ハードコート層として活性線硬化樹脂を含有する層を設けることが、反射防止フィルムの取り扱い性や、反射防止フィルムを後述する偏光板にする際の工程で、傷が付きにくくなることから好ましい。
Moreover, after forming a low refractive index layer, you may include the process of heat-processing at the temperature of 50-160 degreeC. The period of the heat treatment may be appropriately determined depending on the set temperature. For example, if it is 50 ° C., it is preferably a period of 3 days or more and less than 30 days, and if it is 160 ° C., a range of 10 minutes or more and 1 day or less is preferable. .
(Hard coat layer: actinic radiation curable resin layer)
In the antireflection film of the present invention, it is possible to provide a layer containing an active ray curable resin as a hard coat layer between the transparent resin film and the antireflection layer. This is preferable because scratches are less likely to occur in the step of making the polarizing plate described later.

活性線硬化樹脂層とは、紫外線や電子線のような活性線(以下、活性エネルギー線ともいう。)照射により架橋反応等を経て硬化する樹脂を主たる成分とする層をいう。活性線硬化樹脂としては、エチレン性不飽和二重結合を有するモノマーを含む成分が好ましく用いられ、紫外線や電子線のような活性線を照射することによって硬化させて活性線硬化樹脂層が形成される。活性線硬化樹脂としては紫外線硬化性樹脂や電子線硬化性樹脂等が代表的なものとして挙げられるが、紫外線照射によって硬化する樹脂が好ましい。   The actinic radiation curable resin layer refers to a layer mainly composed of a resin that is cured through a crosslinking reaction or the like by irradiation with actinic rays (hereinafter also referred to as actinic energy rays) such as ultraviolet rays and electron beams. As the actinic radiation curable resin, a component containing a monomer having an ethylenically unsaturated double bond is preferably used, and an actinic radiation curable resin layer is formed by curing by irradiation with actinic radiation such as ultraviolet rays or electron beams. The Typical examples of the actinic radiation curable resin include an ultraviolet curable resin and an electron beam curable resin, and a resin curable by ultraviolet irradiation is preferable.

紫外線硬化性樹脂としては、例えば、紫外線硬化型ウレタンアクリレート系樹脂、紫外線硬化型ポリエステルアクリレート系樹脂、紫外線硬化型エポキシアクリレート系樹脂、紫外線硬化型ポリオールアクリレート系樹脂、または紫外線硬化型エポキシ樹脂等が好ましく用いられる。中でも紫外線硬化型アクリレート系樹脂が好ましい。   As the ultraviolet curable resin, for example, an ultraviolet curable urethane acrylate resin, an ultraviolet curable polyester acrylate resin, an ultraviolet curable epoxy acrylate resin, an ultraviolet curable polyol acrylate resin, or an ultraviolet curable epoxy resin is preferable. Used. Of these, ultraviolet curable acrylate resins are preferred.

紫外線硬化型アクリルウレタン系樹脂は、一般にポリエステルポリオールにイソシアネートモノマー、またはプレポリマーを反応させて得られた生成物にさらに2−ヒドロキシエチルアクリレート、2−ヒドロキシエチルメタクリレート(以下アクリレートにはメタクリレートを包含するものとしてアクリレートのみを表示する)、2−ヒドロキシプロピルアクリレート等の水酸基を有するアクリレート系のモノマーを反応させることによって容易に得ることができる。例えば、特開昭59−151110号公報に記載のものを用いることができる。   The UV curable acrylic urethane resin generally includes 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate (hereinafter referred to as acrylate) in addition to a product obtained by reacting a polyester polyol with an isocyanate monomer or a prepolymer. It can be easily obtained by reacting an acrylate monomer having a hydroxyl group such as 2-hydroxypropyl acrylate. For example, those described in JP-A-59-151110 can be used.

例えば、ユニディック17−806(大日本インキ株式会社製)100部とコロネートL(日本ポリウレタン株式会社製)1部との混合物等が好ましく用いられる。   For example, a mixture of 100 parts Unidic 17-806 (Dainippon Ink Co., Ltd.) and 1 part Coronate L (Nihon Polyurethane Co., Ltd.) is preferably used.

紫外線硬化型ポリエステルアクリレート系樹脂としては、一般にポリエステルポリオールに2−ヒドロキシエチルアクリレート、2−ヒドロキシアクリレート系のモノマーを反応させると容易に形成されるものを挙げることができ、特開昭59−151112号公報に記載のものを用いることができる。   Examples of UV curable polyester acrylate resins include those which are easily formed when 2-hydroxyethyl acrylate and 2-hydroxy acrylate monomers are generally reacted with polyester polyols. JP-A-59-151112 Those described in the publication can be used.

紫外線硬化型エポキシアクリレート系樹脂の具体例としては、エポキシアクリレートをオリゴマーとし、これに反応性希釈剤、光重合開始剤を添加し、反応させて生成するものを挙げることができ、特開平1−105738号公報に記載のものを用いることができる。   Specific examples of the ultraviolet curable epoxy acrylate resin include an epoxy acrylate as an oligomer, a reactive diluent and a photopolymerization initiator added thereto, and reacted to form an oligomer. Those described in Japanese Patent No. 105738 can be used.

紫外線硬化型ポリオールアクリレート系樹脂の具体例としては、トリメチロールプロパントリアクリレート、ジトリメチロールプロパンテトラアクリレート、ペンタエリスリトールトリアクリレート、ペンタエリスリトールテトラアクリレート、ジペンタエリスリトールヘキサアクリレート、アルキル変性ジペンタエリスリトールペンタアクリレート等を挙げることができる。   Specific examples of UV curable polyol acrylate resins include trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, alkyl-modified dipentaerythritol pentaacrylate, etc. Can be mentioned.

これら紫外線硬化性樹脂の光重合開始剤としては、具体的には、ベンゾイン及びその誘導体、アセトフェノン、ベンゾフェノン、ヒドロキシベンゾフェノン、ミヒラーズケトン、α−アミロキシムエステル、チオキサントン等及びこれらの誘導体を挙げることができる。光増感剤と共に使用してもよい。上記光重合開始剤も光増感剤として使用できる。また、エポキシアクリレート系の光重合開始剤の使用の際、n−ブチルアミン、トリエチルアミン、トリ−n−ブチルホスフィン等の増感剤を用いることができる。紫外線硬化樹脂組成物に用いられる光重合開始剤また光増感剤は該組成物100質量部に対して0.1〜15質量部であり、好ましくは1〜10質量部である。   Specific examples of photopolymerization initiators for these ultraviolet curable resins include benzoin and its derivatives, acetophenone, benzophenone, hydroxybenzophenone, Michler's ketone, α-amyloxime ester, thioxanthone, and derivatives thereof. You may use with a photosensitizer. The photopolymerization initiator can also be used as a photosensitizer. In addition, when using an epoxy acrylate photopolymerization initiator, a sensitizer such as n-butylamine, triethylamine, tri-n-butylphosphine can be used. The photopolymerization initiator or photosensitizer used in the ultraviolet curable resin composition is 0.1 to 15 parts by mass, preferably 1 to 10 parts by mass with respect to 100 parts by mass of the composition.

樹脂モノマーとしては、例えば、不飽和二重結合が一つのモノマーとして、メチルアクリレート、エチルアクリレート、ブチルアクリレート、ベンジルアクリレート、シクロヘキシルアクリレート、酢酸ビニル、スチレン等の一般的なモノマーを挙げることができる。また不飽和二重結合を二つ以上持つモノマーとして、エチレングリコールジアクリレート、プロピレングリコールジアクリレート、ジビニルベンゼン、1,4−シクロヘキサンジアクリレート、1,4−シクロヘキシルジメチルアジアクリレート、前出のトリメチロールプロパントリアクリレート、ペンタエリスリトールテトラアクリルエステル等を挙げることができる。市販品としては、アデカオプトマーKR・BYシリーズ:KR−400、KR−410、KR−550、KR−566、KR−567、BY−320B(旭電化株式会社製);コーエイハードA−101−KK、A−101−WS、C−302、C−401−N、C−501、M−101、M−102、T−102、D−102、NS−101、FT−102Q8、MAG−1−P20、AG−106、M−101−C(広栄化学株式会社製);セイカビームPHC2210(S)、PHC X−9(K−3)、PHC2213、DP−10、DP−20、DP−30、P1000、P1100、P1200、P1300、P1400、P1500、P1600、SCR900(大日精化工業株式会社製);KRM7033、KRM7039、KRM7130、KRM7131、UVECRYL29201、UVECRYL29202(ダイセル・ユーシービー株式会社製);RC−5015、RC−5016、RC−5020、RC−5031、RC−5100、RC−5102、RC−5120、RC−5122、RC−5152、RC−5171、RC−5180、RC−5181(大日本インキ化学工業株式会社製);オーレックスNo.340クリヤ(中国塗料株式会社製);サンラッドH−601、RC−750、RC−700、RC−600、RC−500、RC−611、RC−612(三洋化成工業株式会社製);SP−1509、SP−1507(昭和高分子株式会社製);RCC−15C(グレース・ジャパン株式会社製)、アロニックスM−6100、M−8030、M−8060(東亞合成株式会社製)等を適宜選択して利用できる。また、具体的化合物例としては、トリメチロールプロパントリアクリレート、ジトリメチロールプロパンテトラアクリレート、ペンタエリスリトールトリアクリレート、ペンタエリスリトールテトラアクリレート、ジペンタエリスリトールヘキサアクリレート、アルキル変性ジペンタエリスリトールペンタアクリレート等を挙げることができる。   Examples of the resin monomer may include general monomers such as methyl acrylate, ethyl acrylate, butyl acrylate, benzyl acrylate, cyclohexyl acrylate, vinyl acetate, and styrene as monomers having one unsaturated double bond. In addition, monomers having two or more unsaturated double bonds include ethylene glycol diacrylate, propylene glycol diacrylate, divinylbenzene, 1,4-cyclohexane diacrylate, 1,4-cyclohexyldimethyl adiacrylate, and the above trimethylolpropane. Examples thereof include triacrylate and pentaerythritol tetraacryl ester. As commercial products, Adekaoptomer KR / BY series: KR-400, KR-410, KR-550, KR-566, KR-567, BY-320B (manufactured by Asahi Denka Co., Ltd.); Koei Hard A-101- KK, A-101-WS, C-302, C-401-N, C-501, M-101, M-102, T-102, D-102, NS-101, FT-102Q8, MAG-1- P20, AG-106, M-101-C (manufactured by Guangei Chemical Co., Ltd.); Seika Beam PHC2210 (S), PHC X-9 (K-3), PHC2213, DP-10, DP-20, DP-30, P1000 , P1100, P1200, P1300, P1400, P1500, P1600, SCR900 (manufactured by Dainichi Seika Kogyo Co., Ltd.); KRM7033, KRM7039 KRM 7130, KRM 7131, UVECRYL 29201, UVECRYL 29202 (manufactured by Daicel UC Corporation); RC-5015, RC-5016, RC-5020, RC-5031, RC-5100, RC-5102, RC-5120, RC-5122, RC -5152, RC-5171, RC-5180, RC-5181 (Dainippon Ink Chemical Co., Ltd.); 340 clear (manufactured by China Paint Co., Ltd.); Sun Rad H-601, RC-750, RC-700, RC-600, RC-500, RC-611, RC-612 (Sanyo Chemical Industries Co., Ltd.); SP-1509 , SP-1507 (manufactured by Showa Polymer Co., Ltd.); RCC-15C (manufactured by Grace Japan Co., Ltd.), Aronix M-6100, M-8030, M-8060 (manufactured by Toagosei Co., Ltd.), etc. Available. Examples of specific compounds include trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, alkyl-modified dipentaerythritol pentaacrylate, and the like. .

また、硬化樹脂層には耐傷性、滑り性や屈折率を調整するために無機化合物または有機化合物の微粒子を含んでもよい。   Further, the cured resin layer may contain fine particles of an inorganic compound or an organic compound in order to adjust the scratch resistance, slipperiness and refractive index.

無機微粒子としては、酸化珪素、酸化チタン、酸化アルミニウム、酸化スズ、酸化インジウム、ITO、酸化亜鉛、酸化ジルコニウム、酸化マグネシウム、炭酸カルシウム、炭酸カルシウム、タルク、クレイ、焼成カオリン、焼成ケイ酸カルシウム、水和ケイ酸カルシウム、ケイ酸アルミニウム、ケイ酸マグネシウム及びリン酸カルシウムを挙げることができる。特に、酸化珪素、酸化チタン、酸化アルミニウム、酸化ジルコニウム、酸化マグネシウム等が好ましく用いられる。有機粒子としては、ポリメタアクリル酸メチルアクリレート樹脂粉末、アクリルスチレン系樹脂粉末、ポリメチルメタクリレート樹脂粉末、シリコン系樹脂粉末、ポリスチレン系樹脂粉末、ポリカーボネート樹脂粉末、ベンゾグアナミン系樹脂粉末、メラミン系樹脂粉末、ポリオレフィン系樹脂粉末、ポリエステル系樹脂粉末、ポリアミド系樹脂粉末、ポリイミド系樹脂粉末、またはポリ弗化エチレン系樹脂粉末等を添加することができる。好ましい微粒子は、架橋ポリスチレン粒子(例えば、綜研化学製SX−130H、SX−200H、SX−350H)、ポリメチルメタクリレート系粒子(例えば、綜研化学製MX150、MX300)が挙げられる。   Inorganic fine particles include silicon oxide, titanium oxide, aluminum oxide, tin oxide, indium oxide, ITO, zinc oxide, zirconium oxide, magnesium oxide, calcium carbonate, calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, water Mention may be made of Japanese calcium silicate, aluminum silicate, magnesium silicate and calcium phosphate. In particular, silicon oxide, titanium oxide, aluminum oxide, zirconium oxide, magnesium oxide and the like are preferably used. As organic particles, polymethacrylic acid methyl acrylate resin powder, acrylic styrene resin powder, polymethyl methacrylate resin powder, silicon resin powder, polystyrene resin powder, polycarbonate resin powder, benzoguanamine resin powder, melamine resin powder, A polyolefin resin powder, a polyester resin powder, a polyamide resin powder, a polyimide resin powder, a polyfluoroethylene resin powder, or the like can be added. Preferred fine particles include crosslinked polystyrene particles (for example, SX-130H, SX-200H, SX-350H manufactured by Soken Chemical) and polymethyl methacrylate-based particles (for example, MX150, MX300 manufactured by Soken Chemical).

これらの微粒子の平均粒径としては、0.01〜5μmが好ましく0.1〜5.0μm、さらには、0.1〜4.0μmであることがハードコート層を形成する塗布組成物に添加した際の組成物の安定性から好ましい。   The average particle diameter of these fine particles is preferably from 0.01 to 5 μm, more preferably from 0.1 to 5.0 μm, and further preferably from 0.1 to 4.0 μm added to the coating composition for forming the hard coat layer. It is preferable from the stability of the composition.

また、粒径の異なる2種以上の微粒子を含有しても良い。紫外線硬化性樹脂と微粒子の割合は、樹脂100質量部に対して、0.1〜30質量部となるように配合することが望ましい。   Moreover, you may contain 2 or more types of microparticles | fine-particles from which a particle size differs. The proportion of the ultraviolet curable resin and the fine particles is desirably blended so as to be 0.1 to 30 parts by mass with respect to 100 parts by mass of the resin.

また、ハードコート層はグラビアコーター、ディップコーター、リバースコーター、ワイヤーバーコーター、ダイコーター、インクジェット法等公知の方法を用いて、ハードコート層を形成する塗布組成物を塗布し、塗布後、加熱乾燥し、UV硬化処理することで形成できる。塗布量はウェット膜厚として0.1〜40μmが適当で、好ましくは、0.5〜30μmである。また、ドライ膜厚としては平均膜厚0.1〜30μm、好ましくは1〜20μmである。   Also, the hard coat layer is coated with a coating composition for forming the hard coat layer using a known method such as a gravure coater, dip coater, reverse coater, wire bar coater, die coater, ink jet method, etc. And can be formed by UV curing. The coating amount is suitably 0.1 to 40 μm, preferably 0.5 to 30 μm, as the wet film thickness. Moreover, as a dry film thickness, it is an average film thickness of 0.1-30 micrometers, Preferably it is 1-20 micrometers.

UV硬化処理の光源としては、紫外線を発生する光源であれば制限なく使用できる。例えば、低圧水銀灯、中圧水銀灯、高圧水銀灯、超高圧水銀灯、カーボンアーク灯、メタルハライドランプ、キセノンランプ等を用いることができる。照射条件はそれぞれのランプによって異なるが、活性線の照射量は、通常5〜500mJ/cm2、好ましくは5〜150mJ/cm2であるが、特に好ましくは20〜100mJ/cm2である。 As a light source for UV curing treatment, any light source that generates ultraviolet rays can be used without limitation. For example, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultrahigh pressure mercury lamp, a carbon arc lamp, a metal halide lamp, a xenon lamp, or the like can be used. Irradiation conditions vary depending on each lamp, but the irradiation amount of active rays is usually 5 to 500 mJ / cm 2 , preferably 5 to 150 mJ / cm 2 , and particularly preferably 20 to 100 mJ / cm 2 .

また、活性線を照射する際には、フィルムの搬送方向に張力を付与しながら行うことが好ましく、さらに好ましくは幅方向にも張力を付与しながら行うことである。付与する張力は30〜300N/mが好ましい。張力を付与する方法は特に限定されず、バックロール上で搬送方向に張力を付与してもよく、テンターにて幅方向、または2軸方向に張力を付与してもよい。これによってさらに平面性優れたフィルムを得ることができる。   Moreover, when irradiating actinic radiation, it is preferable to carry out while applying tension | tensile_strength in the conveyance direction of a film, More preferably, it is performing applying tension | tensile_strength also in the width direction. The tension to be applied is preferably 30 to 300 N / m. The method for applying tension is not particularly limited, and tension may be applied in the conveying direction on the back roll, or tension may be applied in the width direction or biaxial direction by a tenter. This makes it possible to obtain a film having further excellent flatness.

ハードコート層の形成する塗布組成物には溶媒が含まれていてもよい。塗布組成物に含有される有機溶媒としては、例えば、炭化水素類(トルエン、キシレン、)、アルコール類(メタノール、エタノール、イソプロパノール、ブタノール、シクロヘキサノール)、ケトン類(アセトン、メチルエチルケトン、メチルイソブチルケトン)、エステル類(酢酸メチル、酢酸エチル、乳酸メチル)、グリコールエーテル類、その他の有機溶媒からも適宜選択し、またはこれらを混合し利用できる。   The coating composition formed by the hard coat layer may contain a solvent. Examples of the organic solvent contained in the coating composition include hydrocarbons (toluene, xylene), alcohols (methanol, ethanol, isopropanol, butanol, cyclohexanol), and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone). , Esters (methyl acetate, ethyl acetate, methyl lactate), glycol ethers, and other organic solvents may be appropriately selected or mixed for use.

有機溶媒としては、プロピレングリコールモノアルキルエーテル(アルキル基の炭素原子数として1〜4)またはプロピレングリコールモノアルキルエーテル酢酸エステル(アルキル基の炭素原子数として1〜4)等が好ましい。また、有機溶媒の含有量としては塗布組成物中、5〜80質量%が好ましい。   As the organic solvent, propylene glycol monoalkyl ether (1 to 4 carbon atoms of the alkyl group) or propylene glycol monoalkyl ether acetate (1 to 4 carbon atoms of the alkyl group) is preferable. Moreover, as content of an organic solvent, 5-80 mass% is preferable in a coating composition.

ハードコート層は、JIS B 0601で規定される中心線平均粗さ(Ra)が0.001〜0.1μmのクリアハードコート層、または微粒子等を添加しRaが0.1〜1μmに調整された防眩性ハードコート層であることが好ましい。中心線平均粗さ(Ra)は光干渉式の表面粗さ測定器で測定することが好ましく、例えばWYKO社製の非接触表面微細形状計測装置「WYKO NT−2000」を用いて測定することができる。   The hard coat layer has a center line average roughness (Ra) defined by JIS B 0601 of 0.001 to 0.1 μm, or a fine hard coat layer and Ra is adjusted to 0.1 to 1 μm. An antiglare hard coat layer is preferred. The center line average roughness (Ra) is preferably measured by an optical interference type surface roughness measuring instrument, for example, by using a non-contact surface fine shape measuring device “WYKO NT-2000” manufactured by WYKO. it can.

さらにハードコート層には、低屈折率層で記載した上記シリコーン系界面活性剤あるいはポリオキシエーテル化合物を含有させることが好ましい。これらは塗布性を高める。また、これら成分は、塗布液中の固形分成分に対し、0.01〜3質量%の範囲で添加することが好ましい。   Further, the hard coat layer preferably contains the silicone surfactant or polyoxyether compound described in the low refractive index layer. These enhance the applicability. Moreover, it is preferable to add these components in 0.01-3 mass% with respect to the solid content component in a coating liquid.

ポリオキシエーテル化合物としては、例えば、ポリオキシエチレンアルキルエーテル、ポリオキシエチレンラウリルエーテル、ポリオキシエチレンセチルエーテル、ポリオキシエチレンステアリルエーテル等のポリオキシエチレンアルキルエーテル化合物、ポリオキシエチレンノニルフェニルエーテル、ポリオキシエチレンオクチルフェニルエーテル等のポリオキシアルキルフェニルエーテル化合物、ポリオキシアルキレンアルキルエーテル、ポリオキシエチレン高級アルコールエーテル、ポリオキシエチレンオクチルドデシルエーテル等が挙げられる。ポリオキシエチレンアルキルエーテルの市販品としては、エマルゲン1108、エマルゲン1118S−70(以上、花王社製)、ポリオキシエチレンラウリルエーテルの市販品としては、エマルゲン103、エマルゲン104P、エマルゲン105、エマルゲン106、エマルゲン108、エマルゲン109P、エマルゲン120、エマルゲン123P、エマルゲン147、エマルゲン150、エマルゲン130K(以上、花王社製)、ポリオキシエチレンセチルエーテルの市販品としては、エマルゲン210P、エマルゲン220(以上、花王社製)、ポリオキシエチレンステアリルエーテルの市販品としては、エマルゲン220、エマルゲン306P(以上、花王社製)、ポリオキシアルキレンアルキルエーテルの市販品としては、エマルゲンLS−106、エマルゲンLS−110、エマルゲンLS−114、エマルゲンMS−110(以上、花王社製)ポリオキシエチレン高級アルコールエーテルの市販品としては、エマルゲン705,エマルゲン707、エマルゲン709等が挙げられる。   Examples of the polyoxyether compound include polyoxyethylene alkyl ether, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene alkyl ether compounds such as polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene Polyoxyalkyl phenyl ether compounds such as ethylene octyl phenyl ether, polyoxyalkylene alkyl ether, polyoxyethylene higher alcohol ether, polyoxyethylene octyldodecyl ether and the like can be mentioned. Commercial products of polyoxyethylene alkyl ether include Emulgen 1108, Emulgen 1118S-70 (above, manufactured by Kao Corporation), and commercially available products of polyoxyethylene lauryl ether include Emulgen 103, Emulgen 104P, Emulgen 105, Emulgen 106, Emulgen 108, Emulgen 109P, Emulgen 120, Emulgen 123P, Emulgen 147, Emulgen 150, Emulgen 130K (above, manufactured by Kao Corporation), and polyoxyethylene cetyl ether are commercially available products of Emulgen 210P, Emulgen 220 (above, manufactured by Kao Corporation) As commercially available products of polyoxyethylene stearyl ether, Emulgen 220, Emulgen 306P (above, manufactured by Kao Corporation), and commercially available products of polyoxyalkylene alkyl ether include Examples of commercially available products of Rugen LS-106, Emulgen LS-110, Emulgen LS-114, Emulgen MS-110 (manufactured by Kao Corporation) polyoxyethylene higher alcohol ether include Emulgen 705, Emulgen 707, and Emulgen 709. .

これら非イオン性のポリオキシエーテル化合物の中でも好ましくは、ポリオキシエチレンオレイルエーテル化合物であり、下記の一般式(4)で表わされる化合物である。   Among these nonionic polyoxyether compounds, polyoxyethylene oleyl ether compounds are preferable, and are compounds represented by the following general formula (4).

1835−O(C24O)nH ・・・(4)
式中、nは2〜40を表わす。
C 18 H 35 -O (C 2 H 4 O) n H ··· (4)
In the formula, n represents 2 to 40.

オレイル部分に対するエチレンオキシドの平均付加個数(n)は、2〜40であり、好ましくは2〜10である。また、上記一般式(4)の化合物はエチレンオキシドとオレイルアルコールとを反応させて得られる。   The average addition number (n) of ethylene oxide with respect to the oleyl part is 2 to 40, preferably 2 to 10. Moreover, the compound of the said General formula (4) is obtained by making ethylene oxide and oleyl alcohol react.

具体的商品としては、エマルゲン404〔ポリオキシエチレン(4)オレイルエーテル〕、エマルゲン408〔ポリオキシエチレン(8)オレイルエーテル〕、エマルゲン409P〔ポリオキシエチレン(9)オレイルエーテル〕、エマルゲン420〔ポリオキシエチレン(13)オレイルエーテル〕、エマルゲン430〔ポリオキシエチレン(30)オレイルエーテル〕(以上、花王社製)、日本油脂製NOFABLEEAO−9905(ポリオキシエチレン(5)オレイルエーテル)等が挙げられる。   Specific products include Emulgen 404 [polyoxyethylene (4) oleyl ether], Emulgen 408 [polyoxyethylene (8) oleyl ether], Emulgen 409P [polyoxyethylene (9) oleyl ether], Emulgen 420 [polyoxy Ethylene (13) oleyl ether], Emulgen 430 [polyoxyethylene (30) oleyl ether] (above, manufactured by Kao Corporation), NOFBLEEAO-9905 (polyoxyethylene (5) oleyl ether) manufactured by NOF Corporation.

なお、( )がnの数字を表す。非イオン性のポリオキシエーテル化合物は単独或いは2種以上を併用しても良い。   Note that () represents the number n. Nonionic polyoxyether compounds may be used alone or in combination of two or more.

シリコーン界面活性剤とポリオキシエーテル化合物とのハードコート層中の含有質量比は、1.0:1.0〜0.10:1.0であり、さらに好ましくは0.70:1.0〜0.20:1.0であり、前記質量比で含有することが本発明の効果を得る上で好ましい。   The mass ratio of the silicone surfactant and the polyoxyether compound in the hard coat layer is 1.0: 1.0 to 0.10: 1.0, more preferably 0.70: 1.0 to In order to obtain the effects of the present invention, it is preferably 0.20: 1.0.

ハードコート層中の非イオン性のポリオキシエーテル化合物とシリコーン界面活性剤の好ましい含有量は、両者の総含有量で0.1質量%〜8.0質量%が好ましく、さらに好ましくは、0.2質量%〜4.0質量%であり、該範囲で添加することでハードコート層で安定に存在する。   The preferable content of the nonionic polyoxyether compound and the silicone surfactant in the hard coat layer is preferably 0.1% by mass to 8.0% by mass, more preferably 0.0% by mass in terms of the total content of both. It is 2 mass%-4.0 mass%, and it exists stably in a hard-coat layer by adding in this range.

また、上記フッ素界面活性剤、アクリル系共重合物、アセチレングリコール系化合物または非イオン性界面活性剤、ラジカル重合性の非イオン性界面活性剤等を併用しても良い。   Moreover, you may use together the said fluorosurfactant, an acryl-type copolymer, an acetylene glycol type compound or a nonionic surfactant, a radically polymerizable nonionic surfactant, etc.

非イオン性界面活性剤としては、ポリオキシエチレンモノラウレート、ポリオキシエチレンモノステアレート、ポリオキシエチレンモノオレート等のポリオキシアルキルエステル化合物、ソルビタンモノラウレート、ソルビタンモノステアレート、ソルビタンモノオレート等のソルビタンエステル化合物、等が挙げられる。   Nonionic surfactants include polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyalkyl ester compounds such as polyoxyethylene monooleate, sorbitan monolaurate, sorbitan monostearate, sorbitan monooleate, etc. Sorbitan ester compounds, and the like.

アセチレングリコール系化合物としてはサーフィノール104E、サーフィノール104PA、サーフィノール420、サーフィノール440、ダイノール604(以上、日信化学工業株式会社製)などが挙げられる。   Examples of the acetylene glycol compounds include Surfinol 104E, Surfinol 104PA, Surfinol 420, Surfinol 440, and Dynal 604 (manufactured by Nissin Chemical Industry Co., Ltd.).

ラジカル重合性の非イオン性界面活性剤としては、例えば、「RMA−564」、「RMA−568」、「RMA−1114」[以上、商品名、日本乳化剤株式会社製]等のポリオキシアルキレンアルキルフェニルエーテル(メタ)アクリレート系重合性界面活性剤などを挙げることができる。   Examples of the radical polymerizable nonionic surfactant include polyoxyalkylene alkyl such as “RMA-564”, “RMA-568”, “RMA-1114” [trade name, manufactured by Nippon Emulsifier Co., Ltd.]. Examples include phenyl ether (meth) acrylate polymerizable surfactants.

また、ハードコート層は、2層以上の重層構造を有していてもよい。その中の1層は例えば導電性微粒子、または、イオン性ポリマーを含有する所謂帯電防止層としてもよいし、また、種々の表示素子に対する色補正用フィルターとして色調調整機能を有する色調調整剤(染料もしくは顔料等)を含有させてもよいし、また電磁波遮断剤または赤外線吸収剤等を含有させそれぞれの機能を有するようにしてもよい。
(バックコート層)
本発明の反射防止フィルムは、ハードコート層を設けた側と反対側の面にバックコート層を設けてもよい。バックコート層は、反射防止層を設けることで生じるカールを矯正するために設けられる。すなわち、バックコート層を設けた面を内側にして丸まろうとする性質を持たせることにより、カールの度合いをバランスさせることができる。なお、バックコート層は好ましくはブロッキング防止層を兼ねて塗設され、その場合、バックコート層塗布組成物には、ブロッキング防止機能を持たせるために微粒子が添加されることが好ましい。
The hard coat layer may have a multilayer structure of two or more layers. One of the layers may be, for example, a so-called antistatic layer containing conductive fine particles or an ionic polymer, or a color tone adjusting agent (dye having a color tone adjusting function as a color correction filter for various display elements. Alternatively, a pigment or the like may be contained, or an electromagnetic wave blocking agent or an infrared absorber may be contained to have each function.
(Back coat layer)
In the antireflection film of the present invention, a back coat layer may be provided on the surface opposite to the side provided with the hard coat layer. The back coat layer is provided in order to correct curling caused by providing the antireflection layer. That is, the degree of curling can be balanced by imparting the property of being rounded with the surface on which the backcoat layer is provided facing inward. The back coat layer is preferably applied also as an anti-blocking layer. In this case, it is preferable that fine particles are added to the back coat layer coating composition in order to provide an anti-blocking function.

バックコート層に添加される微粒子としては無機化合物の例として、二酸化珪素、二酸化チタン、酸化アルミニウム、酸化ジルコニウム、炭酸カルシウム、炭酸カルシウム、タルク、クレイ、焼成カオリン、焼成ケイ酸カルシウム、酸化錫、酸化インジウム、酸化亜鉛、ITO、水和ケイ酸カルシウム、ケイ酸アルミニウム、ケイ酸マグネシウム及びリン酸カルシウムを挙げることができる。   As fine particles added to the back coat layer, examples of inorganic compounds include silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, calcium carbonate, calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, tin oxide, and oxidation. Mention may be made of indium, zinc oxide, ITO, hydrated calcium silicate, aluminum silicate, magnesium silicate and calcium phosphate.

これらの微粒子は、例えば、アエロジルR972、R972V、R974、R812、200、200V、300、R202、OX50、TT600(以上、日本アエロジル株式会社製)、シーホスターKE−P10、同KE−P30、同KE−P50、同KE−P100、同KE−P150、同KE−P250(以上、日本触媒株式会社製)の商品名で市販されており、使用することができる。   These fine particles include, for example, Aerosil R972, R972V, R974, R812, 200, 200V, 300, R202, OX50, TT600 (manufactured by Nippon Aerosil Co., Ltd.), Seahoster KE-P10, KE-P30, KE- P50, KE-P100, KE-P150, and KE-P250 (above, manufactured by Nippon Shokubai Co., Ltd.) are commercially available and can be used.

ポリマーの例として、シリコーン樹脂、フッ素樹脂及びアクリル樹脂を挙げることができる。シリコーン樹脂が好ましく、特に三次元の網状構造を有するものが好ましく、例えば、トスパール103、同105、同108、同120、同145、同3120及び同240(以上東芝シリコーン株式会社製)の商品名で市販されており、使用することができる。   Examples of the polymer include silicone resin, fluororesin, and acrylic resin. Silicone resins are preferable, and those having a three-dimensional network structure are particularly preferable. For example, Tospearl 103, 105, 108, 120, 145, 3120, and 240 (manufactured by Toshiba Silicone Co., Ltd.) Are commercially available and can be used.

これらの中でもでアエロジル200V、アエロジルR972V、シーホスターKE−P30、同KE−P50、及び同KE−P100がヘイズを低く保ちながら、ブロッキング防止効果が大きいため特に好ましく用いられる。本発明で用いられる反射防止フィルムは、活性エネルギー線硬化樹脂層の裏面側の動摩擦係数が0.9以下、特に0.1〜0.9であることが好ましい。   Among these, Aerosil 200V, Aerosil R972V, Seahoster KE-P30, KE-P50, and KE-P100 are particularly preferably used because they have a large anti-blocking effect while keeping haze low. The antireflection film used in the present invention preferably has a dynamic friction coefficient on the back side of the active energy ray-curable resin layer of 0.9 or less, particularly 0.1 to 0.9.

バックコート層に含まれる微粒子は、バインダーに対して0.1〜50質量%好ましくは0.1〜10質量%であることが好ましい。バックコート層を設けた場合のヘイズの増加は1%以下であることが好ましく0.5%以下であることが好ましく、特に0.0〜0.1%であることが好ましい。   The fine particles contained in the backcoat layer are 0.1 to 50% by weight, preferably 0.1 to 10% by weight, based on the binder. When the back coat layer is provided, the increase in haze is preferably 1% or less, more preferably 0.5% or less, and particularly preferably 0.0 to 0.1%.

バックコート層の塗布に用いられる溶媒としては、例えば、ジオキサン、アセトン、メチルエチルケトン、メチルイソブチルケトン、N,N−ジメチルホルムアミド、酢酸メチル、酢酸エチル、トリクロロエチレン、メチレンクロライド、エチレンクロライド、テトラクロロエタン、トリクロロエタン、クロロホルム、水、メタノール、エタノール、n−プロピルアルコール、i−プロピルアルコール、n−ブタノール、シクロヘキサノン、シクロヘキサノール、プロピレングリコールモノメチルエーテル、プロピレングリコールモノエチルエーテル、または炭化水素類(トルエン、キシレン)等があげられ、適宜組み合わされて用いられる。   Examples of the solvent used for coating the backcoat layer include dioxane, acetone, methyl ethyl ketone, methyl isobutyl ketone, N, N-dimethylformamide, methyl acetate, ethyl acetate, trichloroethylene, methylene chloride, ethylene chloride, tetrachloroethane, trichloroethane, Chloroform, water, methanol, ethanol, n-propyl alcohol, i-propyl alcohol, n-butanol, cyclohexanone, cyclohexanol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, or hydrocarbons (toluene, xylene) Are used in appropriate combinations.

バックコート層のバインダーとして用いられる樹脂としては、例えば塩化ビニル−酢酸ビニル共重合体、塩化ビニル樹脂、酢酸ビニル樹脂、酢酸ビニルとビニルアルコールの共重合体、部分加水分解した塩化ビニル−酢酸ビニル共重合体、塩化ビニル−塩化ビニリデン共重合体、塩化ビニル−アクリロニトリル共重合体、エチレン−ビニルアルコール共重合体、塩素化ポリ塩化ビニル、エチレン−塩化ビニル共重合体、エチレン−酢酸ビニル共重合体等のビニル系重合体または共重合体、ニトロセルロース、セルロースアセテートプロピオネート(好ましくはアセチル基置換度1.8〜2.3、プロピオニル基置換度0.1〜1.0)、ジアセチルセルロース、セルロースアセテートブチレート樹脂等のセルロース誘導体、マレイン酸及び/またはアクリル酸の共重合体、アクリル酸エステル共重合体、アクリロニトリル−スチレン共重合体、塩素化ポリエチレン、アクリロニトリル−塩素化ポリエチレン−スチレン共重合体、メチルメタクリレート−ブタジエン−スチレン共重合体、アクリル樹脂、ポリビニルアルコール樹脂、ポリビニルアセタール樹脂、ポリビニルブチラール樹脂、ウレタン樹脂、ポリエステルポリウレタン樹脂、ポリエーテルポリウレタン樹脂、ポリカーボネートポリウレタン樹脂、ポリエステル樹脂、ポリエーテル樹脂、ポリアミド樹脂、アミノ樹脂、スチレン−ブタジエン樹脂、ブタジエン−アクリロニトリル樹脂等のゴム系樹脂、シリコーン系樹脂、フッ素系樹脂等を挙げることができるが、これらに限定されるものではない。   Examples of the resin used as the binder of the backcoat layer include vinyl chloride-vinyl acetate copolymer, vinyl chloride resin, vinyl acetate resin, vinyl acetate-vinyl alcohol copolymer, partially hydrolyzed vinyl chloride-vinyl acetate copolymer. Polymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, ethylene-vinyl alcohol copolymer, chlorinated polyvinyl chloride, ethylene-vinyl chloride copolymer, ethylene-vinyl acetate copolymer, etc. Vinyl polymer or copolymer, nitrocellulose, cellulose acetate propionate (preferably acetyl group substitution degree 1.8-2.3, propionyl group substitution degree 0.1-1.0), diacetyl cellulose, cellulose Cellulose derivatives such as acetate butyrate resin, maleic acid and / or Or acrylic acid copolymer, acrylic ester copolymer, acrylonitrile-styrene copolymer, chlorinated polyethylene, acrylonitrile-chlorinated polyethylene-styrene copolymer, methyl methacrylate-butadiene-styrene copolymer, acrylic resin , Polyvinyl alcohol resin, polyvinyl acetal resin, polyvinyl butyral resin, urethane resin, polyester polyurethane resin, polyether polyurethane resin, polycarbonate polyurethane resin, polyester resin, polyether resin, polyamide resin, amino resin, styrene-butadiene resin, butadiene-acrylonitrile Examples thereof include, but are not limited to, rubber resins such as resins, silicone resins, fluorine resins, and the like.

