JP2006007699A - Printing plate material and image forming method - Google Patents

Printing plate material and image forming method Download PDF

Info

Publication number
JP2006007699A
JP2006007699A JP2004191111A JP2004191111A JP2006007699A JP 2006007699 A JP2006007699 A JP 2006007699A JP 2004191111 A JP2004191111 A JP 2004191111A JP 2004191111 A JP2004191111 A JP 2004191111A JP 2006007699 A JP2006007699 A JP 2006007699A
Authority
JP
Japan
Prior art keywords
printing plate
image forming
plate material
image
layer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2004191111A
Other languages
Japanese (ja)
Inventor
Tomonori Kawamura
朋紀 河村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Konica Minolta Medical and Graphic Inc
Original Assignee
Konica Minolta Medical and Graphic Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Konica Minolta Medical and Graphic Inc filed Critical Konica Minolta Medical and Graphic Inc
Priority to JP2004191111A priority Critical patent/JP2006007699A/en
Publication of JP2006007699A publication Critical patent/JP2006007699A/en
Pending legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To provide a printing plate material which facilitates the confirmation of an exposed image and is excellent in press developabilities, and an image forming method. <P>SOLUTION: In a negative type printing plate material having an on printing press developable thermosensitive image forming layer on a hydrophilically surfaced base material, (a) the visible light reflection density of the hydrophilic surface is at least 0.5, (b) a visible image imparting layer, which decreases the visible light reflection density of an exposed part than the visible light reflection density of an unexposed part by at least 0.2 under the exposure condition for exposing with the energy quantity of 400 mJ/cm<SP>2</SP>by an infrared laser light having a peak maximum wavelength of 830 nm, is provided on the thermosensitive image forming layer side. <P>COPYRIGHT: (C)2006,JPO&NCIPI

Description

本発明は印刷版材料及びその画像形成方法に関し、特にコンピューター・トゥー・プレート(CTP)方式により画像形成が可能な印刷版材料及び画像形成方法に関する。   The present invention relates to a printing plate material and an image forming method thereof, and more particularly to a printing plate material and an image forming method capable of forming an image by a computer-to-plate (CTP) method.

現在、印刷の分野においては、印刷画像データのデジタル化に伴い、CTP方式による印刷が行われるようになってきているが、この印刷においては、安価で取り扱いが容易で従来の所謂PS版と同等の印刷適性を有したCTP方式用印刷版材料が求められている。   At present, in the field of printing, printing by the CTP method has been performed with the digitization of print image data. However, this printing is inexpensive and easy to handle and is equivalent to a conventional so-called PS plate. Therefore, there is a demand for a printing plate material for a CTP system having the following printability.

特に近年、特別な薬剤(例えばアルカリ、酸、溶媒など)を含む処理液による現像処理を必要とせず、従来の印刷機に適用可能である印刷版材料が求められており、例えば、全く現像処理を必要としない相変化タイプの印刷版材料、水もしくは水を主体とした実質的に中性の処理液で処理をする印刷版材料、印刷機上で印刷の初期段階で現像処理を行い特に現像工程を必要としない印刷版材料などの、ケミカルフリータイプ印刷版材料やプロセスレスタイプ印刷版材料と呼ばれる印刷版材料が知られている。   In particular, in recent years, there has been a demand for a printing plate material that does not require development processing using a processing solution containing a special agent (for example, alkali, acid, solvent, etc.) and can be applied to a conventional printing machine. Phase change type printing plate material that does not require water, printing plate material that is processed with water or a substantially neutral processing liquid mainly composed of water, and development processing is performed at an initial stage of printing on a printing press. There are known printing plate materials called chemical-free type printing plate materials and processless type printing plate materials, such as printing plate materials that do not require a process.

上記の全く現像処理を必要としない印刷版材料や印刷機上で現像を行うプロセスレスタイプの印刷版材料においても、印刷機に取り付ける際に必要なパンチングを露光後に行うため、従来のPSと同様に所謂露光可視画性をもつことが必要とされている。   The above-described printing plate materials that do not require any development processing and processless type printing plate materials that are developed on a printing press perform punching necessary for attachment to the printing press after exposure, so that they are the same as conventional PS In addition, it is required to have so-called exposure visible image quality.

また、プロセスレスタイプの印刷版材料の画像形成に主として用いられるのは近赤外〜赤外線の波長を有するサーマルレーザー記録方式であり、この方式で画像形成可能なサーマルプロセスレスプレートには、大きく分けて、アブレーションタイプと熱融着画像層機上現像タイプ、および相変化タイプが知られている。   In addition, the thermal laser recording method having a wavelength of near infrared to infrared is mainly used for image formation of processless type printing plate materials. The thermal processless plate that can form an image by this method is roughly divided. An ablation type, a heat fusion image layer on-machine development type, and a phase change type are known.

一方これらのプロセスレスタイプの印刷版材料に露光可視画性を持たせた印刷版材料として以下の印刷版材料が知られている。   On the other hand, the following printing plate materials are known as printing plate materials obtained by imparting exposure visibility to these processless type printing plate materials.

例えば、画像形成層中にロイコ色素とその顕色剤といったような感熱発色する素材を含有させた層や、熱によってスルホン酸を発生する官能基を有する高分子化合物および発生した酸によって変色する化合物とを含有する親油層、を有する印刷版材料(特許文献1、2参照)、画像形成要素の露出によりその光学濃度を変化させることができるIR−色素を含有する層を有する印刷版材料(特許文献3参照)、露光によって光学濃度を変化させることのできるシアニン系赤外線吸収色素を20質量%以上含有させた、印刷機上で除去可能な親水性オーバーコート層を有する印刷版材料(特許文献4参照)が知られている。   For example, a layer containing a heat-sensitive coloring material such as a leuco dye and its developer in the image forming layer, a polymer compound having a functional group that generates sulfonic acid by heat, and a compound that changes color by the generated acid A printing plate material having a layer containing an IR-dye that can change its optical density by exposure of an imaging element (Patent Documents 1 and 2) Reference 3), a printing plate material having a hydrophilic overcoat layer that can be removed on a printing press, containing 20% by mass or more of a cyanine infrared absorbing dye whose optical density can be changed by exposure (Patent Document 4) See).

しかしながら、これらの印刷版材料においては、露光により発色あるいは退色、変色する色素を含有するため、機上現像において、これらの色素による印刷インキ、湿し水に対する汚染を避けるのは困難であり、機上現像時に正常な印刷物を得るまでに要する損紙の量が多い場合あるといった問題があった。   However, since these printing plate materials contain dyes that develop, fade, or change color upon exposure, it is difficult to avoid contamination of the printing ink and fountain solution by these dyes during on-machine development. There has been a problem that the amount of damaged paper required for obtaining a normal printed matter at the time of top development may be large.

また、これらの印刷版材料では、充分な露光可視画性を得ようとすると印刷版材料の感度、機上現像性が不充分となり、印刷適性と露光可視画性を両立させるのは困難であった。
特開2000−225780号公報 特開2002−211150号公報 特開平11−240270号公報 特開2002−205466号公報
In addition, in these printing plate materials, if sufficient exposure visible image properties are obtained, the sensitivity of the printing plate materials and on-machine developability are insufficient, and it is difficult to achieve both printability and exposure visible image properties. It was.
JP 2000-225780 A Japanese Patent Laid-Open No. 2002-211150 JP-A-11-240270 JP 2002-205466 A

本発明の目的は、露光画像の確認が容易で、機上現像性に優れる印刷版材料及び画像形成方法を提供することである。   An object of the present invention is to provide a printing plate material and an image forming method which are easy to confirm an exposed image and excellent in on-press development property.

本発明の目的は、下記の構成により達成される。   The object of the present invention is achieved by the following constitution.

(請求項1)
親水性表面を有する基材上に、印刷機上現像可能な感熱画像形成層を有するネガ型印刷版材料であって、a)該親水性表面の可視光反射濃度が0.5以上であり、b)該基材の感熱画像形成層側に、極大波長が830nmの赤外レーザー光により400mJ/cm2のエネルギー量で露光する露光条件下において、露光部の可視光反射濃度を未露光部の可視光反射濃度に対して0.2以上減少し得る、可視画付与層を有することを特徴とする印刷版材料。
(Claim 1)
A negative type printing plate material having a thermal image forming layer developable on a printing machine on a substrate having a hydrophilic surface, wherein a) the visible light reflection density of the hydrophilic surface is 0.5 or more, b) On the thermal image forming layer side of the substrate, the visible light reflection density of the exposed part is set to the unexposed part under the exposure conditions in which the maximum wavelength is exposed to an infrared laser beam having a wavelength of 830 nm at an energy amount of 400 mJ / cm 2 . A printing plate material having a visible image providing layer which can be reduced by 0.2 or more with respect to the visible light reflection density.

(請求項2)
請求項1に記載の印刷版材料をレーザー光で画像露光し、画像形成することを特徴とする画像形成方法。
(Claim 2)
An image forming method, wherein the printing plate material according to claim 1 is image-exposed with a laser beam to form an image.

本発明の上記構成により、露光画像の確認が容易で、機上現像性に優れる印刷版材料及び画像形成方法が提供できる。   With the above-described configuration of the present invention, it is possible to provide a printing plate material and an image forming method in which an exposure image can be easily confirmed and the on-press developability is excellent.

本発明は、親水性表面を有する基材上に、印刷機上現像可能な感熱画像形成層を有するネガ型印刷版材料において、a)該親水性表面の可視光反射濃度が0.5以上であり、b)該基材の感熱画像形成層側に、極大波長が830nmの赤外レーザー光により400mJ/cm2のエネルギー量で露光する露光条件下において、露光部の可視光反射濃度を未露光部の可視光反射濃度に対して0.2以上減少し得る、可視画付与層を有することを特徴とする。 The present invention relates to a negative type printing plate material having a thermal image-forming layer that can be developed on a printing machine on a substrate having a hydrophilic surface. A) The visible light reflection density of the hydrophilic surface is 0.5 or more. Yes, b) The visible light reflection density of the exposed portion is unexposed on the heat-sensitive image forming layer side of the substrate under the exposure conditions where the maximum wavelength is exposed to an energy of 400 mJ / cm 2 with infrared laser light having a wavelength of 830 nm. It has a visible image providing layer that can be reduced by 0.2 or more with respect to the visible light reflection density of the portion.

本発明は、上記特定の反射濃度を有する基材と可視画付与層とを組み合わせ有することにより、良好な露光可視画性と機上現像性を得るものである。   In the present invention, a good exposure visible image property and on-press developability are obtained by combining the base material having the specific reflection density and the visible image providing layer.

以下、本発明について詳細に説明する。   Hereinafter, the present invention will be described in detail.

〔基材〕
本発明に係る親水性表面を有する基材は、基材の表面を親水化処理する方法あるいは基材上に親水性層を設ける方法により得られる。
〔Base material〕
The substrate having a hydrophilic surface according to the present invention can be obtained by a method of hydrophilizing the surface of the substrate or a method of providing a hydrophilic layer on the substrate.