例えば、アクリル樹脂としては、アクリペットMD、VH、MF、V(三菱レーヨン株式会社製)、ハイパールM−4003、M−4005、M−4006、M−4202、M−5000、M−5001、M−4501(根上工業株式会社製)、ダイヤナールBR−50、BR−52、BR−53、BR−60、BR−64、BR−73、BR−75、BR−77、BR−79、BR−80、BR−82、BR−83、BR−85、BR−87、BR−88、BR−90、BR−93、BR−95、BR−100、BR−101、BR−102、BR−105、BR−106、BR−107、BR−108、BR−112、BR−113、BR−115、BR−116、BR−117、BR−118等(三菱レーヨン株式会社製)のアクリル及びメタクリル系モノマーを原料として製造した各種ホモポリマー並びにコポリマー等が市販されており、この中から好ましいモノを適宜選択することもできる。   For example, as an acrylic resin, Acrypet MD, VH, MF, V (manufactured by Mitsubishi Rayon Co., Ltd.), Hyperl M-4003, M-4005, M-4006, M-4202, M-5000, M-5001, M -4501 (manufactured by Negami Kogyo Co., Ltd.), Dialnal BR-50, BR-52, BR-53, BR-60, BR-64, BR-73, BR-75, BR-77, BR-79, BR- 80, BR-82, BR-83, BR-85, BR-87, BR-88, BR-90, BR-93, BR-95, BR-100, BR-101, BR-102, BR-105, BR-106, BR-107, BR-108, BR-112, BR-113, BR-115, BR-116, BR-117, BR-118, etc. (Mitsubishi Rayon Co., Ltd.) acrylic Fine methacrylic monomer are commercially available various homopolymers and copolymers, etc. was prepared as a raw material, it is also possible to select a preferred mono from this appropriate.

例えば、バインダーとして用いられる樹脂としてはセルロースジアセテート、セルロースアセテートプロヒオネートなどのセルロースエステルとアクリル樹脂のブレンド物を用いることが好ましく、アクリル樹脂からなる微粒子を用いて、微粒子とバインダーとの屈折率差を0〜0.02未満とすることで透明性の高いバックコート層とすることができる。   For example, as a resin used as a binder, it is preferable to use a blend of cellulose ester such as cellulose diacetate and cellulose acetate prothionate and an acrylic resin, and the refractive index of the fine particles and the binder using fine particles made of an acrylic resin. By setting the difference to be less than 0 to 0.02, a highly transparent back coat layer can be obtained.

これらの塗布組成物をグラビアコーター、ディップコーター、リバースコーター、ワイヤーバーコーター、ダイコーター、またはスプレー塗布、インクジェット塗布等を用いて透明樹脂フィルムの表面にウェット膜厚1〜100μmで塗布するのが好ましいが、特に5〜30μmであることが好ましい。   These coating compositions are preferably applied to the surface of the transparent resin film with a wet film thickness of 1 to 100 μm using a gravure coater, dip coater, reverse coater, wire bar coater, die coater, spray coating, ink jet coating or the like. Is particularly preferably 5 to 30 μm.

また、塗布後、加熱乾燥し、必要に応じて硬化処理することで、バックコート層は形成される。硬化処理は低屈折率層で記載した内容を用いることができる。バックコート層は2回以上に分けて塗布することもできる。また、バックコート層は偏光子との接着性を改善するための易接着層を兼ねても良い。   Moreover, a backcoat layer is formed by heat-drying after application | coating and carrying out the hardening process as needed. The content described in the low refractive index layer can be used for the curing treatment. The backcoat layer can be applied in two or more steps. Further, the backcoat layer may also serve as an easy adhesion layer for improving the adhesion with the polarizer.

上記のように各層を塗布により形成するに際して、透明樹脂フィルムの幅が1.4〜4mでロール状に巻き取られた状態から繰り出して、上記塗布を行い、乾燥・硬化処理した後、ロール状に巻き取られることが好ましい。また、反射防止層を積層した後、ロール状に巻き取った状態で50〜160℃で加熱処理を行う製造方法によって製造されることが、反射防止フィルムを長尺塗布した際の効率性や安定性から好ましい。加熱処理期間は、設定される温度によって適宜決定すればよく、例えば、50℃であれば、好ましくは3日間以上30日未満の期間、160℃であれば10分以上1日以下の範囲が好ましい。通常は、巻外部、巻中央部、巻き芯部の加熱処理効果が偏らないように、比較的低温に設定することが好ましく、50〜60℃付近で7日間程度行うことが好ましい。   When each layer is formed by coating as described above, the transparent resin film is unwound in a roll shape with a width of 1.4 to 4 m, applied, dried and cured, and then rolled. It is preferable to be wound around. Moreover, after laminating | stacking an antireflection layer, it is manufactured by the manufacturing method which heat-processes at 50-160 degreeC in the state wound up by roll shape, and the efficiency and stability at the time of apply | coating an antireflection film long It is preferable from the property. The heat treatment period may be appropriately determined depending on the set temperature. For example, if it is 50 ° C., it is preferably a period of 3 days or more and less than 30 days, and if it is 160 ° C., a range of 10 minutes or more and 1 day or less is preferable. . Usually, it is preferably set at a relatively low temperature so that the heat treatment effect at the outside of the winding, the center of the winding, and the core is not biased, and is preferably performed at around 50 to 60 ° C. for about 7 days.

加熱処理を安定して行うためには、温湿度が調整可能な場所で行うことが必要であり、塵のないクリーンルーム等の加熱処理室で行うことが好ましい。   In order to stably perform the heat treatment, it is necessary to perform in a place where the temperature and humidity can be adjusted, and it is preferable to perform in a heat treatment chamber such as a clean room without dust.

反射防止フィルムをロール状に巻き取る際の、巻きコアとしては、円筒上のコアであれは、特に限定されないが、好ましくは中空プラスチックコアであり、プラスチック材料としては加熱処理温度に耐える耐熱性プラスチックが好ましく、例えばフェノール樹脂、キシレン樹脂、メラミン樹脂、ポリエステル樹脂、エポキシ樹脂などの樹脂が挙げられる。またガラス繊維などの充填材により強化した熱硬化性樹脂が好ましい。これらの巻きコアへの巻き数は、100巻き以上であることが好ましく、500巻き以上であることがさらに好ましく、巻き厚は5cm以上であることが好ましい。
(反射防止フィルムの反射率)
本発明の反射防止フィルムの反射率は、分光光度計により測定を行うことができる。その際、サンプルの測定側の裏面を粗面化処理した後、黒色のスプレーを用いて光吸収処理を行ってから、可視光領域(400〜700nm)の反射光を測定する。反射率は低いほど好ましいが、可視光領域の波長における平均値が2.5%以下であることが好ましく、最低反射率は1.5%以下であることが好ましい。また、反射率が2.5%以下であれば、本発明の反射防止フィルムと見なすことができる。
The winding core for winding the antireflection film into a roll is not particularly limited as long as it is a cylindrical core, but is preferably a hollow plastic core, and the plastic material is a heat resistant plastic that can withstand heat treatment temperatures. Preferred examples include resins such as phenol resins, xylene resins, melamine resins, polyester resins, and epoxy resins. A thermosetting resin reinforced with a filler such as glass fiber is preferable. The number of windings on these winding cores is preferably 100 windings or more, more preferably 500 windings or more, and the winding thickness is preferably 5 cm or more.
(Reflectivity of antireflection film)
The reflectance of the antireflection film of the present invention can be measured with a spectrophotometer. At that time, after the surface on the measurement side of the sample is roughened, the light absorption treatment is performed using a black spray, and then the reflected light in the visible light region (400 to 700 nm) is measured. The lower the reflectivity, the better. However, the average value in the visible light wavelength is preferably 2.5% or less, and the minimum reflectivity is preferably 1.5% or less. Moreover, if a reflectance is 2.5% or less, it can be regarded as the antireflection film of this invention.

可視光の波長領域において、平坦な形状の反射スペクトルを有することが好ましい。   It is preferable to have a flat reflection spectrum in the visible light wavelength region.

また、反射防止処理を施した画像表示装置表面の反射色相は、反射防止膜の設計上可視光領域において短波長域や長波長域の反射率が高くなることから赤や青に色づくことが多いが、反射光の色味は用途によって要望が異なり、薄型テレビ等の最表面に使用する場合にはニュートラルな色調が好まれる。   Also, the reflection hue on the surface of the image display device subjected to the antireflection treatment is often colored red or blue because the reflectance of the short wavelength region or the long wavelength region is high in the visible light region due to the design of the antireflection film. However, the color tone of reflected light varies depending on the application, and when used on the outermost surface of a flat-screen television or the like, a neutral color tone is preferred.

この場合、一般的に反射色相範囲は、XYZ表色系(CIE1931表色系)上で、
0.17≦x≦0.33、
0.10≦y≦0.33
であれば実用上問題はないが、xy平面上において(x、y)=(0.31、0.31)からの距離Δxyが0.05以下となる範囲が、より色味がないニュートラルに近いため好ましく、0.03以下がさらに好ましい。
In this case, generally, the reflection hue range is on the XYZ color system (CIE 1931 color system).
0.17 ≦ x ≦ 0.33,
0.10 ≦ y ≦ 0.33
If there is no practical problem, the range in which the distance Δxy from (x, y) = (0.31, 0.31) on the xy plane is 0.05 or less is neutral with less color. Since it is near, 0.03 or less is more preferable.

導電層と低屈折率層の膜厚は、各々の層の屈折率より反射率、反射光の色味を考慮して常法に従って計算で求められる。   The film thicknesses of the conductive layer and the low refractive index layer can be obtained by calculation according to a conventional method in consideration of the reflectance and the color of reflected light based on the refractive index of each layer.

各層を塗布する前に表面処理することが好ましい。表面処理方法としては、洗浄法、アルカリ処理法、フレームプラズマ処理法、高周波放電プラズマ法、電子ビーム法、イオンビーム法、スパッタリング法、酸処理、コロナ処理法、大気圧グロー放電プラズマ法等が挙げられる。   It is preferable to perform a surface treatment before applying each layer. Examples of the surface treatment method include a cleaning method, an alkali treatment method, a flame plasma treatment method, a high frequency discharge plasma method, an electron beam method, an ion beam method, a sputtering method, an acid treatment, a corona treatment method, and an atmospheric pressure glow discharge plasma method. It is done.

コロナ処理とは、大気圧下、電極間に1kV以上の高電圧を印加し、放電することで行う処理のことであり、春日電機株式会社や株式会社トーヨー電機などで市販されている装置を用いて行うことができる。コロナ放電処理の強度は、電極間距離、単位面積当たりの出力、ジェネレーターの周波数に依存する。   The corona treatment is a treatment performed by applying a high voltage of 1 kV or more between the electrodes at atmospheric pressure and discharging it, using an apparatus commercially available from Kasuga Electric Co., Ltd. or Toyo Electric Co., Ltd. Can be done. The intensity of the corona discharge treatment depends on the distance between the electrodes, the output per unit area, and the generator frequency.

コロナ処理装置の一方の電極(A電極)は、市販のものを用いることができるが、材質はアルミニウム、ステンレスなどから選択ができる。もう一方はプラスチックフィルムを抱かせるための電極(B電極)であり、コロナ処理が、安定かつ均一に実施されるように、前記A電極に対して一定の距離に設置されるロール電極である。これも通常市販されているものを用いることができ、材質は、アルミニウム、ステンレス、及びそれらの金属でできたロールに、セラミック、シリコン、EPTゴム、ハイパロンゴムなどがライニングされているロールが好ましく用いられる。   As one electrode (A electrode) of the corona treatment apparatus, a commercially available one can be used, but the material can be selected from aluminum, stainless steel and the like. The other is an electrode (B electrode) for holding a plastic film, and is a roll electrode installed at a certain distance from the A electrode so that the corona treatment is carried out stably and uniformly. A commercially available one can also be used, and the material is preferably a roll made of ceramic, silicon, EPT rubber, hyperon rubber or the like on a roll made of aluminum, stainless steel, or a metal thereof. It is done.

本発明に用いられるコロナ処理に用いる周波数は、20kHz以上100kHz以下の周波数であり、30kHz〜60kHzの周波数が好ましい。周波数が低下するとコロナ処理の均一性が劣化し、コロナ処理のムラが発生する。また、周波数が大きくなると、高出力のコロナ処理を行う場合には、特に問題ないが、低出力のコロナ処理を実施する場合には、安定した処理を行うことが難しくなり、結果として、処理ムラが発生する。   The frequency used for the corona treatment used in the present invention is a frequency of 20 kHz to 100 kHz, and a frequency of 30 kHz to 60 kHz is preferable. When the frequency is lowered, the uniformity of the corona treatment is deteriorated and unevenness of the corona treatment occurs. In addition, when the frequency is increased, there is no particular problem when performing high-output corona treatment, but when performing low-output corona treatment, it is difficult to perform stable processing, resulting in uneven processing. Occurs.

コロナ処理の出力は、1〜5W・min/m2であるが、2〜4W・min/m2の出力が好ましい。電極とフィルムとの距離は、5mm以上50mm以下であるが、好ましくは、10mm以上35mm以下である。間隙が開いてくると、一定の出力を維持するためにより高電圧が必要になり、ムラが発生し易くなる。また、間隙が狭くなりすぎると、印加する電圧が低くなりすぎ、ムラが発生し易くなる。さらにまた、フィルムを搬送して連続処理する際に電極にフィルムが接触し傷が発生する。 The output of the corona treatment is 1 to 5 W · min / m 2 , but an output of 2 to 4 W · min / m 2 is preferable. The distance between the electrode and the film is 5 mm or more and 50 mm or less, preferably 10 mm or more and 35 mm or less. When the gap is opened, a higher voltage is required to maintain a constant output, and unevenness is likely to occur. On the other hand, if the gap is too narrow, the applied voltage becomes too low and unevenness is likely to occur. Furthermore, when the film is transported and continuously processed, the film comes into contact with the electrodes and scratches are generated.

アルカリ処理方法としては、ハードコート層を塗設したフィルムをアルカリ水溶液に浸す方法であれば特に限定されない。アルカリ水溶液としては、水酸化ナトリウム水溶液、水酸化カリウム水溶液、アンモニア水溶液等が使用可能であり、中でも水酸化ナトリウム水溶液が好ましい。   The alkali treatment method is not particularly limited as long as it is a method in which a film coated with a hard coat layer is immersed in an alkaline aqueous solution. As the aqueous alkali solution, an aqueous sodium hydroxide solution, an aqueous potassium hydroxide solution, an aqueous ammonia solution or the like can be used, and an aqueous sodium hydroxide solution is particularly preferable.

アルカリ水溶液のアルカリ濃度、例えば水酸化ナトリウム濃度は0.1〜25質量%が好ましく、0.5〜15質量%がより好ましい。アルカリ処理温度は通常10〜80℃、好ましく20〜60℃である。アルカリ処理時間は5秒〜5分、好ましくは30秒〜3分である。アルカリ処理後のフィルムは酸性水で中和した後、十分に水洗いを行うことが好ましい。
(透明樹脂フィルム)
本発明に用いられる透明樹脂フィルムよりなる透明フィルム基材について、説明する。
The alkali concentration of the alkaline aqueous solution, for example, sodium hydroxide concentration is preferably 0.1 to 25% by mass, and more preferably 0.5 to 15% by mass. The alkali treatment temperature is usually 10 to 80 ° C, preferably 20 to 60 ° C. The alkali treatment time is 5 seconds to 5 minutes, preferably 30 seconds to 3 minutes. The film after the alkali treatment is preferably neutralized with acidic water and then thoroughly washed with water.
(Transparent resin film)
The transparent film base material which consists of a transparent resin film used for this invention is demonstrated.

透明フィルム基材としては、製造が容易であること、活性線硬化型樹脂層との接着性が良好である、光学的に等方性である、光学的に透明であること等が好ましい要件として挙げられる。   As a transparent film base material, it is preferable that the production is easy, the adhesiveness with the actinic radiation curable resin layer is good, the optical isotropic property, the optical transparency, etc. Can be mentioned.

ここでいう透明とは、可視光の透過率60%以上であることをさし、好ましくは80%以上であり、特に好ましくは90%以上である。   The term “transparent” as used herein means that the visible light transmittance is 60% or more, preferably 80% or more, and particularly preferably 90% or more.

上記の性質を有していれば特に限定はないが、例えば、セルロースジアセテートフィルム、セルローストリアセテートフィルム、セルロースアセテートプロピオネートフィルム、セルロースアセテートブチレートフィルム等のセルロースエステル系フィルム、ポリエステル系フィルム、ポリカーボネート系フィルム、ポリアリレート系フィルム、ポリスルホン(ポリエーテルスルホンも含む)系フィルム、ポリエチレンテレフタレート、ポリエチレンナフタレート等のポリエステルフィルム、ポリエチレンフィルム、ポリプロピレンフィルム、セロファン、ポリ塩化ビニリデンフィルム、ポリビニルアルコールフィルム、エチレンビニルアルコールフィルム、シンジオタクティックポリスチレン系フィルム、シクロオレフィンポリマーフィルム(アートン(JSR社製)、ゼオネックス、ゼオノア(以上、日本ゼオン社製))、ポリビニルアセタール、ポリメチルペンテンフィルム、ポリエーテルケトンフィルム、ポリエーテルケトンイミドフィルム、ポリアミドフィルム、フッ素樹脂フィルム、ナイロンフィルム、ポリメチルメタクリレートフィルム、アクリルフィルムまたはガラス板等を挙げることができる。   Although it will not specifically limit if it has said property, For example, cellulose ester films, such as a cellulose diacetate film, a cellulose triacetate film, a cellulose acetate propionate film, a cellulose acetate butyrate film, a polyester film, a polycarbonate Film, polyarylate film, polysulfone (including polyethersulfone) film, polyester film such as polyethylene terephthalate and polyethylene naphthalate, polyethylene film, polypropylene film, cellophane, polyvinylidene chloride film, polyvinyl alcohol film, ethylene vinyl alcohol Film, syndiotactic polystyrene film, cycloolefin polymer fill (Arton (manufactured by JSR), Zeonex, Zeonore (manufactured by Nippon Zeon)), polyvinyl acetal, polymethylpentene film, polyether ketone film, polyether ketone imide film, polyamide film, fluororesin film, nylon film, A polymethyl methacrylate film, an acrylic film, a glass plate, etc. can be mentioned.

中でも、セルロースエステル系フィルム、ポリカーボネート系フィルム、ポリスルホン(ポリエーテルスルホンを含む)系フィルム、シクロオレフィンポリマーフィルムが好ましく、本発明においては、特にセルロースエステル系フィルム(例えば、コニカミノルタタック、製品名KC8UX、KC4UX、KC5UX、KC8UCR3、KC8UCR4、KC8UCR5、KC8UY、KC4UY、KC4UE、KC12UR(以上、コニカミノルタオプト株式会社製))が、製造上、コスト面、透明性、接着性等の観点から好ましく用いられる。   Among these, a cellulose ester film, a polycarbonate film, a polysulfone (including polyether sulfone) film, and a cycloolefin polymer film are preferable. In the present invention, in particular, a cellulose ester film (for example, Konica Minoltack, product name KC8UX, KC4UX, KC5UX, KC8UCR3, KC8UCR4, KC8UCR5, KC8UY, KC4UY, KC4UE, KC12UR (above, manufactured by Konica Minolta Opto Co., Ltd.) are preferably used from the viewpoints of cost, transparency, adhesion and the like.

これらのフィルムは、溶融流延製膜で製造されたフィルムであっても、溶液流延製膜で製造されたフィルムであってもよい。   These films may be films produced by melt casting film formation or films produced by solution casting film formation.

透明フィルム基材としては、セルロースエステル系フィルム(以下セルロースエステルフィルムともいう)を用いることが好ましい。セルロースエステルとしては、セルロースアセテート、セルロースアセテートブチレート、セルロースアセテートプロピオネートが好ましく、中でもセルロースアセテートブチレート、セルロースアセテートフタレート、セルロースアセテートプロピオネートが好ましく用いられる。   As the transparent film substrate, it is preferable to use a cellulose ester film (hereinafter also referred to as a cellulose ester film). As the cellulose ester, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate are preferable. Among them, cellulose acetate butyrate, cellulose acetate phthalate, and cellulose acetate propionate are preferably used.

特に、アセチル基の置換度をX、プロピオニル基またはブチリル基の置換度をYとした時、XとYが下記の範囲にあるセルロースエステルフィルムを用いるのが、好ましい。   In particular, when the substitution degree of the acetyl group is X and the substitution degree of the propionyl group or butyryl group is Y, it is preferable to use a cellulose ester film in which X and Y are in the following ranges.

2.3≦X+Y≦3.0 0.1≦Y≦2.0
特に、2.5≦X+Y≦2.9 3≦Y≦1.2
であることが好ましい。
2.3 ≦ X + Y ≦ 3.0 0.1 ≦ Y ≦ 2.0
In particular, 2.5 ≦ X + Y ≦ 2.9 3 ≦ Y ≦ 1.2
It is preferable that

以下、好ましい透明樹脂フィルムであるセルロースエステルフィルムについて詳細に説明する。   Hereinafter, the cellulose ester film which is a preferable transparent resin film will be described in detail.

セルロースエステルフィルムは、熱処理による基材変形が少なく、平面性に優れた反射防止フィルムを得る上で、陽電子消滅寿命法により求められる自由体積半径が0.250〜0.310nmであることが好ましい。さらに、全自由体積パラメータが1.0〜2.0であるセルロースエステルフィルムであることがより好ましい。   The cellulose ester film preferably has a free volume radius of 0.250 to 0.310 nm determined by the positron annihilation lifetime method in order to obtain an antireflection film with little flatness due to heat treatment and excellent flatness. Furthermore, it is more preferable that it is a cellulose-ester film whose total free volume parameter is 1.0-2.0.

なお、上記自由体積とは、透明樹脂フィルムの分子鎖に占有されていない空隙部分を表している。これは、陽電子消滅寿命法を用いて測定することができる。具体的には、陽電子を試料に入射してから消滅するまでの時間を測定し、その消滅寿命から原子空孔や自由体積の大きさ、数濃度等に関する情報を非破壊的に観察することにより求めることができる。
(陽電子消滅寿命法による自由体積半径と全自由体積パラメータの測定)
下記測定条件にて陽電子消滅寿命と相対強度を測定した。
In addition, the said free volume represents the space | gap part which is not occupied by the molecular chain of a transparent resin film. This can be measured using the positron annihilation lifetime method. Specifically, by measuring the time from the incidence of positrons to the sample until annihilation, non-destructively observing information on the vacancies, the size of free volumes, the number concentration, etc. from the annihilation lifetime Can be sought.
(Measurement of free volume radius and total free volume parameters by positron annihilation lifetime method)
The positron annihilation lifetime and relative intensity were measured under the following measurement conditions.

(測定条件)
陽電子線源:22NaCl(強度1.85MBq)
ガンマ線検出器:プラスチック製シンチレーター+光電子増倍管
装置時間分解能:290ps
測定温度:23℃
総カウント数:100万カウント
試料サイズ:20mm×15mm
20mm×15mmにカットした試料切片を、20枚重ねて約2mmの厚みにした。
(Measurement condition)
Positron beam source: 22 NaCl (strength 1.85 MBq)
Gamma ray detector: Plastic scintillator + photomultiplier tube Time resolution: 290ps
Measurement temperature: 23 ° C
Total count: 1 million counts Sample size: 20 mm x 15 mm
Twenty pieces of sample sections cut to 20 mm × 15 mm were stacked to a thickness of about 2 mm.

試料は測定前に24時間真空乾燥を行った。   The sample was vacuum dried for 24 hours before measurement.

照射面積:約10mmφ
1チャンネルあたりの時間:23.3ps/ch
上記の測定条件に従って、陽電子消滅寿命測定を実施し、非線形最小二乗法により3成分解析して、消滅寿命の小さいものから、τ1、τ2、τ3とし、それに応じた強度をI1,I2,I3(I1+I2+I3=100%)とした。
Irradiation area: About 10mmφ
Time per channel: 23.3ps / ch
In accordance with the above measurement conditions, positron annihilation lifetime measurement is performed, and three-component analysis is performed by the nonlinear least square method, and τ1, τ2, and τ3 are determined from those having a small annihilation lifetime, and the corresponding intensities are I1, I2, I3 ( I1 + I2 + I3 = 100%).

最も寿命の長い平均消滅寿命τ3から、下記式を用いて自由体積半径R3(nm)を求めた。τ3が空孔での陽電子消滅に対応し、τ3が大きいほど空孔サイズが大きいと考えられている。   From the average annihilation lifetime τ3 having the longest lifetime, the free volume radius R3 (nm) was determined using the following formula. τ3 corresponds to positron annihilation in the vacancies, and it is considered that the larger the τ3, the larger the vacancy size.

τ3=(1/2)〔1−{R3/(R3+0.166)}
+(1/2π)sin{2πR3/(R3+0.166)}〕−1
ここで、0.166(nm)は、空孔の壁から浸出している電子層の厚さに相当する。
τ3 = (1/2) [1- {R3 / (R3 + 0.166)}
+ (1 / 2π) sin {2πR3 / (R3 + 0.166)}]-1
Here, 0.166 (nm) corresponds to the thickness of the electron layer leached from the hole wall.

さらに、全自由体積パラメータVPは、下記式により求めた。     Further, the total free volume parameter VP was obtained by the following equation.

3={(4/3)π(R33}(nm3
P=I3(%)×V3(nm3
ここでI3(%)は、空孔の相対的な数濃度に相当するため、VPは相対的な空孔量に相当する。
V 3 = {(4/3) π (R 3 ) 3 } (nm 3 )
V P = I 3 (%) × V 3 (nm 3 )
Here I 3 (%), in order to correspond to the relative number concentrations of vacancies, V P corresponds to the relative vacancy.

以上の測定を2回繰り返し、その平均値を求めた。   The above measurement was repeated twice, and the average value was obtained.

陽電子消滅寿命法は、例えばMATERIAL STAGE vol.4,No.5 2004 p21−25、東レリサーチセンター THE TRC NEWS No.80(Jul.2002)p20−22、「ぶんせき」(1988,pp.11−20)に「陽電子消滅法による高分子の自由体積の評価」が掲載されており、これらを参考にすることができる。   The positron annihilation lifetime method is described in, for example, MATERIAL STAGE vol. 4, no. 5 2004 p21-25, Toray Research Center THE TRC NEWS No. 80 (Jul. 2002) p20-22, “Bunseki” (1988, pp.11-20), “Evaluation of free volume of polymer by positron annihilation method” is published. it can.

セルロースエステルフィルムにおける自由体積半径は、0.250〜0.315nm、好ましくは0.250〜0.310nmであり、さらに好ましい範囲は、0.285〜0.305nmである。自由体積半径が0.250nm未満である。自由体積半径が0.250〜0.315nmでは、熱処理に対する基材変形が小さく、平面性に優れた反射防止フィルムが得られる。   The free volume radius in the cellulose ester film is 0.250 to 0.315 nm, preferably 0.250 to 0.310 nm, and a more preferable range is 0.285 to 0.305 nm. The free volume radius is less than 0.250 nm. When the free volume radius is 0.250 to 0.315 nm, the base material deformation with respect to the heat treatment is small, and an antireflection film excellent in flatness can be obtained.

セルロースエステルフィルムを形成するセルロースエステルの原料としては、特に限定はないが、綿花リンター、木材パルプ(針葉樹由来、広葉樹由来)、ケナフ等を挙げることができる。またそれらから得られたセルロースエステルはそれぞれ任意の割合で混合使用することができる。これらのセルロースエステルは、アシル化剤が酸無水物(無水酢酸、無水プロピオン酸、無水酪酸)である場合には、酢酸のような有機酸やメチレンクロライド等の有機溶媒を用い、硫酸のようなプロトン性触媒を用いてセルロース原料と反応させて得ることができる。   The raw material of the cellulose ester forming the cellulose ester film is not particularly limited, and examples thereof include cotton linter, wood pulp (derived from coniferous tree, derived from broadleaf tree), kenaf and the like. Moreover, the cellulose ester obtained from them can be mixed and used in arbitrary ratios, respectively. When the acylating agent is an acid anhydride (acetic anhydride, propionic anhydride, butyric anhydride), these cellulose esters use an organic solvent such as acetic acid or an organic solvent such as methylene chloride, and It can be obtained by reacting with a cellulose raw material using a protic catalyst.

アシル化剤が、酸クロライド(CH3COCl、C25COCl、C37COCl)の場合には、触媒としてアミンのような塩基性化合物を用いて反応が行われる。具体的には、特開平10−45804号公報に記載の方法等を参考にして合成することができる。 Acylating agent, acid chloride (CH 3 COCl, C 2 H 5 COCl, C 3 H 7 COCl) in the case of the reaction is carried out using a basic compound such as an amine as a catalyst. Specifically, it can be synthesized with reference to the method described in JP-A-10-45804.

また、本発明に用いられるセルロースエステルは各置換度に合わせて上記アシル化剤量を混合して反応させたものであり、セルロースエステルはこれらアシル化剤がセルロース分子の水酸基に反応する。セルロース分子はグルコースユニットが多数連結したものからなっており、グルコースユニットに3個の水酸基がある。この3個の水酸基にアシル基が誘導された数を置換度(モル%)という。例えば、セルローストリアセテートはグルコースユニットの3個の水酸基全てにアセチル基が結合している(実際には2.6〜3.0)。   In addition, the cellulose ester used in the present invention is obtained by mixing and reacting the amount of the acylating agent in accordance with the degree of substitution. In the cellulose ester, these acylating agents react with hydroxyl groups of cellulose molecules. Cellulose molecules are composed of many glucose units linked together, and the glucose unit has three hydroxyl groups. The number of acyl groups derived from these three hydroxyl groups is called the degree of substitution (mol%). For example, cellulose triacetate has acetyl groups bonded to all three hydroxyl groups of the glucose unit (actually 2.6 to 3.0).

アシル基の置換度の測定方法はASTM−D817−96の規定に準じて測定することができる。   The measuring method of the substitution degree of an acyl group can be measured according to the rule of ASTM-D817-96.

セルロースエステルの数平均分子量は、50000〜250000が、成型した場合の機械的強度が強く、かつ、適度なドープ粘度となり好ましく、さらに好ましくは、80000〜150000である。   The number average molecular weight of the cellulose ester is preferably from 50,000 to 250,000 because the mechanical strength when molded is high and an appropriate dope viscosity is obtained, and more preferably from 80,000 to 150,000.

セルロースエステルフィルムは、一般的に溶液流延製膜法と呼ばれるセルロースエステル溶解液(ドープ)を、例えば、無限に移送する無端の金属ベルトまたは回転する金属ドラムの流延用支持体上に加圧ダイからドープを流延(キャスティング)し製膜する方法で製造される。   Cellulose ester film is a solution in which a cellulose ester solution (dope), commonly referred to as a solution casting film forming method, is pressed onto a casting support of an endless metal belt or rotating metal drum, for example. It is manufactured by casting a dope from a die and forming a film.

これらドープの調製に用いられる有機溶媒としては、セルロースエステルを溶解でき、かつ、適度な沸点であることが好ましく、例えば、メチレンクロライド、酢酸メチル、酢酸エチル、酢酸アミル、アセト酢酸メチル、アセトン、テトラヒドロフラン、1,3−ジオキソラン、1,4−ジオキサン、シクロヘキサノン、ギ酸エチル、2,2,2−トリフルオロエタノール、2,2,3,3−テトラフルオロ−1−プロパノール、1,3−ジフルオロ−2−プロパノール、1,1,1,3,3,3−ヘキサフルオロ−2−メチル−2−プロパノール、1,1,1,3,3,3−ヘキサフルオロ−2−プロパノール、2,2,3,3,3−ペンタフルオロ−1−プロパノール、ニトロエタン、1,3−ジメチル−2−イミダゾリジノン等を挙げることができるが、メチレンクロライド等の有機ハロゲン化合物、ジオキソラン誘導体、酢酸メチル、酢酸エチル、アセトン、アセト酢酸メチル等が好ましい有機溶媒(即ち、良溶媒)として挙げられる。   As the organic solvent used for preparing these dopes, it is preferable that the cellulose ester can be dissolved and has an appropriate boiling point. For example, methylene chloride, methyl acetate, ethyl acetate, amyl acetate, methyl acetoacetate, acetone, tetrahydrofuran 1,3-dioxolane, 1,4-dioxane, cyclohexanone, ethyl formate, 2,2,2-trifluoroethanol, 2,2,3,3-tetrafluoro-1-propanol, 1,3-difluoro-2 -Propanol, 1,1,1,3,3,3-hexafluoro-2-methyl-2-propanol, 1,1,1,3,3,3-hexafluoro-2-propanol, 2,2,3 , 3,3-pentafluoro-1-propanol, nitroethane, 1,3-dimethyl-2-imidazolidinone, etc. Can, organic halogen compounds such as methylene chloride, dioxolane derivatives, methyl acetate, ethyl acetate and acetone, methyl acetoacetate, and the like are preferable organic solvents (i.e., good solvent), and as.

また、下記の製膜工程に示すように、溶媒蒸発工程において流延用支持体上に形成されたウェブ(ドープ膜)から溶媒を乾燥させる時に、ウェブ中の発泡を防止する観点から、用いられる有機溶媒の沸点としては、30〜80℃が好ましく、例えば、上記記載の良溶媒の沸点は、メチレンクロライド(沸点40.4℃)、酢酸メチル(沸点56.32℃)、アセトン(沸点56.3℃)、酢酸エチル(沸点76.82℃)等である。   Moreover, as shown in the following film forming process, it is used from the viewpoint of preventing foaming in the web when the solvent is dried from the web (dope film) formed on the casting support in the solvent evaporation process. The boiling point of the organic solvent is preferably 30 to 80 ° C. For example, the good solvent described above has a boiling point of methylene chloride (boiling point 40.4 ° C), methyl acetate (boiling point 56.32 ° C), acetone (boiling point 56.56 ° C). 3 ° C.), ethyl acetate (boiling point 76.82 ° C.) and the like.

上記の良溶媒の中でも溶解性に優れるメチレンクロライド、あるいは酢酸メチルが好ましく用いられる。   Among the above good solvents, methylene chloride or methyl acetate having excellent solubility is preferably used.

上記有機溶媒の他に、0.1〜40質量%の炭素原子数1〜4のアルコールを含有させることが好ましい。特に好ましくは5〜30質量%で前記アルコールが含まれることが好ましい。   In addition to the organic solvent, it is preferable to contain 0.1 to 40% by mass of an alcohol having 1 to 4 carbon atoms. It is particularly preferable that the alcohol is contained at 5 to 30% by mass.

これらは上記のドープを流延用支持体に流延後、溶媒が蒸発を始めアルコールの比率が多くなるとウェブ(ドープ膜)がゲル化し、ウェブを丈夫にし流延用支持体から剥離することを容易にするゲル化溶媒として用いられたり、これらの割合が少ない時は非塩素系有機溶媒のセルロースエステルの溶解を促進する役割もある。   After casting the above dope onto the casting support, the solvent starts to evaporate and the alcohol ratio increases and the web (dope film) gels, making the web strong and peeling from the casting support. When it is used as a gelling solvent for facilitating or the ratio of these is small, it also has a role of promoting the dissolution of the cellulose ester of the non-chlorine organic solvent.

炭素原子数1〜4のアルコールとしては、メタノール、エタノール、n−プロパノール、iso−プロパノール、n−ブタノール、sec−ブタノール、tert−ブタノール等を挙げることができる。   Examples of the alcohol having 1 to 4 carbon atoms include methanol, ethanol, n-propanol, iso-propanol, n-butanol, sec-butanol, tert-butanol and the like.

これらの溶媒のうち、ドープの安定性がよく、沸点も比較的低く、乾燥性もよく、かつ毒性がないこと等からエタノールが好ましい。好ましくは、メチレンクロライド70〜95質量%に対してエタノール5〜30質量%を含む溶媒を用いることが好ましい。メチレンクロライドの代わりに酢酸メチルを用いることもできる。このとき、冷却溶解法によりドープを調製してもよい。   Of these solvents, ethanol is preferred because it has good dope stability, relatively low boiling point, good drying properties, and no toxicity. It is preferable to use a solvent containing 5 to 30% by mass of ethanol with respect to 70 to 95% by mass of methylene chloride. Methyl acetate can be used in place of methylene chloride. At this time, the dope may be prepared by a cooling dissolution method.

セルロースエステルフィルムには、下記のような可塑剤を含有するのが好ましい。可塑剤としては、例えば、リン酸エステル系可塑剤、多価アルコールエステル系可塑剤、フタル酸エステル系可塑剤、トリメリット酸エステル系可塑剤、ピロメリット酸系可塑剤、グリコレート系可塑剤、クエン酸エステル系可塑剤、ポリエステル系可塑剤、脂肪酸エステル系可塑剤、多価カルボン酸エステル系可塑剤等を好ましく用いることができる。   The cellulose ester film preferably contains the following plasticizer. Examples of plasticizers include phosphate ester plasticizers, polyhydric alcohol ester plasticizers, phthalate ester plasticizers, trimellitic ester plasticizers, pyromellitic acid plasticizers, glycolate plasticizers, Citric acid ester plasticizers, polyester plasticizers, fatty acid ester plasticizers, polycarboxylic acid ester plasticizers, and the like can be preferably used.

中でも、多価アルコールエステル系可塑剤、フタル酸エステル系可塑剤、クエン酸エステル系可塑剤、脂肪酸エステル系可塑剤、グリコレート系可塑剤、多価カルボン酸エステル系可塑剤等が好ましい。特に多価アルコールエステル系可塑剤を用いることが好ましく、ハードコート層の鉛筆硬度が4H以上を安定に得ることができるため好ましい。   Among these, polyhydric alcohol ester plasticizers, phthalate ester plasticizers, citrate ester plasticizers, fatty acid ester plasticizers, glycolate plasticizers, polycarboxylic acid ester plasticizers, and the like are preferable. In particular, it is preferable to use a polyhydric alcohol ester plasticizer, which is preferable because the pencil hardness of the hard coat layer can be stably obtained as 4H or more.

多価アルコールエステル系可塑剤は2価以上の脂肪族多価アルコールとモノカルボン酸のエステルよりなる可塑剤であり、分子内に芳香環またはシクロアルキル環を有することが好ましい。好ましくは2〜20価の脂肪族多価アルコールエステルである。   The polyhydric alcohol ester plasticizer is a plasticizer composed of an ester of a divalent or higher aliphatic polyhydric alcohol and a monocarboxylic acid, and preferably has an aromatic ring or a cycloalkyl ring in the molecule. Preferably it is a 2-20 valent aliphatic polyhydric alcohol ester.

本発明に好ましく用いられる多価アルコールは次の一般式(5)で表される。   The polyhydric alcohol preferably used in the present invention is represented by the following general formula (5).

1−(OH)n ・・・(5)
式中、R1はn価の有機基、nは2以上の正の整数、OH基はアルコール性、及び/またはフェノール性水酸基を表わす。
R 1- (OH) n (5)
In the formula, R 1 represents an n-valent organic group, n represents a positive integer of 2 or more, and the OH group represents an alcoholic and / or phenolic hydroxyl group.

好ましい多価アルコールの例としては、例えば以下のようなものを挙げることができるが、本発明はこれらに限定されるものではない。   Examples of preferred polyhydric alcohols include the following, but the present invention is not limited to these.

アドニトール、アラビトール、エチレングリコール、ジエチレングリコール、トリエチレングリコール、テトラエチレングリコール、1,2−プロパンジオール、1,3−プロパンジオール、ジプロピレングリコール、トリプロピレングリコール、1,2−ブタンジオール、1,3−ブタンジオール、1,4−ブタンジオール、ジブチレングリコール、1,2,4−ブタントリオール、1,5−ペンタンジオール、1,6−ヘキサンジオール、ヘキサントリオール、ガラクチトール、マンニトール、3−メチルペンタン−1,3,5−トリオール、ピナコール、ソルビトール、トリメチロールプロパン、トリメチロールエタン、キシリトール等を挙げることができる。特に、トリエチレングリコール、テトラエチレングリコール、ジプロピレングリコール、トリプロピレングリコール、ソルビトール、トリメチロールプロパン、キシリトールが好ましい。   Adonitol, arabitol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3- Butanediol, 1,4-butanediol, dibutylene glycol, 1,2,4-butanetriol, 1,5-pentanediol, 1,6-hexanediol, hexanetriol, galactitol, mannitol, 3-methylpentane- Examples include 1,3,5-triol, pinacol, sorbitol, trimethylolpropane, trimethylolethane, xylitol and the like. In particular, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, sorbitol, trimethylolpropane, and xylitol are preferable.

多価アルコールエステルに用いられるモノカルボン酸としては、特に制限はなく、公知の脂肪族モノカルボン酸、脂環族モノカルボン酸、芳香族モノカルボン酸等を用いることができる。脂環族モノカルボン酸、芳香族モノカルボン酸を用いると透湿性、保留性を向上させる点で好ましい。   There is no restriction | limiting in particular as monocarboxylic acid used for polyhydric alcohol ester, Well-known aliphatic monocarboxylic acid, alicyclic monocarboxylic acid, aromatic monocarboxylic acid, etc. can be used. Use of an alicyclic monocarboxylic acid or aromatic monocarboxylic acid is preferred in terms of improving moisture permeability and retention.

好ましいモノカルボン酸の例としては以下のようなものを挙げることができるが、本発明はこれに限定されるものではない。   Examples of preferred monocarboxylic acids include the following, but the present invention is not limited thereto.

脂肪族モノカルボン酸としては、炭素数1〜32の直鎖または側鎖を有する脂肪酸を好ましく用いることができる。炭素数は1〜20であることがさらに好ましく、1〜10であることが特に好ましい。酢酸を含有させるとセルロースエステルとの相溶性が増すため好ましく、酢酸と他のモノカルボン酸を混合して用いることも好ましい。   As the aliphatic monocarboxylic acid, a fatty acid having a straight chain or a side chain having 1 to 32 carbon atoms can be preferably used. The number of carbon atoms is more preferably 1-20, and particularly preferably 1-10. When acetic acid is contained, the compatibility with the cellulose ester is increased, and it is also preferable to use a mixture of acetic acid and another monocarboxylic acid.

好ましい脂肪族モノカルボン酸としては、酢酸、プロピオン酸、酪酸、吉草酸、カプロン酸、エナント酸、カプリル酸、ペラルゴン酸、カプリン酸、2−エチル−ヘキサン酸、ウンデシル酸、ラウリン酸、トリデシル酸、ミリスチン酸、ペンタデシル酸、パルミチン酸、ヘプタデシル酸、ステアリン酸、ノナデカン酸、アラキン酸、ベヘン酸、リグノセリン酸、セロチン酸、ヘプタコサン酸、モンタン酸、メリシン酸、ラクセル酸等の飽和脂肪酸、ウンデシレン酸、オレイン酸、ソルビン酸、リノール酸、リノレン酸、アラキドン酸等の不飽和脂肪酸等を挙げることができる。   Preferred aliphatic monocarboxylic acids include acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, 2-ethyl-hexanoic acid, undecylic acid, lauric acid, tridecylic acid, Saturated fatty acids such as myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, nonadecanoic acid, arachidic acid, behenic acid, lignoceric acid, serotic acid, heptacosanoic acid, montanic acid, melicic acid, laccelic acid, undecylenic acid, olein Examples thereof include unsaturated fatty acids such as acid, sorbic acid, linoleic acid, linolenic acid, and arachidonic acid.

好ましい脂環族モノカルボン酸の例としては、シクロペンタンカルボン酸、シクロヘキサンカルボン酸、シクロオクタンカルボン酸、またはそれらの誘導体を挙げることができる。   Examples of preferred alicyclic monocarboxylic acids include cyclopentane carboxylic acid, cyclohexane carboxylic acid, cyclooctane carboxylic acid, or derivatives thereof.

好ましい芳香族モノカルボン酸の例としては、安息香酸、トルイル酸等の安息香酸のベンゼン環にアルキル基、メトキシ基あるいはエトキシ基などのアルコキシ基を1〜3個を導入したもの、ビフェニルカルボン酸、ナフタレンカルボン酸、テトラリンカルボン酸等のベンゼン環を2個以上有する芳香族モノカルボン酸、またはそれらの誘導体を挙げることができる。特に安息香酸が好ましい。   Examples of preferred aromatic monocarboxylic acids include those in which 1 to 3 alkoxy groups such as an alkyl group, a methoxy group or an ethoxy group are introduced into the benzene ring of benzoic acid such as benzoic acid or toluic acid, biphenylcarboxylic acid, Examples thereof include aromatic monocarboxylic acids having two or more benzene rings such as naphthalenecarboxylic acid and tetralincarboxylic acid, or derivatives thereof. Benzoic acid is particularly preferable.

多価アルコールエステルの分子量は特に制限はないが、300〜1500であることが好ましく、350〜750であることがさらに好ましい。分子量が大きい方が揮発し難くなるため好ましく、透湿性、セルロースエステルとの相溶性の点では小さい方が好ましい。   The molecular weight of the polyhydric alcohol ester is not particularly limited, but is preferably 300 to 1500, and more preferably 350 to 750. A higher molecular weight is preferred because it is less likely to volatilize, and a smaller one is preferred in terms of moisture permeability and compatibility with cellulose ester.

多価アルコールエステルに用いられるカルボン酸は1種類でもよいし、2種以上の混合であってもよい。また、多価アルコール中のOH基は、全てエステル化してもよいし、一部をOH基のままで残してもよい。   The carboxylic acid used for the polyhydric alcohol ester may be one kind or a mixture of two or more kinds. Moreover, all the OH groups in the polyhydric alcohol may be esterified, or a part of the OH groups may be left as they are.

以下に、多価アルコールエステルの具体的化合物を例示する。   Below, the specific compound of a polyhydric alcohol ester is illustrated.

Figure 2009036817
Figure 2009036817

Figure 2009036817
Figure 2009036817

Figure 2009036817
Figure 2009036817

Figure 2009036817
Figure 2009036817

グリコレート系可塑剤は特に限定されないが、アルキルフタリルアルキルグリコレート類が好ましく用いることができる。アルキルフタリルアルキルグリコレート類としては、例えばメチルフタリルメチルグリコレート、エチルフタリルエチルグリコレート、プロピルフタリルプロピルグリコレート、ブチルフタリルブチルグリコレート、オクチルフタリルオクチルグリコレート、メチルフタリルエチルグリコレート、エチルフタリルメチルグリコレート、エチルフタリルプロピルグリコレート、メチルフタリルブチルグリコレート、エチルフタリルブチルグリコレート、ブチルフタリルメチルグリコレート、ブチルフタリルエチルグリコレート、プロピルフタリルブチルグリコレート、ブチルフタリルプロピルグリコレート、メチルフタリルオクチルグリコレート、エチルフタリルオクチルグリコレート、オクチルフタリルメチルグリコレート、オクチルフタリルエチルグリコレート等が挙げられる。   The glycolate plasticizer is not particularly limited, but alkylphthalylalkyl glycolates can be preferably used. Examples of alkyl phthalyl alkyl glycolates include methyl phthalyl methyl glycolate, ethyl phthalyl ethyl glycolate, propyl phthalyl propyl glycolate, butyl phthalyl butyl glycolate, octyl phthalyl octyl glycolate, methyl phthalyl ethyl Glycolate, ethyl phthalyl methyl glycolate, ethyl phthalyl propyl glycolate, methyl phthalyl butyl glycolate, ethyl phthalyl butyl glycolate, butyl phthalyl methyl glycolate, butyl phthalyl ethyl glycolate, propyl phthalyl butyl glycol Butyl phthalyl propyl glycolate, methyl phthalyl octyl glycolate, ethyl phthalyl octyl glycolate, octyl phthalyl methyl glycolate, octyl phthalate Ethyl glycolate, and the like.

フタル酸エステル系可塑剤としては、ジエチルフタレート、ジメトキシエチルフタレート、ジメチルフタレート、ジオクチルフタレート、ジブチルフタレート、ジ−2−エチルヘキシルフタレート、ジオクチルフタレート、ジシクロヘキシルフタレート、ジシクロヘキシルテレフタレート等が挙げられる。   Examples of the phthalate ester plasticizer include diethyl phthalate, dimethoxyethyl phthalate, dimethyl phthalate, dioctyl phthalate, dibutyl phthalate, di-2-ethylhexyl phthalate, dioctyl phthalate, dicyclohexyl phthalate, and dicyclohexyl terephthalate.

クエン酸エステル系可塑剤としては、クエン酸アセチルトリメチル、クエン酸アセチルトリエチル、クエン酸アセチルトリブチル等が挙げられる。   Examples of the citrate plasticizer include acetyl trimethyl citrate, acetyl triethyl citrate, and acetyl tributyl citrate.

脂肪酸エステル系可塑剤として、オレイン酸ブチル、リシノール酸メチルアセチル、セバシン酸ジブチル等が挙げられる。   Examples of fatty acid ester plasticizers include butyl oleate, methylacetyl ricinoleate, and dibutyl sebacate.

多価カルボン酸エステル系可塑剤も好ましく用いることができる。具体的には特開2002−265639号公報の段落番号[0015]〜[0020]記載の多価カルボン酸エステルを可塑剤の一つとして添加することが好ましい。   Polycarboxylic acid ester plasticizers can also be preferably used. Specifically, it is preferable to add the polyvalent carboxylic acid ester described in paragraphs [0015] to [0020] of JP-A No. 2002-265639 as one of the plasticizers.

また、他の可塑剤としてリン酸エステル系可塑剤を用いることもでき、トリフェニルホスフェート、トリクレジルホスフェート、クレジルジフェニルホスフェート、オクチルジフェニルホスフェート、ジフェニルビフェニルホスフェート、トリオクチルホスフェート、トリブチルホスフェート等が挙げられる。   In addition, phosphate plasticizers can also be used as other plasticizers, such as triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, diphenyl biphenyl phosphate, trioctyl phosphate, tributyl phosphate, etc. It is done.

このほか、特開2003−12859号記載のアクリルポリマーなどを含有させることも好ましい。   In addition, it is also preferable to contain an acrylic polymer described in JP-A-2003-12859.

〈アクリルポリマー〉
セルロースエステルフィルムは、延伸方向に対して負の配向複屈折性を示す重量平均分子量が500以上30000以下であるアクリルポリマーを含有することが好ましい。
<Acrylic polymer>
It is preferable that a cellulose-ester film contains the acrylic polymer whose weight average molecular weight which shows negative orientation birefringence with respect to a extending | stretching direction is 500-30000.

該ポリマーの重量平均分子量が500以上30000以下のもので該ポリマーの組成を制御することで、セルロースエステルと該ポリマーとの相溶性を良好にすることができる。   By controlling the composition of the polymer so that the weight average molecular weight of the polymer is 500 or more and 30000 or less, the compatibility between the cellulose ester and the polymer can be improved.

特に、アクリルポリマー、芳香環を側鎖に有するアクリルポリマーまたはシクロヘキシル基を側鎖に有するアクリルポリマーについて、好ましくは重量平均分子量が500以上10000以下のものであれば、上記に加え、製膜後のセルロースエステルフィルムの透明性が優れ、透湿度も極めて低く、反射防止フィルムとして優れた性能を示す。   In particular, for an acrylic polymer, an acrylic polymer having an aromatic ring in the side chain, or an acrylic polymer having a cyclohexyl group in the side chain, if the weight average molecular weight is preferably 500 or more and 10,000 or less, in addition to the above, The transparency of the cellulose ester film is excellent, the moisture permeability is extremely low, and it exhibits excellent performance as an antireflection film.

該ポリマーは重量平均分子量が500以上30000以下であるから、オリゴマーから低分子量ポリマーの間にあると考えられるものである。このようなポリマーを合成するには、通常の重合では分子量のコントロールが難しく、分子量を余り大きくしない方法でできるだけ分子量を揃えることのできる方法を用いることが望ましい。   Since the polymer has a weight average molecular weight of 500 or more and 30000 or less, it is considered to be between the oligomer and the low molecular weight polymer. In order to synthesize such a polymer, it is difficult to control the molecular weight in normal polymerization, and it is desirable to use a method that can align the molecular weight as much as possible by a method that does not increase the molecular weight too much.

かかる重合方法としては、クメンペルオキシドやt−ブチルヒドロペルオキシドのような過酸化物重合開始剤を使用する方法、重合開始剤を通常の重合より多量に使用する方法、重合開始剤の他にメルカプト化合物や四塩化炭素等の連鎖移動剤を使用する方法、重合開始剤の他にベンゾキノンやジニトロベンゼンのような重合停止剤を使用する方法、さらに特開2000−128911号または同2000−344823号公報にあるような一つのチオール基と2級の水酸基とを有する化合物、或いは、該化合物と有機金属化合物を併用した重合触媒を用いて塊状重合する方法等を挙げることができ、何れも好ましく用いられるが、特に、該公報に記載の方法が好ましい。   Such polymerization methods include a method using a peroxide polymerization initiator such as cumene peroxide and t-butyl hydroperoxide, a method using a polymerization initiator in a larger amount than normal polymerization, and a mercapto compound in addition to the polymerization initiator. And a method using a chain transfer agent such as carbon tetrachloride, a method using a polymerization terminator such as benzoquinone and dinitrobenzene in addition to the polymerization initiator, and further disclosed in JP 2000-128911 or 2000-344823 Examples thereof include a compound having one thiol group and a secondary hydroxyl group, or a bulk polymerization method using a polymerization catalyst in which the compound and an organometallic compound are used in combination. In particular, the method described in the publication is preferable.

なお、本発明のアクリルポリマーとは、芳香環或いはシクロヘキシル基を有するモノマー単位を有しないアクリル酸またはメタクリル酸アルキルエステルのホモポリマーまたはコポリマーを指す。芳香環を側鎖に有するアクリルポリマーというのは、必ず芳香環を有するアクリル酸またはメタクリル酸エステルモノマー単位を含有するアクリルポリマーである。   The acrylic polymer of the present invention refers to a homopolymer or copolymer of acrylic acid or alkyl methacrylate that does not have a monomer unit having an aromatic ring or a cyclohexyl group. An acrylic polymer having an aromatic ring in the side chain is an acrylic polymer that always contains an acrylic acid or methacrylic acid ester monomer unit having an aromatic ring.

また、シクロヘキシル基を側鎖に有するアクリルポリマーというのは、シクロヘキシル基を有するアクリル酸またはメタクリル酸エステルモノマー単位を含有するアクリルポリマーである。   The acrylic polymer having a cyclohexyl group in the side chain is an acrylic polymer containing an acrylic acid or methacrylic acid ester monomer unit having a cyclohexyl group.

芳香環及びシクロヘキシル基を有さないアクリル酸エステルモノマーとしては、例えば、アクリル酸メチル、アクリル酸エチル、アクリル酸プロピル(i−、n−)、アクリル酸ブチル(n−、i−、s−、t−)、アクリル酸ペンチル(n−、i−、s−)、アクリル酸ヘキシル(n−、i−)、アクリル酸ヘプチル(n−、i−)、アクリル酸オクチル(n−、i−)、アクリル酸ノニル(n−、i−)、アクリル酸ミリスチル(n−、i−)、アクリル酸(2−エチルヘキシル)、アクリル酸(ε−カプロラクトン)、アクリル酸(2−ヒドロキシエチル)、アクリル酸(2−ヒドロキシプロピル)、アクリル酸(3−ヒドロキシプロピル)、アクリル酸(4−ヒドロキシブチル)、アクリル酸(2−ヒドロキシブチル)、アクリル酸(2−メトキシエチル)、アクリル酸(2−エトキシエチル)等、または上記アクリル酸エステルをメタクリル酸エステルに変えたものを挙げることができる。   Examples of the acrylate monomer having no aromatic ring and cyclohexyl group include, for example, methyl acrylate, ethyl acrylate, propyl acrylate (i-, n-), butyl acrylate (n-, i-, s-, t-), pentyl acrylate (n-, i-, s-), hexyl acrylate (n-, i-), heptyl acrylate (n-, i-), octyl acrylate (n-, i-) , Nonyl acrylate (n-, i-), myristyl acrylate (n-, i-), acrylic acid (2-ethylhexyl), acrylic acid (ε-caprolactone), acrylic acid (2-hydroxyethyl), acrylic acid (2-hydroxypropyl), acrylic acid (3-hydroxypropyl), acrylic acid (4-hydroxybutyl), acrylic acid (2-hydroxybutyl), acrylic acid 2-methoxy-ethyl), acrylic acid (2-ethoxyethyl), or the acrylic acid ester may include those obtained by changing the methacrylic acid ester.

アクリルポリマーは上記モノマーのホモポリマーまたはコポリマーであるが、アクリル酸メチルエステルモノマー単位が30質量%以上を有していることが好ましく、また、メタクリル酸メチルエステルモノマー単位が40質量%以上有することが好ましい。特にアクリル酸メチルまたはメタクリル酸メチルのホモポリマーが好ましい。   The acrylic polymer is a homopolymer or copolymer of the above-mentioned monomers, but the acrylic acid methyl ester monomer unit preferably has 30% by mass or more, and the methacrylic acid methyl ester monomer unit has 40% by mass or more. preferable. In particular, a homopolymer of methyl acrylate or methyl methacrylate is preferred.

芳香環を有するアクリル酸またはメタクリル酸エステルモノマーとしては、例えば、アクリル酸フェニル、メタクリル酸フェニル、アクリル酸(2または4−クロロフェニル)、メタクリル酸(2または4−クロロフェニル)、アクリル酸(2または3または4−エトキシカルボニルフェニル)、メタクリル酸(2または3または4−エトキシカルボニルフェニル)、アクリル酸(oまたはmまたはp−トリル)、メタクリル酸(oまたはmまたはp−トリル)、アクリル酸ベンジル、メタクリル酸ベンジル、アクリル酸フェネチル、メタクリル酸フェネチル、アクリル酸(2−ナフチル)等を挙げることができるが、アクリル酸ベンジル、メタクリル酸ベンジル、アクリル酸フェニチル、メタクリル酸フェネチルを好ましく用いることができる。   Examples of acrylic acid or methacrylic acid ester monomers having an aromatic ring include phenyl acrylate, phenyl methacrylate, acrylic acid (2 or 4-chlorophenyl), methacrylic acid (2 or 4-chlorophenyl), and acrylic acid (2 or 3 Or 4-ethoxycarbonylphenyl), methacrylic acid (2 or 3 or 4-ethoxycarbonylphenyl), acrylic acid (o or m or p-tolyl), methacrylic acid (o or m or p-tolyl), benzyl acrylate, Benzyl methacrylate, phenethyl acrylate, phenethyl methacrylate, acrylic acid (2-naphthyl) and the like can be mentioned, but benzyl acrylate, benzyl methacrylate, phenethyl acrylate, and phenethyl methacrylate are preferably used. That.

芳香環を側鎖に有するアクリルポリマーの中で、芳香環を有するアクリル酸またはメタクリル酸エステルモノマー単位が20〜40質量%を有し、且つアクリル酸またはメタクリル酸メチルエステルモノマー単位を50〜80質量%有することが好ましい。該ポリマー中、水酸基を有するアクリル酸またはメタクリル酸エステルモノマー単位を2〜20質量%有することが好ましい。   Among acrylic polymers having an aromatic ring in the side chain, the acrylic acid or methacrylic acid ester monomer unit having an aromatic ring has 20 to 40% by mass, and the acrylic acid or methacrylic acid methyl ester monomer unit is 50 to 80% by mass. % Is preferable. The polymer preferably has 2 to 20% by mass of acrylic acid or methacrylic acid ester monomer units having a hydroxyl group.

シクロヘキシル基を有するアクリル酸エステルモノマーとしては、例えば、アクリル酸シクロヘキシル、メタクリル酸シクロヘキシル、アクリル酸(4−メチルシクロヘキシル)、メタクリル酸(4−メチルシクロヘキシル)、アクリル酸(4−エチルシクロヘキシル)、メタクリル酸(4−エチルシクロヘキシル)等を挙げることができるが、アクリル酸シクロヘキシル及びメタクリル酸シクロヘキシルを好ましく用いることができる。   Examples of the acrylate monomer having a cyclohexyl group include cyclohexyl acrylate, cyclohexyl methacrylate, acrylic acid (4-methylcyclohexyl), methacrylic acid (4-methylcyclohexyl), acrylic acid (4-ethylcyclohexyl), and methacrylic acid. (4-ethylcyclohexyl) and the like can be mentioned, but cyclohexyl acrylate and cyclohexyl methacrylate can be preferably used.

シクロヘキシル基を側鎖に有するアクリルポリマー中、シクロヘキシル基を有するアクリル酸またはメタクリル酸エステルモノマー単位を20〜40質量%を有しかつ50〜80質量%有することが好ましい。また、該ポリマー中、水酸基を有するアクリル酸またはメタクリル酸エステルモノマー単位を2〜20質量%有することが好ましい。   In the acrylic polymer having a cyclohexyl group in the side chain, the acrylic acid or methacrylic acid ester monomer unit having a cyclohexyl group has 20 to 40% by mass and preferably 50 to 80% by mass. Moreover, it is preferable to have 2-20 mass% of acrylic acid or methacrylic acid ester monomer units having a hydroxyl group in the polymer.

上述のエチレン性不飽和モノマーを重合して得られるポリマー、アクリルポリマー、芳香環を側鎖に有するアクリルポリマー及びシクロヘキシル基を側鎖に有するアクリルポリマーは何れもセルロース樹脂との相溶性に優れる。   A polymer obtained by polymerizing the above ethylenically unsaturated monomer, an acrylic polymer, an acrylic polymer having an aromatic ring in the side chain, and an acrylic polymer having a cyclohexyl group in the side chain are all excellent in compatibility with the cellulose resin.

これらの水酸基を有するアクリル酸またはメタクリル酸エステルモノマーの場合はホモポリマーではなく、コポリマーの構成単位である。この場合、好ましくは、水酸基を有するアクリル酸またはメタクリル酸エステルモノマー単位がアクリルポリマー中2〜20質量%含有することが好ましい。   In the case of an acrylic acid or methacrylic acid ester monomer having these hydroxyl groups, it is not a homopolymer but a structural unit of a copolymer. In this case, it is preferable that the acrylic acid or methacrylic acid ester monomer unit having a hydroxyl group is contained in the acrylic polymer in an amount of 2 to 20% by mass.

また、側鎖に水酸基を有するポリマーも好ましく用いることができる。水酸基を有するモノマー単位としては、前記したモノマーと同様であるが、アクリル酸またはメタクリル酸エステルが好ましく、例えば、アクリル酸(2−ヒドロキシエチル)、アクリル酸(2−ヒドロキシプロピル)、アクリル酸(3−ヒドロキシプロピル)、アクリル酸(4−ヒドロキシブチル)、アクリル酸(2−ヒドロキシブチル)、アクリル酸−p−ヒドロキシメチルフェニル、アクリル酸−p−(2−ヒドロキシエチル)フェニル、またはこれらアクリル酸をメタクリル酸に置き換えたものを挙げることができ、好ましくは、アクリル酸−2−ヒドロキシエチル及びメタクリル酸−2−ヒドロキシエチルである。ポリマー中に水酸基を有するアクリル酸エステルまたはメタクリル酸エステルモノマー単位はポリマー中2〜20質量%含有することが好ましく、より好ましくは2〜10質量%である。   A polymer having a hydroxyl group in the side chain can also be preferably used. The monomer unit having a hydroxyl group is the same as the monomer described above, but acrylic acid or methacrylic acid ester is preferable. For example, acrylic acid (2-hydroxyethyl), acrylic acid (2-hydroxypropyl), acrylic acid (3 -Hydroxypropyl), acrylic acid (4-hydroxybutyl), acrylic acid (2-hydroxybutyl), acrylic acid-p-hydroxymethylphenyl, acrylic acid-p- (2-hydroxyethyl) phenyl, or these acrylic acids. The thing replaced by methacrylic acid can be mentioned, Preferably, it is 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate. The acrylic acid ester or methacrylic acid ester monomer unit having a hydroxyl group in the polymer is preferably contained in the polymer in an amount of 2 to 20% by mass, more preferably 2 to 10% by mass.

前記のようなポリマーが上記の水酸基を有するモノマー単位を2〜20質量%含有したものは、勿論セルロースエステルとの相溶性、保留性、寸法安定性が優れ、透湿度が小さいばかりでなく、偏光板保護フィルムとしての偏光子との接着性に特に優れ、偏光板の耐久性が向上する効果を有している。   A polymer containing 2 to 20% by mass of the above-mentioned monomer unit having a hydroxyl group, of course, is excellent in compatibility with cellulose ester, retention, dimensional stability, low moisture permeability, and polarized light. It is particularly excellent in adhesiveness with a polarizer as a plate protective film, and has the effect of improving the durability of the polarizing plate.

アクリルポリマーの主鎖の少なくとも一方の末端に水酸基を有するようにする方法は、特に主鎖の末端に水酸基を有するようにする方法であれば限定ないが、アゾビス(2−ヒドロキシエチルブチレート)のような水酸基を有するラジカル重合開始剤を使用する方法、2−メルカプトエタノールのような水酸基を有する連鎖移動剤を使用する方法、水酸基を有する重合停止剤を使用する方法、リビングイオン重合により水酸基を末端に有するようにする方法、特開2000−128911号公報は2000−344823号公報にあるような一つのチオール基と2級の水酸基とを有する化合物、或いは、該化合物と有機金属化合物を併用した重合触媒を用いて塊状重合する方法等により得ることができ、特に該公報に記載の方法が好ましい。   The method of having a hydroxyl group at at least one terminal of the main chain of the acrylic polymer is not particularly limited as long as it has a hydroxyl group at the terminal of the main chain, but azobis (2-hydroxyethylbutyrate) A method using a radical polymerization initiator having such a hydroxyl group, a method using a chain transfer agent having a hydroxyl group such as 2-mercaptoethanol, a method using a polymerization terminator having a hydroxyl group, and terminating a hydroxyl group by living ion polymerization. And a method comprising a compound having one thiol group and a secondary hydroxyl group as described in Japanese Patent Application Laid-Open No. 2000-344823, or a combination of the compound and an organometallic compound. It can be obtained by a bulk polymerization method using a catalyst, and the method described in the publication is particularly preferable.

この公報記載に関連する方法で作られたポリマーは、綜研化学社製のアクトフロー・シリーズとして市販されており、好ましく用いることができる。上記の末端に水酸基を有するポリマー及び/または側鎖に水酸基を有するポリマーは、本発明において、ポリマーの相溶性、透明性を著しく向上する効果を有する。   The polymer produced by the method related to the description in this publication is commercially available as Act Flow Series manufactured by Soken Chemical Co., Ltd., and can be preferably used. In the present invention, the polymer having a hydroxyl group at the terminal and / or the polymer having a hydroxyl group in a side chain has an effect of significantly improving the compatibility and transparency of the polymer.

さらに、延伸方向に対して負の配向複屈折性を示すエチレン性不飽和モノマーとして、スチレン類を用いたポリマーであることが負の屈折性を発現させるために好ましい。スチレン類としては、例えば、スチレン、メチルスチレン、ジメチルスチレン、トリメチルスチレン、エチルスチレン、イソプロピルスチレン、クロロメチルスチレン、メトキシスチレン、アセトキシスチレン、クロロスチレン、ジクロロスチレン、ブロモスチレン、ビニル安息香酸メチルエステルなどが挙げられるが、これらに限定される物ではない。   Furthermore, a polymer using styrene as an ethylenically unsaturated monomer exhibiting negative orientation birefringence with respect to the stretching direction is preferable in order to develop negative refraction. Examples of styrenes include styrene, methyl styrene, dimethyl styrene, trimethyl styrene, ethyl styrene, isopropyl styrene, chloromethyl styrene, methoxy styrene, acetoxy styrene, chloro styrene, dichloro styrene, bromo styrene, and vinyl benzoic acid methyl ester. Although it is mentioned, it is not a thing limited to these.

前記不飽和エチレン性モノマーとして挙げた例示モノマーと共重合してもよく、また複屈折性を制御する目的で、2種以上の上記ポリマーをもちいてセルロースエステルに相溶させて用いても良い。   It may be copolymerized with the exemplified monomers listed as the unsaturated ethylenic monomer, or may be used by being dissolved in a cellulose ester using two or more kinds of the above polymers for the purpose of controlling birefringence.

さらに、セルロースエステルフィルムは、分子内に芳香環と親水性基を有しないエチレン性不飽和モノマーXaと分子内に芳香環を有せず、親水性基を有するエチレン性不飽和モノマーXbとを共重合して得られた重量平均分子量5000以上30000以下のポリマーXと、より好ましくは芳香環を有さないエチレン性不飽和モノマーYaを重合して得られた重量平均分子量500以上3000以下のポリマーYとを含有することが好ましい。
(ポリマーX、ポリマーY)
本発明に用いられるポリマーXは、分子内に芳香環と親水性基を有しないエチレン性不飽和モノマーXaと、分子内に芳香環を有せず、親水性基を有するエチレン性不飽和モノマーXbとを共重合して得られた重量平均分子量5000以上、30000以下のポリマーである。
In addition, the cellulose ester film contains an ethylenically unsaturated monomer Xa having no aromatic ring and a hydrophilic group in the molecule and an ethylenically unsaturated monomer Xb having no aromatic ring in the molecule and having a hydrophilic group. Polymer Y having a weight average molecular weight of 5,000 to 30,000 obtained by polymerization, and more preferably a polymer Y having a weight average molecular weight of 500 to 3,000 obtained by polymerizing an ethylenically unsaturated monomer Ya having no aromatic ring It is preferable to contain.
(Polymer X, Polymer Y)
The polymer X used in the present invention includes an ethylenically unsaturated monomer Xa having no aromatic ring and a hydrophilic group in the molecule, and an ethylenically unsaturated monomer Xb having no aromatic ring in the molecule and having a hydrophilic group. Is a polymer having a weight average molecular weight of 5,000 or more and 30,000 or less obtained by copolymerization.

好ましくは、Xaは、分子内に芳香環と親水性基を有しないアクリルまたはメタクリルモノマー、Xbは、分子内に芳香環を有せず親水性基を有するアクリルまたはメタクリルモノマーである。   Preferably, Xa is an acrylic or methacrylic monomer that does not have an aromatic ring and a hydrophilic group in the molecule, and Xb is an acrylic or methacrylic monomer that does not have an aromatic ring in the molecule and has a hydrophilic group.

ポリマーXは、下記の一般式(6)で表わされる。   The polymer X is represented by the following general formula (6).

−(Xa)m−(Xb)n−(Xc)p− ・・・(6)
さらに好ましくは、下記の一般式(7)で表わされるポリマーである。
− (Xa) m − (Xb) n − (Xc) p − (6)
More preferably, it is a polymer represented by the following general formula (7).

−[CH2−C(−R1)(−CO22)]m−[CH2−C(−R3
(−CO24−OH)−]n−[Xc]p− ・・・(7)
(式中、R1、R3は、HまたはCH3を表わす。R2は炭素数1〜12のアルキル基、シクロアルキル基を表わす。R4は−CH2−、−C24−または−C36−を表わす。Xcは、Xa、Xbに重合可能なモノマー単位を表わす。m、nおよびpは、モル組成比を表わす。ただし、m≠0、n≠0、k≠0、m+n+p=100である。)
本発明において、アクリル系ポリマーXを構成するモノマー単位としてのモノマーを下記に挙げるがこれに限定されない。
- [CH 2 -C (-R 1 ) (- CO 2 R 2)] m - [CH 2 -C (-R 3)
(-CO 2 R 4 -OH) - ] n - [Xc] p - ··· (7)
(In the formula, R 1 and R 3 represent H or CH 3. R 2 represents an alkyl group having 1 to 12 carbon atoms and a cycloalkyl group. R 4 represents —CH 2 —, —C 2 H 4 —. Or -C 3 H 6- , Xc represents a monomer unit polymerizable to Xa and Xb, m, n and p represent molar composition ratios, provided that m ≠ 0, n ≠ 0, k ≠ 0, m + n + p = 100.)
In the present invention, monomers as monomer units constituting the acrylic polymer X are listed below, but are not limited thereto.

アクリル系ポリマーXにおいて、親水性基とは、水酸基、エチレンオキシド連鎖を有する基をいう。   In the acrylic polymer X, the hydrophilic group means a group having a hydroxyl group or an ethylene oxide chain.

分子内に芳香環と親水性基を有しないエチレン性不飽和モノマーXaは、例えばアクリル酸メチル、アクリル酸エチル、アクリル酸プロピル(i−、n−)、アクリル酸ブチル(n−、i−、s−、t−)、アクリル酸ペンチル(n−、i−、s−)、アクリル酸ヘキシル(n−、i−)、アクリル酸ヘプチル(n−、i−)、アクリル酸オクチル(n−、i−)、アクリル酸ノニル(n−、i−)、アクリル酸ミリスチル(n−、i−)、アクリル酸(2−エチルヘキシル)、アクリル酸(ε−カプロラクトン)、等、または上記アクリル酸エステルをメタクリル酸エステルに変えたものを挙げることができる。   The ethylenically unsaturated monomer Xa having no aromatic ring and no hydrophilic group in the molecule includes, for example, methyl acrylate, ethyl acrylate, propyl acrylate (i-, n-), butyl acrylate (n-, i-, s-, t-), pentyl acrylate (n-, i-, s-), hexyl acrylate (n-, i-), heptyl acrylate (n-, i-), octyl acrylate (n-, i-), nonyl acrylate (n-, i-), myristyl acrylate (n-, i-), acrylic acid (2-ethylhexyl), acrylic acid (ε-caprolactone), etc., or the above acrylate ester What changed to the methacrylic acid ester can be mentioned.

中でも、アクリル酸メチル、アクリル酸エチル、メタクリル酸メチル、メタクリル酸エチル、メタクリル酸プロピル(i−、n−)であることが好ましい。   Among these, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, and propyl methacrylate (i-, n-) are preferable.