本発明に係る親水性表面を有する基材は、可視光反射濃度が0.5以上であることが必要であり、さらに0.8以上が好ましく1.0〜1.5が特に好ましい。   The substrate having a hydrophilic surface according to the present invention is required to have a visible light reflection density of 0.5 or more, more preferably 0.8 or more, and particularly preferably 1.0 to 1.5.

可視光反射濃度とは、観測視野2°、絶対白色濃度標準で測定した値で400nmから700nmまでの、各20nm間隔の反射濃度値の平均値をいい、例えば、GretagMacbeth社製分光濃度計Spectrolinoを用いて、フィルター条件D65、観測視野2°、ホワイトベース:絶対白色、濃度標準:Status−Tで測定した値で400nmから700nmまでの、各20nm間隔の反射濃度を測定し、平均値を求めることにより算出することができる。   The visible light reflection density is an average value of reflection density values at intervals of 20 nm from 400 nm to 700 nm as measured with an observation visual field of 2 ° and an absolute white density standard. For example, a spectral densitometer Spectrolino manufactured by GretagMacbeth is used. Using the filter condition D65, the observation field of view 2 °, the white base: absolute white, the density standard: the value measured by Status-T, the reflection density at intervals of 20 nm from 400 nm to 700 nm is measured, and the average value is obtained. Can be calculated.

本発明に係る基材としては、印刷版の基材として使用される公知の材料を使用することができる。   As a base material which concerns on this invention, the well-known material used as a base material of a printing plate can be used.

例えば、金属板、プラスチックフィルム、ポリオレフィン等で処理された紙、上記材料を適宜貼り合わせた複合基材等が挙げられる。基材の厚さとしては、印刷機に取り付け可能であれば特に制限されるものではないが、50〜500μmのものが一般的に取り扱いやすい。   For example, a metal plate, a plastic film, paper treated with a polyolefin, a composite base material obtained by appropriately bonding the above materials, and the like can be given. The thickness of the base material is not particularly limited as long as it can be attached to a printing press, but a thickness of 50 to 500 μm is generally easy to handle.

金属板としては、鉄、ステンレス、アルミニウム等が挙げられるが、比重と剛性との関係から特にアルミニウムが好ましい。アルミニウム板は、通常その表面に存在する圧延・巻取り時に使用されたオイルを除去するためにアルカリ、酸、溶剤等で脱脂した後に使用される。脱脂処理としては特にアルカリ水溶液による脱脂が好ましい。また、塗布層との接着性を向上させるために、塗布面に易接着処理や下引き層の塗布を行なっても良い。   Examples of the metal plate include iron, stainless steel, and aluminum. Aluminum is particularly preferable from the relationship between specific gravity and rigidity. The aluminum plate is usually used after degreasing with an alkali, an acid, a solvent or the like in order to remove oil used during rolling and winding existing on the surface. As the degreasing treatment, degreasing with an alkaline aqueous solution is particularly preferable. Moreover, in order to improve adhesiveness with an application layer, you may perform an easily bonding process and application | coating of an undercoat layer to an application surface.

例えば、ケイ酸塩やシランカップリング剤等のカップリング剤を含有する液に浸漬するか、液を塗布した後、十分な乾燥を行なう方法が挙げられる。陽極酸化処理も易接着処理の一種と考えられ、使用することができる。また、陽極酸化処理と上記浸漬または塗布処理を組み合わせて使用することもできる。また、公知の方法で粗面化されたアルミニウム基材、いわゆるアルミ砂目を、親水性表面を有する基材として使用することもできる。   For example, a method of dipping in a liquid containing a coupling agent such as a silicate or a silane coupling agent or applying a liquid, followed by sufficient drying can be used. Anodizing treatment is also considered as a kind of easy adhesion treatment and can be used. Moreover, it can also use combining an anodizing process and the said immersion or application | coating process. Moreover, the aluminum base material roughened by the well-known method, what is called an aluminum grain can also be used as a base material which has a hydrophilic surface.

本発明の印刷版材料に用いることができるアルミニウム基材には、純アルミニウムおよびアルミニウム合金よりなる基材が含まれる。アルミニウム合金としては種々のものが使用でき、例えば珪素、銅、マンガン、マグネシウム、クロム、亜鉛、鉛、ビスマス、ニッケル、チタン、ナトリウム、鉄等の金属とアルミニウムの合金が用いられる。   Aluminum substrates that can be used for the printing plate material of the present invention include substrates made of pure aluminum and aluminum alloys. Various aluminum alloys can be used. For example, an alloy of a metal such as silicon, copper, manganese, magnesium, chromium, zinc, lead, bismuth, nickel, titanium, sodium, iron, and aluminum is used.

アルミニウム基材は、粗面化処理に先立ってアルミニウム表面の圧延油を除去するために脱脂処理を施すことが好ましい。脱脂処理としては、トリクレン、シンナー等の溶剤を用いる脱脂処理、ケシロン、トリエタノール等のエマルジョンを用いたエマルジョン脱脂処理等が用いられる。また、脱脂処理には、水酸化ナトリウム、水酸化カリウム,炭酸ナトリウム,リン酸ナトリウム等のアルカリの水溶液を用いることもできる。脱脂処理にアルカリ水溶液を用いた場合、上記脱脂処理のみでは除去できない汚れや酸化皮膜も除去することができる。   The aluminum substrate is preferably subjected to a degreasing treatment in order to remove the rolling oil on the aluminum surface prior to the roughening treatment. As the degreasing treatment, a degreasing treatment using a solvent such as trichlene or thinner, an emulsion degreasing treatment using an emulsion such as kesilon or triethanol, or the like is used. In addition, an alkaline aqueous solution such as sodium hydroxide, potassium hydroxide, sodium carbonate, or sodium phosphate can be used for the degreasing treatment. When an alkaline aqueous solution is used for the degreasing treatment, dirt and oxide film that cannot be removed only by the degreasing treatment can be removed.

脱脂処理にアルカリ水溶液を用いた場合には、燐酸、硝酸、塩酸、硫酸、クロム酸等の酸、あるいはそれらの混酸に浸漬し中和処理を施すことが好ましい。中和処理の次に電解粗面化を行う場合は、中和に使用する酸を電解粗面化に使用する酸に合わせることが特に好ましい。   When an alkaline aqueous solution is used for the degreasing treatment, it is preferable to perform a neutralization treatment by immersing in an acid such as phosphoric acid, nitric acid, hydrochloric acid, sulfuric acid, chromic acid, or a mixed acid thereof. When electrolytic surface roughening is performed after the neutralization treatment, it is particularly preferable to match the acid used for neutralization with the acid used for electrolytic surface roughening.

基材の粗面化としては公知の方法での電解粗面化処理を行うが、その前処理として、適度な処理量の化学的粗面化や機械的粗面化を適宜組み合わせた粗面化処理を行なってもかまわない。   As the roughening of the substrate, an electrolytic surface roughening treatment is carried out by a known method, but as a pretreatment, roughening by appropriately combining chemical roughening or mechanical roughening with an appropriate amount of treatment. Processing may be performed.

化学的粗面化は脱脂処理と同様に水酸化ナトリウム、水酸化カリウム,炭酸ナトリウム,リン酸ナトリウム等のアルカリの水溶液を用いる。処理後には燐酸、硝酸、塩酸、硫酸、クロム酸等の酸、あるいはそれらの混酸に浸漬し中和処理を施すことが好ましい。中和処理の次に電解粗面化を行う場合は、中和に使用する酸を電解粗面化に使用する酸に合わせることが特に好ましい。   Chemical roughening uses an aqueous solution of an alkali such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium phosphate as in the degreasing treatment. After the treatment, it is preferable to carry out a neutralization treatment by dipping in an acid such as phosphoric acid, nitric acid, hydrochloric acid, sulfuric acid, chromic acid, or a mixed acid thereof. When electrolytic surface roughening is performed after the neutralization treatment, it is particularly preferable to match the acid used for neutralization with the acid used for electrolytic surface roughening.

機械的粗面化処理方法は特に限定されないがブラシ研磨、ホーニング研磨が好ましい。   The mechanical roughening treatment method is not particularly limited, but brush polishing and honing polishing are preferable.

機械的に粗面化された基材は、基材の表面に食い込んだ研磨剤、アルミニウム屑等を取り除いたり、ピット形状をコントロールしたりする等のために、酸またはアルカリの水溶液に浸漬して表面をエッチングすることが好ましい。酸としては、例えば硫酸、過硫酸、弗酸、燐酸、硝酸、塩酸等が含まれ、塩基としては、例えば、水酸化ナトリウム、水酸化カリウム、炭酸ナトリウム、リン酸ナトリウム等が含まれる。これらの中でもアルカリの水溶液を用いるのが好ましい。   A mechanically roughened substrate is immersed in an aqueous solution of acid or alkali to remove abrasives, aluminum scraps, etc. that have digged into the surface of the substrate, or to control the pit shape. It is preferable to etch the surface. Examples of the acid include sulfuric acid, persulfuric acid, hydrofluoric acid, phosphoric acid, nitric acid, and hydrochloric acid. Examples of the base include sodium hydroxide, potassium hydroxide, sodium carbonate, and sodium phosphate. Among these, it is preferable to use an alkaline aqueous solution.

機械的粗面化処理に#400よりも細かい粒度の研磨剤を用い、かつ、機械的粗面化処理の後にアルカリ水溶液によるエッチング処理を行うことで、機械的粗面化処理による入り組んだ粗面化構造を滑らかな凹凸の表面とすることができる。このため、本発明の画像形成層を設けた際にも機上現像性を損なうことなく数μm〜数十μmの比較的長波長のうねりを形成することができ、これに後述する電解粗面化処理を加えることで、印刷性能が良好で、かつ、耐刷性向上にも寄与するアルミニウム基材とすることができる。また、電解粗面化処理時の電気量を低減することもでき、コストダウンにもつながる。   By using an abrasive having a particle size finer than # 400 for the mechanical surface roughening treatment, and performing an etching treatment with an alkaline aqueous solution after the mechanical surface roughening treatment, an intricate rough surface by the mechanical surface roughening treatment. The structure can be a smooth uneven surface. For this reason, even when the image forming layer of the present invention is provided, a relatively long wavelength undulation of several μm to several tens of μm can be formed without impairing the on-press developability. By adding the crystallization treatment, it is possible to obtain an aluminum substrate that has good printing performance and contributes to improved printing durability. In addition, the amount of electricity during the electrolytic surface roughening treatment can be reduced, leading to cost reduction.

上記をアルカリの水溶液で浸漬処理を行った場合には、燐酸、硝酸、硫酸、クロム酸等の酸、あるいはそれらの混酸に浸漬し中和処理を施すことが好ましい。   When the above is immersed in an alkaline aqueous solution, it is preferably immersed in an acid such as phosphoric acid, nitric acid, sulfuric acid, chromic acid, or a mixed acid thereof for neutralization.

中和処理の次に電解粗面化処理を行う場合は、中和に使用する酸を電解粗面化処理に使用する酸に合わせることが特に好ましい。   When the electrolytic surface-roughening treatment is performed after the neutralization treatment, it is particularly preferable that the acid used for neutralization is matched with the acid used for the electrolytic surface-roughening treatment.