分子内に芳香環を有せず、親水性基を有するエチレン性不飽和モノマーXbは、水酸基を有するモノマー単位として、アクリル酸またはメタクリル酸エステルが好ましく、例えばアクリル酸(2−ヒドロキシエチル)、アクリル酸(2−ヒドロキシプロピル)、アクリル酸(3−ヒドロキシプロピル)、アクリル酸(4−ヒドロキシブチル)、アクリル酸(2−ヒドロキシブチル)、またはこれらアクリル酸をメタクリル酸に置き換えたものを挙げることができ、好ましくは、アクリル酸(2−ヒドロキシエチル)、及びメタクリル酸(2−ヒドロキシエチル)、アクリル酸(2−ヒドロキシプロピル)、アクリル酸(3−ヒドロキシプロピル)である。   The ethylenically unsaturated monomer Xb having no aromatic ring in the molecule and having a hydrophilic group is preferably acrylic acid or methacrylic acid ester as a monomer unit having a hydroxyl group. For example, acrylic acid (2-hydroxyethyl), acrylic Examples include acid (2-hydroxypropyl), acrylic acid (3-hydroxypropyl), acrylic acid (4-hydroxybutyl), acrylic acid (2-hydroxybutyl), or those obtained by replacing these acrylic acids with methacrylic acid. Preferred are acrylic acid (2-hydroxyethyl), methacrylic acid (2-hydroxyethyl), acrylic acid (2-hydroxypropyl), and acrylic acid (3-hydroxypropyl).

Xcとしては、Xa、Xb以外のものでかつ共重合可能なエチレン性不飽和モノマーであれば、特に制限はないが、芳香環を有していないものが好ましい。   Xc is not particularly limited as long as it is an ethylenically unsaturated monomer other than Xa and Xb and copolymerizable, but preferably has no aromatic ring.

Xa、Xb、及びXcのモル組成比=m:nは、99:1〜65:35の範囲が好ましく、さらに好ましくは95:5〜75:25の範囲である。Xcのpは0〜10である。Xcは複数のモノマー単位であってもよい。   The molar composition ratio of Xa, Xb, and Xc = m: n is preferably in the range of 99: 1 to 65:35, and more preferably in the range of 95: 5 to 75:25. P of Xc is 0-10. Xc may be a plurality of monomer units.

Xaのモル組成比が多いと、セルロースエステルとの相溶性が良化するが、フィルム厚み方向リタデーション(Rt)値が大きくなる。Xbのモル組成比が多いと、上記相溶性が悪くなるが、厚み方向リタデーション(Rt)を低減させる効果が高い。また、Xbのモル組成比が上記範囲を超えると、製膜時にヘイズが出る傾向があり、これらの最適化を図り、Xa、Xbのモル組成比を決めることが好ましい。   When the molar composition ratio of Xa is large, compatibility with the cellulose ester is improved, but the film thickness direction retardation (Rt) value is increased. When the molar composition ratio of Xb is large, the compatibility is deteriorated, but the effect of reducing the thickness direction retardation (Rt) is high. Further, if the molar composition ratio of Xb exceeds the above range, haze tends to occur during film formation. It is preferable to optimize these and determine the molar composition ratio of Xa and Xb.

ポリマーXの分子量は、重量平均分子量が5000以上30000以下であり、さらに好ましくは8000以上25000以下である。   As for the molecular weight of the polymer X, the weight average molecular weight is from 5,000 to 30,000, and more preferably from 8,000 to 25,000.

重量平均分子量を5000以上とすることにより、セルロースエステルフィルムの、高温高湿下における寸法変化が少ない、偏光板保護フィルムとしてカールが少ない等の利点が得られ好ましい。重量平均分子量が30000を以内とした場合は、セルロースエステルとの相溶性がより向上し、高温高湿下においてのブリードアウト、さらには製膜直後でのヘイズの発生が抑制される。   By setting the weight average molecular weight to 5,000 or more, it is preferable because the cellulose ester film has advantages such as less dimensional change under high temperature and high humidity and less curling as a polarizing plate protective film. When the weight average molecular weight is 30000 or less, the compatibility with the cellulose ester is further improved, and bleeding out under high temperature and high humidity, and further haze generation immediately after film formation is suppressed.

ポリマーXの重量平均分子量は、公知の分子量調節方法で調整することができる。そのような分子量調節方法としては、例えば四塩化炭素、ラウリルメルカプタン、チオグリコール酸オクチル等の連鎖移動剤を添加する方法等が挙げられる。また、重合温度は通常室温から130℃、好ましくは50℃から100℃で行われるが、この温度または重合反応時間を調整することで可能である。   The weight average molecular weight of the polymer X can be adjusted by a known molecular weight adjusting method. Examples of such a molecular weight adjusting method include a method of adding a chain transfer agent such as carbon tetrachloride, lauryl mercaptan, octyl thioglycolate, and the like. The polymerization temperature is usually room temperature to 130 ° C., preferably 50 ° C. to 100 ° C., and this temperature or the polymerization reaction time can be adjusted.

つぎに、ポリマーYは、芳香環を有さないエチレン性不飽和モノマーYaを重合して得られた重量平均分子量500以上、3000以下のポリマーである。   Next, the polymer Y is a polymer having a weight average molecular weight of 500 or more and 3000 or less obtained by polymerizing an ethylenically unsaturated monomer Ya having no aromatic ring.

ここで、ポリマーYの重量平均分子量が500以上では、ポリマーの残存モノマーが減少するので、好ましい。また、ポリマーYの重量平均分子量を3000以下とすることは、厚み方向リタデーション(Rt)値の低下性能を維持するために好ましい。   Here, when the weight average molecular weight of the polymer Y is 500 or more, the residual monomer of the polymer decreases, which is preferable. Moreover, it is preferable to make the weight average molecular weight of the polymer Y 3000 or less in order to maintain the fall performance of the thickness direction retardation (Rt) value.

Yaは、好ましくは芳香環を有さないアクリルまたはメタクリルモノマーである。   Ya is preferably an acrylic or methacrylic monomer having no aromatic ring.

ポリマーYは、下記の一般式(8)で表される。   The polymer Y is represented by the following general formula (8).

−(Ya)k−(Yb)q− ・・・(8)
さらに好ましくは、下記の一般式(9)で表されるポリマーである。
-(Ya) k- (Yb) q- (8)
More preferably, it is a polymer represented by the following general formula (9).

−[CH2−C(−R5)(−CO26)]k−[Yb]q− …(9)
(式中、R5は、HまたはCH3を表わす。R6は、炭素数1〜12のアルキル基またはシクロアルキル基を表わす。Ybは、Yaと共重合可能なモノマー単位を表わす。kおよびqは、モル組成比を表わす。ただし、k≠0、k+q=100である。)
Ybは、Yaと共重合可能なエチレン性不飽和モノマーであれば特に制限はない。Ybは複数であってもよい。k+q=100、qは好ましくは0〜30である。
- [CH 2 -C (-R 5 ) (- CO 2 R 6)] k- [Yb] q- ... (9)
(In the formula, R 5 represents H or CH 3. R 6 represents an alkyl group or a cycloalkyl group having 1 to 12 carbon atoms. Yb represents a monomer unit copolymerizable with Ya. q represents a molar composition ratio, where k ≠ 0 and k + q = 100.
Yb is not particularly limited as long as it is an ethylenically unsaturated monomer copolymerizable with Ya. Yb may be plural. k + q = 100, q is preferably 0-30.

芳香環を有さないエチレン性不飽和モノマーを重合して得られるポリマーYを構成するエチレン性不飽和モノマーYaは、アクリル酸エステルとして、例えばアクリル酸メチル、アクリル酸エチル、アクリル酸プロピル(i−、n−)、アクリル酸ブチル(n−、i−、s−、t−)、アクリル酸ペンチル(n−、i−、s−)、アクリル酸ヘキシル(n−、i−)、アクリル酸ヘプチル(n−、i−)、アクリル酸オクチル(n−、i−)、アクリル酸ノニル(n−、i−)、アクリル酸ミリスチル(n−、i−)、アクリル酸シクロヘキシル、アクリル酸(2−エチルヘキシル)、アクリル酸(ε−カプロラクトン)、アクリル酸(2−ヒドロキシエチル)、アクリル酸(2−ヒドロキシプロピル)、アクリル酸(3−ヒドロキシプロピル)、アクリル酸(4−ヒドロキシブチル)、アクリル酸(2−ヒドロキシブチル)、メタクリル酸エステルとして、上記アクリル酸エステルをメタクリル酸エステルに変えたもの;不飽和酸として、例えばアクリル酸、メタクリル酸、無水マレイン酸、クロトン酸、イタコン酸等を挙げることができる。   The ethylenically unsaturated monomer Ya constituting the polymer Y obtained by polymerizing an ethylenically unsaturated monomer having no aromatic ring is, for example, methyl acrylate, ethyl acrylate, propyl acrylate (i- , N-), butyl acrylate (n-, i-, s-, t-), pentyl acrylate (n-, i-, s-), hexyl acrylate (n-, i-), heptyl acrylate (N-, i-), octyl acrylate (n-, i-), nonyl acrylate (n-, i-), myristyl acrylate (n-, i-), cyclohexyl acrylate, acrylic acid (2- Ethyl hexyl), acrylic acid (ε-caprolactone), acrylic acid (2-hydroxyethyl), acrylic acid (2-hydroxypropyl), acrylic acid (3-hydroxypropiyl) ), Acrylic acid (4-hydroxybutyl), acrylic acid (2-hydroxybutyl), methacrylic acid ester, the above acrylic acid ester changed to methacrylic acid ester; unsaturated acid such as acrylic acid, methacrylic acid, Mention may be made of maleic anhydride, crotonic acid, itaconic acid and the like.

Ybは、Yaと共重合可能なエチレン性不飽和モノマーであれば、特に制限はないが、ビニルエステルとして、例えば酢酸ビニル、プロピオン酸ビニル、酪酸ビニル、吉草酸ビニル、ピバリン酸ビニル、カプロン酸ビニル、カプリン酸ビニル、ラウリン酸ビニル、ミリスチン酸ビニル、パルミチン酸ビニル、ステアリン酸ビニル、シクロヘキサンカルボン酸ビニル、オクチル酸ビニル、メタクリル酸ビニル、クロトン酸ビニル、ソルビン酸ビニル、桂皮酸ビニル等が好ましい。Ybは複数であってもよい。   Yb is not particularly limited as long as it is an ethylenically unsaturated monomer copolymerizable with Ya. Examples of vinyl esters include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl pivalate, and vinyl caproate. Vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl cyclohexanecarboxylate, vinyl octylate, vinyl methacrylate, vinyl crotonate, vinyl sorbate, vinyl cinnamate and the like are preferred. Yb may be plural.

ポリマーX、及びポリマーYを合成するには、通常の重合では分子量のコントロールが難しく、分子量をあまり大きくしない方法で、できるだけ分子量を揃えることのできる方法を用いることが望ましい。   In order to synthesize the polymer X and the polymer Y, it is difficult to control the molecular weight in normal polymerization, and it is desirable to use a method that can make the molecular weights as uniform as possible without increasing the molecular weight.

ポリマーX、及びポリマーYの重合方法としては、クメンペルオキシドやt−ブチルヒドロペルオキシドのような過酸化物重合開始剤を使用する方法、重合開始剤を通常の重合より多量に使用する方法、重合開始剤の他にメルカプト化合物や四塩化炭素等の連鎖移動剤を使用する方法、重合開始剤の他にベンゾキノンやジニトロベンゼンのような重合停止剤を使用する方法、さらに特開2000−128911号公報または同2000−344823号公報に記載された一つのチオール基と2級の水酸基とを有する化合物、あるいは、該化合物と有機金属化合物を併用した重合触媒を用いて塊状重合する方法等を挙げることができる。   Polymerization methods of polymer X and polymer Y include a method using a peroxide polymerization initiator such as cumene peroxide and t-butyl hydroperoxide, a method using a polymerization initiator in a larger amount than normal polymerization, and a polymerization start. A method using a chain transfer agent such as a mercapto compound or carbon tetrachloride in addition to the agent, a method using a polymerization terminator such as benzoquinone or dinitrobenzene in addition to the polymerization initiator, and JP 2000-128911 A or Examples thereof include a method of bulk polymerization using a compound having one thiol group and a secondary hydroxyl group described in JP-A-2000-344823, or a polymerization catalyst in which the compound and an organometallic compound are used in combination. .

ポリマーYは、分子中にチオール基と2級の水酸基とを有する化合物を連鎖移動剤として使用する重合方法が好ましい。この場合、ポリマーYの末端には、重合触媒および連鎖移動剤に起因する水酸基、チオエーテルを有することとなる。この末端残基により、ポリマーYとセルロースエステルとの相溶性を調整することができる。   The polymer Y is preferably a polymerization method using a compound having a thiol group and a secondary hydroxyl group in the molecule as a chain transfer agent. In this case, the terminal of the polymer Y has a hydroxyl group and a thioether resulting from the polymerization catalyst and the chain transfer agent. By this terminal residue, the compatibility between the polymer Y and the cellulose ester can be adjusted.

ポリマーXおよびポリマーYの水酸基価は30〜150[mgKOH/g]であることが好ましい。   The hydroxyl value of the polymer X and the polymer Y is preferably 30 to 150 [mg KOH / g].

ここで、水酸基価の測定は、JIS K−0070(1992)に準ずる。この水酸基価は、試料1gをアセチル化させたとき、水酸基と結合した酢酸を中和するのに必要とする水酸化カリウムのmg数と定義される。具体的には試料xg(約1g)をフラスコに精秤し、これにアセチル化試薬(無水酢酸20mlにピリジンを加えて400mlにしたもの)20mlを正確に加える。フラスコの口に空気冷却管を装着し、95〜100℃のグリセリン浴にて加熱する。1時間30分後、冷却し、空気冷却管から精製水1mlを加え、無水酢酸を酢酸に分解する。次に電位差滴定装置を用いて0.5mol/L水酸化カリウムエタノール溶液で滴定を行い、得られた滴定曲線の変曲点を終点とする。さらに空試験として、試料を入れないで滴定し、滴定曲線の変曲点を求める。水酸基価は、つぎの式によって算出する。   Here, the measurement of hydroxyl value is based on JIS K-0070 (1992). This hydroxyl value is defined as the number of mg of potassium hydroxide required to neutralize acetic acid bonded to a hydroxyl group when 1 g of a sample is acetylated. Specifically, a sample xg (about 1 g) is precisely weighed in a flask, and 20 ml of an acetylating reagent (a solution obtained by adding pyridine to 20 ml of acetic anhydride to 400 ml) is accurately added thereto. An air cooling tube is attached to the mouth of the flask and heated in a glycerin bath at 95-100 ° C. After 1 hour and 30 minutes, the mixture is cooled, 1 ml of purified water is added from an air condenser, and acetic anhydride is decomposed into acetic acid. Next, titration is performed with a 0.5 mol / L potassium hydroxide ethanol solution using a potentiometric titrator, and the inflection point of the obtained titration curve is set as the end point. Further, as a blank test, titration is performed without a sample, and an inflection point of the titration curve is obtained. The hydroxyl value is calculated by the following formula.

水酸基価={(B−C)×f×28.05/x}+D
(式中、Bは、空試験に用いた0.5mol/Lの水酸化カリウムエタノール溶液の量(ml)、Cは、滴定に用いた0.5mol/Lの水酸化カリウムエタノール溶液の量(ml)、fは、0.5mol/L水酸化カリウムエタノール溶液のファクター、Dは、酸価、また28.05は、水酸化カリウムの1mol量56.11の1/2を表わす)
ポリマーXとポリマーYのセルロースエステルフィルム中での含有量は、下記式(i)、式(ii)を満足する範囲であることが好ましい。ポリマーXの含有量をxg(質量%=ポリマーXの質量/セルロースエステルの質量×100)、ポリマーYの含有量をyg(質量%)とすると、
式(i) 5≦xg+yg≦35(質量%)
式(ii) 0.05≦yg/(xg+yg)≦0.4
式(i)の好ましい範囲は、10〜25質量%である。
Hydroxyl value = {(BC) × f × 28.05 / x} + D
(In the formula, B is the amount of 0.5 mol / L potassium hydroxide ethanol solution (ml) used for the blank test, and C is the amount of 0.5 mol / L potassium hydroxide ethanol solution used for titration ( ml), f is a factor of 0.5 mol / L potassium hydroxide ethanol solution, D is acid value, and 28.05 is 1/2 of 1 mol amount of potassium hydroxide 56.11)
The content of the polymer X and the polymer Y in the cellulose ester film is preferably in a range satisfying the following formulas (i) and (ii). When the content of the polymer X is xg (mass% = the mass of the polymer X / the mass of the cellulose ester × 100) and the content of the polymer Y is yg (mass%),
Formula (i) 5 ≦ xg + yg ≦ 35 (mass%)
Formula (ii) 0.05 ≦ yg / (xg + yg) ≦ 0.4
A preferable range of the formula (i) is 10 to 25% by mass.

なお、ポリマーの重量平均分子量Mwは、ゲルパーミエーションクロマトグラフィーを用いて測定することができる。   In addition, the weight average molecular weight Mw of a polymer can be measured using gel permeation chromatography.

測定条件は、以下の通りである。   The measurement conditions are as follows.

溶媒: メチレンクロライド
カラム: Shodex K806、K805、K803G
(昭和電工株式会社製を3本接続して使用した)
カラム温度:25℃
試料濃度: 0.1質量%
検出器: RI Model 504(GLサイエンス社製)
ポンプ: L6000(日立製作所株式会社製)
流量: 1.0ml/min
校正曲線: 標準ポリスチレンSTK
standard ポリスチレン(東ソー株式会社製)Mw=1,000,000〜500までの13サンプルによる校正曲線を使用した。13サンプルは、ほぼ等間隔に用いる。
Solvent: Methylene chloride Column: Shodex K806, K805, K803G
(Used by connecting three Showa Denko Co., Ltd.)
Column temperature: 25 ° C
Sample concentration: 0.1% by mass
Detector: RI Model 504 (manufactured by GL Sciences)
Pump: L6000 (manufactured by Hitachi, Ltd.)
Flow rate: 1.0ml / min
Calibration curve: Standard polystyrene STK
Standard polystyrene (manufactured by Tosoh Corporation) Mw = 1,000,000-500 calibration curves with 13 samples were used. Thirteen samples are used at approximately equal intervals.

ポリマーXとポリマーYは、総量として5質量%以上であれば、厚み方向リタデーション(Rt)値の低減に十分な作用をする。また、総量として35質量%以下であれば、偏光子PVAとの接着性が良好である。   If the total amount of the polymer X and the polymer Y is 5% by mass or more, the polymer X and the polymer Y sufficiently act to reduce the thickness direction retardation (Rt) value. Moreover, if it is 35 mass% or less as a total amount, adhesiveness with polarizer PVA is favorable.

ポリマーXとポリマーYは、後述するドープ液を構成する素材として直接添加、溶解するか、もしくはセルロースエステルを溶解する有機溶媒に予め溶解した後ドープ液に添加することができる。   The polymer X and the polymer Y can be directly added and dissolved as a material constituting the dope solution described later, or can be added to the dope solution after being previously dissolved in an organic solvent for dissolving the cellulose ester.

セルロースエステルフィルム中の上記可塑剤の総含有量は、固形分総量に対し、5〜20質量%が好ましく、6〜16質量%がさらに好ましく、特に好ましくは8〜13質量%である。また、2種の可塑剤の含有量は各々少なくとも1質量%以上であり、好ましくは各々2質量%以上含有することである。   The total content of the plasticizer in the cellulose ester film is preferably 5 to 20% by mass, more preferably 6 to 16% by mass, and particularly preferably 8 to 13% by mass with respect to the total solid content. The contents of the two kinds of plasticizers are each at least 1% by mass, preferably 2% by mass or more.

多価アルコールエステル系可塑剤は、1〜15質量%含有することが好ましく、特に3〜11質量%含有することが好ましい。多価アルコールエステル系可塑剤の含有量が、少ないと平面性の劣化が認められ、また多すぎると、ブリードアウトがしやすい。多価アルコールエステル系可塑剤とその他の可塑剤との質量比率は、1:4〜4:1の範囲であることが好ましく、1:3〜3:1であることがさらに好ましい。可塑剤の添加量が多すぎても、また少なすぎてもフィルムが変形しやすく好ましくない。
(溶液流延製膜法)
セルロースエステルフィルムの溶液流延製膜法による製造は、セルロースエステル及び添加剤を溶剤に溶解させてドープを調製する工程、ドープをベルト状もしくはドラム状の金属支持体上に流延する工程、流延したドープをウェブとして乾燥する工程、金属支持体から剥離する工程、延伸または幅保持する工程、さらに乾燥する工程、仕上がったフィルムを巻取る工程により行われる。
The polyhydric alcohol ester plasticizer is preferably contained in an amount of 1 to 15% by mass, particularly preferably 3 to 11% by mass. If the content of the polyhydric alcohol ester plasticizer is small, deterioration of planarity is recognized, and if it is too large, bleeding out is likely to occur. The mass ratio of the polyhydric alcohol ester plasticizer and the other plasticizer is preferably in the range of 1: 4 to 4: 1, and more preferably 1: 3 to 3: 1. If the amount of the plasticizer added is too large or too small, the film is liable to be deformed, which is not preferable.
(Solution casting film forming method)
The cellulose ester film is produced by a solution casting method, in which a cellulose ester and an additive are dissolved in a solvent to prepare a dope, a dope is cast on a belt-shaped or drum-shaped metal support, It is performed by a step of drying the stretched dope as a web, a step of peeling from the metal support, a step of stretching or maintaining the width, a step of further drying, and a step of winding the finished film.

まず、ドープを調製する工程について述べる。ドープ中のセルロースエステルの濃度は、濃度が高い方が金属支持体に流延した後の乾燥負荷が低減できて好ましいが、セルロースエステルの濃度が高過ぎると濾過時の負荷が増えて、濾過精度が悪くなる。これらを両立する濃度としては、10〜35質量%が好ましく、さらに好ましくは、15〜25質量%である。   First, the process for preparing the dope will be described. The concentration of cellulose ester in the dope is preferably higher because the drying load after casting on the metal support can be reduced. However, if the concentration of cellulose ester is too high, the load during filtration increases and the filtration accuracy increases. Becomes worse. The concentration for achieving both of these is preferably 10 to 35% by mass, and more preferably 15 to 25% by mass.

ドープで用いられる溶剤は、単独で用いても2種以上を併用してもよいが、セルロースエステルの良溶剤と貧溶剤を混合して使用することが生産効率の点で好ましく、良溶剤が多い方がセルロースエステルの溶解性の点で好ましい。良溶剤と貧溶剤の混合比率の好ましい範囲は、良溶剤が70〜98質量%であり、貧溶剤が2〜30質量%である。良溶剤、貧溶剤とは、使用するセルロースエステルを単独で溶解するものを良溶剤、単独で膨潤するかまたは溶解しないものを貧溶剤と定義している。そのため、セルロースエステルのアシル基置換度によっては、良溶剤、貧溶剤が変わり、例えばアセトンを溶剤として用いる時には、セルロースエステルの酢酸エステル(アセチル基置換度2.4)、セルロースアセテートプロピオネートでは良溶剤になり、セルロースの酢酸エステル(アセチル基置換度2.8)では貧溶剤となる。   The solvent used in the dope may be used alone or in combination of two or more, but it is preferable to use a mixture of a good solvent and a poor solvent of cellulose ester in terms of production efficiency, and there are many good solvents. This is preferable from the viewpoint of the solubility of the cellulose ester. The preferable range of the mixing ratio of the good solvent and the poor solvent is 70 to 98% by mass for the good solvent and 2 to 30% by mass for the poor solvent. With a good solvent and a poor solvent, what dissolve | melts the cellulose ester to be used independently is defined as a good solvent, and what poorly swells or does not melt | dissolve is defined as a poor solvent. Therefore, depending on the acyl group substitution degree of the cellulose ester, the good solvent and the poor solvent change. For example, when acetone is used as the solvent, the cellulose ester acetate ester (acetyl group substitution degree 2.4) and cellulose acetate propionate are good. As a solvent, cellulose acetate (acetyl group substitution degree 2.8) is a poor solvent.

本発明に用いられる良溶剤は、特に限定されないが、メチレンクロライド等の有機ハロゲン化合物やジオキソラン類、アセトン、酢酸メチル、アセト酢酸メチル等が挙げられる。特に好ましくはメチレンクロライドまたは酢酸メチルが挙げられる。   The good solvent used in the present invention is not particularly limited, and examples thereof include organic halogen compounds such as methylene chloride, dioxolanes, acetone, methyl acetate, and methyl acetoacetate. Particularly preferred is methylene chloride or methyl acetate.

また、本発明に用いられる貧溶剤は特に限定されないが、例えば、メタノール、エタノール、n−ブタノール、シクロヘキサン、シクロヘキサノン等が好ましく用いられる。また、ドープ中には水が0.01〜2質量%含有していることが好ましい。   Moreover, although the poor solvent used for this invention is not specifically limited, For example, methanol, ethanol, n-butanol, cyclohexane, cyclohexanone, etc. are used preferably. Moreover, it is preferable that 0.01-2 mass% of water contains in dope.

上記記載のドープを調製する時の、セルロースエステルの溶解方法としては、一般的な方法を用いることができる。加熱と加圧を組み合わせると常圧における沸点以上に加熱できる。溶剤の常圧での沸点以上でかつ加圧下で溶剤が沸騰しない範囲の温度で加熱しながら攪拌溶解すると、ゲルやママコと呼ばれる塊状未溶解物の発生を防止するため好ましい。また、セルロースエステルを貧溶剤と混合して湿潤または膨潤させた後、さらに良溶剤を添加して溶解する方法も好ましく用いられる。   A general method can be used as a dissolution method of the cellulose ester when preparing the dope described above. When heating and pressurization are combined, it is possible to heat above the boiling point at normal pressure. It is preferable to stir and dissolve while heating at a temperature that is equal to or higher than the boiling point of the solvent at normal pressure and does not boil under pressure, in order to prevent the formation of massive undissolved material called gel or mamako. Moreover, after mixing a cellulose ester with a poor solvent and making it wet or swell, the method of adding a good solvent and melt | dissolving is also used preferably.

加圧は、窒素ガス等の不活性気体を圧入する方法や、加熱によって溶剤の蒸気圧を上昇させる方法によって行ってもよい。加熱は外部から行うことが好ましく、例えばジャケットタイプのものは温度コントロールが容易で好ましい。   The pressurization may be performed by a method of injecting an inert gas such as nitrogen gas or a method of increasing the vapor pressure of the solvent by heating. Heating is preferably performed from the outside. For example, a jacket type is preferable because temperature control is easy.

溶剤を添加しての加熱温度は、高い方がセルロースエステルの溶解性の観点から好ましいが、加熱温度が高すぎると必要とされる圧力が大きくなり生産性が悪くなる。好ましい加熱温度は45〜120℃であり、60〜110℃がより好ましく、70℃〜105℃がさらに好ましい。また、圧力は設定温度で溶剤が沸騰しないように調整される。   The heating temperature with the addition of the solvent is preferably higher from the viewpoint of the solubility of the cellulose ester, but if the heating temperature is too high, the required pressure increases and the productivity deteriorates. A preferable heating temperature is 45 to 120 ° C, more preferably 60 to 110 ° C, and still more preferably 70 ° C to 105 ° C. The pressure is adjusted so that the solvent does not boil at the set temperature.

または冷却溶解法も、好ましく用いられ、これによって酢酸メチル等の溶媒にセルロースエステルを溶解させることができる。   Alternatively, a cooling dissolution method is also preferably used, whereby the cellulose ester can be dissolved in a solvent such as methyl acetate.

つぎに、このセルロースエステル溶液を濾紙等の適当な濾過材を用いて濾過する。濾過材としては、不溶物等を除去するために、絶対濾過精度が小さい方が好ましいが、絶対濾過精度が小さすぎると濾過材の目詰まりが発生しやすいという問題がある。このため、絶対濾過精度0.008mm以下の濾材が好ましく、0.001〜0.008mmの濾材がより好ましく、0.003〜0.006mmの濾材がさらに好ましい。   Next, this cellulose ester solution is filtered using a suitable filter medium such as filter paper. As the filter medium, in order to remove insoluble matters and the like, it is preferable that the absolute filtration accuracy is small. However, if the absolute filtration accuracy is too small, there is a problem that the filter medium is likely to be clogged. For this reason, a filter medium with an absolute filtration accuracy of 0.008 mm or less is preferable, a filter medium with 0.001 to 0.008 mm is more preferable, and a filter medium with 0.003 to 0.006 mm is more preferable.

濾材の材質は、特に制限はなく、通常の濾材を使用することができるが、ポリプロピレン、テフロン(登録商標)等のプラスチック製の濾材や、ステンレススティール等の金属製の濾材が繊維の脱落等がなく好ましい。濾過により、原料のセルロースエステルに含まれていた不純物、特に輝点異物を除去、低減することが好ましい。   The material of the filter medium is not particularly limited, and a normal filter medium can be used. However, a plastic filter medium such as polypropylene or Teflon (registered trademark), or a metal filter medium such as stainless steel may cause fibers to fall off. Less preferred. It is preferable to remove and reduce impurities, particularly bright spot foreign matter, contained in the raw material cellulose ester by filtration.

この明細書において、輝点異物とは、2枚の偏光板をクロスニコル状態にして配置し、その間にセルロースエステルフィルムを置き、一方の偏光板の側から光を当てて、他方の偏光板の側から観察した時に反対側からの光が漏れて見える点(異物)のことであり、径が0.01mm以上である輝点数が200個/cm2以下であることが好ましい。より好ましくは100個/cm2以下であり、さらに好ましくは50個/m2以下であり、さらに好ましくは0〜10個/cm2以下である。また、0.01mm以下の輝点も少ない方が好ましい。 In this specification, the bright spot foreign material is arranged in a crossed Nicol state with two polarizing plates, a cellulose ester film is placed between them, light is applied from one polarizing plate side, It is a point (foreign matter) that light from the opposite side appears to leak when observed from the side, and the number of bright spots having a diameter of 0.01 mm or more is preferably 200 / cm 2 or less. More preferably, it is 100 pieces / cm < 2 > or less, More preferably, it is 50 pieces / m < 2 > or less, More preferably, it is 0-10 pieces / cm < 2 > or less. Further, it is preferable that the number of bright spots of 0.01 mm or less is small.

ドープの濾過は、通常の方法で行うことができるが、溶剤の常圧での沸点以上で、かつ加圧下で溶剤が沸騰しない範囲の温度で加熱しながら濾過する方法が、濾過前後の濾圧の差(差圧という)の上昇が小さく、好ましい。好ましい温度は45〜120℃であり、45〜70℃がより好ましく、45〜55℃であることがさらに好ましい。   The dope can be filtered by a normal method, but the method of filtering while heating at a temperature not lower than the boiling point at normal pressure of the solvent and at which the solvent does not boil under pressure is the filtration pressure before and after filtration. The increase in the difference (referred to as differential pressure) is small and preferable. A preferred temperature is 45 to 120 ° C, more preferably 45 to 70 ° C, and even more preferably 45 to 55 ° C.

濾圧は小さい方が好ましい。濾圧は1.6MPa以下であることが好ましく、1.2MPa以下であることがより好ましく、1.0MPa以下であることがさらに好ましい。   A smaller filtration pressure is preferred. The filtration pressure is preferably 1.6 MPa or less, more preferably 1.2 MPa or less, and further preferably 1.0 MPa or less.

つぎに、ドープの流延について説明する。   Next, dope casting will be described.

流延(キャスト)工程における金属支持体は、表面を鏡面仕上げしたものが好ましく、金属支持体としては、ステンレススティールベルトもしくは鋳物で表面をメッキ仕上げしたドラムが好ましく用いられる。   The metal support in the casting (casting) step preferably has a mirror-finished surface. As the metal support, a stainless steel belt or a drum whose surface is plated with a casting is preferably used.

キャストの幅は1〜4mとすることができる。流延工程の金属支持体の表面温度は−50℃〜溶剤が沸騰して発泡しない温度以下に設定される。温度が高い方がウェブの乾燥速度が速くできるので好ましいが、余り高すぎるとウェブが発泡したり、平面性が劣化する場合がある。好ましい支持体温度としては0〜100℃で適宜決定され、5〜30℃がさらに好ましい。または、冷却することによって、ウェブをゲル化させて残留溶媒を多く含んだ状態でドラムから剥離することも好ましい方法である。   The cast width can be 1 to 4 m. The surface temperature of the metal support in the casting step is set to −50 ° C. to a temperature at which the solvent boils and does not foam. A higher temperature is preferred because the web can be dried faster, but if it is too high, the web may foam or the flatness may deteriorate. A preferable support temperature is appropriately determined at 0 to 100 ° C, and more preferably 5 to 30 ° C. Alternatively, it is also a preferable method that the web is gelled by cooling and peeled from the drum in a state containing a large amount of residual solvent.

金属支持体の温度を制御する方法は特に制限されないが、温風または冷風を吹きかける方法や、温水を金属支持体の裏側に接触させる方法がある。温水を用いる方が熱の伝達が効率的に行われるため、金属支持体の温度が一定になるまでの時間が短く好ましい。温風を用いる場合は溶媒の蒸発潜熱によるウェブの温度低下を考慮して、溶媒の沸点以上の温風を使用しつつ、発泡も防ぎながら、目的の温度よりも高い温度の風を使う場合がある。特に、流延から剥離するまでの間で支持体の温度及び乾燥風の温度を変更し、効率的に乾燥を行うことが好ましい。   The method for controlling the temperature of the metal support is not particularly limited, and there are a method of blowing hot air or cold air, and a method of contacting hot water with the back side of the metal support. It is preferable to use warm water because heat transfer is performed efficiently, so that the time until the temperature of the metal support becomes constant is short. When using warm air, considering the temperature drop of the web due to the latent heat of vaporization of the solvent, while using warm air above the boiling point of the solvent and preventing foaming, there are cases where wind at a temperature higher than the target temperature is used. is there. In particular, it is preferable to perform drying efficiently by changing the temperature of the support and the temperature of the drying air during the period from casting to peeling.

セルロースエステルフィルムが良好な平面性を示すためには、金属支持体からウェブを剥離する際の残留溶媒量は10〜150質量%が好ましく、さらに好ましくは20〜40質量%または60〜130質量%であり、特に好ましくは、20〜30質量%または70〜120質量%である。   In order for the cellulose ester film to exhibit good flatness, the residual solvent amount when peeling the web from the metal support is preferably 10 to 150% by mass, more preferably 20 to 40% by mass or 60 to 130% by mass. Especially preferably, it is 20-30 mass% or 70-120 mass%.

本発明においては、残留溶媒量は、下記式で定義される。   In the present invention, the residual solvent amount is defined by the following formula.

残留溶媒量(質量%)={(M−N)/N}×100
ここで、Mは、ウェブまたはフィルムを製造中または製造後の任意の時点で採取した試料の質量で、Nは、Mを115℃で1時間の加熱後の質量である。
Residual solvent amount (% by mass) = {(MN) / N} × 100
Here, M is the mass of a sample taken at any time during or after the production of the web or film, and N is the mass after heating M at 115 ° C. for 1 hour.

また、セルロースエステルフィルムの乾燥工程においては、ウェブを金属支持体より剥離し、さらに乾燥し、残留溶媒量を1質量%以下にすることが好ましく、さらに好ましくは0.1質量%以下であり、特に好ましくは0〜0.01質量%以下である。   Further, in the drying step of the cellulose ester film, the web is peeled off from the metal support, and further dried, and the residual solvent amount is preferably 1% by mass or less, more preferably 0.1% by mass or less, Especially preferably, it is 0-0.01 mass% or less.

フィルム乾燥工程では一般にロール乾燥方式(上下に配置した多数のロールをウェブを交互に通し乾燥させる方式)やテンター方式でウェブを搬送させながら乾燥する方式が採られる。   In the film drying process, generally, a roll drying method (a method in which a plurality of rolls arranged on the upper and lower sides are alternately passed through and dried) or a method of drying while transporting the web by a tenter method is adopted.

本発明の反射防止フィルム用のセルロースエステルフィルムを作製するためには、金属支持体より剥離した直後のウェブの残留溶剤量の多いところで搬送方向に延伸し、さらにウェブの両端をクリップ等で把持するテンター方式で幅方向に延伸を行うことが特に好ましい。縦方向、横方向ともに好ましい延伸倍率は1.01〜1.3倍であり、1.05〜1.15倍がさらに好ましい。縦方向及び横方向延伸により面積が1.12〜1.44倍となっていることが好ましく、1.15〜1.32倍となっていることが好ましい。これは縦方向の延伸倍率×横方向の延伸倍率で求めることができる。縦方向と横方向の延伸倍率のいずれかが1.01倍未満ではハードコート層を形成する際の紫外線照射による平面性の劣化が生じやすくなる。   In order to produce the cellulose ester film for the antireflection film of the present invention, the web is stretched in the conveying direction where the residual solvent amount of the web immediately after peeling from the metal support is large, and both ends of the web are gripped with clips or the like. It is particularly preferable to perform stretching in the width direction by a tenter method. A preferable draw ratio in both the machine direction and the transverse direction is 1.01 to 1.3 times, and more preferably 1.05 to 1.15 times. It is preferable that the area is 1.12 to 1.44 times, and preferably 1.15 to 1.32 times due to longitudinal and lateral stretching. This can be determined by the draw ratio in the longitudinal direction × the draw ratio in the transverse direction. If one of the stretching ratios in the machine direction and the transverse direction is less than 1.01, the flatness is likely to deteriorate due to ultraviolet irradiation when the hard coat layer is formed.

剥離直後に縦方向に延伸するために、剥離張力及びその後の搬送張力によって延伸することが好ましい。例えば剥離張力を210N/m以上で剥離することが好ましく、特に好ましくは220〜300N/mである。   In order to stretch in the machine direction immediately after peeling, it is preferable to stretch by peeling tension and subsequent transport tension. For example, it is preferable to peel at a peeling tension of 210 N / m or more, and particularly preferably 220 to 300 N / m.

ウェブを乾燥させる手段は特に制限なく、一般的に熱風、赤外線、加熱ロール、マイクロ波等で行うことができるが、簡便さの点で熱風で行うことが好ましい。   The means for drying the web is not particularly limited, and can be generally performed with hot air, infrared rays, a heating roll, microwave, or the like, but it is preferably performed with hot air in terms of simplicity.

ウェブの乾燥工程における乾燥温度は30〜200℃で段階的に高くしていくことが好ましく、50〜180℃の範囲で段階的に高くすることが寸法安定性をよくするためさらに好ましい。   The drying temperature in the web drying step is preferably increased stepwise from 30 to 200 ° C, and more preferably stepwise increased from 50 to 180 ° C in order to improve dimensional stability.

セルロースエステルフィルムの膜厚は、特に限定はされないが10〜200μmが好ましく用いられる。特に10〜70μmの薄膜フィルムでは平面性と耐擦傷性に優れた反射防止フィルムを得ることが困難であったが、本発明によれば、平面性と耐擦傷性に優れた薄膜の反射防止フィルムが得られ、また生産性にも優れているため、セルロースエステルフィルムの膜厚は10〜70μmであることが特に好ましい。さらに好ましくは20〜60μmである。最も好ましくは35〜60μmである。また、共流延法によって多層構成としたセルロースエステルフィルムも好ましく用いることができる。セルロースエステルが多層構成の場合でも紫外線吸収剤と可塑剤を含有する層を有しており、それがコア層、スキン層、もしくはその両方であってもよい。   Although the film thickness of a cellulose-ester film is not specifically limited, 10-200 micrometers is used preferably. In particular, it was difficult to obtain an antireflection film excellent in flatness and scratch resistance with a thin film of 10 to 70 μm. According to the present invention, a thin antireflection film excellent in flatness and scratch resistance was obtained. And the film thickness of the cellulose ester film is particularly preferably 10 to 70 μm. More preferably, it is 20-60 micrometers. Most preferably, it is 35-60 micrometers. Moreover, the cellulose ester film made into the multilayer structure by the co-casting method can also be used preferably. Even when the cellulose ester has a multilayer structure, it has a layer containing an ultraviolet absorber and a plasticizer, and it may be a core layer, a skin layer, or both.

本発明の反射防止フィルムは、幅1m以上であり、幅1.4〜4mのものが好ましく用いられる。特に好ましくは1.4〜3mである。4mを超えると搬送が困難となる。また、セルロースエステルフィルムのハードコート層を設ける面の中心線平均粗さ(Ra)は0.001〜1μmのものを用いることができる。
(溶融流延製膜法)
セルロースエステルフィルムは、溶融流延製膜法によって形成することも、好ましい。
The antireflection film of the present invention has a width of 1 m or more and preferably has a width of 1.4 to 4 m. Especially preferably, it is 1.4-3 m. If it exceeds 4 m, conveyance becomes difficult. Moreover, the centerline average roughness (Ra) of the surface which provides the hard-coat layer of a cellulose-ester film can use a 0.001-1 micrometer thing.
(Melt casting method)
The cellulose ester film is also preferably formed by a melt casting film forming method.

溶液流延製膜法において用いられる溶媒(例えば塩化メチレン等)を用いずに、加熱溶融する溶融流延による成形法は、さらに詳細には、溶融押出成形法、プレス成形法、インフレーション法、射出成形法、ブロー成形法、延伸成形法等に分類できる。これらの中で、機械的強度及び表面精度等に優れるセルロースエステルフィルムを得るためには、溶融押し出し法が優れている。   The molding method by melt casting that is heated and melted without using the solvent (for example, methylene chloride, etc.) used in the solution casting film forming method, more specifically, melt extrusion molding method, press molding method, inflation method, injection It can be classified into molding method, blow molding method, stretch molding method and the like. Among these, in order to obtain a cellulose ester film excellent in mechanical strength, surface accuracy and the like, the melt extrusion method is excellent.

セルロースエステル及び添加剤の混合物を熱風乾燥または真空乾燥した後、溶融押出し、T型ダイよりフィルム状に押出して、静電印加法等により冷却ドラムに密着させ、冷却固化させ、未延伸フィルムを得る。冷却ドラムの温度は90〜150℃に維持されていることが好ましい。   A mixture of cellulose ester and additives is dried with hot air or vacuum, then melt extruded, extruded into a film from a T-die, and brought into close contact with a cooling drum by an electrostatic application method, etc., and cooled and solidified to obtain an unstretched film . The temperature of the cooling drum is preferably maintained at 90 to 150 ° C.

セルロースエステルと、その他、必要により添加される安定化剤等の添加剤は、溶融する前に混合しておくことが好ましく、セルロースエステルと添加剤を加熱前に混合することが、さらに好ましい。混合は、混合機等により行ってもよく、また、セルロースエステル調製過程において混合してもよい。混合機を使用する場合は、V型混合機、円錐スクリュー型混合機、水平円筒型混合機等、ヘンシェルミキサー、リボンミキサー一般的な混合機を用いることができる。   The cellulose ester and other additives such as a stabilizer added as necessary are preferably mixed before melting, and more preferably mixed before heating. Mixing may be performed by a mixer or the like, or may be performed in the cellulose ester preparation process. When a mixer is used, a general mixer such as a V-type mixer, a conical screw type mixer, a horizontal cylindrical type mixer, a Henschel mixer, or a ribbon mixer can be used.

上記のようにフィルム構成材料を混合した後に、その混合物を押出し機を用いて直接溶融して製膜するようにしてもよいが、一旦、フィルム構成材料をペレット化した後、該ペレットを押出し機で溶融して製膜するようにしてもよい。また、フィルム構成材料が、融点の異なる複数の材料を含む場合には、融点の低い材料のみが溶融する温度で一旦、いわゆるおこし状の半溶融物を作製し、半溶融物を押出し機に投入して製膜することも可能である。フィルム構成材料に熱分解しやすい材料が含まれる場合には、溶融回数を減らす目的で、ペレットを作製せずに直接製膜する方法や、上記のようなおこし状の半溶融物を作ってから製膜する方法が好ましい。   After the film constituent materials are mixed as described above, the mixture may be directly melted and formed into a film using an extruder, but once the film constituent materials are pelletized, the pellets are extruded. The film may be melted to form a film. In addition, when the film constituent material includes a plurality of materials having different melting points, a so-called braided semi-melt is once produced at a temperature at which only a material having a low melting point is melted, and the semi-melt is put into an extruder. It is also possible to form a film. If the film component contains a material that is easily pyrolyzed, in order to reduce the number of times of melting, a method of directly forming a film without producing pellets, or after making a paste-like semi-molten material as described above A method of forming a film is preferred.

押出し機は、市場で入手可能な種々の押出し機を使用可能であるが、溶融混練押出し機が好ましく、単軸押出し機でも2軸押出し機でもよい。フィルム構成材料からペレットを作製せずに、直接製膜を行う場合、適当な混練度が必要であるため2軸押出し機を用いることが好ましいが、単軸押出し機でも、スクリューの形状をマドック型、ユニメルト、ダルメージ等の混練型のスクリューに変更することにより、適度の混練が得られるので、使用可能である。フィルム構成材料として、一旦、ペレットやおこし状の半溶融物を使用する場合は、単軸押出し機でも2軸押出し機でも使用可能である。   As the extruder, various commercially available extruders can be used, but a melt-kneading extruder is preferable, and a single-screw extruder or a twin-screw extruder may be used. When forming a film directly without producing pellets from film constituent materials, it is preferable to use a twin-screw extruder because an appropriate degree of kneading is necessary, but even with a single-screw extruder, the screw shape is a Maddock type. By changing to a kneading type screw such as unimelt or dull mage, moderate kneading can be obtained, so that it can be used. When a pellet or braided semi-melt is once used as a film constituent material, it can be used in either a single screw extruder or a twin screw extruder.

押出し機内及び押出した後の冷却工程は、窒素ガス等の不活性ガスで置換するか、あるいは減圧することにより、酸素の濃度を下げることが好ましい。   In the extruder and in the cooling step after extrusion, it is preferable to reduce the oxygen concentration by replacing with an inert gas such as nitrogen gas or reducing the pressure.

押出し機内のフィルム構成材料の溶融温度は、フィルム構成材料の粘度や吐出量、製造するシートの厚み等によって好ましい条件が異なるが、一般的には、フィルムのガラス転移温度(Tg)に対して、Tg以上、Tg+100℃以下、好ましくはTg+10℃以上、Tg+90℃以下である。具体的には、溶融押出し時の温度は、150〜300℃であることが好ましく、特に180〜270℃の範囲であることが好ましい。さらに200〜250℃の範囲であることが好ましい。   The melting temperature of the film constituent material in the extruder varies depending on the viscosity and discharge amount of the film constituent material, the thickness of the sheet to be manufactured, etc., but generally, with respect to the glass transition temperature (Tg) of the film, Tg or more and Tg + 100 ° C. or less, preferably Tg + 10 ° C. or more and Tg + 90 ° C. or less. Specifically, the temperature during melt extrusion is preferably 150 to 300 ° C, and particularly preferably 180 to 270 ° C. Furthermore, it is preferable that it is the range of 200-250 degreeC.

押出し時の溶融粘度は、10〜100000ポイズ、好ましくは100〜10000ポイズである。   The melt viscosity at the time of extrusion is 10 to 100,000 poise, preferably 100 to 10,000 poise.

また、押出し機内でのフィルム構成材料の滞留時間は、短い方が好ましく、5分以内、好ましくは3分以内、より好ましくは2分以内である。滞留時間は、押出し機1の種類、押出す条件にも左右されるが、材料の供給量やL/D、スクリュー回転数、スクリューの溝の深さ等を調整することにより短縮することが可能である。   Further, the residence time of the film constituting material in the extruder is preferably shorter, and is within 5 minutes, preferably within 3 minutes, more preferably within 2 minutes. Although the residence time depends on the type of the extruder 1 and the extrusion conditions, it can be shortened by adjusting the material supply amount, L / D, screw rotation speed, screw groove depth, etc. It is.

上記押出し機でフィルム状に押出して、静電印加法等により冷却ドラムに密着させ、冷却固化させ、未延伸フィルムを得る。冷却ドラムの温度は90〜150℃に維持されていることが好ましい。   Extruded into a film by the above extruder, brought into close contact with a cooling drum by an electrostatic application method or the like, cooled and solidified to obtain an unstretched film. The temperature of the cooling drum is preferably maintained at 90 to 150 ° C.

本発明に用いられるセルロースエステルフィルムは、幅手方向もしくは製膜方向に延伸製膜されたフィルムであることが特に好ましい。   The cellulose ester film used in the present invention is particularly preferably a film stretched in the width direction or the film forming direction.

前述の冷却ドラムから剥離され、得られた未延伸フィルムを複数のロール群及び/または赤外線ヒーター等の加熱装置を介して、セルロースエステルのガラス転移温度(Tg)から、Tg+100℃の範囲内に加熱し、一段または多段縦延伸することが好ましい。   The unstretched film peeled off from the cooling drum is heated within a range of Tg + 100 ° C. from the glass transition temperature (Tg) of the cellulose ester via a plurality of roll groups and / or a heating device such as an infrared heater. In addition, it is preferable to perform single-stage or multistage longitudinal stretching.

つぎに、上記のようにして得られた縦方向に延伸されたセルロースエステルフィルムを横延伸し、ついで熱処理することが好ましい。   Next, the cellulose ester film stretched in the longitudinal direction obtained as described above is preferably stretched in the transverse direction and then heat-treated.

熱処理は、ガラス転移温度(Tg)−20℃〜延伸温度の範囲内で、通常0.5〜300秒間搬送しながら行うことが好ましい。   It is preferable to perform heat processing within the range of glass transition temperature (Tg) -20 degreeC-extending | stretching temperature, normally conveying for 0.5 to 300 second.

熱処理されたフィルムは、通常、ガラス転移温度(Tg)以下まで冷却され、フィルム両端のクリップ把持部分をカットし巻き取られる。また冷却は、最終熱処理温度からガラス転移温度(Tg)までを、毎秒100℃以下の冷却速度で徐冷することが好ましい。   The heat-treated film is usually cooled to a glass transition temperature (Tg) or lower, and clip holding portions at both ends of the film are cut and wound. Further, the cooling is preferably performed by gradually cooling from the final heat treatment temperature to the glass transition temperature (Tg) at a cooling rate of 100 ° C. or less per second.

冷却する手段は特に限定はなく、従来公知の手段で行えるが、特に複数の温度領域で順次冷却しながら、これらの処理を行うことがフィルムの寸法安定性向上の点で好ましい。なお、冷却速度は、最終熱処理温度をT1、フィルムが最終熱処理温度からTgに達するまでの時間をtとしたとき、(T1−Tg)/tで求めた値である。   The means for cooling is not particularly limited, and can be performed by a conventionally known means. In particular, it is preferable to perform these treatments while sequentially cooling in a plurality of temperature ranges from the viewpoint of improving the dimensional stability of the film. The cooling rate is a value obtained by (T1−Tg) / t, where T1 is the final heat treatment temperature and t is the time until the film reaches Tg from the final heat treatment temperature.

セルロースエステルフィルムには、紫外線吸収剤が好ましく用いられる。   An ultraviolet absorber is preferably used for the cellulose ester film.

紫外線吸収剤としては、波長370nm以下の紫外線の吸収能に優れ、かつ良好な液晶表示性の観点から、波長400nm以上の可視光の吸収が少ないものが好ましく用いられる。   As the ultraviolet absorber, those excellent in the ability to absorb ultraviolet rays having a wavelength of 370 nm or less and having little absorption of visible light having a wavelength of 400 nm or more are preferably used from the viewpoint of good liquid crystal display properties.

紫外線吸収剤の具体例としては、例えば、オキシベンゾフェノン系化合物、ベンゾトリアゾール系化合物、サリチル酸エステル系化合物、ベンゾフェノン系化合物、シアノアクリレート系化合物、トリアジン系化合物、ニッケル錯塩系化合物等が挙げられるが、これらに限定されない。   Specific examples of the ultraviolet absorber include, for example, oxybenzophenone compounds, benzotriazole compounds, salicylic acid ester compounds, benzophenone compounds, cyanoacrylate compounds, triazine compounds, nickel complex compounds, and the like. It is not limited to.

ベンゾトリアゾール系紫外線吸収剤としては、例えば下記の紫外線吸収剤を具体例として挙げるが、本発明はこれらに限定されない。   Specific examples of the benzotriazole-based ultraviolet absorbers include the following ultraviolet absorbers, but the present invention is not limited thereto.

UV−1:2−(2′−ヒドロキシ−5′−メチルフェニル)ベンゾトリアゾール
UV−2:2−(2′−ヒドロキシ−3′,5′−ジ−tert−ブチルフェニル)ベンゾトリアゾール
UV−3:2−(2′−ヒドロキシ−3′−tert−ブチル−5′−メチルフェニル)ベンゾトリアゾール
UV−4:2−(2′−ヒドロキシ−3′,5′−ジ−tert−ブチルフェニル)−5−クロロベンゾトリアゾール
UV−5:2−(2′−ヒドロキシ−3′−(3″,4″,5″,6″−テトラヒドロフタルイミドメチル)−5′−メチルフェニル)ベンゾトリアゾール
UV−6:2,2−メチレンビス(4−(1,1,3,3−テトラメチルブチル)−6−(2H−ベンゾトリアゾール−2−イル)フェノール)
UV−7:2−(2′−ヒドロキシ−3′−tert−ブチル−5′−メチルフェニル)−5−クロロベンゾトリアゾール
UV−8:2−(2H−ベンゾトリアゾール−2−イル)−6−(直鎖及び側鎖ドデシル)−4−メチルフェノール(TINUVIN171、Ciba製)
UV−9:オクチル−3−〔3−tert−ブチル−4−ヒドロキシ−5−(クロロ−2H−ベンゾトリアゾール−2−イル)フェニル〕プロピオネートと2−エチルヘキシル−3−〔3−tert−ブチル−4−ヒドロキシ−5−(5−クロロ−2H−ベンゾトリアゾール−2−イル)フェニル〕プロピオネートの混合物(TINUVIN109、Ciba製)
また、ベンゾフェノン系紫外線吸収剤としては下記の具体例を示すが、本発明はこれらに限定されない。
UV-1: 2- (2'-hydroxy-5'-methylphenyl) benzotriazole UV-2: 2- (2'-hydroxy-3 ', 5'-di-tert-butylphenyl) benzotriazole UV-3 : 2- (2'-hydroxy-3'-tert-butyl-5'-methylphenyl) benzotriazole UV-4: 2- (2'-hydroxy-3 ', 5'-di-tert-butylphenyl)- 5-Chlorobenzotriazole UV-5: 2- (2'-hydroxy-3 '-(3 ", 4", 5 ", 6" -tetrahydrophthalimidomethyl) -5'-methylphenyl) benzotriazole UV-6: 2,2-methylenebis (4- (1,1,3,3-tetramethylbutyl) -6- (2H-benzotriazol-2-yl) phenol)
UV-7: 2- (2'-hydroxy-3'-tert-butyl-5'-methylphenyl) -5-chlorobenzotriazole UV-8: 2- (2H-benzotriazol-2-yl) -6 (Linear and side chain dodecyl) -4-methylphenol (TINUVIN171, manufactured by Ciba)
UV-9: Octyl-3- [3-tert-butyl-4-hydroxy-5- (chloro-2H-benzotriazol-2-yl) phenyl] propionate and 2-ethylhexyl-3- [3-tert-butyl- 4-Hydroxy-5- (5-chloro-2H-benzotriazol-2-yl) phenyl] propionate (TINUVIN109, manufactured by Ciba)
Moreover, although the following specific example is shown as a benzophenone series ultraviolet absorber, this invention is not limited to these.

UV−10:2,4−ジヒドロキシベンゾフェノン
UV−11:2,2′−ジヒドロキシ−4−メトキシベンゾフェノン
UV−12:2−ヒドロキシ−4−メトキシ−5−スルホベンゾフェノン
UV−13:ビス(2−メトキシ−4−ヒドロキシ−5−ベンゾイルフェニルメタン)
好ましく用いられる紫外線吸収剤としては、透明性が高く、偏光板や液晶の劣化を防ぐ効果に優れたベンゾトリアゾール系紫外線吸収剤やベンゾフェノン系紫外線吸収剤が好ましく、不要な着色がより少ないベンゾトリアゾール系紫外線吸収剤が特に好ましく用いられる。また、市販品として、チヌビン(TINUVIN)326、チヌビン(TINUVIN)109、チヌビン(TINUVIN)171、チヌビン(TINUVIN)900、チヌビン(TINUVIN)928、チヌビン(TINUVIN)360(いずれもチバスペシャルティケミカルズ社製)、LA31(旭電化社製)、Sumisorb250(住友化学社製)、RUVA−100(大塚化学製)が挙げられる。
UV-10: 2,4-dihydroxybenzophenone UV-11: 2,2'-dihydroxy-4-methoxybenzophenone UV-12: 2-hydroxy-4-methoxy-5-sulfobenzophenone UV-13: Bis (2-methoxy -4-hydroxy-5-benzoylphenylmethane)
As the UV absorber preferably used, a benzotriazole UV absorber and a benzophenone UV absorber that are highly transparent and excellent in preventing the deterioration of the polarizing plate and the liquid crystal are preferable, and the benzotriazole system that has less unnecessary coloring. A UV absorber is particularly preferably used. As commercial products, TINUVIN 326, TINUVIN 109, TINUVIN 171, TINUVIN 900, TINUVIN 928, TINUVIN 928, TINUVIN 360 (all manufactured by Ciba Specialty Chemicals) LA31 (manufactured by Asahi Denka), Sumisorb 250 (manufactured by Sumitomo Chemical), and RUVA-100 (manufactured by Otsuka Chemical).

また、特開2001−187825号公報に記載されている分配係数が9.2以上の紫外線吸収剤は、長尺フィルムの面品質を向上させ、塗布性にも優れている。特に分配係数が10.1以上の紫外線吸収剤を用いることが好ましい。   Moreover, the ultraviolet absorber whose distribution coefficient described in Unexamined-Japanese-Patent No. 2001-187825 is 9.2 or more improves the surface quality of a long film, and is excellent also in applicability | paintability. In particular, it is preferable to use an ultraviolet absorber having a distribution coefficient of 10.1 or more.

また、セルロースエステルフィルムには滑り性を付与するため、前述の活性線硬化型樹脂を含む塗布層で記載するものと同様の微粒子を用いることができる。   Moreover, in order to provide slipperiness to a cellulose-ester film, the microparticles | fine-particles similar to what is described with the application layer containing the above-mentioned actinic radiation curable resin can be used.

微粒子としては、無機化合物の例としては、二酸化珪素、二酸化チタン、酸化アルミニウム、酸化ジルコニウム、炭酸カルシウム、炭酸カルシウム、タルク、クレイ、焼成カオリン、焼成ケイ酸カルシウム、水和ケイ酸カルシウム、ケイ酸アルミニウム、ケイ酸マグネシウム及びリン酸カルシウムを挙げることができる。微粒子は珪素を含むものが濁度が低くなる点で好ましく、特に二酸化珪素が好ましい。   As fine particles, examples of inorganic compounds include silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, calcium carbonate, calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, hydrated calcium silicate, aluminum silicate And magnesium silicate and calcium phosphate. Fine particles containing silicon are preferable in terms of low turbidity, and silicon dioxide is particularly preferable.

微粒子の一次粒子の平均粒子径は5〜50nmが好ましく、さらに好ましいのは7〜20nmである。これらは、主に粒子径0.05〜0.3μmの2次凝集体として含有されることが好ましい。含有量は0.05〜1質量%であることが好ましく、特に0.1〜0.5質量%が好ましい。   The average primary particle diameter of the fine particles is preferably 5 to 50 nm, and more preferably 7 to 20 nm. These are preferably contained mainly as secondary aggregates having a particle size of 0.05 to 0.3 μm. The content is preferably 0.05 to 1% by mass, particularly preferably 0.1 to 0.5% by mass.

二酸化珪素の微粒子は、例えば、アエロジルR972、R972V、R974、R812、200、200V、300、R202、OX50、TT600(以上日本アエロジル株式会社製)の商品名で市販されており、これらの微粒子を使用することができる。   Silicon dioxide fine particles are commercially available under the trade names of, for example, Aerosil R972, R972V, R974, R812, 200, 200V, 300, R202, OX50, TT600 (manufactured by Nippon Aerosil Co., Ltd.), and these fine particles are used. can do.

酸化ジルコニウムの微粒子は、例えば、アエロジルR976及びR811(以上、日本アエロジル株式会社製)の商品名で市販されており、使用することができる。   Zirconium oxide fine particles are commercially available, for example, under the trade names Aerosil R976 and R811 (manufactured by Nippon Aerosil Co., Ltd.), and can be used.

微粒子としてポリマー粒子を用いることもでき、ポリマーの例として、シリコーン樹脂、フッ素樹脂及びアクリル樹脂を挙げることができる。シリコーン樹脂が好ましく、特に三次元の網状構造を有するものが好ましく、例えば、トスパール103、同105、同108、同120、同145、同3120及び同240(以上東芝シリコーン株式会社製)の商品名で市販されており、使用することができる。   Polymer particles can also be used as the fine particles, and examples of the polymer include silicone resins, fluororesins, and acrylic resins. Silicone resins are preferable, and those having a three-dimensional network structure are particularly preferable. For example, Tospearl 103, 105, 108, 120, 145, 3120, and 240 (manufactured by Toshiba Silicone Co., Ltd.) Are commercially available and can be used.

これらの中でもアエロジル200V、アエロジルR972Vが濁度を低く保ちながら、摩擦係数を下げる効果が大きいため、特に好ましく用いられる。   Among these, Aerosil 200V and Aerosil R972V are particularly preferably used because they have a large effect of reducing the friction coefficient while keeping turbidity low.

また、セルロースエステルフィルムには、以下に説明する劣化防止剤を含有することが好ましい。つぎに劣化防止剤について説明する。
(劣化防止剤)
劣化防止剤とは、高分子が熱や酸素、水分、酸などによって分解されることを化学的な作用によって抑制する材料のことである。本発明に用いられる透明基材フィルムは、溶融流延法の場合、特に200℃以上の高温下で成形されるため、高分子の分解・劣化が起きやすい系であり、劣化防止剤をフィルム形成材料中に含有させることが好ましい。
Moreover, it is preferable to contain the deterioration inhibitor demonstrated below in a cellulose-ester film. Next, the deterioration preventing agent will be described.
(Deterioration inhibitor)
A deterioration inhibitor is a material that suppresses decomposition of a polymer by heat, oxygen, moisture, acid, or the like by a chemical action. In the case of the melt casting method, the transparent substrate film used in the present invention is formed at a high temperature of 200 ° C. or more. It is preferable to make it contain in material.

フィルム形成材料の酸化防止、分解して発生した酸の捕捉、光または熱によるラジカル種基因の分解反応を抑制または禁止する等、解明できていない分解反応を含めて、着色や分子量低下に代表される変質や材料の分解による揮発成分の生成を抑制するために劣化防止剤を用いる。   It is represented by coloring and molecular weight reduction, including decomposition reactions that have not been elucidated, such as preventing oxidation of film-forming materials, capturing acid generated by decomposition, and suppressing or prohibiting decomposition reactions caused by radical species due to light or heat. Degradation inhibitors are used to suppress the generation of volatile components due to deterioration and material decomposition.

劣化防止剤としては、例えば、酸化防止剤、ヒンダードアミン光安定剤、酸捕捉剤、金属不活性化剤などが挙げられるが、これらに限定されない。これらは、特開平3−199201号公報、特開平5−1907073号公報、特開平5−194789号公報、特開平5−271471号公報、特開平6−107854号公報などに記載がある。これらの中でも、本発明の目的のためには、フィルム形成材料中に劣化防止剤として酸化防止剤を含むことが好ましい。   Examples of the degradation inhibitor include, but are not limited to, an antioxidant, a hindered amine light stabilizer, an acid scavenger, and a metal deactivator. These are described in JP-A-3-199201, JP-A-5-1907073, JP-A-5-194789, JP-A-5-271471, JP-A-6-107854, and the like. Among these, for the purpose of the present invention, it is preferable to include an antioxidant as a deterioration preventing agent in the film forming material.

フィルム形成材料中の劣化防止剤は、少なくとも1種以上選択でき、フィルムの透明性から添加する量は、透明基材フィルムを形成する透明基材樹脂100質量%に対して、劣化防止剤の添加量は0.01質量%以上、10質量%以下が好ましく、より好ましくは0.1質量%以上、5.0質量%以下であり、さらに好ましくは0.2質量%以上、2.0質量%以下である。   At least one or more kinds of deterioration preventing agents in the film forming material can be selected, and the amount added from the transparency of the film is the addition of the deterioration preventing agent with respect to 100% by mass of the transparent substrate resin forming the transparent substrate film. The amount is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.1% by mass or more and 5.0% by mass or less, and further preferably 0.2% by mass or more and 2.0% by mass. It is as follows.

フィルム形成材料は、材料の変質や吸湿性を回避する目的で、構成する材料が1種または複数種のペレットに分割して保存することができる。ペレット化は、加熱時の溶融物の混合性または相溶性が向上でき、または得られたフィルムの光学的な均一性が確保できることもある。
(酸化防止剤)
また、セルロースエステルフィルムには以下に説明する酸化防止剤を含有することが好ましい。酸化防止剤としては、酸素によるフィルム形成材料の劣化を抑制する化合物であれば制限なく用いることができるが、中でもフェノール系酸化防止剤、リン系酸化防止剤、イオウ系酸化防止剤、アルキルラジカル捕捉剤、過酸化物分解剤、酸素スカベンジャー等が挙げられる。これらの中でもフェノール系酸化防止剤、リン系酸化防止剤、アルキルラジカル捕捉剤が好ましいが、フェノール系酸化防止剤とリン系酸化防止剤の2者の組み合わせを用いることがより好ましく、フェノール系酸化防止剤とリン系酸化防止剤とアルキルラジカル捕捉剤の3者の組み合わせを用いることが最も好ましい。これらの酸化防止剤を配合することにより、透明性、耐熱性等を低下させることなく、溶融成型時の熱や熱酸化劣化等による成形体の着色や強度低下を防止できる。これらの酸化防止剤は、それぞれ単独で、或いは2種以上を組み合わせて用いることができ、その配合量は、本発明の目的を損なわない範囲で適宜選択されるが、本発明に用いられるセルロースエステルの質量に対して、0.01質量%以上10質量%以下が好ましく、より好ましくは0.1質量%以上5.0質量%以下であり、さらに好ましくは0.2質量%以上2.0質量%以下である。
(フェノール系酸化防止剤)
フェノール系酸化防止剤は既知の化合物であり、パラ−t−ブチルフェノール、パラ−(1,1,3,3−テトラメチルブチル)フェノール等のアルキル基置換フェノールの他、例えば、米国特許第4,839,405号明細書の第12〜14欄に記載の、2,6−ジアルキルフェノール誘導体化合物、いわゆるヒンダードフェノール系化合物が挙げられるが、これらの中で、ヒンダードフェノール系化合物が好ましい。
The film-forming material can be stored by dividing the material constituting the material into one or more kinds of pellets for the purpose of avoiding material alteration and hygroscopicity. Pelletization may improve the mixing or compatibility of the melt during heating, or may ensure the optical uniformity of the resulting film.
(Antioxidant)
Moreover, it is preferable to contain the antioxidant demonstrated below in a cellulose-ester film. Any antioxidant can be used without limitation as long as it is a compound that suppresses the deterioration of the film-forming material due to oxygen. Among them, a phenol-based antioxidant, a phosphorus-based antioxidant, a sulfur-based antioxidant, an alkyl radical scavenger, and the like. Agents, peroxide decomposers, oxygen scavengers and the like. Among these, phenolic antioxidants, phosphorus antioxidants, and alkyl radical scavengers are preferable, but it is more preferable to use a combination of two of a phenolic antioxidant and a phosphorus antioxidant, and phenolic antioxidants. It is most preferable to use a combination of three of an agent, a phosphorus-based antioxidant, and an alkyl radical scavenger. By blending these antioxidants, it is possible to prevent coloration or strength reduction of the molded product due to heat during heat molding or deterioration due to thermal oxidation without lowering transparency, heat resistance and the like. These antioxidants can be used alone or in combination of two or more, and the blending amount thereof is appropriately selected within a range not impairing the object of the present invention, but the cellulose ester used in the present invention. Is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.1% by mass or more and 5.0% by mass or less, and still more preferably 0.2% by mass or more and 2.0% by mass. % Or less.
(Phenolic antioxidant)
Phenol-based antioxidants are known compounds. In addition to alkyl group-substituted phenols such as para-t-butylphenol and para- (1,1,3,3-tetramethylbutyl) phenol, for example, US Pat. Examples include 2,6-dialkylphenol derivative compounds, so-called hindered phenol compounds, described in columns 12 to 14 of the specification of 839,405. Among these, hindered phenol compounds are preferable.

ヒンダードフェノールフェノール系化合物の具体例としては、n−オクタデシル3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)−プロピオネート、n−オクタデシル3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)−アセテート、n−オクタデシル3,5−ジ−t−ブチル−4−ヒドロキシベンゾエート、n−ヘキシル3,5−ジ−t−ブチル−4−ヒドロキシフェニルベンゾエート、n−ドデシル3,5−ジ−t−ブチル−4−ヒドロキシフェニルベンゾエート、ネオ−ドデシル3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート、ドデシルβ(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート、エチルα−(4−ヒドロキシ−3,5−ジ−t−ブチルフェニル)イソブチレート、オクタデシルα−(4−ヒドロキシ−3,5−ジ−t−ブチルフェニル)イソブチレート、オクタデシルα−(4−ヒドロキシ−3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート、2−(n−オクチルチオ)エチル3,5−ジ−t−ブチル−4−ヒドロキシ−ベンゾエート、2−(n−オクチルチオ)エチル3,5−ジ−t−ブチル−4−ヒドロキシ−フェニルアセテート、2−(n−オクタデシルチオ)エチル3,5−ジ−t−ブチル−4−ヒドロキシフェニルアセテート、2−(n−オクタデシルチオ)エチル3,5−ジ−t−ブチル−4−ヒドロキシ−ベンゾエート、2−(2−ヒドロキシエチルチオ)エチル3,5−ジ−t−ブチル−4−ヒドロキシベンゾエート、ジエチルグリコールビス−(3,5−ジ−t−ブチル−4−ヒドロキシ−フェニル)プロピオネート、2−(n−オクタデシルチオ)エチル3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート、ステアルアミドN,N−ビス−[エチレン3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、n−ブチルイミノN,N−ビス−[エチレン3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、2−(2−ステアロイルオキシエチルチオ)エチル3,5−ジ−t−ブチル−4−ヒドロキシベンゾエート、2−(2−ステアロイルオキシエチルチオ)エチル7−(3−メチル−5−t−ブチル−4−ヒドロキシフェニル)ヘプタノエート、1,2−プロピレングリコールビス−[3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、エチレングリコールビス−[3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、ネオペンチルグリコールビス−[3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、エチレングリコールビス−(3,5−ジ−t−ブチル−4−ヒドロキシフェニルアセテート)、グリセリン−l−n−オクタデカノエート−2,3−ビス−(3,5−ジ−t−ブチル−4−ヒドロキシフェニルアセテート)、ペンタエリスリトール−テトラキス−[3−(3′,5′−ジ−t−ブチル−4′−ヒドロキシフェニル)プロピオネート]、1,1,1−トリメチロールエタン−トリス−[3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、ソルビトールヘキサ−[3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、2−ヒドロキシエチル7−(3−メチル−5−tブチル−4−ヒドロキシフェニル)プロピオネート、2−ステアロイルオキシエチル7−(3−メチル−5−t−ブチル−4−ヒドロキシフェニル)ヘプタノエート、1,6−n−ヘキサンジオール−ビス[(3′,5′−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオネート]、ペンタエリスリトール−テトラキス(3,5−ジ−t−ブチル−4−ヒドロキシヒドロシンナメート)が含まれる。上記タイプのフェノール化合物は、例えば、チバスペシャルティケミカルズから、「IRGANOX1076」及び「IRGANOX1010」という商品名で市販されている。
(リン系酸化防止剤)
リン系酸化防止剤として、ホスファイト系化合物、及びホスホナイト系化合物が挙げられる。ホスファイト系化合物の具体例としては、トリフェニルホスファイト、ジフェニルイソデシルホスファイト、フェニルジイソデシルホスファイト、トリス(ノニルフェニル)ホスファイト、トリス(ジノニルフェニル)ホスファイト、トリス(2,4−ジ−t−ブチルフェニル)ホスファイト、トリス(2,4−ジ−t−ブチル−5−メチルフェニル)ホスファイト、10−(3,5−ジ−t−ブチル−4−ヒドロキシベンジル)−9,10−ジヒドロ−9−オキサ−10−ホスファフェナントレン−10−オキサイド、6−[3−(3−t−ブチル−4−ヒドロキシ−5−メチルフェニル)プロポキシ]−2,4,8,10−テトラ−t−ブチルジベンズ[d,f][1.3.2]ジオキサホスフェピン、トリデシルホスファイト等のモノホスファイト系化合物;4,4′−ブチリデン−ビス(3−メチル−6−t−ブチルフェニル−ジ−トリデシルホスファイト)、4,4′−イソプロピリデン−ビス(フェニル−ジ−アルキル(C12〜C15)ホスファイト)等のジホスファイト系化合物;等が挙げられる。上記タイプのホスファイト系化合物は、例えば、住友化学株式会社から、「SumilizerGP」、旭電化工業株式会社から「ADK STAB PEP−24G」、「ADK STAB PEP−36」、「ADK STAB 3010」、「ADK STAB HP−10」及び「ADK STAB 2112」という商品名で市販されている。
Specific examples of the hindered phenol phenol compound include n-octadecyl 3- (3,5-di-t-butyl-4-hydroxyphenyl) -propionate, n-octadecyl 3- (3,5-di-t- Butyl-4-hydroxyphenyl) -acetate, n-octadecyl 3,5-di-t-butyl-4-hydroxybenzoate, n-hexyl 3,5-di-t-butyl-4-hydroxyphenylbenzoate, n-dodecyl 3,5-di-t-butyl-4-hydroxyphenylbenzoate, neo-dodecyl 3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate, dodecyl β (3,5-di-t- Butyl-4-hydroxyphenyl) propionate, ethyl α- (4-hydroxy-3,5-di-t-butylphenyl) isobuty Rate, octadecyl α- (4-hydroxy-3,5-di-t-butylphenyl) isobutyrate, octadecyl α- (4-hydroxy-3,5-di-t-butyl-4-hydroxyphenyl) propionate, 2- (N-octylthio) ethyl 3,5-di-t-butyl-4-hydroxy-benzoate, 2- (n-octylthio) ethyl 3,5-di-t-butyl-4-hydroxy-phenyl acetate, 2- ( n-octadecylthio) ethyl 3,5-di-t-butyl-4-hydroxyphenyl acetate, 2- (n-octadecylthio) ethyl 3,5-di-t-butyl-4-hydroxy-benzoate, 2- ( 2-hydroxyethylthio) ethyl 3,5-di-t-butyl-4-hydroxybenzoate, diethyl glycol bis- (3,5-di -T-butyl-4-hydroxy-phenyl) propionate, 2- (n-octadecylthio) ethyl 3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate, stearamide N, N-bis- [ Ethylene 3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate], n-butylimino N, N-bis- [ethylene 3- (3,5-di-t-butyl-4-hydroxyphenyl) ) Propionate], 2- (2-stearoyloxyethylthio) ethyl 3,5-di-t-butyl-4-hydroxybenzoate, 2- (2-stearoyloxyethylthio) ethyl 7- (3-methyl-5- t-butyl-4-hydroxyphenyl) heptanoate, 1,2-propylene glycol bis- [3- (3,5-di-t-butyl- -Hydroxyphenyl) propionate], ethylene glycol bis- [3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate], neopentylglycol bis- [3- (3,5-di-t- Butyl-4-hydroxyphenyl) propionate], ethylene glycol bis- (3,5-di-t-butyl-4-hydroxyphenyl acetate), glycerin-1-n-octadecanoate-2,3-bis- ( 3,5-di-t-butyl-4-hydroxyphenyl acetate), pentaerythritol-tetrakis- [3- (3 ', 5'-di-t-butyl-4'-hydroxyphenyl) propionate], 1,1 , 1-Trimethylolethane-tris- [3- (3,5-di-tert-butyl-4-hydroxyphenyl) propione ), Sorbitol hexa- [3- (3,5-di-t-butyl-4-hydroxyphenyl) propionate], 2-hydroxyethyl 7- (3-methyl-5-tbutyl-4-hydroxyphenyl) propionate 2-stearoyloxyethyl 7- (3-methyl-5-t-butyl-4-hydroxyphenyl) heptanoate, 1,6-n-hexanediol-bis [(3 ', 5'-di-t-butyl- 4-hydroxyphenyl) propionate], pentaerythritol-tetrakis (3,5-di-t-butyl-4-hydroxyhydrocinnamate). The above type of phenolic compounds are commercially available from Ciba Specialty Chemicals under the trade names “IRGANOX1076” and “IRGANOX1010”, for example.
(Phosphorus antioxidant)
Examples of phosphorus antioxidants include phosphite compounds and phosphonite compounds. Specific examples of the phosphite compound include triphenyl phosphite, diphenylisodecyl phosphite, phenyl diisodecyl phosphite, tris (nonylphenyl) phosphite, tris (dinonylphenyl) phosphite, tris (2,4-di -T-butylphenyl) phosphite, tris (2,4-di-t-butyl-5-methylphenyl) phosphite, 10- (3,5-di-t-butyl-4-hydroxybenzyl) -9, 10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 6- [3- (3-tert-butyl-4-hydroxy-5-methylphenyl) propoxy] -2,4,8,10- Mono such as tetra-t-butyldibenz [d, f] [1.3.2] dioxaphosphine, tridecyl phosphite Sphite compounds; 4,4'-butylidene-bis (3-methyl-6-tert-butylphenyl-di-tridecyl phosphite), 4,4'-isopropylidene-bis (phenyl-di-alkyl (C12- And diphosphite compounds such as C15) phosphite). The above type of phosphite compounds are, for example, Sumitomo Chemical Co., Ltd., “Sumilizer GP”, Asahi Denka Kogyo Co., Ltd. “ADK STAB PEP-24G”, “ADK STAB PEP-36”, “ADK STAB 3010”, “ It is marketed under the brand names of “ADK STAB HP-10” and “ADK STAB 2112”.