電解粗面化処理は一般に酸性電解液中で交流電流を用いて粗面化を行うものである。酸性電解液は通常の電解粗面化法に用いられるものが使用できるが、塩酸系または硝酸系電解液を用いるのが好ましく、本発明においては塩酸系電解液を用いるのが特に好ましい。   The electrolytic surface roughening treatment is generally a surface roughening using an alternating current in an acidic electrolyte. As the acidic electrolytic solution, those used in a general electrolytic surface roughening method can be used, but a hydrochloric acid-based or nitric acid-based electrolytic solution is preferably used, and in the present invention, a hydrochloric acid-based electrolytic solution is particularly preferable.

電解に使用する電源波形は、矩形波、台形波、のこぎり波等さまざまな波形を用いることができるが、特に正弦波が好ましい。   Various waveforms such as a rectangular wave, a trapezoidal wave, and a sawtooth wave can be used as the power supply waveform used for electrolysis, and a sine wave is particularly preferable.

また、特開平10−869号公報に開示されているような分割電解粗面化処理も好ましく用いることができる。   Further, a divided electrolytic surface roughening treatment as disclosed in JP-A-10-869 can also be preferably used.

硝酸系電解液を用いての電解粗面化において印加される電圧は、1〜50Vが好ましく、5〜30Vが更に好ましい。電流密度(ピーク値)は、10〜200A/dm2が好ましく、20〜150A/dm2が更に好ましい。 1-50V is preferable and, as for the voltage applied in the electrolytic surface roughening using nitric acid type electrolyte solution, 5-30V is still more preferable. The current density (peak value) is preferably from 10 to 200 A / dm 2, more preferably 20 to 150 A / dm 2.

電気量は全処理工程を合計して、100〜2000C/dm2、好ましくは200〜1500C/dm2、より好ましくは200〜1000C/dm2である。 Quantity of electricity by summing all the processing steps, 100~2000C / dm 2, preferably not 200~1500C / dm 2, more preferably a 200~1000C / dm 2.

温度は、10〜50℃が好ましく、15〜45℃が更に好ましい。硝酸濃度は0.1〜5質量%が好ましい。   The temperature is preferably 10 to 50 ° C, more preferably 15 to 45 ° C. The concentration of nitric acid is preferably 0.1 to 5% by mass.

電解液には、必要に応じて硝酸塩、塩化物、アミン類、アルデヒド類、燐酸、クロム酸、ホウ酸、酢酸、蓚酸等を加えることが出来る。   If necessary, nitrates, chlorides, amines, aldehydes, phosphoric acid, chromic acid, boric acid, acetic acid, oxalic acid, and the like can be added to the electrolytic solution.

本発明においては、電解粗面化処理された基材は、表面のスマット等を取り除いたり、ピット形状をコントロールしたりする等のために、アルカリの水溶液に浸漬して表面のエッチングを行う。   In the present invention, the electrolytically roughened substrate is etched by immersing it in an aqueous alkali solution in order to remove surface smut or the like or to control the pit shape.

アルカリ水溶液としては、水酸化ナトリウム、水酸化カリウム、炭酸ナトリウム、リン酸ナトリウム等が含まれる。   Examples of the alkaline aqueous solution include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium phosphate and the like.

アルカリ水溶液によるエッチング処理を行うことで、本発明の画像形成層を設けた際の刷り出し性や地汚れが非常に良好となる。   By performing the etching treatment with an alkaline aqueous solution, the printability and the background stain when the image forming layer of the present invention is provided are very good.

アルカリの水溶液で浸漬処理を行った後には、燐酸、硝酸、硫酸、クロム酸等の酸、あるいはそれらの混酸に浸漬し中和処理を施すことが好ましい。中和処理の次に陽極酸化処理を行う場合は、中和に使用する酸を陽極酸化処理に使用する酸に合わせることが特に好ましい。   After the immersion treatment with an alkaline aqueous solution, it is preferable to perform a neutralization treatment by immersion in an acid such as phosphoric acid, nitric acid, sulfuric acid, chromic acid, or a mixed acid thereof. When the anodizing treatment is performed after the neutralizing treatment, it is particularly preferable that the acid used for the neutralization is matched with the acid used for the anodizing treatment.

粗面化処理の次に、陽極酸化処理を行う。   Following the roughening treatment, an anodizing treatment is performed.

本発明で用いられる陽極酸化処理の方法には特に制限はなく、公知の方法を用いることができる。陽極酸化処理により基材上には酸化皮膜が形成される。本発明において、陽極酸化処理には、硫酸および/または燐酸等を10〜50%の濃度で含む水溶液を電解液として、電流密度1〜10A/dm2で電解する方法が好ましく用いられるが、他に米国特許第1,412,768号に記載されている硫酸中で高電流密度で電解する方法や、米国特許第3,511,661号に記載されている燐酸を用いて電解する方法等を用いることができる。 There is no restriction | limiting in particular in the method of the anodizing process used by this invention, A well-known method can be used. An oxide film is formed on the substrate by anodizing. In the present invention, a method of electrolyzing with an aqueous solution containing sulfuric acid and / or phosphoric acid or the like at a concentration of 10 to 50% as an electrolytic solution at an electric current density of 1 to 10 A / dm 2 is preferably used for the anodizing treatment. US Pat. No. 1,412,768 describes a method of electrolysis at a high current density in sulfuric acid, and a method of electrolysis using phosphoric acid described in US Pat. No. 3,511,661. Can be used.

陽極酸化処理された基材は、必要に応じ封孔処理を施してもよい。これら封孔処理は、熱水処理、沸騰水処理、水蒸気処理、重クロム酸塩水溶液処理、亜硝酸塩処理、酢酸アンモニウム処理等公知の方法を用いて行うことができる。   The anodized base material may be subjected to a sealing treatment as necessary. These sealing treatments can be performed using known methods such as hot water treatment, boiling water treatment, water vapor treatment, dichromate aqueous solution treatment, nitrite treatment, ammonium acetate treatment.

また、陽極酸化処理された基材は適宜、上記封孔処理以外の表面処理を行うこともできる。表面処理としては、ケイ酸塩処理、リン酸塩処理、各種有機酸処理、PVPA処理、ベーマイト化処理といった公知の処理が挙げられる。また、特開平8−314157号に記載の炭酸水素塩を含有する水溶液による処理や、炭酸水素塩を含有する水溶液による処理に続けてクエン酸のような有機酸処理を行ってもよい。   In addition, the anodized base material can be appropriately subjected to a surface treatment other than the sealing treatment. Examples of the surface treatment include known treatments such as silicate treatment, phosphate treatment, various organic acid treatments, PVPA treatment, and boehmite treatment. Further, an organic acid treatment such as citric acid may be performed following the treatment with an aqueous solution containing a bicarbonate described in JP-A-8-314157 or the treatment with an aqueous solution containing a bicarbonate.

本発明に係る基材としてのプラスチックフィルムとしては、ポリエチレンテレフタレート、ポリエチレンナフタレート、ポリイミド、ポリアミド、ポリカーボネート、ポリスルホン、ポリフェニレンオキサイド、セルロースエステル類等を挙げることができる。   Examples of the plastic film as the substrate according to the present invention include polyethylene terephthalate, polyethylene naphthalate, polyimide, polyamide, polycarbonate, polysulfone, polyphenylene oxide, and cellulose esters.

また、裏面のすべり性を制御する(例えば版胴表面との摩擦係数を低減させる)目的で、裏面コート層を設けた基材も好ましく使用することができる。   In addition, for the purpose of controlling the slipperiness of the back surface (for example, reducing the friction coefficient with the plate cylinder surface), a substrate provided with a back surface coating layer can also be preferably used.

(アルミニウム基材の着色)
基材の親水性表面の可視光反射濃度は、親水性表面を着色させることにより0.5以上とすることができる。
(Coloring of aluminum substrate)
The visible light reflection density of the hydrophilic surface of the substrate can be 0.5 or more by coloring the hydrophilic surface.

良好な可視画視認性を得るためには、濃色に着色できることが好ましい。   In order to obtain good visible image visibility, it is preferable that the film can be colored deeply.

具体的には、反射濃度として、0.5以上が必要であるが、視認性、網点画像の光学濃度の測定精度などの面から0.8以上が好ましく1.0〜1.5がさらに好ましい。   Specifically, the reflection density is required to be 0.5 or higher, but 0.8 or higher is preferable from the viewpoint of visibility, optical density measurement accuracy of halftone image, and 1.0 to 1.5 is more preferable. preferable.

本発明においては、基材としてアルミニウムを用いその親水性表面を着色するのが好ましい態様である。   In the present invention, it is a preferred embodiment that aluminum is used as the substrate and the hydrophilic surface is colored.

アルミニウム基材を着色する手段として、下記の様な方法が挙げられる。   As a means for coloring the aluminum substrate, the following methods may be mentioned.

たとえば『電解法による着色皮膜』馬場宣良著(槇書店)記載の電解着色法等を用いることができる。   For example, the electrolytic coloring method described in “Colored film by electrolytic method” written by Nobuyoshi Baba (Tsubaki Shoten) can be used.

硫酸浴中で交流電解により作った交流アルマイトは各種金属塩水溶液に浸漬すると下記に示すカラー・アルマイトが得られ、この着色が利用できる。   When an alternating current alumite prepared by alternating current electrolysis in a sulfuric acid bath is immersed in various metal salt aqueous solutions, the following color anodized is obtained, and this coloring can be used.

(浸漬液:アルマイトの色)
酒石酸ナトリウム・アンチモン:オレンジ
ヒ素酸ナトリウム:黄色
クエン酸アンモニウム・ビスマス:黄褐色
硫酸銅:緑
酢酸コバルト:黒
酢酸カドミウム:黄色
塩化金:紫
酢酸鉛:こげ茶
シュウ酸アンモニウム鉄:黒
モリブデン酸ナトリウム:オレンジ
硫酸アンモニウム・ニッケル:ブロンズ
セレン酸ナトリウム:赤褐色
硝酸銀:灰褐色
塩化アンモニウム・第2スズ:黄色
塩化アンモニウム・第1スズ:褐色
酢酸ウラニウム:褐色
また、Al−Si合金、Al−Cr合金、Al−Mn合金などは硫酸浴で陽極酸化するだけでカラー・アルマイトができ、これらのカラー・アルマイトを「合金発色」というが、これらの着色も利用できる。
(Immersion solution: Anodized color)
Sodium tartrate / antimony: sodium orange arsenate: yellow ammonium citrate / bismuth: tan copper sulfate: cobalt cobalt acetate: cadmium black acetate: yellow gold chloride: purple lead acetate: dark iron ammonium oxalate iron: black sodium molybdate: Orange ammonium sulfate, nickel: bronze sodium selenate: reddish brown silver nitrate: gray brown ammonium chloride, stannic: yellow ammonium chloride, stannous: brown uranium acetate: brown Al-Si alloy, Al-Cr alloy, Al-Mn Alloys and the like can be colored and anodized simply by anodizing in a sulfuric acid bath, and these colored anodized are called “alloy coloring”, but these colors can also be used.