ホスホナイト系化合物の具体例としては、ジメチル−フェニルホスホナイト、ジ−t−ブチル−フェニルホスホナイト、ジフェニル−フェニルホスホナイト、ジ−(4−ペンチル−フェニル)−フェニルホスホナイト、ジ−(2−t−ブチル−フェニル)−フェニルホスホナイト、ジ−(2−メチル−3−ペンチル−フェニル)−フェニルホスホナイト、ジ−(2−メチル−4−オクチル−フェニル)−フェニルホスホナイト、ジ−(3−ブチル−4−メチル−フェニル)−フェニルホスホナイト、ジ−(3−ヘキシル−4−エチル−フェニル)−フェニルホスホナイト、ジ−(2,4,6−トリメチルフェニル)−フェニルホスホナイト、ジ−(2,3−ジメチル−4−エチル−フェニル)−フェニルホスホナイト、ジ−(2,6−ジエチル−3−ブチルフェニル)−フェニルホスホナイト、ジ−(2,3−ジプロピル−5−ブチルフェニル)−フェニルホスホナイト、ジ−(2,4,6−トリ−t−ブチルフェニル)−フェニルホスホナイト、ビス(2,4−ジ−t−ブチル−5−メチルフェニル)ビフェニル−4−イル−ホスホナイト、ビス(2,4−ジ−t−ブチル−5−メチルフェニル)−4′−(ビス(2,4−ジ−t−ブチル−5−メチルフェノキシ)ホスフィノ)ビフェニル−4−イル−ホスホナイト、テトラキス(2,4−ジ−t−ブチル−フェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−フェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(3,5−ジ−t−ブチル−フェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3,4−トリメチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジメチル−5−エチル−フェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジメチル−4−プロピルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジメチル−5−t−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジメチル−4−t−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジエチル−5−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジエチル−4−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4,5−トリエチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジエチル−4−プロピルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジエチル−6−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジエチル−5−t−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジエチル−6−t−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジプロピル−5−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジプロピル−4−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジプロピル−5−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジプロピル−6−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジプロピル−5−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジブチル−4−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジブチル−3−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジブチル−4−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジ−t−ブチル−3−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジ−t−ブチル−5−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジ−t−ブチル−6−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−3−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−4−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−6−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジ−t−ブチル−3−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジ−t−ブチル−4−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジ−t−ブチル−5−メチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3−ジブチル−4−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジブチル−3−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジブチル−4−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジ−t−ブチル−3−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジ−t−ブチル−5−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4−ジ−t−ブチル−6−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−3−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−4−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,5−ジ−t−ブチル−6−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジ−t−ブチル−3−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジ−t−ブチル−4−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,6−ジ−t−ブチル−5−エチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,3,4−トリブチルフェニル)−4,4′−ビフェニレンジホスホナイト、テトラキス(2,4,6−トリ−t−ブチルフェニル)−4,4′−ビフェニレンジホスホナイト等が挙げられる。上記タイプのリン系化合物は、例えば、チバ・スペシャルティ・ケミカルズ株式会社から「IRGAFOSP−EPQ」、堺化学工業株式会社から「GSY−P101」という商品名で市販されている。   Specific examples of the phosphonite compound include dimethyl-phenylphosphonite, di-t-butyl-phenylphosphonite, diphenyl-phenylphosphonite, di- (4-pentyl-phenyl) -phenylphosphonite, di- (2- t-butyl-phenyl) -phenylphosphonite, di- (2-methyl-3-pentyl-phenyl) -phenylphosphonite, di- (2-methyl-4-octyl-phenyl) -phenylphosphonite, di- ( 3-butyl-4-methyl-phenyl) -phenylphosphonite, di- (3-hexyl-4-ethyl-phenyl) -phenylphosphonite, di- (2,4,6-trimethylphenyl) -phenylphosphonite, Di- (2,3-dimethyl-4-ethyl-phenyl) -phenylphosphonite, di- (2,6-diethi -3-butylphenyl) -phenylphosphonite, di- (2,3-dipropyl-5-butylphenyl) -phenylphosphonite, di- (2,4,6-tri-t-butylphenyl) -phenylphosphonite Bis (2,4-di-t-butyl-5-methylphenyl) biphenyl-4-yl-phosphonite, bis (2,4-di-t-butyl-5-methylphenyl) -4 '-(bis ( 2,4-di-tert-butyl-5-methylphenoxy) phosphino) biphenyl-4-yl-phosphonite, tetrakis (2,4-di-tert-butyl-phenyl) -4,4'-biphenylenediphosphonite, Tetrakis (2,5-di-t-butyl-phenyl) -4,4'-biphenylenediphosphonite, tetrakis (3,5-di-t-butyl-phenyl) -4,4'-bif Nylene diphosphonite, tetrakis (2,3,4-trimethylphenyl) -4,4'-biphenylene diphosphonite, tetrakis (2,3-dimethyl-5-ethyl-phenyl) -4,4'-biphenylene diphospho Knight, tetrakis (2,3-dimethyl-4-propylphenyl) -4,4'-biphenylene diphosphonite, tetrakis (2,3-dimethyl-5-t-butylphenyl) -4,4'-biphenylene diphospho Knight, tetrakis (2,5-dimethyl-4-t-butylphenyl) -4,4'-biphenylene diphosphonite, tetrakis (2,3-diethyl-5-methylphenyl) -4,4'-biphenylene diphospho Knight, tetrakis (2,6-diethyl-4-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4,5-triethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-diethyl-4-propylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2, 5-diethyl-6-butylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,3-diethyl-5-t-butylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2, 5-diethyl-6-tert-butylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,3-dipropyl-5-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2, 6-dipropyl-4-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-dipropyl-5- Tilphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,3-dipropyl-6-butylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-dipropyl-5-butylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,3-dibutyl-4-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,5-dibutyl-3-methylphenyl) -4 , 4'-biphenylenediphosphonite, tetrakis (2,6-dibutyl-4-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4-di-t-butyl-3-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4-di-t-butyl-5-methylphenyl) -4 4'-biphenylenediphosphonite, tetrakis (2,4-di-t-butyl-6-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,5-di-t-butyl-3- Methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,5-di-t-butyl-4-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,5-di-) t-butyl-6-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-di-t-butyl-3-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis ( 2,6-di-t-butyl-4-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-di-t-butyl-5-methylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,3-dibutyl-4-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4-dibutyl-3-ethylphenyl) -4 , 4'-biphenylenediphosphonite, tetrakis (2,5-dibutyl-4-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4-di-t-butyl-3-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4-di-t-butyl-5-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4-di-t-butyl) -6-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,5-di-t-butyl-3-ethylphenyl) -4,4'- Phenylenediphosphonite, tetrakis (2,5-di-t-butyl-4-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,5-di-t-butyl-6-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-di-t-butyl-3-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-di-t-butyl) -4-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,6-di-t-butyl-5-ethylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,3 , 4-tributylphenyl) -4,4'-biphenylenediphosphonite, tetrakis (2,4,6-tri-t-butylphenyl) -4,4'-biphenylene Phosphonite, and the like. The phosphorus compound of the above type is commercially available, for example, from Ciba Specialty Chemicals Co., Ltd. under the trade name “IRGAFOSP-EPQ” and from Sakai Chemical Industry Co., Ltd. as “GSY-P101”.

リン系酸化防止剤として、ホスホナイト系化合物が好ましく、中でも、テトラキス(2,4−ジ−t−ブチル−フェニル)−4,4′−ビフェニレンジホスホナイト等の4,4′−ビフェニレンジホスホナイト化合物が好ましく、特に好ましいものはテトラキス(2,4−ジ−t−ブチル−5−メチルフェニル)−4,4′−ビフェニレンジホスホナイトである。
(アルキルラジカル捕捉剤)
セルロースエステルフィルムには以下に説明するアルキルラジカル捕捉剤を含有することが好ましい。ここでいうアルキルラジカル捕捉剤とは、アルキルラジカルが速やかに反応しうる基を有し、かつアルキルラジカルと反応後に後続反応が起こらない安定な生成物を与える化合物を意味する。
As the phosphorus antioxidant, phosphonite compounds are preferable, and among them, 4,4′-biphenylene diphosphonite such as tetrakis (2,4-di-t-butyl-phenyl) -4,4′-biphenylene diphosphonite. Compounds are preferred, and particularly preferred is tetrakis (2,4-di-t-butyl-5-methylphenyl) -4,4'-biphenylenediphosphonite.
(Alkyl radical scavenger)
The cellulose ester film preferably contains an alkyl radical scavenger described below. The term “alkyl radical scavenger” as used herein means a compound that has a group with which an alkyl radical can react rapidly and gives a stable product in which no subsequent reaction occurs after the reaction with the alkyl radical.

アルキルラジカル捕捉剤として、住友化学株式会社から、「SumilizerGM」、「SumilizerGS」という商品名で市販されている。
(ヒンダードアミン光安定剤)
セルロースエステルフィルムには、フィルム形成材料の熱溶融時の劣化防止剤、また製造後に偏光子保護フィルムとして晒される外光や液晶ディスプレイのバックライトからの光に対する劣化防止剤として、ヒンダードアミン光安定剤(HALS)化合物を添加することが好ましい。ヒンダードアミン光安定剤としては、例えば、米国特許第4,619,956号明細書の第5〜11欄及び米国特許第4,839,405号明細書の第3〜5欄に記載されているように、2,2,6,6−テトラアルキルピペリジン化合物、またはそれらの酸付加塩もしくはそれらと金属化合物との錯体が含まれる。
Alkyl radical scavengers are commercially available from Sumitomo Chemical Co., Ltd. under the trade names “Sumilizer GM” and “Sumilizer GS”.
(Hindered amine light stabilizer)
Cellulose ester films include hindered amine light stabilizers (degradation inhibitors for film-forming materials during heat melting, and as degradation inhibitors for external light exposed as a polarizer protective film after production and light from backlights of liquid crystal displays) It is preferred to add a HALS) compound. Examples of the hindered amine light stabilizer are described in US Pat. No. 4,619,956, columns 5 to 11 and US Pat. No. 4,839,405, columns 3 to 5. 2,2,6,6-tetraalkylpiperidine compounds, or their acid addition salts or complexes of them with metal compounds.

ヒンダードアミン光安定剤の具体例としては、ビス(2,2,6,6−テトラメチル−4−ピペリジル)セバケート、ビス(2,2,6,6−テトラメチル−4−ピペリジル)スクシネート、ビス(1,2,2,6,6−ペンタメチル−4−ピペリジル)セバケート、ビス(N−オクトキシ−2,2,6,6−テトラメチル−4−ピペリジル)セバケート、ビス(N−ベンジルオキシ−2,2,6,6−テトラメチル−4−ピペリジル)セバケート、ビス(N−シクロヘキシルオキシ−2,2,6,6−テトラメチル−4−ピペリジル)セバケート、ビス(1,2,2,6,6−ペンタメチル−4−ピペリジル)2−(3,5−ジ−t−ブチル−4−ヒドロキシベンジル)−2−ブチルマロネート、ビス(1−アクロイル−2,2,6,6−テトラメチル−4−ピペリジル)2,2−ビス(3,5−ジ−t−ブチル−4−ヒドロキシベンジル)−2−ブチルマロネート、ビス(1,2,2,6,6−ペンタメチル−4−ピペリジル)デカンジオエート、2,2,6,6−テトラメチル−4−ピペリジルメタクリレート、4−[3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオニルオキシ]−1−[2−(3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオニルオキシ)エチル]−2,2,6,6−テトラメチルピペリジン、2−メチル−2−(2,2,6,6−テトラメチル−4−ピペリジル)アミノ−N−(2,2,6,6−テトラメチル−4−ピペリジル)プロピオンアミド、テトラキス(2,2,6,6−テトラメチル−4−ピペリジル)1,2,3,4−ブタンテトラカルボキシレート、テトラキス(1,2,2,6,6−ペンタメチル−4−ピペリジル)1,2,3,4−ブタンテトラカルボキシレート等が挙げられる。   Specific examples of the hindered amine light stabilizer include bis (2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis (2,2,6,6-tetramethyl-4-piperidyl) succinate, bis ( 1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, bis (N-octoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis (N-benzyloxy-2, 2,6,6-tetramethyl-4-piperidyl) sebacate, bis (N-cyclohexyloxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis (1,2,2,6,6) -Pentamethyl-4-piperidyl) 2- (3,5-di-t-butyl-4-hydroxybenzyl) -2-butylmalonate, bis (1-acryloyl-2,2,6,6- Tramethyl-4-piperidyl) 2,2-bis (3,5-di-tert-butyl-4-hydroxybenzyl) -2-butylmalonate, bis (1,2,2,6,6-pentamethyl-4- Piperidyl) decanedioate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, 4- [3- (3,5-di-tert-butyl-4-hydroxyphenyl) propionyloxy] -1- [ 2- (3- (3,5-di-tert-butyl-4-hydroxyphenyl) propionyloxy) ethyl] -2,2,6,6-tetramethylpiperidine, 2-methyl-2- (2,2, 6,6-tetramethyl-4-piperidyl) amino-N- (2,2,6,6-tetramethyl-4-piperidyl) propionamide, tetrakis (2,2,6,6-tetramethyl-4-piperidyl) 1,2,3,4-butane tetracarboxylate, tetrakis (1,2,2,6,6-pentamethyl-4-piperidyl) 1,2,3,4-butane tetracarboxylate, and the like.

また、高分子タイプの化合物でもよく、具体例としては、N,N′,N″,N″′−テトラキス−[4,6−ビス−〔ブチル−(N−メチル−2,2,6,6−テトラメチルピペリジン−4−イル)アミノ〕−トリアジン−2−イル]−4,7−ジアザデカン−1,10−ジアミン、ジブチルアミンと1,3,5−トリアジン−N,N′−ビス(2,2,6,6−テトラメチル−4−ピペリジル)−1,6−ヘキサメチレンジアミンとN−(2,2,6,6−テトラメチル−4−ピペリジル)ブチルアミンとの重縮合物、ジブチルアミンと1,3,5−トリアジンとN,N′−ビス(2,2,6,6−テトラメチル−4−ピペリジル)ブチルアミンとの重縮合物、ポリ〔{(1,1,3,3−テトラメチルブチル)アミノ−1,3,5−トリアジン−2,4−ジイル}{(2,2,6,6−テトラメチル−4−ピペリジル)イミノ}ヘキサメチレン{(2,2,6,6−テトラメチル−4−ピペリジル)イミノ}〕、1,6−ヘキサンジアミン−N,N′−ビス(2,2,6,6−テトラメチル−4−ピペリジル)とモルホリン−2,4,6−トリクロロ−1,3,5−トリアジンとの重縮合物、ポリ[(6−モルホリノ−s−トリアジン−2,4−ジイル)〔(2,2,6,6−テトラメチル−4−ピペリジル)イミノ〕−ヘキサメチレン〔(2,2,6,6−テトラメチル−4−ピペリジル)イミノ〕]等の、ピペリジン環がトリアジン骨格を介して複数結合した高分子量HALS;コハク酸ジメチルと4−ヒドロキシ−2,2,6,6−テトラメチル−1−ピペリジンエタノールとの重合物、1,2,3,4−ブタンテトラカルボン酸と1,2,2,6,6−ペンタメチル−4−ピペリジノールと3,9−ビス(2−ヒドロキシ−1,1−ジメチルエチル)−2,4,8,10−テトラオキサスピロ[5,5]ウンデカンとの混合エステル化物等の、ピペリジン環がエステル結合を介して結合した化合物等が挙げられるが、これらに限定されるものではない。   Further, it may be a polymer type compound. As specific examples, N, N ′, N ″, N ″ ′-tetrakis- [4,6-bis- [butyl- (N-methyl-2,2,6, 6-tetramethylpiperidin-4-yl) amino] -triazin-2-yl] -4,7-diazadecane-1,10-diamine, dibutylamine and 1,3,5-triazine-N, N′-bis ( 2,2,6,6-tetramethyl-4-piperidyl) -1,6-hexamethylenediamine and N- (2,2,6,6-tetramethyl-4-piperidyl) butylamine polycondensate, di Polycondensate of butylamine, 1,3,5-triazine and N, N′-bis (2,2,6,6-tetramethyl-4-piperidyl) butylamine, poly [{(1,1,3,3 -Tetramethylbutyl) amino-1,3,5-tri Gin-2,4-diyl} {(2,2,6,6-tetramethyl-4-piperidyl) imino} hexamethylene {(2,2,6,6-tetramethyl-4-piperidyl) imino}], Weight of 1,6-hexanediamine-N, N'-bis (2,2,6,6-tetramethyl-4-piperidyl) and morpholine-2,4,6-trichloro-1,3,5-triazine Condensate, poly [(6-morpholino-s-triazine-2,4-diyl) [(2,2,6,6-tetramethyl-4-piperidyl) imino] -hexamethylene [(2,2,6, 6-tetramethyl-4-piperidyl) imino]] and other high molecular weight HALS in which a plurality of piperidine rings are bonded via a triazine skeleton; dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1 -Piperidine Etano 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and 3,9-bis (2-hydroxy-1,1-dimethyl) (Ethyl) -2,4,8,10-tetraoxaspiro [5,5] undecane and the like, and the like are exemplified by compounds in which a piperidine ring is bonded through an ester bond, but the present invention is not limited thereto. It is not a thing.

これらの中でも、ジブチルアミンと1,3,5−トリアジンとN,N′−ビス(2,2,6,6−テトラメチル−4−ピペリジル)ブチルアミンとの重縮合物、ポリ〔{(1,1,3,3−テトラメチルブチル)アミノ−1,3,5−トリアジン−2,4−ジイル}{(2,2,6,6−テトラメチル−4−ピペリジル)イミノ}ヘキサメチレン{(2,2,6,6−テトラメチル−4−ピペリジル)イミノ}〕、コハク酸ジメチルと4−ヒドロキシ−2,2,6,6−テトラメチル−1−ピペリジンエタノールとの重合物等で、数平均分子量(Mn)が2,000〜5,000のものが好ましい。   Among these, polycondensates of dibutylamine, 1,3,5-triazine and N, N′-bis (2,2,6,6-tetramethyl-4-piperidyl) butylamine, poly [{(1, 1,3,3-tetramethylbutyl) amino-1,3,5-triazine-2,4-diyl} {(2,2,6,6-tetramethyl-4-piperidyl) imino} hexamethylene {(2 , 2,6,6-tetramethyl-4-piperidyl) imino}], a polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol, etc. Those having a molecular weight (Mn) of 2,000 to 5,000 are preferred.

上記タイプのヒンダードアミン化合物は、例えばチバスペシャルティケミカルズから、「TINUVIN144」及び「TINUVIN770」、旭電化工業株式会社から「ADK STAB LA−52」という商品名で市販されている。   Hindered amine compounds of the above type are commercially available, for example, from Ciba Specialty Chemicals under the trade names “TINUVIN 144” and “TINUVIN 770”, and from Asahi Denka Kogyo Co., Ltd. under the name “ADK STAB LA-52”.

ヒンダードアミン光安定剤は、本発明に用いられるセルロースエステルの質量に対して、0.1〜10質量%添加することが好ましく、さらに0.2〜5質量%添加することが好ましく、さらに0.5〜2質量%添加することが好ましい。これらは2種以上を併用してもよい。
(酸捕捉剤)
セルロースエステルフィルムには、酸捕捉剤が、高温環境下では酸による分解を抑制することから、含有されることが好ましい。酸捕捉剤としては、酸と反応して酸を不活性化する化合物であれば制限なく用いることができるが、中でも米国特許第4,137,201号明細書に記載されているような、エポキシ基を有する化合物が好ましい。
The hindered amine light stabilizer is preferably added in an amount of 0.1 to 10% by mass, more preferably 0.2 to 5% by mass, more preferably 0.5 to the mass of the cellulose ester used in the present invention. It is preferable to add ~ 2 mass%. Two or more of these may be used in combination.
(Acid scavenger)
It is preferable that an acid scavenger is contained in the cellulose ester film because it suppresses decomposition by an acid in a high temperature environment. The acid scavenger can be used without limitation as long as it is a compound that reacts with an acid to inactivate the acid, and among them, an epoxy as described in US Pat. Compounds having a group are preferred.

このような酸捕捉剤としてのエポキシ化合物は当該技術分野において既知であり、種々のポリグリコールのジグリシジルエーテル、特にポリグリコール1モル当たりに約8〜40モルのエチレンオキシド等の縮合によって誘導されるポリグリコール、グリセロールのジグリシジルエーテル等、金属エポキシ化合物(例えば、塩化ビニルポリマー組成物において、及び塩化ビニルポリマー組成物と共に、従来から利用されているもの)、エポキシ化エーテル縮合生成物、ビスフェノールAのジグリシジルエーテル(すなわち、4,4′−ジヒドロキシジフェニルジメチルメタン)、エポキシ化不飽和脂肪酸エステル(特に、2〜22個の炭素原子の脂肪酸の4〜2個程度の炭素原子のアルキルのエステル(例えば、ブチルエポキシステアレート)等)、及び種々のエポキシ化長鎖脂肪酸トリグリセリド等(例えば、エポキシ化大豆油、エポキシ化亜麻仁油等)の組成物によって代表され例示され得るエポキシ化植物油及び他の不飽和天然油(これらはときとしてエポキシ化天然グリセリドまたは不飽和脂肪酸と称され、これらの脂肪酸は一般に12〜22個の炭素原子を含有している)が含まれる。また、市販のエポキシ基含有エポキシド樹脂化合物として、EPON 815Cやその他のエポキシ化エーテルオリゴマー縮合生成物も好ましく用いることができる。   Epoxy compounds as such acid scavengers are known in the art and are derived by condensation of various polyglycol diglycidyl ethers, particularly about 8 to 40 moles of ethylene oxide per mole of polyglycol. Glycol, diglycidyl ether of glycerol, etc., metal epoxy compounds (such as those conventionally used in and with vinyl chloride polymer compositions), epoxidized ether condensation products, diphenols of bisphenol A Glycidyl ether (ie, 4,4′-dihydroxydiphenyldimethylmethane), epoxidized unsaturated fatty acid ester (especially an ester of an alkyl of about 4 to 2 carbon atoms of a fatty acid of 2 to 22 carbon atoms (for example, Butyl epoxy stearate Epoxidized vegetable oils and other unsaturated natural oils, which may be represented and exemplified by compositions of various epoxidized long chain fatty acid triglycerides and the like (eg, epoxidized soybean oil, epoxidized linseed oil, etc.) As epoxidized natural glycerides or unsaturated fatty acids, which generally contain from 12 to 22 carbon atoms). Moreover, EPON 815C and other epoxidized ether oligomer condensation products can also be preferably used as commercially available epoxy group-containing epoxide resin compounds.

さらに上記以外に用いることが可能な酸捕捉剤としては、オキセタン化合物やオキサゾリン化合物、あるいはアルカリ土類金属の有機酸塩やアセチルアセトナート錯体、特開平5−194788号公報の段落番号[0068]〜[0105]に記載されているものが含まれる。   In addition to the above, acid scavengers that can be used include oxetane compounds, oxazoline compounds, alkaline earth metal organic acid salts and acetylacetonate complexes, and paragraphs [0068] to JP-A-5-194788. [0105] are included.

本発明においては、酸捕捉剤は、本発明に用いられるセルロースエステルの質量に対して、0.1〜10質量%添加することが好ましく、さらに0.2〜5質量%添加することが好ましく、さらに0.5〜2質量%添加することが好ましい。これらは2種以上を併用してもよい。   In the present invention, the acid scavenger is preferably added in an amount of 0.1 to 10% by mass, more preferably 0.2 to 5% by mass, based on the mass of the cellulose ester used in the present invention. Furthermore, it is preferable to add 0.5-2 mass%. Two or more of these may be used in combination.

なお酸捕捉剤は、酸掃去剤、酸捕獲剤、酸キャッチャー等と称されることもあるが、本発明においてはこれらの呼称による差異なく用いることができる。
(金属不活性剤)
セルロースエステルフィルムには、金属不活性剤も含まれることも好ましい。金属不活性剤とは、酸化反応において開始剤あるいは触媒として作用する金属イオン不活性化する化合物を意味し、ヒドラジド系化合物、シュウ酸ジアミド系化合物、トリアゾール系化合物等が挙げられ、例えば、N,N′−ビス〔3−(3,5−ジ−t−ブチル−4−ヒドロキシフェニル)プロピオニル〕ヒドラジン、2−ヒドロキシエチルシュウ酸ジアミド、2−ヒドロキシ−N−(1H−1,2,4−トリアゾール−3−イル)ベンズアミド、N−(5−tert−ブチル−2−エトキシフェニル)−N′−(2−エチルフェニル)シュウ酸アミド等が挙げられる。
In addition, although an acid scavenger may be called an acid scavenger, an acid capture agent, an acid catcher, etc., in this invention, it can use without a difference by these names.
(Metal deactivator)
It is also preferred that the cellulose ester film contains a metal deactivator. A metal deactivator means a metal ion deactivating compound that acts as an initiator or a catalyst in an oxidation reaction, and examples thereof include hydrazide compounds, oxalic acid diamide compounds, triazole compounds, and the like. N'-bis [3- (3,5-di-t-butyl-4-hydroxyphenyl) propionyl] hydrazine, 2-hydroxyethyl oxalic acid diamide, 2-hydroxy-N- (1H-1,2,4- And triazol-3-yl) benzamide and N- (5-tert-butyl-2-ethoxyphenyl) -N '-(2-ethylphenyl) oxalic acid amide.

金属不活性剤は、透明基材フィルムの樹脂100質量%に対して、0.0002〜2質量%添加することが好ましく、さらに0.0005〜2質量%添加することが好ましく、さらに0.001〜1質量%添加することが好ましい。これらは2種以上を併用してもよい。
(その他の添加剤)
セルロースエステルフィルムには、その他の添加剤として、例えば、染料、顔料、蛍光体、二色性色素、リタデーション制御剤、屈折率調整剤、ガス透過抑制剤、抗菌剤、生分解性付与剤などを添加しても良い。
The metal deactivator is preferably added in an amount of 0.0002 to 2% by mass, more preferably 0.0005 to 2% by mass, and more preferably 0.001 to 100% by mass of the resin of the transparent base film. It is preferable to add ~ 1 mass%. Two or more of these may be used in combination.
(Other additives)
For the cellulose ester film, other additives such as dyes, pigments, phosphors, dichroic dyes, retardation control agents, refractive index adjusters, gas permeation inhibitors, antibacterial agents, biodegradability imparting agents, etc. It may be added.

そして、これらの添加剤をセルロースエステルフィルムに含有させる方法としては、各々の材料を固体或いは液体のまま混合し、加熱溶融し混練して均一な溶融物とした後、流延してセルロースエステルフィルムを形成する方法であっても、予め全ての材料を溶媒等を用いて、溶解して均一溶液とした後、溶媒を除去して、添加剤とセルロースエステルフィルムの混合物で含有させても良い。
(偏光板)
本発明による反射防止フィルムを用いた偏光板について述べる。
And, as a method of incorporating these additives into the cellulose ester film, the respective materials are mixed as solid or liquid, heated and melted and kneaded to obtain a uniform melt, and then cast into a cellulose ester film. Even in the method of forming a film, all materials may be dissolved in advance using a solvent or the like to obtain a uniform solution, and then the solvent may be removed and contained in a mixture of an additive and a cellulose ester film.
(Polarizer)
The polarizing plate using the antireflection film according to the present invention will be described.

偏光板は、一般的な方法で作製することができる。本発明の反射防止フィルムの裏面側をアルカリ鹸化処理し、処理した反射防止フィルムを、ヨウ素溶液中に浸漬延伸して作製した偏光膜の少なくとも一方の面に、完全鹸化型ポリビニルアルコール水溶液を用いて貼り合わせることが好ましい。もう一方の面に該反射防止フィルムを用いても、別の偏光板保護フィルムを用いてもよい。   The polarizing plate can be produced by a general method. The back surface side of the antireflection film of the present invention is subjected to alkali saponification treatment, and a completely saponified polyvinyl alcohol aqueous solution is used on at least one surface of a polarizing film prepared by immersing and stretching the treated antireflection film in an iodine solution. It is preferable to bond them together. The antireflection film may be used on the other surface, or another polarizing plate protective film may be used.

本発明の反射防止フィルムに対して、もう一方の面に用いられる偏光板保護フィルムは、面内リタデーション(Ro)が、20〜70nm、厚み方向リタデーション(Rt)が100〜400nmの位相差を有する光学補償フィルム(位相差フィルム)であることが好ましい。   With respect to the antireflection film of the present invention, the polarizing plate protective film used on the other surface has an in-plane retardation (Ro) of 20 to 70 nm and a thickness direction retardation (Rt) of 100 to 400 nm. It is preferably an optical compensation film (retardation film).

なお、リタデーション値Ro、Rtは、自動複屈折率計を用いて測定することができる。例えば、KOBRA−21ADH(王子計測機器株式会社製)を用いて、温度23℃、湿度55%RHの環境下で、波長が590nmで求めることができる。   The retardation values Ro and Rt can be measured using an automatic birefringence meter. For example, using KOBRA-21ADH (manufactured by Oji Scientific Instruments Co., Ltd.), the wavelength can be obtained at 590 nm in an environment of a temperature of 23 ° C. and a humidity of 55% RH.

これらは例えば、特開2002−71957号、特願2002−155395号記載の方法で作製することができる。または、さらにディスコチック液晶等の液晶化合物を配向させて形成した光学異方層を有している光学補償フィルムを兼ねる偏光板保護フィルムを用いることが好ましい。例えば、特開2003−98348号記載の方法で光学異方性層を形成することができる。あるいは面内リタデーション(Ro)が、0〜5nm、厚み方向リタデーション(Rt)が−20〜+20nmの無配向フィルムも好ましく用いられる。   These can be prepared, for example, by the methods described in JP-A No. 2002-71957 and Japanese Patent Application No. 2002-155395. Alternatively, it is preferable to use a polarizing plate protective film that also serves as an optical compensation film having an optically anisotropic layer formed by aligning a liquid crystal compound such as a discotic liquid crystal. For example, the optically anisotropic layer can be formed by the method described in JP-A-2003-98348. Alternatively, an unoriented film having an in-plane retardation (Ro) of 0 to 5 nm and a thickness direction retardation (Rt) of -20 to +20 nm is also preferably used.

本発明の反射防止フィルムと組み合わせて使用することによって、平面性に優れ、安定した視野角拡大効果を有する偏光板を得ることができる。   By using in combination with the antireflection film of the present invention, a polarizing plate having excellent flatness and a stable viewing angle expansion effect can be obtained.

裏面側に用いられる偏光板保護フィルムとしては、市販のセルロースエステルフィルムとして、KC8UX2MW、KC4UX、KC5UX、KC4UY、KC8UY、KC12UR、KC4UEW、KC8UCR−3、KC8UCR−4、KC8UCR−5、KC4FR−1、KC4FR−2(コニカミノルタオプト株式会社製)等が好ましく用いられる。   As a polarizing plate protective film used on the back side, as a commercially available cellulose ester film, KC8UX2MW, KC4UX, KC5UX, KC4UY, KC8UY, KC12UR, KC4UEW, KC8UCR-3, KC8UCR-4, KC8UCR-5, KC4FR-1, KC4F-1, -2 (manufactured by Konica Minolta Opto Co., Ltd.) and the like are preferably used.

偏光板の主たる構成要素である偏光膜とは、一定方向の偏波面の光だけを通す素子であり、現在知られている代表的な偏光膜は、ポリビニルアルコール系偏光フィルムで、これはポリビニルアルコール系フィルムにヨウ素を染色させたものと二色性染料を染色させたものがあるがこれのみに限定されるものではない。偏光膜は、ポリビニルアルコール水溶液を製膜し、これを一軸延伸させて染色するか、染色した後一軸延伸してから、好ましくはホウ素化合物で耐久性処理を行ったものが用いられている。偏光膜の膜厚は5〜30μm、好ましくは8〜15μmの偏光膜が好ましく用いられる。該偏光膜の面上に、本発明の反射防止フィルムの片面を貼り合わせて偏光板を形成する。好ましくは完全鹸化ポリビニルアルコール等を主成分とする水系の接着剤によって貼り合わせる。
(画像表示装置)
本発明の反射防止フィルム面を画像表示装置の鑑賞面側に組み込むことによって、種々の視認性に優れた本発明の画像表示装置を作製することができる。
The polarizing film, which is the main component of the polarizing plate, is an element that transmits only light having a polarization plane in a certain direction. A typical polarizing film known at present is a polyvinyl alcohol polarizing film, which is a polyvinyl alcohol film. There are ones in which iodine is dyed on a system film and ones in which a dichroic dye is dyed, but it is not limited to this. As the polarizing film, a polyvinyl alcohol aqueous solution is formed and dyed by uniaxially stretching or dyed, or uniaxially stretched after dyeing, and then preferably subjected to a durability treatment with a boron compound. A polarizing film having a thickness of 5 to 30 μm, preferably 8 to 15 μm, is preferably used. On the surface of the polarizing film, one side of the antireflection film of the present invention is bonded to form a polarizing plate. It is preferably bonded with an aqueous adhesive mainly composed of completely saponified polyvinyl alcohol or the like.
(Image display device)
By incorporating the antireflection film surface of the present invention on the viewing surface side of the image display device, the image display device of the present invention having various visibility can be produced.

本発明の反射防止フィルムは、偏光板に組み込まれ、反射型、透過型、半透過型LCDまたはTN型、STN型、OCB型、HAN型、VA型(PVA型、MVA型)、IPS型等の各種駆動方式のLCDで好ましく用いられる。また、本発明の反射防止フィルムは反射防止層の反射光の色ムラが著しく少なく、また、反射率が低く、平面性に優れ、プラズマディスプレイ、フィールドエミッションディスプレイ、有機ELディスプレイ、無機ELディスプレイ、電子ペーパー等の各種画像表示装置にも好ましく用いられる。   The antireflection film of the present invention is incorporated in a polarizing plate, and is a reflection type, transmission type, transflective LCD or TN type, STN type, OCB type, HAN type, VA type (PVA type, MVA type), IPS type, etc. It is preferably used in LCDs of various drive systems. In addition, the antireflection film of the present invention has significantly less color unevenness in the reflected light of the antireflection layer, and has a low reflectance and excellent flatness, and is a plasma display, field emission display, organic EL display, inorganic EL display, electronic It is also preferably used for various image display devices such as paper.

特に、本発明の反射防止フィルムを、プラズマディスプレイの前面板フイルターとして加工し、装着したプラズマディスプレイは、光干渉ムラもなく優れた視認性を有する画像表示装置である。また、30型以上の大画面のプラズマディスプレイ画像表示装置でも、色ムラや波打ちムラが少なく、長時間の鑑賞でも目が疲れないという効果がある。また本発明の反射防止フィルムは、良好な帯電防止性も有しているものである。   In particular, a plasma display in which the antireflection film of the present invention is processed as a front plate filter of a plasma display and is mounted is an image display device having excellent visibility without uneven light interference. In addition, even a 30-inch or larger plasma display image display device has an effect that there is little color unevenness and wavy unevenness, and eyes are not tired even during long-time viewing. The antireflection film of the present invention also has good antistatic properties.

以下、本発明の実施例を説明するが、本発明はこれらに限定されるものではない。
実施例1
本発明による反射防止フィルムを作製するにあたり、まず、透明フィルム基材を作製した。
(ドープ組成物)
セルローストリアセテート(平均酢化度61.0%) 100質量部
トリフェニルフォスフェート 8質量部
エチルフタリルエチルグリコレート 2質量部
チヌビン109(チバスペシャルティケミカルズ株式会社製) 1質量部
チヌビン171(チバスペシャルティケミカルズ株式会社製) 1質量部
メチレンクロライド 430質量部
メタノール 90質量部
上記の材料を密閉容器に投入し、加圧下で温度80℃に保温し、攪拌しながら完全に溶解して、ドープ組成物を得た。
Examples of the present invention will be described below, but the present invention is not limited thereto.
Example 1
In preparing the antireflection film according to the present invention, first, a transparent film substrate was prepared.
(Dope composition)
Cellulose triacetate (average degree of acetylation 61.0%) 100 parts by weight Triphenyl phosphate 8 parts by weight Ethylphthalyl ethyl glycolate 2 parts by weight Tinuvin 109 (manufactured by Ciba Specialty Chemicals) 1 part by weight Tinuvin 171 (Ciba Specialty Chemicals) 1 part by weight Methylene chloride 430 parts by weight Methanol 90 parts by weight The above materials are put into a sealed container, kept at a temperature of 80 ° C. under pressure, and completely dissolved with stirring to obtain a dope composition. It was.

つぎに、このドープ組成物を濾過し、冷却して温度33℃に保ち、ステンレスバンド上に均一に流延し、剥離が可能になるまで溶媒を蒸発させたところでステンレスバンドから剥離し、テンターで幅方向に1.1倍に延伸した後、多数のロールで搬送させながら乾燥させ、両端部に高さ10μmのナーリングを設けて巻き取り、透明なセルローストリアセテートフィルムよりなる透明フィルム基材1を作製した。ここで、透明フィルム基材1は、膜厚80μm、幅1.5m、及び長さ3900mを有するものであった。   Next, the dope composition is filtered, cooled and kept at a temperature of 33 ° C., cast evenly on a stainless steel band, and the solvent is evaporated until peeling is possible. After stretching 1.1 times in the width direction, the film is dried while being conveyed by a large number of rolls, wound with 10 μm height knurling on both ends, and a transparent film substrate 1 made of a transparent cellulose triacetate film is produced. did. Here, the transparent film base material 1 had a film thickness of 80 μm, a width of 1.5 m, and a length of 3900 m.

また、膜厚及び長さを変更した以外は、上記の場合と同様にして、膜厚40μm、幅1.5m、長さ5200mのセルローストリアセテートフィルムよりなる透明フィルム基材2を作製した。
(反射防止フィルム1の作製)
上記作製した透明フィルム基材1上に、下記のように導電層1、ついで、低屈折率層1の順に塗設し、反射防止フィルム1を作製した。
Moreover, the transparent film base material 2 which consists of a cellulose triacetate film with a film thickness of 40 micrometers, a width | variety of 1.5 m, and length of 5200 m was produced like the said case except having changed the film thickness and length.
(Preparation of antireflection film 1)
On the transparent film substrate 1 produced as described above, the antireflection film 1 was produced by coating the conductive layer 1 and then the low refractive index layer 1 in this order.

なお、以下の実施例において、反射防止層を構成する各層の屈折率は、下記方法により測定した。
(屈折率)
各屈折率層の屈折率は、各層を単独で下記で作製したハードコートフィルム上に塗設したサンプルについて、分光光度計の分光反射率の測定結果から求めた。分光光度計はU−4000型(日立製作所製)を用いて、サンプルの測定側の裏面を粗面化処理した後、黒色のスプレーで光吸収処理を行って裏面での光の反射を防止して、5度正反射の条件にて可視光領域(400nm〜700nm)の反射率の測定を行った。
(導電層1の形成)
透明フィルム基材1上に、ポリチオフェン含有多官能アクリレート塗剤(製品名:ELコートUVH−D003、出光テクノファイン株式会社製)をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが5μmの導電層1を設けた。なお、この導電層1の屈折率は1.51であった。
In the following examples, the refractive index of each layer constituting the antireflection layer was measured by the following method.
(Refractive index)
The refractive index of each refractive index layer was calculated | required from the measurement result of the spectral reflectance of the spectrophotometer about the sample which coated each layer on the hard coat film produced below. The spectrophotometer uses U-4000 type (manufactured by Hitachi, Ltd.), and after roughening the back side of the measurement side of the sample, light absorption treatment is performed with black spray to prevent reflection of light on the back side. The reflectance in the visible light region (400 nm to 700 nm) was measured under the condition of regular reflection at 5 degrees.
(Formation of conductive layer 1)
A polythiophene-containing polyfunctional acrylate coating (product name: EL coat UVH-D003, manufactured by Idemitsu Technofine Co., Ltd.) is die-coated on the transparent film substrate 1 and dried at 70 ° C. for 1 minute. The conductive layer 1 having a thickness of 5 μm was provided by being cured by / cm 2 irradiation. The refractive index of this conductive layer 1 was 1.51.

さらに、下記バックコート層用塗布組成物を、透明フィルム基材1の裏面側にウェット膜厚14μmとなるようにダイコートし、80℃にて乾燥し、巻き取り、バックコート層を設けた。
(バックコート層用塗布組成物)
ジアセチルセルロース 0.6質量部
アセトン 35質量部
メチルエチルケトン 35質量部
メタノール 35質量部
シリカ微粒子の2%メタノール分散液 16質量部
(KE−P30、日本触媒株式会社製)
(低屈折率層1の形成)
上記導電層1の表面上に、下記低屈折率層用塗布組成物1をダイコートし、80℃で1分間乾燥させ、ついで紫外線を0.3J/cm2照射して硬化させて厚さが100nmとなるように低屈折率層1を設け、反射防止フィルム1を作製した。なお、この低屈折率層1の屈折率は1.35であった。
(低屈折率層用塗布組成物1)
トリアクリロイルヘプタデカフルオロノネニルペンタエリスリトールとペンタエリスリトールテトラアクリレートの混合物 30質量部
(LINC−3A、共栄社化学株式会社製)
中空シリカ系粒子分散液1 100質量部
2−メチル−1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 5質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
メチルイソブチルケトン 300質量部
メチルエチルケトン 300質量部
(中空シリカ系粒子分散液1の調製)
平均粒径5nm、SiO2濃度20質量%のシリカゾル100gと、純水1900gとの混合物を80℃に加温した。この反応母液のpHは10.5であり、同母液にSiO2として0.98質量%のケイ酸ナトリウム水溶液9000gとAl23として1.02質量%のアルミン酸ナトリウム水溶液9000gとを同時に添加した。その間、反応液の温度を80℃に保持した。反応液のpHは添加直後、12.5に上昇し、その後、ほとんど変化しなかった。添加終了後、反応液を室温まで冷却し、限外濾過膜で洗浄して固形分濃度20質量%のSiO2・Al23核粒子分散液を調製した。(工程a)。
Furthermore, the following backcoat layer coating composition was die-coated on the back side of the transparent film substrate 1 so as to have a wet film thickness of 14 μm, dried at 80 ° C., wound up, and a backcoat layer was provided.
(Coating composition for back coat layer)
Diacetylcellulose 0.6 parts by weight Acetone 35 parts by weight Methyl ethyl ketone 35 parts by weight Methanol 35 parts by weight Silica fine particle 2% methanol dispersion 16 parts by weight (KE-P30, manufactured by Nippon Shokubai Co., Ltd.)
(Formation of low refractive index layer 1)
The following coating composition 1 for low refractive index layer is die-coated on the surface of the conductive layer 1, dried at 80 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.3 J / cm 2 to a thickness of 100 nm. The low refractive index layer 1 was provided so that the antireflection film 1 was produced. The refractive index of the low refractive index layer 1 was 1.35.
(Coating composition 1 for low refractive index layer)
30 parts by mass of a mixture of triacryloylheptadecafluorononenyl pentaerythritol and pentaerythritol tetraacrylate (LINC-3A, manufactured by Kyoeisha Chemical Co., Ltd.)
Hollow silica-based particle dispersion 1 100 parts by mass 2-methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 5 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
Methyl isobutyl ketone 300 parts by weight Methyl ethyl ketone 300 parts by weight (Preparation of hollow silica-based particle dispersion 1)
A mixture of 100 g of silica sol having an average particle size of 5 nm and a SiO 2 concentration of 20% by mass and 1900 g of pure water was heated to 80 ° C. The pH of the reaction mother liquor is 10.5, uterine solution added as SiO 2 as a 0.98 wt% aqueous solution of sodium silicate 9000g and Al 2 O 3 of 1.02% by weight sodium aluminate solution 9000g simultaneously did. Meanwhile, the temperature of the reaction solution was kept at 80 ° C. The pH of the reaction solution rose to 12.5 immediately after the addition and hardly changed thereafter. After completion of the addition, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to prepare a SiO 2 .Al 2 O 3 core particle dispersion having a solid content concentration of 20% by mass. (Step a).

この核粒子分散液500gに純水1700gを加えて98℃に加温し、この温度を保持しながら、ケイ酸ナトリウム水溶液を陽イオン交換樹脂で脱アルカリして得られたケイ酸液(SiO2濃度3.5質量%)3000gを添加して、第1シリカ被覆層を形成した核粒子の分散液を得た。(工程b)。 1700 g of pure water is added to 500 g of this core particle dispersion and heated to 98 ° C., and while maintaining this temperature, a silicate solution (SiO 2) obtained by dealkalizing a sodium silicate aqueous solution with a cation exchange resin. A dispersion of core particles in which a first silica coating layer was formed was obtained by adding 3000 g (concentration: 3.5% by mass). (Step b).

ついで、限外濾過膜で洗浄して固形分濃度13質量%になった第1シリカ被覆層を形成した核粒子分散液500gに純水1125gを加え、さらに濃塩酸(35.5%)を滴下してpH1.0とし、脱アルミニウム処理を行った。   Next, 1125 g of pure water is added to 500 g of the core particle dispersion liquid on which the first silica coating layer having a solid content concentration of 13 mass% is formed by washing with an ultrafiltration membrane, and concentrated hydrochloric acid (35.5%) is further added dropwise. The pH was adjusted to 1.0 and dealumination was performed.

ついで、pH3の塩酸水溶液10Lと純水5Lを加えながら、限外濾過膜で溶解したアルミニウム塩を分離し、第1シリカ被覆層を形成した核粒子の構成成分の一部を除去したSiO2・Al23多孔質粒子の分散液を調製した。(工程c)。 Then, while adding pH3 hydrochloric acid aqueous 10L of pure water 5L, to separate the aluminum salt dissolved in the ultrafiltration membrane, SiO 2 · removing a part of the constituting components of the core particles forming the first silica coating layer A dispersion of Al 2 O 3 porous particles was prepared. (Step c).

上記多孔質粒子分散液1500gと、純水500g、エタノール1750g、及び28%アンモニア水626gとの混合液を35℃に加温した後、エチルシリケート(SiO228質量%)104gを添加し、第1シリカ被覆層を形成した多孔質粒子の表面をエチルシリケートの加水分解重縮合物で被覆して第2シリカ被覆層を形成した。ついで、限外濾過膜を用いて溶媒をエタノールに置換した固形分濃度20質量%の中空シリカ系粒子分散液1を調製した。 A mixture of 1500 g of the above porous particle dispersion, 500 g of pure water, 1750 g of ethanol, and 626 g of 28% ammonia water is heated to 35 ° C., and then 104 g of ethyl silicate (SiO 2 28 mass%) is added. The surface of the porous particles on which the silica coating layer was formed was coated with a hydrolyzed polycondensate of ethyl silicate to form a second silica coating layer. Next, a hollow silica-based particle dispersion 1 having a solid content concentration of 20% by mass was prepared by replacing the solvent with ethanol using an ultrafiltration membrane.

この中空シリカ系粒子の第1シリカ被覆層の厚さは3nm、平均粒径は45nm、MOX/SiO2(モル比)は0.0017、屈折率は1.28であった。ここで、平均粒径は動的光散乱法により測定した。
実施例2
(反射防止フィルム2の作製)
上記作製した透明フィルム基材2上に、下記導電層用塗布組成物2を使用して導電層を形成した以外は実施例1と同様にして反射防止フィルム2を作製した。
(導電層用塗布組成物2)
ポリアニリン含有塗剤 40質量部
(ORMECON D1000、ORMECON CHEMIE Gmbh & Co.KG社製)
ジペンタエリスリトールヘキサアクリレート 120質量部
(NKエステルA−DPH、新中村化学工業株式会社製)
2−メチルー1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 10質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
N−メチル−2−ピロリドン 200質量部
実施例3
(反射防止フィルム3の作製)
上記作製した透明フィルム基材1上に、下記のように導電層3、ついで、低屈折率層2の順に塗設し、反射防止フィルム3を作製した。
(導電層3の形成)
透明フィルム基材1上に、下記の導電層用塗布組成物3をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが5μmの導電層3を設けた。なお、この導電層3の屈折率は1.51であった。
(導電層用塗布組成物3)
テトラシアノテトラアザナフタレンドープポリピロール溶液 18質量部
(SSPY、ティーエーケミカル株式会社製)
ジペンタエリスリトールヘキサアクリレート 30質量部
(NKエステルA−DPH、新中村化学工業株式会社製)
2−メチルー1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 4質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
N−メチル−2−ピロリドン 70質量部
さらに、実施例1と同様にして透明フィルム基材1の裏面側にバックコート層を設けた。
(低屈折率層2の形成)
上記導電層3の表面上に、下記低屈折率層用塗布組成物2をダイコートし、80℃で1分間乾燥させ、ついで紫外線を0.3J/cm2照射して硬化させて厚さが100nmとなるように低屈折率層2を設け、反射防止フィルム3を作製した。なお、この低屈折率層2の屈折率は1.39であった。
(低屈折率層用塗布組成物2)
トリアクリロイルヘプタデカフルオロノネニルペンタエリスリトールとペンタエリスリトールテトラアクリレートの混合物 30質量部
(LINC−3A、共栄社化学株式会社製)
酸化アンチモン被覆中空シリカ系粒子分散液1 100質量部
2−メチル−1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 5質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
メチルイソブチルケトン 300質量部
メチルエチルケトン 300質量部
(酸化アンチモン被覆中空シリカ系粒子分散液1の調製)
平均粒径5nm、SiO2濃度20質量%のシリカゾル100gと、純水1900gとの混合物を80℃に加温した。この反応母液のpHは10.5であり、同母液にSiO2として1.17質量%のケイ酸ナトリウム水溶液9000gとAl23として0.83質量%のアルミン酸ナトリウム水溶液9000gとを同時に添加した。その間、反応液の温度を80℃に保持した。反応液のpHは添加直後、12.5に上昇し、その後、ほとんど変化しなかった。添加終了後、反応液を室温まで冷却し、限外濾過膜で洗浄して固形分濃度20質量%のSiO2・Al23核粒子分散液を調製した。(工程d)。
The thickness of the first silica coating layer of the hollow silica-based particles was 3 nm, the average particle size was 45 nm, MOX / SiO 2 (molar ratio) was 0.0017, and the refractive index was 1.28. Here, the average particle diameter was measured by a dynamic light scattering method.
Example 2
(Preparation of antireflection film 2)
An antireflection film 2 was produced in the same manner as in Example 1 except that a conductive layer was formed on the produced transparent film substrate 2 using the following conductive layer coating composition 2.
(Coating composition 2 for conductive layer)
40 parts by mass of polyaniline-containing coating (ORMECON D1000, ORMECON CHEMIE Gmbh & Co. KG)
120 parts by mass of dipentaerythritol hexaacrylate (NK ester A-DPH, manufactured by Shin-Nakamura Chemical Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 10 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
N-methyl-2-pyrrolidone 200 parts by weight Example 3
(Preparation of antireflection film 3)
On the transparent film substrate 1 produced as described above, the conductive layer 3 and then the low refractive index layer 2 were applied in this order to produce the antireflection film 3.
(Formation of conductive layer 3)
The following conductive layer coating composition 3 is die-coated on the transparent film substrate 1, dried at 70 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.2 J / cm 2 to have a thickness of 5 μm. Layer 3 was provided. The refractive index of the conductive layer 3 was 1.51.
(Coating composition 3 for conductive layer)
18 parts by mass of tetracyanotetraazanaphthalene-doped polypyrrole solution (SSPY, manufactured by TA Chemical Co., Ltd.)
30 parts by mass of dipentaerythritol hexaacrylate (NK ester A-DPH, manufactured by Shin-Nakamura Chemical Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 4 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
N-methyl-2-pyrrolidone 70 parts by mass Further, a back coat layer was provided on the back side of the transparent film substrate 1 in the same manner as in Example 1.
(Formation of low refractive index layer 2)
The following coating composition 2 for a low refractive index layer is die-coated on the surface of the conductive layer 3, dried at 80 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.3 J / cm 2 to a thickness of 100 nm. A low refractive index layer 2 was provided so that an antireflection film 3 was produced. The refractive index of the low refractive index layer 2 was 1.39.
(Coating composition 2 for low refractive index layer)
30 parts by mass of a mixture of triacryloylheptadecafluorononenyl pentaerythritol and pentaerythritol tetraacrylate (LINC-3A, manufactured by Kyoeisha Chemical Co., Ltd.)
Antimony oxide-coated hollow silica particle dispersion 1 100 parts by mass 2-methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 5 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals Co., Ltd. )
300 parts by weight of methyl isobutyl ketone 300 parts by weight of methyl ethyl ketone (Preparation of antimony oxide-coated hollow silica particle dispersion 1)
A mixture of 100 g of silica sol having an average particle size of 5 nm and a SiO 2 concentration of 20% by mass and 1900 g of pure water was heated to 80 ° C. The pH of this reaction mother liquor was 10.5, and 9000 g of a 1.17 mass% sodium silicate aqueous solution as SiO 2 and 9000 g of a 0.83 mass% sodium aluminate aqueous solution as Al 2 O 3 were simultaneously added to the mother liquor. did. Meanwhile, the temperature of the reaction solution was kept at 80 ° C. The pH of the reaction solution rose to 12.5 immediately after the addition and hardly changed thereafter. After completion of the addition, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to prepare a SiO 2 .Al 2 O 3 core particle dispersion having a solid content concentration of 20% by mass. (Step d).

この核粒子分散液500gに純水1700gを加えて98℃に加温し、この温度を保持しながら、濃度0.5質量%の硫酸アンモニウム53200gを添加し、ついでSiO2として濃度1.17質量%のケイ酸ナトリウム水溶液3000gとAl23として濃度0.5質量%のアルミン酸ナトリウム水溶液9000gを添加して複合酸化物粒子1の分散液を得た。(工程e)。 1700 g of pure water was added to 500 g of this core particle dispersion and heated to 98 ° C., while maintaining this temperature, 53200 g of ammonium sulfate having a concentration of 0.5% by mass was added, and then SiO 2 having a concentration of 1.17% by mass. A dispersion of composite oxide particles 1 was obtained by adding 3000 g of an aqueous sodium silicate solution and 9000 g of an aqueous sodium aluminate solution having a concentration of 0.5% by mass as Al 2 O 3 . (Step e).

これを限外濾過膜で洗浄して固形分濃度13質量%になった複合酸化物粒子1の分散液500gに純水1125gを加え、さらに濃塩酸(濃度35.5質量%)を滴下してpH1.0とし、脱アルミニウム処理を行った。次いで、pH3の塩酸水溶液10Lと純水5Lを加えながら限外濾過膜で溶解したアルミニウム塩を分離して固形分濃度20質量%のシリカ系粒子分散液を得た。(工程f)。   1125 g of pure water was added to 500 g of the dispersion of composite oxide particles 1 having a solid content of 13% by mass by washing with an ultrafiltration membrane, and concentrated hydrochloric acid (concentration 35.5% by mass) was further added dropwise. The pH was adjusted to 1.0 and dealumination was performed. Subsequently, while adding 10 L of hydrochloric acid aqueous solution of pH 3 and 5 L of pure water, the aluminum salt dissolved in the ultrafiltration membrane was separated to obtain a silica-based particle dispersion having a solid concentration of 20% by mass. (Step f).

純水1800gに苛性カリ(旭硝子(株)製:純度85質量%)57gを溶解した溶液中に三酸化アンチモン(住友金属鉱山(株)製:KN 純度98.5質量%)111gを懸濁させた。この懸濁液を95℃に加熱し、次いで、過酸化水素水(林純薬(株)製:特級、純度35質量%)32.8gを純水110.7gで希釈した水溶液を9時間で添加(0.1mol/hr)し、三酸化アンチモンを溶解し、その後11時間熟成した。冷却後、得られた溶液から1000gを取り、この溶液を純水6000gで希釈した後、陽イオン交換樹脂に通して脱イオン処理を行った。このときのpHは2.1、電導度は2.4mS/cmであった。(工程g)。   111 g of antimony trioxide (manufactured by Sumitomo Metal Mining Co., Ltd .: KN purity 98.5 mass%) was suspended in a solution of 57 g of caustic potash (Asahi Glass Co., Ltd .: purity 85 mass%) dissolved in 1800 g of pure water. . This suspension was heated to 95 ° C., and then an aqueous solution obtained by diluting 32.8 g of hydrogen peroxide (produced by Hayashi Pure Chemical Co., Ltd .: special grade, purity 35% by mass) with 110.7 g of pure water was added in 9 hours. Added (0.1 mol / hr) to dissolve antimony trioxide, and then aged for 11 hours. After cooling, 1000 g was taken from the resulting solution, and this solution was diluted with 6000 g of pure water, and then passed through a cation exchange resin for deionization treatment. At this time, the pH was 2.1 and the conductivity was 2.4 mS / cm. (Step g).

上記で調製したシリカ系粒子分散液を、固形分濃度1質量%に希釈した分散液400gに、固形分濃度1質量%のアンチモン酸40gを加え、70℃で10時間攪拌し、限外濾過膜で濃縮し、固形分濃度20質量%の酸化アンチモン被覆シリカ系粒子(i)分散液を調製した。(工程h)。   40 g of antimonic acid with a solid content concentration of 1% by mass was added to 400 g of the dispersion solution prepared by diluting the silica-based particle dispersion prepared above to a solid content concentration of 1% by mass, and the mixture was stirred at 70 ° C. for 10 hours to obtain an ultrafiltration membrane. To obtain an antimony oxide-coated silica-based particle (i) dispersion having a solid concentration of 20% by mass. (Step h).

この酸化アンチモン被覆シリカ系粒子(i)分散液100gに、純水300gとメタノール400gを加え、これに正ケイ酸エチル(SiO2濃度28質量%)3.57gを混合し、50℃で15時間加熱攪拌してシリカ被覆層を形成した酸化アンチモン被覆シリカ系粒子(ii)分散液を調製した。この分散液を限外濾過膜を用いてメタノールに溶媒置換するとともに、固形分濃度20質量%になるまで濃縮した。次いで、ロータリーエバポレーターにてイソプロピルアルコールに溶媒置換して濃度20質量%のシリカ系粒子(ii)のイソプロピルアルコール分散液とした。(工程i)。 300 g of pure water and 400 g of methanol are added to 100 g of this antimony oxide-coated silica-based particle (i) dispersion, and 3.57 g of normal ethyl silicate (SiO 2 concentration: 28% by mass) is mixed therewith, and then at 50 ° C. for 15 hours. An antimony oxide-coated silica-based particle (ii) dispersion in which a silica coating layer was formed by heating and stirring was prepared. The dispersion was subjected to solvent substitution with methanol using an ultrafiltration membrane and concentrated to a solid content concentration of 20% by mass. Subsequently, the solvent was replaced with isopropyl alcohol by a rotary evaporator to obtain an isopropyl alcohol dispersion of silica-based particles (ii) having a concentration of 20% by mass. (Step i).