合金発色法においては、合金成分だけでなくて、合金の熱処理状況によって発色しなかったり、色調が変化したりする。すなわち、アルミ合金が固溶体であるか、共晶であるかが発色に影響を与え、例えば下記のような色が得られる。   In the alloy coloring method, the coloring does not occur or the color tone changes depending on the heat treatment status of the alloy as well as the alloy components. That is, whether the aluminum alloy is a solid solution or a eutectic affects the color development, and for example, the following colors are obtained.

(アルミ合金:色)
Al−Si:黒、灰色
Al−Cr:黄金色、灰色
Al−Mn:紅褐色
Al−Mn−Cr:黒、灰色、黄色
又、無色のアルマイトを作ったあとに、改めて色をつける方法を着色法と呼び、アルマイトの着色法としては染料着色法、無機塩浸漬着色法、電解着色法があるが、これらの着色方も利用できる。また、そのほかの特殊な着色法として、アルミニウム上に機械的に非常に細い多数のミゾを作り、光の干渉で色をつける方法も利用できる。
(Aluminum alloy: Color)
Al-Si: black, gray Al-Cr: golden, gray Al-Mn: reddish brown Al-Mn-Cr: black, gray, yellow In addition, after making colorless anodized, coloring method to add color again The alumite coloring methods include dye coloring methods, inorganic salt immersion coloring methods, and electrolytic coloring methods, and these coloring methods can also be used. In addition, as another special coloring method, a method can be used in which a large number of mechanically fine grooves are formed on aluminum and colored by light interference.

〔親水性層〕
親水性表面を有する基材は、上記のような基材の表面を親水化処理する方法あるいは基材上に親水性層を設ける方法により得られる。
[Hydrophilic layer]
The substrate having a hydrophilic surface can be obtained by a method of hydrophilizing the surface of the substrate as described above or a method of providing a hydrophilic layer on the substrate.

親水性を設ける場合、親水性層は親水性素材を含み、親水性素材としては、金属酸化物が好ましく用いられる。   In the case of providing hydrophilicity, the hydrophilic layer includes a hydrophilic material, and a metal oxide is preferably used as the hydrophilic material.

金属酸化物としては、金属酸化物の粒子を含むことが好ましい。   The metal oxide preferably contains metal oxide particles.

例えば、コロイダルシリカ、アルミナゾル、チタニアゾル、その他の金属酸化物のゾルが挙げられる。   Examples thereof include colloidal silica, alumina sol, titania sol, and other metal oxide sols.

この金属酸化物粒子の形態としては、球状、針状、羽毛状、その他の何れの形態でも良い。平均粒径としては、3〜100nmであることが好ましく、平均粒径が異なる数種の金属酸化物粒子を併用することもできる。又、粒子表面に表面処理がなされていても良い。   The form of the metal oxide particles may be spherical, needle-like, feather-like, or any other form. The average particle diameter is preferably 3 to 100 nm, and several kinds of metal oxide particles having different average particle diameters can be used in combination. The surface of the particles may be surface treated.

上記金属酸化物粒子はその造膜性を利用して結合剤としての使用が可能である。有機の結合剤を用いるよりも親水性の低下が少なく、親水性層への使用に適している。   The metal oxide particles can be used as a binder by utilizing the film forming property. The decrease in hydrophilicity is less than when an organic binder is used, and it is suitable for use in a hydrophilic layer.

本発明には、上記の中でも特にコロイダルシリカが好ましく使用できる。コロイダルシリカは比較的低温の乾燥条件であっても造膜性が高いという利点があり、良好な強度を得ることができる。   Among the above, colloidal silica can be preferably used in the present invention. Colloidal silica has the advantage of high film-forming properties even under relatively low temperature drying conditions, and can provide good strength.

上記コロイダルシリカとしては、ネックレス状コロイダルシリカ、平均粒径20nm以下の微粒子コロイダルシリカを含むことが好ましく、さらに、コロイダルシリカはコロイド溶液としてアルカリ性を呈することが好ましい。   The colloidal silica preferably includes necklace-like colloidal silica and fine particle colloidal silica having an average particle size of 20 nm or less, and the colloidal silica preferably exhibits alkalinity as a colloidal solution.

本発明に用いることができる親水性層は金属酸化物として多孔質金属酸化物粒子を含むことが好ましい。   The hydrophilic layer that can be used in the present invention preferably contains porous metal oxide particles as a metal oxide.

多孔質金属酸化物粒子としては、多孔質シリカ又は多孔質アルミノシリケート粒子もしくはゼオライト粒子を好ましく用いることができる。   As the porous metal oxide particles, porous silica, porous aluminosilicate particles, or zeolite particles can be preferably used.

多孔質無機粒子の粒径としては、親水性層に含有されている状態で、実質的に1μm以下であることが好ましく、0.5μm以下であることが更に好ましい。   The particle diameter of the porous inorganic particles is preferably substantially 1 μm or less, and more preferably 0.5 μm or less, when contained in the hydrophilic layer.

親水性層にはその他の添加素材として、ケイ酸塩水溶液も使用することができる。ケイ酸Na、ケイ酸K、ケイ酸Liといったアルカリ金属ケイ酸塩が好ましく、そのSiO2/M2O比率はケイ酸塩を添加した際の塗布液全体のpHが13を超えない範囲となるように選択することが無機粒子の溶解を防止する上で好ましい。 A silicate aqueous solution can also be used as another additive material for the hydrophilic layer. Alkali metal silicates such as silicate Na, silicate K, and silicate Li are preferred, and the SiO 2 / M 2 O ratio is in a range where the pH of the entire coating solution does not exceed 13 when silicate is added. It is preferable to select such that the inorganic particles are not dissolved.

また、金属アルコキシドを用いた、いわゆるゾル−ゲル法による無機ポリマーもしくは有機−無機ハイブリッドポリマーも使用することができる。ゾル−ゲル法による無機ポリマーもしくは有機−無機ハイブリッドポリマーの形成については、例えば「ゾル−ゲル法の応用」(作花済夫著/アグネ承風社発行)に記載されているもの、又は本書に引用されている文献に記載されている公知の方法を使用することができる。   Further, an inorganic polymer or an organic-inorganic hybrid polymer using a metal alkoxide by a so-called sol-gel method can also be used. Regarding the formation of inorganic polymers or organic-inorganic hybrid polymers by the sol-gel method, for example, those described in “Application of the sol-gel method” (Sakuo Sakuo / Agne Jofusha) or in this book Known methods described in the cited documents can be used.

本発明の好ましい態様として、親水性層には後述の光熱変換剤を含有させることができる。   As a preferred embodiment of the present invention, the hydrophilic layer can contain a photothermal conversion agent described later.

光熱変換素剤としては下記のような素材を挙げることができる。   Examples of the photothermal conversion material include the following materials.

一般的な赤外吸収色素であるシアニン系色素、クロコニウム系色素、ポリメチン系色素、アズレニウム系色素、スクワリウム系色素、チオピリリウム系色素、ナフトキノン系色素、アントラキノン系色素などの有機化合物、フタロシアニン系、ナフタロシアニン系、アゾ系、チオアミド系、ジチオール系、インドアニリン系の有機金属錯体などが挙げられる。具体的には、特開昭63−139191号、特開昭64−33547号、特開平1−160683号、特開平1−280750号、特開平1−293342号、特開平2−2074号、特開平3−26593号、特開平3−30991号、特開平3−34891号、特開平3−36093号、特開平3−36094号、特開平3−36095号、特開平3−42281号、特開平3−97589号、特開平3−103476号等に記載の化合物が挙げられる。これらは一種又は二種以上を組み合わせて用いることができる。   General infrared absorbing dyes such as cyanine dyes, croconium dyes, polymethine dyes, azurenium dyes, squalium dyes, thiopyrylium dyes, naphthoquinone dyes, anthraquinone dyes, organic compounds such as phthalocyanine dyes and naphthalocyanine dyes , Azo-based, thioamide-based, dithiol-based, and indoaniline-based organometallic complexes. Specifically, JP-A-63-139191, JP-A-64-33547, JP-A-1-160683, JP-A-1-280750, JP-A-1-293342, JP-A-2-2074, Kaihei 3-26593, JP-A-3-30991, JP-A-3-34891, JP-A-3-36093, JP-A-3-36094, JP-A-3-36095, JP-A-3-42281, JP-A-3-42281 Examples thereof include compounds described in JP-A-3-97589, JP-A-3-103476, and the like. These can be used alone or in combination of two or more.

また、特開平11−240270号、特開平11−265062号、特開2000−309174号、特開2002−49147号、特開2001−162965号、特開2002−144750号、特開2001−219667号に記載の化合物も好ましく用いることができる。   JP-A-11-240270, JP-A-11-265062, JP-A-2000-309174, JP-A-2002-49147, JP-A-2001-162965, JP-A-2002-144750, JP-A-2001-219667. The compounds described in (1) can also be preferably used.

親水性層を設ける場合は、この親水性層の表面の可視光反射濃度が0.5以上であり、後述の可視画付与層が露光により濃度が低下した領域との濃度差が0.5以上であることが好ましい。   When the hydrophilic layer is provided, the visible light reflection density on the surface of the hydrophilic layer is 0.5 or more, and the density difference from the area where the density of the visible image providing layer described below is lowered by exposure is 0.5 or more. It is preferable that

〔感熱画像形成層〕
本発明に係る感熱画像形成層(以下画像形成層と略記)は、像様加熱により画像形成可能な層であり、印刷機上現像可能な層である。
(Thermal image forming layer)
The heat-sensitive image forming layer (hereinafter abbreviated as “image forming layer”) according to the present invention is a layer capable of forming an image by imagewise heating, and is a layer that can be developed on a printing press.

像様に加熱するには、直接熱源で画像様に加熱する方法、あるいはレーザーなどで、画像露光を行い、露光することにより発生する熱により加熱する方法があるが、本発明においては、レーザー光を用いた画像露光による方法が好ましく用いられる。   There are two methods for imagewise heating: a method of heating imagewise with a direct heat source, or a method of performing image exposure with a laser or the like and heating with heat generated by exposure. In the present invention, laser light is used. A method by image exposure using is preferably used.

画像形成層の加熱された部分は印刷時印刷インキ受容性である画像部となる。   The heated portion of the image forming layer becomes an image portion that is printing ink receptive during printing.

画像形成層は熱により変形、溶融、軟化等の変化を生じる感熱性素材を含有する。   The image forming layer contains a heat-sensitive material that causes changes such as deformation, melting, and softening due to heat.

画像形成層には、前述の親水性層に記載の光熱変換剤を含有させるのが好ましい態様である。   In a preferred embodiment, the image forming layer contains the photothermal conversion agent described in the hydrophilic layer.

感熱性素材としては、天然または合成ワックス類、ポリエステル、ポリスチレン、ポリアクリル、ポリウレタン系樹脂もしくはこれらの共重合体樹脂あるいはブロックイソシアネートなどの熱反応性の素材などが挙げられる。   Examples of the heat-sensitive material include natural or synthetic waxes, polyester, polystyrene, polyacryl, polyurethane-based resins, copolymer resins thereof, or thermally reactive materials such as blocked isocyanate.