次いで、このシリカ被覆層を形成した酸化アンチモン被覆シリカ系粒子(ii)のイソプロピルアルコール分散液100gにメタクリル系シランカップリング剤(信越化学工業(株)製:KBM−503)0.73gを加え、50℃で15時間加熱攪拌し、シランカップリング剤により表面処理されたシリカ被覆層を形成した酸化アンチモン被覆シリカ系粒子分散液1を調製した。この粒子の屈折率は1.39、体積抵抗値は1500Ω/cm、平均粒子径は61nm、酸化アンチモン被覆層の厚さは1nmであった。
実施例4
(反射防止フィルム4の作製)
上記作製した透明フィルム基材2上に、下記のように導電層4、ついで、低屈折率層3の順に塗設し、反射防止フィルム4を作製した。
(導電層4の形成)
透明フィルム基材2上に、下記の導電層用塗布組成物4をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが5μmの導電層4を設けた。なお、この導電層4の屈折率は1.51であった。
(導電層用塗布組成物4)
ポリスチレンスルホン酸ドープポリ(3,4−エチレンジオキシチオフェン)溶液
18質量部
(BAYTRON P ET V2、H.C.Stark社製)
ジペンタエリスリトールヘキサアクリレート 30質量部
(NKエステルA−DPH、新中村化学工業株式会社製)
2−メチルー1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 3質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
エタノール 300質量部
さらに、実施例1と同様にして透明フィルム基材2の裏面側にバックコート層を設けた。
(低屈折率層3の形成)
上記導電層4の表面上に、下記低屈折率層用塗布組成物3をダイコートし、80℃で1分間乾燥させ、ついで紫外線を0.3J/cm2照射して硬化させて厚さが100nmとなるように低屈折率層3を設け、反射防止フィルム4を作製した。なお、この低屈折率層2の屈折率は1.38であった。
(低屈折率層用塗布組成物3)
トリアクリロイルヘプタデカフルオロノネニルペンタエリスリトールとペンタエリスリトールテトラアクリレートの混合物 30質量部
(LINC−3A、共栄社化学株式会社製)
フッ化マグネシウム粒子分散液1 150質量部
(MFANB15WT%−F16、シーアイ化成株式会社製)
2−メチル−1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 5質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
メチルイソブチルケトン 300質量部
メチルエチルケトン 300質量部
実施例5
(反射防止フィルム5の作製)
上記作製した透明フィルム基材1上に、下記のように導電層5、ついで、低屈折率層2の順に塗設し、反射防止フィルム5を作製した。
(導電層5の形成)
透明フィルム基材1上に、下記の導電層用塗布組成物5をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが5μmの導電層5を設けた。なお、この導電層5の屈折率は1.51であった。
(導電層用塗布組成物5)
ポリフェニルアセチレン 10質量部
ジペンタエリスリトールヘキサアクリレート 30質量部
(NKエステルA−DPH、新中村化学工業株式会社製)
2−メチルー1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 3質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
酢酸エチル 40質量部
プロピレングリコールモノメチルエーテル 60質量部
さらに、実施例1と同様にして透明フィルム基材2の裏面側にバックコート層を設けた。
実施例6
(反射防止フィルム6の作製)
上記作製した透明フィルム基材1上に、下記のようにハードコート層、導電層6、ついで、低屈折率層2の順に塗設し、反射防止フィルム6を作製した。
(ハードコート層の形成)
上記透明フィルム基材1に、下記のハードコート層用塗布組成物をダイコートし、80℃で乾燥の後、0.2J/cm2の紫外線を高圧水銀灯で照射して硬化させ、厚さ6μmのハードコート層を形成しハードコートフィルムを作製した。なお、このハードコートの屈折率は1.51であった。
(ハードコート層用塗布組成物)
ペンタエリスリトールトリアクリレート 30質量部
ペンタエリスリトールテトラアクリレート 45質量部
ウレタンアクリレート 25質量部
(U−4HA、新中村化学工業株式会社製)
1−ヒドロキシ−シクロヘキシル−フェニル−ケトン 5質量部
(イルガキュア184、チバスペシャルティケミカルズ株式会社製)
2−メチル−1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 3質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
ポリオキシエチレンオレイルエーテル 0.5質量部
(エマルゲン404、花王株式会社製)
プロピレングリコールモノメチルエーテル 10質量部
酢酸メチル 45質量部
アセトン 45質量部
さらに、実施例1と同様にして透明フィルム基材1の裏面側にバックコート層を設けた。
(導電層6の形成)
上記ハードコートフィルム1上に、ポリチオフェン含有多官能アクリレート塗剤(製品名:ELコートUVH−515、出光テクノファイン株式会社製)をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが0.2μmの導電層5を設けた。なお、この導電層6の屈折率は1.51であった。
(低屈折率層2の形成)
上記導電層6の表面上に、実施例3と同様にして低屈折率層2を設け、反射防止フィルム6を作製した。
実施例7
(反射防止フィルム7の作製)
上記作製した透明フィルム基材2上に、導電層用塗布組成物2と低屈折率層用塗布組成物3を使用して導電層と低屈折率層を形成した以外は実施例6と同様にして反射防止フィルム7を作製した。
実施例8
(反射防止フィルム8の作製)
上記作製した透明フィルム基材1上に、導電層用塗布組成物3と低屈折率層用塗布組成物1を使用して導電層と低屈折率層を形成した以外は実施例6と同様にして反射防止フィルム8を作製した。
実施例9
(反射防止フィルム9の作製)
上記作製した透明フィルム基材2上に、導電層用塗布組成物4と低屈折率層用塗布組成物1を使用して導電層と低屈折率層を形成した以外は実施例6と同様にして反射防止フィルム9を作製した。
(反射防止フィルム10の作製)
上記作製した透明フィルム基材1上に、導電層用塗布組成物5と低屈折率層用塗布組成物3を使用して導電層と低屈折率層を形成した以外は実施例6と同様にして反射防止フィルム10を作製した。
実施例11
(反射防止フィルム11の作製)
上記作製した透明フィルム基材1上に、実施例6と同様にしてハードコート層及びバックコート層を設け、下記導電層用塗布組成物7と低屈折率層用塗布組成物4を使用して導電層と低屈折率層を形成し、反射防止フィルム11を作製した。
(導電層7の形成)
ハードコート層上に、下記の導電層用塗布組成物7をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが0.2μmの導電層7を設けた。なお、この導電層7の屈折率は1.51であった。
(導電層用塗布組成物7)
ポリチオフェン含有多官能アクリレート塗剤 60質量部
(ELコートUVH−515、出光テクノファイン株式会社製)
3−アクリロキシプロピルトリメトキシシラン 15質量部
(KBM−5103、信越化学工業株式会社製)
2−メチルー1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 3質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
(低屈折率層4の形成)
上記の導電層7の表面上に、下記低屈折率層用塗布組成物4をダイコートし、80℃で1分間乾燥させ、ついで紫外線を0.1J/cm2照射して硬化させ、さらに120℃で1分間熱硬化させて厚さが100nmとなるように低屈折率層4を設け、反射防止フィルム11を作製した。なお、この低屈折率層4の屈折率は1.35であった。
(低屈折率層用塗布組成物4)
テトラエトキシシラン加水分解物1 90質量部
中空シリカ系粒子分散液1 30質量部
3−アクリロキシプロピルトリメトキシシラン 3質量部
(KBM−5103、信越化学工業株式会社製)
アルミニウムエチルアセトアセテートジイソプロピレート 1質量部
(ALCH、川研ファインケミカル株式会社製)
α−ブチル−ω−[3−(2,2−ビス(ヒドロキシメチル)ブトキシ)プロピル]ポリジメチルシロキサンの10%イソプロピルアルコール液 2質量部
(サイラプレーンFM−DA21、チッソ株式会社製)
プロピレングリコールモノメチルエーテル 450質量部
イソプロピルアルコール 450質量部
(テトラエトキシシラン加水分解物1の調製)
テトラエトキシシラン230gと、エタノール440gとを混和し、これに2%酢酸水溶液120gを添加した後、25℃のウォーターバス中で20時間攪拌することで、テトラエトキシシラン加水分解物1を調製した。
実施例12
(反射防止フィルム12の作製)
上記作製した透明フィルム基材2上に、下記低屈折率層用塗布組成物5を使用して低屈折率層を形成した以外は実施例11と同様にして反射防止フィルム12を作製した。
(低屈折率層用塗布組成物5)
テトラエトキシシラン加水分解物1 90質量部
酸化アンチモン被覆中空シリカ系粒子分散液1 30質量部
3−アクリロキシプロピルトリメトキシシラン 3質量部
(KBM−5103、信越化学工業株式会社製)
アルミニウムエチルアセトアセテートジイソプロピレート 1質量部
(ALCH、川研ファインケミカル株式会社製)
α−ブチル−ω−[3−(2,2−ビス(ヒドロキシメチル)ブトキシ)プロピル]ポリジメチルシロキサンの10%イソプロピルアルコール液 2質量部
(サイラプレーンFM−DA21、チッソ株式会社製)
プロピレングリコールモノメチルエーテル 450質量部
イソプロピルアルコール 450質量部
実施例13
(反射防止フィルム13の作製)
上記作製した透明フィルム基材1上に、下記低屈折率層用塗布組成物6を使用して低屈折率層を形成した以外は実施例11と同様にして反射防止フィルム13を作製した。
(低屈折率層用塗布組成物6)
テトラエトキシシラン加水分解物1 90質量部
フッ化マグネシウム粒子分散液1 45質量部
(MFANB15WT%−F16、シーアイ化成株式会社製)
3−アクリロキシプロピルトリメトキシシラン 3質量部
(KBM−5103、信越化学工業株式会社製)
アルミニウムエチルアセトアセテートジイソプロピレート 1質量部
(ALCH、川研ファインケミカル株式会社製)
α−ブチル−ω−[3−(2,2−ビス(ヒドロキシメチル)ブトキシ)プロピル]ポリジメチルシロキサンの10%イソプロピルアルコール液 2質量部
(サイラプレーンFM−DA21、チッソ株式会社製)
プロピレングリコールモノメチルエーテル 450質量部
イソプロピルアルコール 450質量部
実施例14
(反射防止フィルム14の作製)
上記作製した透明フィルム基材1上に、下記低屈折率層用塗布組成物7を使用して低屈折率層を形成した以外は実施例11と同様にして反射防止フィルム14を作製した。
(低屈折率層用塗布組成物7)
1%ポリシロキサン塗剤 100質量部
(LR−204−50C、日産化学工業株式会社製)
中空シリカ系粒子分散液1 5質量部
3−アクリロキシプロピルトリメトキシシラン 2質量部
(KBM−5103、信越化学工業株式会社製)
実施例15
(反射防止フィルム15の作製)
上記作製した透明フィルム基材2上に、下記低屈折率層用塗布組成物8を使用して低屈折率層を形成した以外は実施例11と同様にして反射防止フィルム15を作製した。
(低屈折率層用塗布組成物8)
1%ポリシロキサン塗剤 100質量部
(LR−204−50C、日産化学工業株式会社製)
酸化アンチモン被覆中空シリカ系粒子分散液1 5質量部
3−アクリロキシプロピルトリメトキシシラン 2質量部
(KBM−5103、信越化学工業株式会社製)
実施例16
(反射防止フィルム16の作製)
上記作製した透明フィルム基材1上に、下記低屈折率層用塗布組成物9を使用して低屈折率層を形成した以外は実施例11と同様にして反射防止フィルム16を作製した。
(低屈折率層用塗布組成物9)
1%ポリシロキサン塗剤 100質量部
(LR−204−50C、日産化学工業株式会社製)
フッ化マグネシウム粒子分散液1 8質量部
(MFANB15WT%−F16、シーアイ化成株式会社製)
3−アクリロキシプロピルトリメトキシシラン 2質量部
(KBM−5103、信越化学工業株式会社製)
実施例17
(反射防止フィルム17の作製)
上記作製した透明フィルム基材1上に、導電層6、ハードコート層、ついで、低屈折率層1の順に塗設し、反射防止フィルム17を作製した。
実施例18
(反射防止フィルム18の作製)
上記作製した透明フィルム基材2上に、低屈折率層用塗布組成物2を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム18を作製した。
実施例19
(反射防止フィルム19の作製)
上記作製した透明フィルム基材1上に、低屈折率層用塗布組成物3を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム19を作製した。
実施例20
(反射防止フィルム20の作製)
上記作製した透明フィルム基材2上に、低屈折率層用塗布組成物4を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム20を作製した。
実施例21
(反射防止フィルム21の作製)
上記作製した透明フィルム基材1上に、低屈折率層用塗布組成物5を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム21を作製した。
実施例22
(反射防止フィルム22の作製)
上記作製した透明フィルム基材2上に、低屈折率層用塗布組成物6を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム22を作製した。
実施例23
(反射防止フィルム23の作製)
上記作製した透明フィルム基材1上に、低屈折率層用塗布組成物7を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム23を作製した。
実施例24
(反射防止フィルム24作製)
上記作製した透明フィルム基材2上に、低屈折率層用塗布組成物8を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム24を作製した。
実施例25
(反射防止フィルム25の作製)
上記作製した透明フィルム基材1上に、低屈折率層用塗布組成物9を使用して低屈折率層を形成した以外は実施例17と同様にして反射防止フィルム25を作製した。
比較例1
(反射防止フィルム26の作製)
上記作製した透明フィルム基材1上に、下記のように導電層8、ついで、低屈折率層1の順に塗設し、反射防止フィルム26を作製した。
(導電層8の形成)
透明フィルム基材1上に、下記の導電層用塗布組成物8をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが5μmの導電層8を設けた。なお、この導電層8の屈折率は1.57であった。
(導電層用塗布組成物8)
イソプロパノール分散アンチモンドープ酸化スズゾル 30質量部
(ELCOM P−30、触媒化成工業株式会社製)
ジペンタエリスリトールヘキサアクリレート 80質量部
(NKエステルA−DPH、新中村化学工業株式会社製)
2−メチルー1−[4−(メチルチオ)フェニル]−2−モルフォリノプロパン−1−オン 3質量部
(イルガキュア907、チバスペシャルティケミカルズ株式会社製)
イソプロパノール 45質量部
メチルエチルケトン 45質量部
さらに、実施例1と同様にして透明フィルム基材1の裏面側にバックコート層を設け、導電層8上に低屈折率層1を設けて反射防止フィルム26を作製した。
比較例2
(反射防止フィルム27の作製)
上記作製した透明フィルム基材2上に、実施例6と同様にしてハードコート層及びバックコート層を設け、導電層用塗布組成物8と低屈折率層用塗布組成物1を使用して導電層9と低屈折率層1を形成し、反射防止フィルム27を作製した。
(導電層9の形成)
ハードコート層上に、導電層用塗布組成物8をダイコートし、70℃で1分間乾燥させ、ついで紫外線を0.2J/cm2照射して硬化させて厚さが0.1μmの導電層9を設けた。なお、この導電層9の屈折率は1.57であった。
比較例3
(反射防止フィルム28の作製)
上記作製した透明フィルム基材1上に、導電層用塗布組成物8と低屈折率層用塗布組成物10を使用して導電層9と低屈折率層10を形成した以外は実施例17と同様にして反射防止フィルム28を作製した。
(低屈折率層用塗布組成物10)
テトラエトキシシラン加水分解物1 95質量部
中空シリカ系粒子分散液1 30質量部
プロピレングリコールモノメチルエーテル 450質量部
イソプロピルアルコール 450質量部
比較例4
(反射防止フィルム29の作製)
上記作製した透明フィルム基材1上に、下記のように導電層10を気相反応にて形成し、ついで、実施例17と同様にしてハードコート層、及び低屈折率層1の順に塗設し、反射防止フィルム29を作製した。
(導電層10の形成)
酸化剤としてFeCl2を、メタノール、2−ブタノール、及びエチルセロソルブが6:3:1の割合で混合された溶媒に3質量%溶解させて触媒溶液を調製した。この触媒溶液を透明フィルム基材1上にスピンコートした後、得られた触媒塗膜を60℃で3分間乾燥させた。
Next, 0.73 g of a methacrylic silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd .: KBM-503) is added to 100 g of an isopropyl alcohol dispersion of antimony oxide-coated silica-based particles (ii) on which this silica coating layer has been formed, An antimony oxide-coated silica-based particle dispersion 1 in which a silica coating layer surface-treated with a silane coupling agent was formed by heating and stirring at 50 ° C. for 15 hours was prepared. The refractive index of this particle was 1.39, the volume resistance value was 1500 Ω / cm, the average particle size was 61 nm, and the thickness of the antimony oxide coating layer was 1 nm.
Example 4
(Preparation of antireflection film 4)
The antireflection film 4 was produced by coating the produced transparent film substrate 2 in the order of the conductive layer 4 and then the low refractive index layer 3 as described below.
(Formation of conductive layer 4)
The following conductive layer coating composition 4 is die-coated on the transparent film substrate 2, dried at 70 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.2 J / cm 2 to have a thickness of 5 μm. Layer 4 was provided. The conductive layer 4 had a refractive index of 1.51.
(Coating composition 4 for conductive layer)
Polystyrene sulfonic acid doped poly (3,4-ethylenedioxythiophene) solution
18 parts by mass (BAYTRON PET V2, manufactured by HC Stark)
30 parts by mass of dipentaerythritol hexaacrylate (NK ester A-DPH, manufactured by Shin-Nakamura Chemical Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 3 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
300 parts by mass of ethanol Further, a back coat layer was provided on the back side of the transparent film substrate 2 in the same manner as in Example 1.
(Formation of low refractive index layer 3)
The following coating composition 3 for low refractive index layer is die-coated on the surface of the conductive layer 4, dried at 80 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.3 J / cm 2 to a thickness of 100 nm. The low refractive index layer 3 was provided so that the antireflection film 4 was produced. The refractive index of the low refractive index layer 2 was 1.38.
(Coating composition 3 for low refractive index layer)
30 parts by mass of a mixture of triacryloylheptadecafluorononenyl pentaerythritol and pentaerythritol tetraacrylate (LINC-3A, manufactured by Kyoeisha Chemical Co., Ltd.)
Magnesium fluoride particle dispersion 1 150 parts by mass (MFANB15WT% -F16, manufactured by CI Kasei Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 5 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
300 parts by weight of methyl isobutyl ketone 300 parts by weight of methyl ethyl ketone Example 5
(Preparation of antireflection film 5)
On the transparent film substrate 1 produced as described above, the antireflection film 5 was produced by coating the conductive layer 5 and then the low refractive index layer 2 in this order.
(Formation of conductive layer 5)
The following conductive layer coating composition 5 is die-coated on the transparent film substrate 1, dried at 70 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.2 J / cm 2 to give a thickness of 5 μm. Layer 5 was provided. The refractive index of this conductive layer 5 was 1.51.
(Coating composition 5 for conductive layer)
10 parts by mass of polyphenylacetylene 30 parts by mass of dipentaerythritol hexaacrylate (NK ester A-DPH, manufactured by Shin-Nakamura Chemical Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 3 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
Ethyl acetate 40 parts by mass Propylene glycol monomethyl ether 60 parts by mass Further, a back coat layer was provided on the back side of the transparent film substrate 2 in the same manner as in Example 1.
Example 6
(Preparation of antireflection film 6)
On the transparent film substrate 1 produced as described above, a hard coat layer, a conductive layer 6 and then a low refractive index layer 2 were coated in this order to produce an antireflection film 6.
(Formation of hard coat layer)
The transparent film substrate 1 is die-coated with the following coating composition for hard coat layer, dried at 80 ° C., and then cured by irradiating 0.2 J / cm 2 of ultraviolet light with a high-pressure mercury lamp, and having a thickness of 6 μm A hard coat layer was formed to produce a hard coat film. The hard coat had a refractive index of 1.51.
(Coating composition for hard coat layer)
Pentaerythritol triacrylate 30 parts by mass Pentaerythritol tetraacrylate 45 parts by mass Urethane acrylate 25 parts by mass (U-4HA, manufactured by Shin-Nakamura Chemical Co., Ltd.)
1-hydroxy-cyclohexyl-phenyl-ketone 5 parts by mass (Irgacure 184, manufactured by Ciba Specialty Chemicals Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 3 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
0.5 parts by mass of polyoxyethylene oleyl ether (Emulgen 404, manufactured by Kao Corporation)
Propylene glycol monomethyl ether 10 parts by mass Methyl acetate 45 parts by mass Acetone 45 parts by mass Further, a back coat layer was provided on the back side of the transparent film substrate 1 in the same manner as in Example 1.
(Formation of conductive layer 6)
A polythiophene-containing polyfunctional acrylate coating (product name: EL coat UVH-515, manufactured by Idemitsu Technofine Co., Ltd.) is die-coated on the hard coat film 1 and dried at 70 ° C. for 1 minute, and then ultraviolet rays are 0.2 J. A conductive layer 5 having a thickness of 0.2 μm was provided by being cured by / cm 2 irradiation. The refractive index of the conductive layer 6 was 1.51.
(Formation of low refractive index layer 2)
On the surface of the conductive layer 6, the low refractive index layer 2 was provided in the same manner as in Example 3 to produce an antireflection film 6.
Example 7
(Preparation of antireflection film 7)
Except that the conductive layer and the low refractive index layer were formed on the produced transparent film substrate 2 using the conductive layer coating composition 2 and the low refractive index layer coating composition 3, the same procedure as in Example 6 was performed. Thus, an antireflection film 7 was produced.
Example 8
(Preparation of antireflection film 8)
Except that the conductive layer and the low refractive index layer were formed on the prepared transparent film substrate 1 using the conductive layer coating composition 3 and the low refractive index layer coating composition 1, the same manner as in Example 6 was performed. Thus, an antireflection film 8 was produced.
Example 9
(Preparation of antireflection film 9)
Except that the conductive layer and the low refractive index layer were formed on the prepared transparent film substrate 2 using the conductive layer coating composition 4 and the low refractive index layer coating composition 1, the same manner as in Example 6 was performed. Thus, an antireflection film 9 was produced.
(Preparation of antireflection film 10)
Except that the conductive layer and the low refractive index layer were formed on the prepared transparent film substrate 1 using the conductive layer coating composition 5 and the low refractive index layer coating composition 3, the same manner as in Example 6 was performed. Thus, an antireflection film 10 was produced.
Example 11
(Preparation of antireflection film 11)
A hard coat layer and a back coat layer were provided on the produced transparent film substrate 1 in the same manner as in Example 6, and the following conductive layer coating composition 7 and low refractive index layer coating composition 4 were used. A conductive layer and a low refractive index layer were formed to produce an antireflection film 11.
(Formation of conductive layer 7)
The following conductive layer coating composition 7 is die-coated on the hard coat layer, dried at 70 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.2 J / cm 2 to have a thickness of 0.2 μm. Layer 7 was provided. The refractive index of the conductive layer 7 was 1.51.
(Coating composition 7 for conductive layer)
60 parts by mass of polythiophene-containing polyfunctional acrylate coating (EL coat UVH-515, manufactured by Idemitsu Techno Fine Co., Ltd.)
15 parts by mass of 3-acryloxypropyltrimethoxysilane (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 3 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
(Formation of low refractive index layer 4)
On the surface of the conductive layer 7, the following coating composition 4 for a low refractive index layer is die-coated, dried at 80 ° C. for 1 minute, then cured by irradiation with ultraviolet rays of 0.1 J / cm 2 , and further 120 ° C. The antireflective film 11 was produced by providing the low refractive index layer 4 so as to have a thickness of 100 nm. The refractive index of the low refractive index layer 4 was 1.35.
(Coating composition 4 for low refractive index layer)
Tetraethoxysilane hydrolyzate 1 90 parts by mass Hollow silica-based particle dispersion 1 30 parts by mass 3-acryloxypropyltrimethoxysilane 3 parts by mass (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
1 part by mass of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemical Co., Ltd.)
α-Butyl-ω- [3- (2,2-bis (hydroxymethyl) butoxy) propyl] polydimethylsiloxane 10% isopropyl alcohol solution 2 parts by mass (Silaplane FM-DA21, manufactured by Chisso Corporation)
Propylene glycol monomethyl ether 450 parts by weight Isopropyl alcohol 450 parts by weight (Preparation of tetraethoxysilane hydrolyzate 1)
Tetraethoxysilane hydrolyzate 1 was prepared by mixing 230 g of tetraethoxysilane and 440 g of ethanol, adding 120 g of 2% aqueous acetic acid solution thereto, and then stirring in a water bath at 25 ° C. for 20 hours.
Example 12
(Preparation of antireflection film 12)
An antireflection film 12 was produced in the same manner as in Example 11 except that the low refractive index layer was formed on the produced transparent film substrate 2 using the following coating composition 5 for low refractive index layer.
(Coating composition 5 for low refractive index layer)
Tetraethoxysilane hydrolyzate 1 90 parts by mass Antimony oxide-coated hollow silica-based particle dispersion 1 30 parts by mass 3-acryloxypropyltrimethoxysilane 3 parts by mass (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
1 part by mass of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemical Co., Ltd.)
α-Butyl-ω- [3- (2,2-bis (hydroxymethyl) butoxy) propyl] polydimethylsiloxane 10% isopropyl alcohol solution 2 parts by mass (Silaplane FM-DA21, manufactured by Chisso Corporation)
Propylene glycol monomethyl ether 450 parts by weight Isopropyl alcohol 450 parts by weight Example 13
(Preparation of antireflection film 13)
An antireflection film 13 was produced in the same manner as in Example 11 except that a low refractive index layer was formed on the produced transparent film substrate 1 using the following coating composition 6 for low refractive index layer.
(Coating composition 6 for low refractive index layer)
Tetraethoxysilane hydrolyzate 1 90 parts by mass Magnesium fluoride particle dispersion 1 45 parts by mass (MFANB15WT% -F16, manufactured by CI Chemical Co., Ltd.)
3-Acryloxypropyltrimethoxysilane 3 parts by mass (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
1 part by mass of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemical Co., Ltd.)
α-Butyl-ω- [3- (2,2-bis (hydroxymethyl) butoxy) propyl] polydimethylsiloxane 10% isopropyl alcohol solution 2 parts by mass (Silaplane FM-DA21, manufactured by Chisso Corporation)
Propylene glycol monomethyl ether 450 parts by weight Isopropyl alcohol 450 parts by weight Example 14
(Preparation of antireflection film 14)
An antireflection film 14 was produced in the same manner as in Example 11 except that a low refractive index layer was formed on the produced transparent film substrate 1 using the following coating composition 7 for a low refractive index layer.
(Coating composition 7 for low refractive index layer)
1% polysiloxane coating agent 100 parts by mass (LR-204-50C, manufactured by Nissan Chemical Industries, Ltd.)
Hollow silica-based particle dispersion 1 5 parts by mass 3-acryloxypropyltrimethoxysilane 2 parts by mass (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
Example 15
(Preparation of antireflection film 15)
An antireflection film 15 was produced in the same manner as in Example 11 except that a low refractive index layer was formed on the produced transparent film substrate 2 using the following coating composition 8 for low refractive index layer.
(Coating composition 8 for low refractive index layer)
1% polysiloxane coating agent 100 parts by mass (LR-204-50C, manufactured by Nissan Chemical Industries, Ltd.)
Antimony oxide-coated hollow silica-based particle dispersion 1 5 parts by mass 3-acryloxypropyltrimethoxysilane 2 parts by mass (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
Example 16
(Preparation of antireflection film 16)
An antireflection film 16 was produced in the same manner as in Example 11 except that a low refractive index layer was formed on the produced transparent film substrate 1 using the following coating composition 9 for low refractive index layer.
(Coating composition 9 for low refractive index layer)
1% polysiloxane coating agent 100 parts by mass (LR-204-50C, manufactured by Nissan Chemical Industries, Ltd.)
Magnesium fluoride particle dispersion 1 8 parts by mass (MFANB15WT% -F16, manufactured by CI Kasei Co., Ltd.)
2-Acryloxypropyltrimethoxysilane 2 parts by mass (KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.)
Example 17
(Preparation of antireflection film 17)
On the transparent film substrate 1 produced as described above, an antireflection film 17 was produced by coating the conductive layer 6, the hard coat layer, and then the low refractive index layer 1 in this order.
Example 18
(Preparation of antireflection film 18)
An antireflection film 18 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 2 using the coating composition 2 for low refractive index layer.
Example 19
(Preparation of antireflection film 19)
An antireflection film 19 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 1 using the coating composition 3 for low refractive index layer.
Example 20
(Preparation of antireflection film 20)
An antireflection film 20 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 2 using the coating composition 4 for low refractive index layer.
Example 21
(Preparation of antireflection film 21)
An antireflection film 21 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 1 using the coating composition 5 for low refractive index layer.
Example 22
(Preparation of antireflection film 22)
An antireflection film 22 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 2 using the coating composition 6 for low refractive index layer.
Example 23
(Preparation of antireflection film 23)
An antireflection film 23 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 1 using the coating composition 7 for low refractive index layer.
Example 24
(Preparation of antireflection film 24)
An antireflection film 24 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 2 using the coating composition 8 for low refractive index layer.
Example 25
(Preparation of antireflection film 25)
An antireflection film 25 was produced in the same manner as in Example 17 except that the low refractive index layer was formed on the produced transparent film substrate 1 using the coating composition 9 for low refractive index layer.
Comparative Example 1
(Preparation of antireflection film 26)
On the transparent film substrate 1 produced as described above, the conductive layer 8 and then the low refractive index layer 1 were applied in the following order to produce an antireflection film 26.
(Formation of conductive layer 8)
The following conductive layer coating composition 8 is die-coated on the transparent film substrate 1, dried at 70 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.2 J / cm 2 to give a thickness of 5 μm. Layer 8 was provided. The conductive layer 8 had a refractive index of 1.57.
(Coating composition 8 for conductive layer)
30 parts by mass of isopropanol-dispersed antimony-doped tin oxide sol (ELCOM P-30, manufactured by Catalyst Kasei Kogyo Co., Ltd.)
80 parts by mass of dipentaerythritol hexaacrylate (NK ester A-DPH, manufactured by Shin-Nakamura Chemical Co., Ltd.)
2-Methyl-1- [4- (methylthio) phenyl] -2-morpholinopropan-1-one 3 parts by mass (Irgacure 907, manufactured by Ciba Specialty Chemicals)
45 parts by mass of isopropanol 45 parts by mass of methyl ethyl ketone Further, in the same manner as in Example 1, a back coat layer was provided on the back side of the transparent film substrate 1, and a low refractive index layer 1 was provided on the conductive layer 8 to provide an antireflection film 26. Produced.
Comparative Example 2
(Preparation of antireflection film 27)
A hard coat layer and a back coat layer are provided on the produced transparent film substrate 2 in the same manner as in Example 6, and conductive using the conductive layer coating composition 8 and the low refractive index layer coating composition 1. Layer 9 and low refractive index layer 1 were formed, and antireflection film 27 was produced.
(Formation of conductive layer 9)
A conductive layer coating composition 8 is die-coated on the hard coat layer, dried at 70 ° C. for 1 minute, and then cured by irradiation with ultraviolet rays of 0.2 J / cm 2 to form a conductive layer 9 having a thickness of 0.1 μm. Was provided. The conductive layer 9 had a refractive index of 1.57.
Comparative Example 3
(Preparation of antireflection film 28)
Example 17 except that the conductive layer 9 and the low refractive index layer 10 were formed on the produced transparent film substrate 1 using the conductive layer coating composition 8 and the low refractive index layer coating composition 10. Similarly, an antireflection film 28 was produced.
(Coating composition 10 for low refractive index layer)
Tetraethoxysilane hydrolyzate 1 95 parts by mass Hollow silica-based particle dispersion 1 30 parts by mass Propylene glycol monomethyl ether 450 parts by mass Isopropyl alcohol 450 parts by mass Comparative Example 4
(Preparation of antireflection film 29)
On the transparent film substrate 1 produced as described above, the conductive layer 10 was formed by a gas phase reaction as described below, and then the hard coat layer and the low refractive index layer 1 were applied in the same manner as in Example 17. Thus, an antireflection film 29 was produced.
(Formation of conductive layer 10)
A catalyst solution was prepared by dissolving 3% by mass of FeCl 2 as an oxidizing agent in a solvent in which methanol, 2-butanol, and ethyl cellosolve were mixed at a ratio of 6: 3: 1. After spin-coating this catalyst solution on the transparent film substrate 1, the obtained catalyst coating film was dried at 60 ° C. for 3 minutes.

ついで、この触媒塗膜が形成された基材フィルムを、飽和状態の3,4−エチレンジオキシチオフェン単量体が生成されるように設計されたCVDチャンバーに設置して30秒間気相重合反応させた後、未反応物を除去するためにメタノールで洗浄し、導電層10を作製した。
(評価方法)
上記のようにして作製した反射防止フィルム1〜29の試料について、下記方法により評価した。得られた結果を、下記の表1にまとめて示した。
(防塵性)
反射防止フィルムの帯電防止性能の評価として、反射防止フィルムのバックコート側をCRT表面に貼り付け、0.5μm以上のホコリ及びティッシュペーパー屑を1ft3あたり100〜200万個有する部屋で24時間使用した。その後、表面100cm2あたり、付着したホコリとティッシュペーパー屑の数を測定し、10個未満を◎、20個未満を○、20〜49個を△、50〜199個を×、200個以上を××として評価した。20個未満であれば実用上問題ないが、10個未満がより好ましい。
(ヘイズ)
JIS K−7361−1に準拠して、濁度計NDH2000(日本電色製)を用いて、得られた反射防止フィルムのヘイズを測定した。
(反射色相の測定)
分光光度計V−550(日本分光製)を用いて、標準C光源にて2度視野で測定し、反射色相x、y値を算出した。その後、(x、y)=(0.31、0.31)からの距離Δxyを算出し、反射防止フィルムの色味を評価した。Δxyが大きいほど反射防止フィルムの色味がきつく好ましくない。Δxyが0.05以下であれば実用上問題ないが、0.03以下がより好ましい。
(密着性)
反射防止フィルムを、温度60℃、湿度95%RHで1000時間保持した後、JIS K5600−5−6に準拠して、碁盤目テープ剥離試験を行った。試料表面にカッターで切り込みを入れて100個のマス目をつくり、粘着テープ(日東電工製No.31B)を圧着してから剥離することを同じ場所で3回繰り返して行った。その後、テープ剥離後の試料表面を目視観察し、以下の基準で評価を行った。
Next, the base film on which this catalyst coating film was formed was placed in a CVD chamber designed to produce a saturated 3,4-ethylenedioxythiophene monomer, and a gas phase polymerization reaction was performed for 30 seconds. Then, in order to remove unreacted substances, the conductive layer 10 was produced by washing with methanol.
(Evaluation methods)
The samples of the antireflection films 1 to 29 produced as described above were evaluated by the following methods. The obtained results are summarized in Table 1 below.
(Dustproof)
As an evaluation of the antistatic performance of the antireflection film, the back coat side of the antireflection film is attached to the CRT surface, and used in a room having 1 to 2 million pieces of dust and tissue paper scraps of 0.5 μm or more per 1 ft 3. did. Thereafter, the number of adhering dust and tissue paper waste is measured per 100 cm 2 of the surface, less than 10 ◎, less than 20 ○, 20 to 49 Δ, 50 to 199 ×, 200 or more XX was evaluated. If it is less than 20, there is no practical problem, but less than 10 is more preferable.
(Haze)
Based on JIS K-7361-1, the haze of the obtained antireflection film was measured using a turbidimeter NDH2000 (manufactured by Nippon Denshoku).
(Measurement of reflection hue)
Using a spectrophotometer V-550 (manufactured by JASCO), measurement was performed twice with a standard C light source, and the reflection hue x and y values were calculated. Thereafter, a distance Δxy from (x, y) = (0.31, 0.31) was calculated, and the color of the antireflection film was evaluated. As Δxy is larger, the color of the antireflection film is not preferable. If Δxy is 0.05 or less, there is no practical problem, but 0.03 or less is more preferable.
(Adhesion)
After holding the antireflection film at a temperature of 60 ° C. and a humidity of 95% RH for 1000 hours, a cross-cut tape peeling test was performed in accordance with JIS K5600-5-6. The sample surface was cut with a cutter to make 100 squares, and pressure-sensitive adhesive tape (Nitto Denko No. 31B) was pressed and then peeled off at the same place three times. Then, the sample surface after tape peeling was observed visually, and the following references | standards evaluated.

密着性評価基準
○:全く剥離しない
△:剥離が認められる
×:全面剥離する
Evaluation criteria for adhesion ○: No peeling at all △: Peeling is observed ×: Peeling over the entire surface

Figure 2009036817
Figure 2009036817

上記表1の結果から明らかなように、本発明による実施例1〜25の反射防止フィルムは、比較例1〜4の反射防止フィルムに比べ、防塵性(帯電防止性)、透明性、色付き、密着性及び高温高湿に対する耐久性が良好であることが分かる。
実施例26
つぎに、実施例1〜25、及び比較例1〜4で作製した各反射防止フィルム1〜29と、セルロースエステル系光学補償フィルムであるKC4FR−1(コニカミノルタオプト株式会社製)の各々1枚を、偏光板用保護フィルムとして用いて、偏光板101〜125及び比較用偏光板126〜129を作製した。
(偏光フィルムの作製)
けん化度99.95モル%、重合度2400のポリビニルアルコール(以下PVAと略す)100質量部に、グリセリン10質量部及び水170質量部を含浸させたものを溶融混錬し、脱泡後、Tダイから金属ロール上に溶融押し出しし、製膜した。その後、乾燥、熱処理してPVAフィルムを得た。得られたPVAフィルムは平均厚みが40μm、水分率が4.4%、フィルム幅が3mであった。
As is clear from the results of Table 1 above, the antireflection films of Examples 1 to 25 according to the present invention are dustproof (antistatic), transparent, colored, compared to the antireflection films of Comparative Examples 1 to 4. It can be seen that the adhesion and durability against high temperature and high humidity are good.
Example 26
Next, each one of antireflection films 1 to 29 produced in Examples 1 to 25 and Comparative Examples 1 to 4, and KC4FR-1 (manufactured by Konica Minolta Opto Co., Ltd.) which is a cellulose ester optical compensation film. Were used as a protective film for polarizing plates, and polarizing plates 101 to 125 and comparative polarizing plates 126 to 129 were produced.
(Preparation of polarizing film)
100 mass parts of polyvinyl alcohol (hereinafter abbreviated as PVA) having a saponification degree of 99.95 mol% and a polymerization degree of 2400 were melt-kneaded with 10 mass parts of glycerin and 170 mass parts of water, and after degassing, T The film was melt-extruded from a die onto a metal roll to form a film. Then, it dried and heat-processed and obtained the PVA film. The obtained PVA film had an average thickness of 40 μm, a moisture content of 4.4%, and a film width of 3 m.

このPVAフィルムを予備膨潤、染色、湿式法による一軸延伸、固定処理、乾燥、熱処理の順番で連続的に処理して偏光フィルムを作製した。   This PVA film was continuously processed in the order of pre-swelling, dyeing, uniaxial stretching by a wet method, fixing treatment, drying, and heat treatment to prepare a polarizing film.

すなわち、上記のPVAフィルムを、30℃の水中に30秒間浸して予備膨潤し、ヨウ素濃度0.4g/L、ヨウ化カリウム濃度40g/Lの35℃の水溶液中に3分間浸した。ついで、ホウ酸濃度4%の50℃の水溶液中でフィルムにかかる張力が700N/mの条件下で6倍に一軸延伸を行い、ヨウ化カリウム濃度40g/L、ホウ酸濃度40g/L、塩化亜鉛濃度10g/Lの30℃の水溶液中に5分間浸して固定処理を行った。その後、PVAフィルムを取り出し、40℃で熱風乾燥し、さらに100℃で5分間熱処理を行った。得られた偏光フィルムは平均厚みは、15μmであった。
(偏光板の作製)
ついで、下記の工程1〜工程5に従って、偏光フィルムと偏光板用保護フィルムとを貼り合わせて、偏光板101〜129を作製した。
That is, the PVA film was immersed in 30 ° C. water for 30 seconds and pre-swelled, and then immersed in an aqueous solution at 35 ° C. having an iodine concentration of 0.4 g / L and a potassium iodide concentration of 40 g / L for 3 minutes. Next, the film was uniaxially stretched 6 times under the condition that the tension applied to the film was 700 N / m in a 50 ° C. aqueous solution having a boric acid concentration of 4%, a potassium iodide concentration of 40 g / L, a boric acid concentration of 40 g / L, The fixing treatment was performed by immersing in an aqueous solution having a zinc concentration of 10 g / L at 30 ° C for 5 minutes. Thereafter, the PVA film was taken out, dried with hot air at 40 ° C., and further subjected to heat treatment at 100 ° C. for 5 minutes. The obtained polarizing film had an average thickness of 15 μm.
(Preparation of polarizing plate)
Subsequently, according to the following process 1-process 5, the polarizing film and the protective film for polarizing plates were bonded together, and the polarizing plates 101-129 were produced.

工程1:光学補償フィルムと反射防止フィルムを2mol/Lの水酸化ナトリウム溶液に、温度60℃で、90秒間浸漬し、ついで水洗、乾燥させた。反射防止フィルムの反射防止層を設けた面には、予め剥離性の保護フィルム(PET製)を張り付けて保護した。   Step 1: The optical compensation film and the antireflection film were immersed in a 2 mol / L sodium hydroxide solution at a temperature of 60 ° C. for 90 seconds, then washed with water and dried. The surface of the antireflection film provided with the antireflection layer was previously protected with a peelable protective film (PET).

工程2:ついで、偏光フィルムを、固形分2質量%のポリビニルアルコール接着剤槽中に1〜2秒間浸漬した。   Step 2: Next, the polarizing film was immersed in a polyvinyl alcohol adhesive tank having a solid content of 2% by mass for 1 to 2 seconds.

工程3:工程2で偏光フィルムに付着した過剰の接着剤を軽く取り除き、それを工程1でアルカリ処理した光学補償フィルムと反射防止フィルムで挟み込んで、積層配置した。   Step 3: Excess adhesive adhered to the polarizing film in Step 2 was lightly removed, and it was sandwiched between the optical compensation film and the antireflection film that had been subjected to alkali treatment in Step 1 and laminated.

工程4:2つの回転するローラにて20〜30N/cm2の圧力で約2m/minの速度で張り合わせた。 Process 4: It bonded together at the speed | rate of about 2 m / min with the pressure of 20-30 N / cm < 2 > with the two rotating rollers.

工程5:80℃の乾燥機中にて、工程4で作製した試料を2分間乾燥処理し、偏光板を作製した。
(試験用液晶表示パネルの作製)
ついで、市販の液晶表示パネル(VA型)の最表面の偏光板を注意深く剥離し、ここに上記作製した反射防止フィルムを用いた偏光板101〜129を張り付けた。
Step 5: The sample prepared in Step 4 was dried for 2 minutes in a dryer at 80 ° C. to prepare a polarizing plate.
(Production of liquid crystal display panel for testing)
Next, the polarizing plate on the outermost surface of a commercially available liquid crystal display panel (VA type) was carefully peeled off, and polarizing plates 101 to 129 using the prepared antireflection film were attached thereto.

上記のようにして得られた液晶パネル201〜229を床から80cmの高さの机上に配置し、床から3mの高さの天井部に昼色光直管蛍光灯(FLR40S・D/M−X松下電器産業株式会社製)40W×2本を1セットとして1.5m間隔で10セット配置した。   The liquid crystal panels 201 to 229 obtained as described above are arranged on a desk 80 cm high from the floor, and a daylight direct fluorescent lamp (FLR40S · D / MX) is placed on the ceiling 3 m high from the floor. Matsushita Electric Industrial Co., Ltd.) 10 sets of 40W × 2 were set as one set at intervals of 1.5 m.

ここで、評価者が液晶パネル表示面正面にいるときに、評価者の頭上より後方に向けて天井部に前記蛍光灯がくるように配置した。液晶パネルは机に対する垂直方向から25°傾けて蛍光灯が写り込むようにして画面の見易さ(視認性)を下記のようにランク評価した。   Here, when the evaluator is in front of the liquid crystal panel display surface, the fluorescent lamp is arranged so that the fluorescent lamp comes to the ceiling portion from the evaluator's overhead to the rear. The liquid crystal panel was tilted by 25 ° from the vertical direction with respect to the desk, and a fluorescent lamp was reflected so that the visibility of the screen (visibility) was evaluated as follows.

A:最も近い蛍光灯の写り込みから気にならず、フォントの大きさ8以下の文字もはっきりと読める
B:近くの蛍光灯の写り込みはやや気になるが、遠くは気にならず、フォントの大きさ8以下の文字もなんとかと読める
C:遠くの蛍光灯の写り込みも気になり、フォントの大きさ8以下の文字を読むのは困難である
D:蛍光灯の写り込みがかなり気になり、写り込みの部分はフォントの大きさ8以下の文字を読むことはできない
評価の結果、本発明の反射防止フィルム1〜25、及び偏光板101〜125を用いた液晶パネル201〜225はいずれもB以上の評価結果であり、比較の液晶パネル226〜229より視認性が良好であった。特に、本発明によるπ共役系導電性ポリマーと電離放射線硬化型樹脂を導電層に含有させた反射防止フィルムを用いた液晶パネルのランクは、いずれも視認性評価がAであった。
A: I don't mind from the reflection of the nearest fluorescent lamp, and I can clearly read characters with a font size of 8 or less. B: The reflection of the nearby fluorescent lamp is a little worrisome, but I don't care about the distance. Can manage to read characters with a font size of 8 or less C: It is difficult to read characters with a font size of 8 or less. Anxious, the portion of the reflection can not read the characters of the font size of 8 or less As a result of the evaluation, the liquid crystal panels 201-225 using the antireflection films 1-25 of the present invention and the polarizing plates 101-125 Are evaluation results of B or more, and visibility was better than comparative liquid crystal panels 226 to 229. In particular, all of the ranks of the liquid crystal panels using the antireflection film containing the π-conjugated conductive polymer according to the present invention and the ionizing radiation curable resin in the conductive layer had a visibility evaluation of A.

Claims (11)

透明フィルム基材上に、導電層と、基材よりも屈折率の低い低屈折率層が、直接または他の層を介してこの順に塗設された反射防止フィルムであって、前記導電層がπ共役系導電性ポリマーと電離放射線硬化型樹脂を含有することを特徴とする反射防止フィルム。 An antireflection film in which a conductive layer and a low refractive index layer having a refractive index lower than that of the base material are coated on the transparent film base material in this order, directly or via another layer, and the conductive layer is An antireflection film comprising a π-conjugated conductive polymer and an ionizing radiation curable resin. 前記π共役系導電性ポリマーが、ポリチオフェン誘導体、ポリピロール誘導体、ポリアニリン誘導体、ポリアセチレン誘導体のうちの、少なくとも1種であることを特徴とする請求項1に記載の反射防止フィルム。 The antireflection film according to claim 1, wherein the π-conjugated conductive polymer is at least one of a polythiophene derivative, a polypyrrole derivative, a polyaniline derivative, and a polyacetylene derivative. 前記電離放射線硬化型樹脂が、分子中に重合可能な不飽和結合を2個以上有するアクリル系化合物を含有することを特徴とする請求項1又は2に記載の反射防止フィルム。 3. The antireflection film according to claim 1, wherein the ionizing radiation curable resin contains an acrylic compound having two or more polymerizable unsaturated bonds in the molecule. 前記導電層が、下記一般式(1)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物を含有することを特徴とする請求項1乃至3の何れか1項に記載の反射防止フィルム。
1 nSiX1 4-n (1)
式中、R1は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X1は水酸基または加水分解可能な置換基であり、nは1〜3の整数である。
4. The reflection according to claim 1, wherein the conductive layer contains an organosilicon compound represented by the following general formula (1), a hydrolyzate thereof, or a polycondensate thereof. Prevention film.
R 1 n SiX 1 4-n (1)
In the formula, R 1 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 1 is a hydroxyl group or a hydrolyzable substituent, and n is an integer of 1 to 3.
前記低屈折率層が、コロイダルシリカ、フッ化マグネシウム、及び外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子よりなる群の中から選ばれた少なくとも1種の無機粒子を含有することを特徴とする請求項1乃至4の何れか1項に記載の反射防止フィルム。 The low refractive index layer comprises at least one inorganic particle selected from the group consisting of colloidal silica, magnesium fluoride, and hollow silica-based particles having an outer shell layer and the inside being porous or hollow. The antireflection film according to claim 1, wherein the antireflection film is contained. 外殻層を有しかつ内部が多孔質または空洞である前記中空シリカ系粒子が、導電性金属酸化物被覆層を有することを特徴とする、請求項5に記載の反射防止フィルム。 6. The antireflection film according to claim 5, wherein the hollow silica-based particles having an outer shell layer and having a porous or hollow interior have a conductive metal oxide coating layer. 前記導電性金属酸化物被覆層が、酸化アンチモン化合物からなることを特徴とする請求項6に記載の反射防止フィルム。 The antireflection film according to claim 6, wherein the conductive metal oxide coating layer is made of an antimony oxide compound. 前記低屈折率層が、下記一般式(2)で表される有機珪素化合物もしくはその加水分解物あるいはその重縮合物と、外殻層を有しかつ内部が多孔質または空洞である中空シリカ系粒子とを含有することを特徴とする、請求項1乃至7の何れか1項に記載の反射防止フィルム。
2 mSiX2 4-m (2)
式中、R2は置換もしくは無置換のアルキル基、または置換もしくは無置換のアリール基、X2は水酸基または加水分解可能な置換基であり、mは0〜3の整数である。
A hollow silica system in which the low refractive index layer has an organosilicon compound represented by the following general formula (2) or a hydrolyzate or polycondensate thereof, and an outer shell layer and is porous or hollow inside The antireflection film according to claim 1, further comprising particles.
R 2 m SiX 2 4-m (2)
In the formula, R 2 is a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, X 2 is a hydroxyl group or a hydrolyzable substituent, and m is an integer of 0 to 3.
前記低屈折率層が、バインダーとの反応性を有する基を少なくとも1つ含むシリコーン化合物を含有することを特徴とする請求項1乃至8の何れか1項に記載の反射防止フィルム。 The antireflective film according to any one of claims 1 to 8, wherein the low refractive index layer contains a silicone compound containing at least one group having reactivity with a binder. 請求項1乃至9の何れか1項に記載の反射防止フィルムを一方の面に用いることを特徴とする偏光板。 A polarizing plate using the antireflection film according to claim 1 on one surface. 請求項1乃至9の何れか1項に記載の反射防止フィルム又は請求項10に記載の偏光板を用いることを特徴とする画像表示装置。 An image display apparatus comprising the antireflection film according to claim 1 or the polarizing plate according to claim 10.
JP2007198716A 2007-07-31 2007-07-31 Antireflective coating, and polarizing plate and image display device using the same Pending JP2009036817A (en)