感熱性素材は、耐刷性、機上現像性等の面でブロックイソシアネート、ウレタン樹脂、ポリエステル樹脂粒子等であることが好ましい。   The heat-sensitive material is preferably a blocked isocyanate, a urethane resin, a polyester resin particle or the like in terms of printing durability, on-press developability, and the like.

これらの樹脂の好ましい物性として、融点、軟化点、ガラス転移点(Tg)などの性質が40℃以上である。   As preferable physical properties of these resins, properties such as a melting point, a softening point, and a glass transition point (Tg) are 40 ° C. or higher.

又、感熱性素材は熱可塑性の樹脂粒子などが好ましく、その平均粒径は機上現像性、解像度の面から0.01〜2μmであることが好ましく、より好ましくは0.1〜1μmである。   The heat-sensitive material is preferably thermoplastic resin particles, and the average particle diameter is preferably 0.01 to 2 μm, more preferably 0.1 to 1 μm from the standpoint of on-press developability and resolution. .

〔画像形成層に含有可能なその他の素材〕
本発明に係る画像形成層にはさらに以下のような素材を含有させることが好ましい。
[Other materials that can be contained in the image forming layer]
The image forming layer according to the present invention preferably further contains the following materials.

画像形成層には水溶性樹脂、水分散性樹脂を含有させることが好ましい。水溶性樹脂、水分散性樹脂としては、オリゴ糖、多糖類、ポリエチレンオキサイド、ポリプロピレンオキサイド、ポリビニルアルコール、ポリエチレングリコール(PEG)、ポリビニルエーテル、スチレン−ブタジエン共重合体、メチルメタクリレート−ブタジエン共重合体の共役ジエン系重合体ラテックス、アクリル系重合体ラテックス、ビニル系重合体ラテックス、ポリアクリル酸、ポリアクリル酸塩、ポリアクリルアミド、ポリビニルピロリドン等の樹脂が挙げられる。   The image forming layer preferably contains a water-soluble resin or a water-dispersible resin. Examples of water-soluble resins and water-dispersible resins include oligosaccharides, polysaccharides, polyethylene oxide, polypropylene oxide, polyvinyl alcohol, polyethylene glycol (PEG), polyvinyl ether, styrene-butadiene copolymers, and methyl methacrylate-butadiene copolymers. Examples thereof include resins such as conjugated diene polymer latex, acrylic polymer latex, vinyl polymer latex, polyacrylic acid, polyacrylate, polyacrylamide, and polyvinylpyrrolidone.

オリゴ糖としては、ラフィノース、トレハロース、マルトース、ガラクトース、スクロース、ラクトースといったものが挙げられるが、特にトレハロースが好ましい。   Examples of the oligosaccharide include raffinose, trehalose, maltose, galactose, sucrose, and lactose, and trehalose is particularly preferable.

多糖類としては、デンプン類、セルロース類、ポリウロン酸、プルランなどが使用可能であるが、特にメチルセルロース塩、カルボキシメチルセルロース塩、ヒドロキシエチルセルロース塩等のセルロース誘導体が好ましく、カルボキシメチルセルロースのナトリウム塩やアンモニウム塩がより好ましい。   As polysaccharides, starches, celluloses, polyuronic acids, pullulans and the like can be used, but cellulose derivatives such as methyl cellulose salts, carboxymethyl cellulose salts, hydroxyethyl cellulose salts are particularly preferable, and sodium salts and ammonium salts of carboxymethyl cellulose are preferable. More preferred.

ポリアクリル酸、ポリアクリル酸、ポリアクリル酸塩(Na塩等)、ポリアクリルアミドとしては、分子量3000〜500万であることが好ましく、5000〜100万であることがより好ましい。   The polyacrylic acid, polyacrylic acid, polyacrylate (Na salt, etc.), and polyacrylamide preferably have a molecular weight of 3,000 to 5,000,000, and more preferably 5,000 to 1,000,000.

水溶性樹脂、水分散性樹脂は印刷版材料の経時保存後の地汚れや耐熱性、および機上現像性を向上させるために添加させる場合があるが、添加量を増やした場合、印刷版画像部の耐久性を低下させる場合があるため添加量は必要最低限であることが好ましく、通常50質量%以下の範囲が好ましく、30%以下の範囲がより好ましい。   Water-soluble resins and water-dispersible resins may be added to improve background stains and heat resistance after storage of printing plate materials over time, and on-press developability. Since the durability of the part may be lowered, the addition amount is preferably the minimum necessary, usually in the range of 50% by mass or less, more preferably in the range of 30% or less.

また、画像形成層には、水溶性の界面活性剤を含有させることができる。Si系、F系、アセチレングリコール系等の界面活性剤を使用することができる。   The image forming layer can contain a water-soluble surfactant. Surfactants such as Si, F, and acetylene glycol can be used.

さらに、pH調整のための酸(リン酸、酢酸等)またはアルカリ(水酸化ナトリウム、ケイ酸塩、リン酸塩等)を含有していても良い。   Further, it may contain an acid (phosphoric acid, acetic acid, etc.) or an alkali (sodium hydroxide, silicate, phosphate, etc.) for pH adjustment.

画像形成層の付き量としては、0.01〜10g/m2であり、好ましくは0.1〜3g/m2であり、さらに好ましくは0.2〜2g/m2である。 The amount per image forming layer, a 0.01 to 10 g / m 2, preferably from 0.1 to 3 g / m 2, more preferably from 0.2 to 2 g / m 2.

〔可視画付与層〕
本発明に係る可視画付与層は、極大波長が830nmの赤外レーザー光により400mJ/cm2のエネルギー量で露光する露光条件下において、露光部の可視光反射濃度を未露光部の可視光反射濃度に対して0.2以上減少し得る層であり、像様加熱時に少なくとも熱または光により、透明度の低下、光散乱性の増大が生じることによって可視光反射濃度が低下する。
[Visible image layer]
The visible image-imparting layer according to the present invention has a visible light reflection density of an exposed portion reflected by an visible light reflection of an unexposed portion under an exposure condition where exposure is performed with an infrared laser beam having a maximum wavelength of 830 nm at an energy amount of 400 mJ / cm 2. It is a layer that can be reduced by 0.2 or more with respect to the density, and the visible light reflection density is lowered by causing a decrease in transparency and an increase in light scattering property due to at least heat or light during imagewise heating.

これにより、印刷版材料の露光部と未露光部で反射濃度差が生じ、画像の判別が可能となる。   Thereby, a difference in reflection density occurs between the exposed portion and the unexposed portion of the printing plate material, and the image can be discriminated.

本発明に係る可視画付与層は、反射濃度を低下させる素材を含み、この素材としては下記のものが挙げられる。   The visible image providing layer according to the present invention includes a material that lowers the reflection density, and examples of the material include the following.

(金属酸化物)
金属酸化物としては、金属酸化物粒子を含むことが好ましい。
(Metal oxide)
The metal oxide preferably contains metal oxide particles.

例えば、コロイダルシリカ、アルミナゾル、チタニアゾル、その他の金属酸化物のゾルが挙げられる。   Examples thereof include colloidal silica, alumina sol, titania sol, and other metal oxide sols.

この金属酸化物粒子の形態としては、球状、針状、羽毛状、その他の何れの形態でも良い。平均粒径としては、3〜2000nmであることが好ましく、平均粒径が異なる数種の金属酸化物粒子を併用することもできる。又、粒子表面に表面処理がなされていても良い。   The form of the metal oxide particles may be spherical, needle-like, feather-like, or any other form. The average particle size is preferably 3 to 2000 nm, and several types of metal oxide particles having different average particle sizes can be used in combination. The surface of the particles may be surface treated.

その他、金属酸化物として多孔質金属酸化物粒子を含むことが好ましい。多孔質金属酸化物粒子としては、後述する多孔質シリカ又は多孔質アルミノシリケート粒子もしくはゼオライト粒子を好ましく用いることができる。   In addition, it is preferable that porous metal oxide particles are included as the metal oxide. As the porous metal oxide particles, porous silica, porous aluminosilicate particles, or zeolite particles described later can be preferably used.

(多孔質シリカ多孔質シリカ又は多孔質アルミノシリケート粒子)
多孔質シリカ粒子は一般に湿式法又は乾式法により製造される。湿式法ではケイ酸塩水溶液を中和して得られるゲルを乾燥、粉砕するか、中和して析出した沈降物を粉砕することで得ることができる。乾式法では四塩化珪素を水素と酸素と共に燃焼し、シリカを析出することで得られる。これらの粒子は製造条件の調整により多孔性や粒径を制御することが可能である。
(ゼオライト粒子)
ゼオライトは結晶性のアルミノケイ酸塩であり、細孔径が0.3〜1nmの規則正しい三次元網目構造の空隙を有する多孔質体である。
(Porous silica porous silica or porous aluminosilicate particles)
The porous silica particles are generally produced by a wet method or a dry method. In the wet method, it can be obtained by drying and pulverizing a gel obtained by neutralizing an aqueous silicate solution, or by pulverizing a precipitate deposited after neutralization. In the dry method, silicon tetrachloride is burned together with hydrogen and oxygen to obtain silica. These particles can be controlled in porosity and particle size by adjusting the production conditions.
(Zeolite particles)
Zeolite is a crystalline aluminosilicate and is a porous body having regular three-dimensional network voids having a pore diameter of 0.3 to 1 nm.

多孔質無機粒子の粒径としては、実質的に1μm以下であることが好ましく、0.5μm以下であることが更に好ましい。   The particle diameter of the porous inorganic particles is preferably substantially 1 μm or less, and more preferably 0.5 μm or less.

また、本発明の印刷版材料の可視画付与層は金属酸化物として、層状鉱物粒子が好ましく用いられる。   Further, in the visible image imparting layer of the printing plate material of the present invention, layered mineral particles are preferably used as a metal oxide.

この層状鉱物粒子としては、カオリナイト、ハロイサイト、タルク、スメクタイト(モンモリロナイト、バイデライト、ヘクトライト、サボナイト等)、バーミキュライト、マイカ(雲母)、クロライトといった粘土鉱物及び、ハイドロタルサイト、層状ポリケイ酸塩(カネマイト、マカタイト、アイアライト、マガディアイト、ケニヤアイト等)等が挙げられる。中でも、単位層(ユニットレイヤー)の電荷密度が高いほど極性が高く、親水性も高いと考えられる。好ましい電荷密度としては0.25以上、更に好ましくは0.6以上である。このような電荷密度を有する層状鉱物としては、スメクタイト(電荷密度0.25〜0.6;陰電荷)、バーミキュライト(電荷密度0.6〜0.9;陰電荷)等が挙げられる。特に、合成フッ素雲母は粒径等安定した品質のものを入手することができ好ましい。又、合成フッ素雲母の中でも、膨潤性であるものが好ましく、自由膨潤であるものが更に好ましい。   The layered mineral particles include kaolinite, halloysite, talc, smectite (montmorillonite, beidellite, hectorite, saponite, etc.), vermiculite, mica (mica), chlorite, and hydrotalcite, layered polysilicate ( Kanemite, macatite, ialite, magadiite, kenyaite, etc.). Among them, it is considered that the higher the charge density of the unit layer (unit layer), the higher the polarity and the higher the hydrophilicity. The charge density is preferably 0.25 or more, more preferably 0.6 or more. Examples of the layered mineral having such a charge density include smectite (charge density 0.25 to 0.6; negative charge), vermiculite (charge density 0.6 to 0.9; negative charge) and the like. In particular, synthetic fluoromica is preferable because it can be obtained with stable quality such as particle size. Among the synthetic fluorine mica, those that are swellable are preferable, and those that are free swell are more preferable.

又、上記の層状鉱物粒子のインターカレーション化合物(ピラードクリスタル等)や、イオン交換処理を施したもの、表面処理(シランカップリング処理、有機バインダとの複合化処理等)を施したものも使用することができる。   Also, intercalation compounds of the above-mentioned layered mineral particles (pillar crystals, etc.), those subjected to ion exchange treatment, and those subjected to surface treatment (silane coupling treatment, compounding treatment with organic binder, etc.) Can be used.

状層状鉱物粒子のサイズとしては、層中に含有されている状態で(膨潤工程、分散剥離工程を経た場合も含めて)、平均粒径(粒子の最大長)が20μm以下であり、又平均アスペクト比(粒子の最大長/粒子の厚さ)が20以上の薄層状であることが好ましく、平均粒径が5μm以下であり、平均アスペクト比が50以上であることが更に好ましく、平均粒径が1μm以下であり、平均アスペクト比が50以上であることが更に好ましい。粒子サイズが上記範囲にある場合、薄層状粒子の特徴である平面方向の連続性及び柔軟性が塗膜に付与され、クラックが入りにくく乾燥状態で強靭な塗膜とすることができる。また、粒子物を多く含有する塗布液においては、層状粘土鉱物の増粘効果によって、粒子物の沈降を抑制することができる。   As the size of the layered mineral particles, the average particle size (maximum particle length) is 20 μm or less in the state of being contained in the layer (including the case of undergoing the swelling process and dispersion peeling process). Preferably, the aspect ratio (maximum particle length / particle thickness) is 20 or more, the average particle size is 5 μm or less, the average aspect ratio is more preferably 50 or more, and the average particle size Is more preferably 1 μm or less and the average aspect ratio is 50 or more. When the particle size is in the above range, the continuity and flexibility in the planar direction, which are the characteristics of the thin layered particles, are imparted to the coating film, and it is difficult for cracks to occur, and a tough coating film can be obtained in a dry state. Moreover, in the coating liquid containing many particulate matters, sedimentation of particulate matter can be suppressed by the thickening effect of the layered clay mineral.

層状鉱物粒子を含む場合の含有量としては、層全体の1〜90質量%であることが好ましく、4〜80質量%であることがより好ましく、特に4〜50%質量%であることが好ましい。   When the layered mineral particles are included, the content is preferably 1 to 90% by mass of the entire layer, more preferably 4 to 80% by mass, and particularly preferably 4 to 50% by mass. .

特に膨潤性合成フッ素雲母やスメクタイトは少量の添加でも効果が見られるため好ましい。層状鉱物粒子は、塗布液に粉体で添加してもよいが、簡便な調液方法(メディア分散等の分散工程を必要としない)でも良好な分散度を得るために、層状鉱物粒子を単独で水に膨潤させたゲルを作成した後、塗布液に添加することが好ましい。   In particular, swellable synthetic fluorinated mica and smectite are preferable because they are effective even when added in a small amount. The layered mineral particles may be added as a powder to the coating solution, but in order to obtain a good degree of dispersion even with a simple preparation method (no need for a dispersion step such as media dispersion), the layered mineral particles are used alone. After the gel swollen in water is prepared, it is preferably added to the coating solution.

また、金属アルコキシドを用いた、いわゆるゾル−ゲル法による無機ポリマーもしくは有機−無機ハイブリッドポリマーも使用することができる。ゾル−ゲル法による無機ポリマーもしくは有機−無機ハイブリッドポリマーの形成については、例えば「ゾル−ゲル法の応用」(作花済夫著/アグネ承風社発行)に記載されているか、又は本書に引用されている文献に記載されている公知の方法を使用することができる。   Further, an inorganic polymer or an organic-inorganic hybrid polymer using a metal alkoxide by a so-called sol-gel method can also be used. The formation of an inorganic polymer or an organic-inorganic hybrid polymer by the sol-gel method is described in, for example, “Application of the sol-gel method” (Sakuo Sakuo / Published by Agne Jofusha) or cited in this book. Known methods described in the published literature can be used.

本発明に係る可視画付与層において、像様に熱または光を与えた領域の反射濃度が低下するのは、レーザー光等により短時間に急激な温度変化が生じるために、可視画付与層中に極微小なクラックを生じたり、層中にガスを包含するために観察光源の入射光が散乱されて、その結果印刷版材料表面の濃度が低下するものと推定される。   In the visible image imparting layer according to the present invention, the reflection density of the region where image-like heat or light is applied decreases because a rapid temperature change occurs in a short time due to laser light or the like. It is presumed that the microscopic cracks are generated in the layer, or the incident light of the observation light source is scattered because the gas is included in the layer, and as a result, the density of the surface of the printing plate material is lowered.

本発明の印刷版材料の好ましい態様としては、前述の表面を親水化処理されたアルミニウム基材、もしくは基材上に設けられた親水性層上に、画像形成層を設け、画像形成層またはそれ以外の基材上の構成層のいずれかに、光熱変換剤を含有する印刷版材料である。   As a preferable embodiment of the printing plate material of the present invention, an image forming layer is provided on an aluminum substrate whose surface has been hydrophilized, or a hydrophilic layer provided on the substrate, and the image forming layer or the same. A printing plate material containing a photothermal conversion agent in any of the constituent layers on the substrate other than the above.

可視画付与層は、基材の画像形成層側に設けられるが、画像形成層と別層として設けても良いが、塗布工程数の低減、光熱変換効率の向上の観点から、画像形成層と可視画付与層が1つの層として機能することも好ましい態様である。   The visible image providing layer is provided on the image forming layer side of the substrate, but may be provided as a separate layer from the image forming layer, but from the viewpoint of reducing the number of coating steps and improving the photothermal conversion efficiency, It is also a preferable aspect that the visible image providing layer functions as one layer.

画像形成層の上層として保護層を設けることもできる。保護層に用いる素材としては、水溶性樹脂、水分散性樹脂を好ましく用いることができる。   A protective layer may be provided as an upper layer of the image forming layer. As a material used for the protective layer, a water-soluble resin or a water-dispersible resin can be preferably used.

また、特開2002−019318号や特開2002−086948号に記載されている親水性オーバーコート層も好ましく用いることができる。保護層の付き量としては、0.01〜10g/m2であり、好ましくは0.1〜3g/m2であり、さらに好ましくは0.2〜2g/m2である。 Further, hydrophilic overcoat layers described in JP-A No. 2002-019318 and JP-A No. 2002-086948 can also be preferably used. The amount per the protective layer is 0.01 to 10 g / m 2, preferably from 0.1 to 3 g / m 2, more preferably from 0.2 to 2 g / m 2.

本発明においては保護層に可視画付与層の機能を付与することも出来る。   In the present invention, the function of a visible image imparting layer can be imparted to the protective layer.

画像形成層は、印刷機上現像可能な層である。   The image forming layer is a layer that can be developed on a printing press.

印刷機上現像可能とは、露光後、平版印刷における湿し水及びまたは印刷インキにより非画像部の画像形成層が除去され得ることをいう。印刷機上現像可能とするには、上述の感熱性素材、水溶性樹脂、水分散性樹脂などを含有させることにより得られる。   “Developable on a printing press” means that the image forming layer in the non-image area can be removed by dampening water and / or printing ink in lithographic printing after exposure. In order to make it developable on a printing press, it can be obtained by including the above-mentioned heat-sensitive material, water-soluble resin, water-dispersible resin and the like.

本発明の可視画付与層において、反射濃度を0.2以上減少させる好ましい態様としては、反射濃度を低下させる素材として、モンモリロナイト等の層状鉱物粒子を可視画付与層の全固形分の4〜50質量%程度の比率で添加する。これらは、水と混ぜることで膨潤し粘度の高い溶液のような状態を形成するため、前述の感熱性素材としてのポリエステルエマルジョン、水溶性の赤外吸収色素と水溶媒中で混合して可視画付与層兼画像形成層塗布液とすることができる。感熱性素材の固形分は40〜95%、赤外吸収色素は0.5〜30%のとなるのが好ましい。   In the visible image imparting layer of the present invention, as a preferred embodiment for reducing the reflection density by 0.2 or more, as a material for reducing the reflection density, layered mineral particles such as montmorillonite are used in an amount of 4 to 50 in the total solid content of the visible image imparting layer. Add at a ratio of about mass%. These are swelled by mixing with water to form a solution-like state, so the above-mentioned polyester emulsion as the heat-sensitive material, water-soluble infrared absorbing dye and water solvent are mixed in a visible image. It can be set as a coating liquid for an application layer / image forming layer. The solid content of the heat-sensitive material is preferably 40 to 95%, and the infrared absorbing dye is preferably 0.5 to 30%.

可視画付与層の付量としては、0.1〜10g/m2が好ましく、0.2〜5g/m2がより好ましい。 The amount with the visible image imparting layer is preferably 0.1~10g / m 2, 0.2~5g / m 2 is more preferable.

可視画付与層兼画像形成層塗布液を親水性表面を有する基材上に塗布後の乾燥は、20℃〜200℃で10秒〜30分程度で行うのが好ましい。   Drying after applying the coating solution for the visible image providing layer / image forming layer onto a substrate having a hydrophilic surface is preferably performed at 20 ° C. to 200 ° C. for about 10 seconds to 30 minutes.

その際、感熱性素材が熱により、その後に水洗で除去不可能な程度に軟化、溶融して親水性表面に密着しない条件に、温度と時間を調整することが必要であるが、上記の温度範囲のなかで調製することで可能となる。   At that time, it is necessary to adjust the temperature and time so that the heat-sensitive material is softened and melted to the extent that it cannot be removed by washing with water and does not adhere to the hydrophilic surface. It becomes possible by preparing within the range.

このような条件で形成された層は、比較的透明性が高く基材表面の濃度を損ねない。この印刷版材料に極大波長が830nmの赤外レーザー光により400mJ/cm2のエネルギー量で露光した場合、露光領域の可視画付与層兼画像形成層が粗面化、白濁化して非露光領域とのコントラストを生じさせることができ、その結果画像が目視で容易に確認が出来るようになる。 The layer formed under such conditions is relatively transparent and does not impair the concentration of the substrate surface. When this printing plate material is exposed with an energy amount of 400 mJ / cm 2 by an infrared laser beam having a maximum wavelength of 830 nm, the visible image providing layer and the image forming layer in the exposed region become roughened and white turbid, resulting in a non-exposed region. Thus, the image can be easily confirmed visually.

〔画像形成方法〕
本発明の画像形成方法には、印刷版としての画像形成と、可視画像の付与のための画像形成の、2つの画像形成工程が存在する。
(Image forming method)
The image forming method of the present invention includes two image forming steps, that is, image formation as a printing plate and image formation for providing a visible image.

これらを別々の工程で行っても良いが、簡略化の点から同時に行われることが好ましい。   These may be performed in separate steps, but are preferably performed simultaneously from the viewpoint of simplification.

本発明の画像形成方法においては、印刷版材料をレーザー光を用いて画像を形成するが、中でも特にサーマルレーザーによる露光によって画像形成を行うことが好ましい。   In the image forming method of the present invention, an image is formed on the printing plate material using laser light, and it is particularly preferable to perform image formation by exposure with a thermal laser.

例えば赤外及び/または近赤外領域で発光する、即ち700〜1500nmの波長範囲で発光するレーザーを使用した走査露光が好ましい。   For example, scanning exposure using a laser that emits light in the infrared and / or near infrared region, that is, emits light in the wavelength range of 700 to 1500 nm is preferable.

レーザーとしてはガスレーザーを用いてもよいが、近赤外領域で発光する半導体レーザーを使用することが特に好ましい。   A gas laser may be used as the laser, but it is particularly preferable to use a semiconductor laser that emits light in the near infrared region.

走査露光に好適な装置としては、この半導体レーザーを用いてコンピュータからの画像信号に応じて印刷版材料表面に画像を形成可能な装置であればどのような方式の装置であってもよい。   As an apparatus suitable for scanning exposure, any apparatus may be used as long as it can form an image on the surface of the printing plate material in accordance with an image signal from a computer using this semiconductor laser.

一般的には、(1)平板状保持機構に保持された印刷版材料に一本もしくは複数本のレーザービームを用いて2次元的な走査を行って印刷版材料全面を露光する方式、(2)固定された円筒状の保持機構の内側に、円筒面に沿って保持された印刷版材料に、円筒内部から一本もしくは複数本のレーザービームを用いて円筒の周方向(主走査方向)に走査しつつ、周方向に直角な方向(副走査方向)に移動させて印刷版材料全面を露光する方式、(3)回転体としての軸を中心に回転する円筒状ドラム表面に保持された印刷版材料に、円筒外部から一本もしくは複数本のレーザービームを用いてドラムの回転によって周方向(主走査方向)に走査しつつ、周方向に直角な方向(副走査方向)に移動させて印刷版材料全面を露光する方式が挙げられる。又特に印刷装置上で露光を行う装置においては、(3)の露光方式が用いられる。   In general, (1) a printing plate material held by a flat plate holding mechanism is exposed two-dimensionally using one or a plurality of laser beams to expose the entire surface of the printing plate material. ) The printing plate material held along the cylindrical surface inside the fixed cylindrical holding mechanism is used in the circumferential direction of the cylinder (main scanning direction) using one or more laser beams from inside the cylinder. A method in which the entire surface of the printing plate material is exposed by moving in a direction perpendicular to the circumferential direction (sub-scanning direction) while scanning, and (3) printing held on the surface of a cylindrical drum that rotates about an axis as a rotating body The plate material is printed by moving in the direction perpendicular to the circumferential direction (sub-scanning direction) while scanning in the circumferential direction (main scanning direction) by rotating the drum using one or multiple laser beams from the outside of the cylinder. A method that exposes the entire plate material That. In particular, in an apparatus that performs exposure on a printing apparatus, the exposure method (3) is used.

〔機上現像方法〕
印刷機上での画像形成層の未露光部の除去は、版胴を回転させながら水付けローラーやインクローラーを接触させて行なうことができるが、下記に挙げる例のような、もしくは、それ以外の種々のシークエンスによって行なうことができる。
[On-press development method]
The removal of the unexposed part of the image forming layer on the printing machine can be performed by contacting a watering roller or an ink roller while rotating the plate cylinder. The various sequences can be performed.

また、その際には、印刷時に必要な湿し水水量に対して、水量を増加させたり、減少させたりといった水量調整を行ってもよく、水量調整を多段階に分けて、もしくは、無段階に変化させて行ってもよい。
(1)印刷開始のシークエンスとして、水付けローラーを接触させて版胴を1回転〜数十回転回転させ、次いで、インクローラーを接触させて版胴を1回転〜数十回転回転させ、次いで、印刷を開始する。
(2)印刷開始のシークエンスとして、インクローラーを接触させて版胴を1回転〜数十回転回転させ、次いで、水付けローラーを接触させて版胴を1回転〜数十回転回転させ、次いで、印刷を開始する。
(3)印刷開始のシークエンスとして、水付けローラーとインクローラーとを実質的に同時に接触させて版胴を1回転〜数十回転回転させ、次いで、印刷を開始する。
In that case, the water amount may be adjusted by increasing or decreasing the amount of dampening water required for printing, and the water amount adjustment may be divided into multiple stages or steplessly. You may change it to.
(1) As a sequence for starting printing, a watering roller is brought into contact with the plate cylinder to make one to several dozen rotations, then an ink roller is brought into contact with the plate cylinder to make one to several dozen rotations, and then Start printing.
(2) As a sequence for starting printing, an ink roller is contacted to rotate the plate cylinder 1 to several tens of turns, then a watering roller is contacted to rotate the plate cylinder 1 to tens of rotations, Start printing.
(3) As a sequence for starting printing, the watering roller and the ink roller are brought into contact with each other substantially simultaneously to rotate the plate cylinder 1 to several tens of times, and then printing is started.

以下、実施例により本発明を具体的に説明するが、本発明はこれらに限定されない。なお、実施例中「部」は特に断りのないかぎり「質量部」を表す。   EXAMPLES Hereinafter, the present invention will be specifically described with reference to examples, but the present invention is not limited thereto. In the examples, “parts” represents “parts by mass” unless otherwise specified.

〔基材の作製〕
厚さ0.24mmのアルミニウム板(材質1050、調質H16)を、50℃の1質量%水酸化ナトリウム水溶液中に浸漬し、溶解量が2g/m2になるように溶解処理を行い水洗した後、25℃の0.1質量%塩酸水溶液中に30秒間浸漬し、中和処理した後水洗した。
[Preparation of substrate]
An aluminum plate (material 1050, tempered H16) having a thickness of 0.24 mm was immersed in a 1% by mass sodium hydroxide aqueous solution at 50 ° C., dissolved so that the dissolved amount became 2 g / m 2 , and washed with water. Then, it was immersed in 0.1 mass% hydrochloric acid aqueous solution at 25 ° C. for 30 seconds, neutralized, and then washed with water.

次いでこのアルミニウム板を、塩酸10g/L、アルミを0.5g/L含有する電解液により、正弦波の交流を用いて、ピーク電流密度が50A/dm2の条件で電解粗面化処理を行なった。 Next, this aluminum plate was subjected to an electrolytic surface roughening treatment with an electrolytic solution containing hydrochloric acid 10 g / L and aluminum 0.5 g / L using a sine wave alternating current and a peak current density of 50 A / dm 2. It was.

この際の電極と試料表面との距離は10mmとした。電解粗面化処理は12回に分割して行い、一回の処理電気量(陽極時)を40C/dm2とし、合計で480C/dm2の処理電気量(陽極時)とした。また、各回の粗面化処理の間に5秒間の休止時間を設けた。 The distance between the electrode and the sample surface at this time was 10 mm. Perform electrolytic graining treatment is divided into 12 times, and the quantity of electricity used in one treatment (at a positive polarity) as the 40C / dm 2, treatment quantity of electricity 480C / dm 2 in total (at a positive polarity). In addition, a rest period of 5 seconds was provided between each surface roughening treatment.

電解粗面化後は、50℃に保たれた1質量%水酸化ナトリウム水溶液中に浸漬して、粗面化された面のスマット含めた溶解量が1.2g/m2になるようにエッチングし、水洗し、次いで25℃に保たれた10%硫酸水溶液中に10秒間浸漬し、中和処理した後水洗した。次いで、20%硫酸水溶液中で、20Vの定電圧条件で電気量が150C/dm2となるように陽極酸化処理を行い、さらに水洗した。 After electrolytic surface roughening, it is immersed in a 1% by weight sodium hydroxide aqueous solution kept at 50 ° C. and etched so that the amount of dissolution including the smut of the roughened surface becomes 1.2 g / m 2. Then, it was washed with water, then immersed in a 10% aqueous sulfuric acid solution maintained at 25 ° C. for 10 seconds, neutralized, and then washed with water. Next, anodization was performed in a 20% sulfuric acid aqueous solution so that the amount of electricity was 150 C / dm 2 under a constant voltage condition of 20 V, followed by washing with water.

次いで、水洗後の表面水をスクイーズした後、70℃に保たれた1質量%のリン酸二水素ナトリウム水溶液に30秒間浸漬し、水洗を行った後に80℃で5分間乾燥し、基材1を得た。   Next, after squeezing the surface water after washing with water, it was immersed in a 1% by mass sodium dihydrogen phosphate aqueous solution maintained at 70 ° C. for 30 seconds, washed with water, dried at 80 ° C. for 5 minutes, Got.

基材1のRaは460nmであった(WYKO社製RST Plusを使用し、40倍で測定した)。   Ra of the substrate 1 was 460 nm (measured at 40 times using RST Plus manufactured by WYKO).

続いて、酢酸アンモニウム(関東化学社製)を固形分濃度0.1質量%の水溶液とし、90℃に液温を保った浴中に、撹拌しながら60秒浸漬処理後、水洗、乾燥した後、カルボキシメチルセルロース1150(ダイセル化学株式会社製)を固形分濃度0.1質量%の水溶液とし、80℃に液温を保った浴中に、撹拌しながら30秒浸漬処理後、水洗、乾燥した。   Subsequently, ammonium acetate (manufactured by Kanto Chemical Co., Inc.) was made into an aqueous solution having a solid concentration of 0.1% by mass, immersed in a bath maintained at 90 ° C. for 60 seconds with stirring, washed with water and dried. Carboxymethylcellulose 1150 (manufactured by Daicel Chemical Industries, Ltd.) was made into an aqueous solution having a solid content concentration of 0.1% by mass, immersed in a bath maintained at 80 ° C. for 30 seconds with stirring, washed with water and dried.

〔基材の着色〕
電解着色法を用い、陽極酸化膜を10μmつけて、金属イオン含有の電解液中で交流の定電圧法にて3〜10分処理することで陽極酸化中のポア内に金属微粒子を析出させた。
[Coloring of substrate]
Using an electrolytic coloring method, 10 μm of an anodic oxide film was applied, and metal fine particles were deposited in the pores during anodic oxidation by treatment for 3 to 10 minutes by an AC constant voltage method in an electrolytic solution containing metal ions. .

表面を黒くするために、硫酸第一錫を用い、下記の電解条件で着色を行った。   In order to make the surface black, stannous sulfate was used and coloring was performed under the following electrolytic conditions.

電解液:硫酸第一錫10g/L、硫酸10g/L、カテコール5g/L
処理温度28度、電圧15V、15秒立ち上げのソフトスタート
着色後のアルミニウム基材表面の反射濃度は0.75であった。濃度測定は、GretagMacbeth社製分光濃度計Spectrolinoを用いて、フィルター条件D65、観測視野2°、ホワイトベース:絶対白色、濃度標準:Status−Tで測定した値で400nmから700nmまでの、各20nm間隔の反射濃度を測定し、平均値を求めた。
Electrolytic solution: stannous sulfate 10 g / L, sulfuric acid 10 g / L, catechol 5 g / L
Soft start with a treatment temperature of 28 degrees, a voltage of 15 V, and a rise of 15 seconds. The reflection density on the surface of the aluminum substrate after coloring was 0.75. Concentration measurement was performed using a GretagMacbeth spectrodensitometer Spectrolino, with filter conditions D65, observation field 2 °, white base: absolute white, density standard: values measured at 400 nm to 700 nm at intervals of 20 nm, 20 nm intervals. The reflection density was measured and the average value was determined.

〔印刷版材料の作製〕
[印刷版材料1]
下記組成の素材を、十分に撹拌混合した後、純水で濃度を適宜希釈調整し、濾過して、固形分2.5質量%の可視画付与層兼画像形成層(1)の塗布液を得た。
[Preparation of printing plate materials]
[Printing plate material 1]
After sufficiently stirring and mixing the materials having the following composition, the concentration is appropriately adjusted by dilution with pure water and filtered to obtain a coating solution for the visible image providing layer / image forming layer (1) having a solid content of 2.5% by mass. Obtained.

次いで、親水性層上に、可視画付与層兼画像形成層(1)の塗布液を、ワイヤーバーを用いて乾燥後の付量が0.8g/m2となるように塗布し、温度50℃で3分間乾燥した。 Next, the coating solution for the visible image providing layer / image forming layer (1) is applied onto the hydrophilic layer using a wire bar so that the applied amount after drying is 0.8 g / m 2, and the temperature is 50. Dry at 3 ° C. for 3 minutes.

次いで、35℃24時間のエイジング処理を行って、印刷版材料1を得た。質量部比は乾燥後の固形分中の質量比率を表す。   Next, an aging treatment at 35 ° C. for 24 hours was performed to obtain a printing plate material 1. A mass part ratio represents the mass ratio in solid content after drying.

可視画付与層兼画像形成層(1)塗布液組成
感熱性素材:水分散型共重合ポリエステル樹脂エマルジョン(東洋紡績(株)社製、バイロナールPMD1200(lot.NoF22524)、固形分41質量%)
163部
水溶性樹脂:ポリアクリル酸ナトリウム、アクアリックDL522(日本触媒社製)の水溶液、固形分10質量% 50部
赤外吸収色素:ADS830WS(AmericanDyeSource 社製)の1質量%水溶液 800部
層状鉱物粒子:コープケミカル株式会社製親水性スメクタイトSWN 20部
[印刷版材料2〜6]
印刷版材料1における着色後のアルミニウム基材表面の反射濃度を表1の様に調整した以外は印刷版材料1と同様にして平版印刷版材料2〜6を得た。
Visible image imparting layer and image forming layer (1) Coating liquid composition Thermosensitive material: Water-dispersed copolyester resin emulsion (manufactured by Toyobo Co., Ltd., Vironal PMD1200 (lot. NoF22524), solid content 41% by mass)
163 parts Water-soluble resin: Sodium polyacrylate, Aquaric DL522 (manufactured by Nippon Shokubai Co., Ltd.), solid content 10 mass% 50 parts Infrared absorbing dye: 1 mass% aqueous solution of ADS830WS (American DyeSource) 800 parts layered mineral Particle: 20 parts hydrophilic smectite SWN manufactured by Coop Chemical Co., Ltd. [printing plate materials 2-6]
Lithographic printing plate materials 2 to 6 were obtained in the same manner as the printing plate material 1 except that the reflection density on the surface of the aluminum base after coloring in the printing plate material 1 was adjusted as shown in Table 1.

[印刷版材料7]
比較の印刷版材料として、印刷版材料1における可視画付与層兼画像形成層(1)の塗布液組成のうち、層状粘土鉱物粒子を除いた以外は同様にして、印刷版材料7を作製した。
[Printing plate material 7]
As a comparative printing plate material, a printing plate material 7 was prepared in the same manner except that the layered clay mineral particles were excluded from the coating solution composition of the visible image providing layer / image forming layer (1) in the printing plate material 1. .

[印刷版材料8]
印刷版材料1におけるアルミニウム基材表面の着色工程を省略した以外は印刷版材料1と同様にして平版印刷版材料8を得た。
[Printing plate material 8]
A lithographic printing plate material 8 was obtained in the same manner as the printing plate material 1 except that the step of coloring the surface of the aluminum substrate in the printing plate material 1 was omitted.

[印刷版材料9]
印刷版材料1における着色後のアルミニウム基材表面の反射濃度を表1の様に調整し、さらに可視画付与層件画像形成層の付き量を1.3/m2に変更した以外は印刷版材料1と同様にして平版印刷版材料9を得た。
[Printing plate material 9]
The printing plate material 1 except that the reflection density on the surface of the aluminum substrate after coloring is adjusted as shown in Table 1 and the amount of the visible image imparting layer and the image forming layer is changed to 1.3 / m 2. A lithographic printing plate material 9 was obtained in the same manner as Material 1.

〔赤外線レーザー露光による画像形成〕
印刷版材料を露光ドラムに巻付け固定した。露光には波長830nm、スポット径約18μmのレーザービームを用い、露光エネルギーを400mJ/cm2として、2400dpi(dpiとは、2.54cm当たりのドット数を表す)、175線で画像を形成した。露光した画像はベタ画像と1〜99%の網点画像とを含むものである。
[Image formation by infrared laser exposure]
The printing plate material was wound around the exposure drum and fixed. A laser beam having a wavelength of 830 nm and a spot diameter of about 18 μm was used for exposure, and the exposure energy was 400 mJ / cm 2 , and an image was formed with 2400 dpi (dpi represents the number of dots per 2.54 cm) and 175 lines. The exposed image includes a solid image and a 1 to 99% halftone dot image.

未露光領域の反射濃度及び露光領域の反射濃度を表1に示す。濃度測定は上記基材1と同様の方法により測定した。   Table 1 shows the reflection density of the unexposed area and the reflection density of the exposed area. The concentration was measured by the same method as that for the substrate 1.

〔印刷方法〕
印刷機:三菱重工業社製DAIYA1F−1を用いて、コート紙、湿し水:アストロマーク3(日研化学研究所社製)2質量%、インク(東洋インク社製TKハイユニティ紅)を使用して印刷を行った。印刷版材料は露光後そのままの状態で版胴に取り付け、PS版と同じ刷り出しシークエンスを用いて印刷した。
[Printing method]
Printing machine: DAIYA1F-1 manufactured by Mitsubishi Heavy Industries, Ltd., coated paper, dampening water: 2% by mass of Astro Mark 3 (manufactured by Nikken Chemical Research Co., Ltd.), ink (TK High Unity Red, manufactured by Toyo Ink Co., Ltd.) And printed. The printing plate material was attached to the plate cylinder as it was after exposure, and printed using the same printing sequence as the PS plate.

〔印刷評価〕
[機上現像性]
各印刷版材料について、刷り出しから何枚目の印刷で機上現像が終了するかを求めた。
[Printing evaluation]
[On-press developability]
For each printing plate material, the number of sheets printed from the start of printing was determined for completion of on-press development.

機上現像終了の指標は、印刷物上で非画像部の汚れがなく、かつ、ベタ画像部の濃度が1.6以上(MacbethRD918を用いてMのモードで測定し)であり、かつ、95%の網点画像が開いていることとした。良好な印刷が得られるまでの損紙の枚数を表1に示した。   The on-machine development end index is that the non-image area is not smudged on the printed material, the density of the solid image area is 1.6 or more (measured in the M mode using Macbeth RD918), and 95% The halftone dot image is open. Table 1 shows the number of damaged paper sheets until satisfactory printing is obtained.

[可視画性の評価]
赤外線レーザー露光による画像形成の印刷版材料をグレタグマクベス社製、標準光源装置プルーフライト(反射用)LD50−440モデルの光源下で観察を行い、網点ステップ部の画像を観察した。
[Evaluation of visibility]
The printing plate material for image formation by infrared laser exposure was observed under the light source of a standard light source device, Proflight (for reflection) LD50-440 model, manufactured by Gretag Macbeth Co., Ltd., and an image of a halftone dot step portion was observed.

その際の網点%の異なるステップ同士の階調差の判別性の可否を比較した。   At this time, the possibility of discriminating gradation differences between steps having different halftone dots% was compared.

評価基準
5:網点1%から99%の全領域において網点の階調差%が5%のステップの差を目視判別可能
4:網点5%から95%の領域において網点の階調差%が5%のステップの差を目視判別可能
3:網点10%から90%の領域において網点の階調差%が20%のステップの差を目視判別可能
2:網点0%(未露光部)と50%および100%(ベタ露光部)のステップの差を目視判別可能
1:網点0%(未露光部)と100%(ベタ露光部)のステップの差を目視判別可能
Evaluation Criteria 5: Step Difference with Halftone Dot Difference% of 5% in All Regions from 1% to 99% Halftone Dots can be Visually Discriminated 4: Halftone Dots in Regions with Halftone Dots of 5% to 95% Step difference with difference% of 5% can be visually discriminated 3: Step difference with halftone dot difference% of 20% can be visually discriminated in the area of 10% to 90% halftone dot 2: Halftone dot 0% ( The difference between the steps of the unexposed area and 50% and 100% (solid exposed area) can be visually discriminated. 1: The difference between the steps of 0% (unexposed area) and 100% (solid exposed area) can be visually discriminated.

Figure 2006007699
Figure 2006007699

表1の結果より、本発明の印刷版材料は、機上現像性に優れ、露光後の目視判別性が良好であり、可視画性に優れることが分かる。   From the results in Table 1, it can be seen that the printing plate material of the present invention is excellent in on-press developability, has good visual discrimination after exposure, and is excellent in visible image properties.

Claims (2)

親水性表面を有する基材上に、印刷機上現像可能な感熱画像形成層を有するネガ型印刷版材料であって、a)該親水性表面の可視光反射濃度が0.5以上であり、b)該基材の感熱画像形成層側に、極大波長が830nmの赤外レーザー光により400mJ/cm2のエネルギー量で露光する露光条件下において、露光部の可視光反射濃度を未露光部の可視光反射濃度に対して0.2以上減少し得る、可視画付与層を有することを特徴とする印刷版材料。 A negative type printing plate material having a thermal image forming layer developable on a printing machine on a substrate having a hydrophilic surface, wherein a) the visible light reflection density of the hydrophilic surface is 0.5 or more, b) On the thermal image forming layer side of the substrate, the visible light reflection density of the exposed part is set to the unexposed part under the exposure conditions in which the maximum wavelength is exposed to an infrared laser beam having a wavelength of 830 nm at an energy amount of 400 mJ / cm 2 . A printing plate material having a visible image providing layer which can be reduced by 0.2 or more with respect to the visible light reflection density. 請求項1に記載の印刷版材料をレーザー光で画像露光し、画像形成することを特徴とする画像形成方法。 An image forming method, wherein the printing plate material according to claim 1 is image-exposed with a laser beam to form an image.
JP2004191111A 2004-06-29 2004-06-29 Printing plate material and image forming method Pending JP2006007699A (en)