JP2003138235A - Pressure-sensitive adhesive composition having opacifying capability and pressure-sensitive adhesive sheet using the same - Google Patents

Pressure-sensitive adhesive composition having opacifying capability and pressure-sensitive adhesive sheet using the same

Info

Publication number
JP2003138235A
JP2003138235A JP2001333802A JP2001333802A JP2003138235A JP 2003138235 A JP2003138235 A JP 2003138235A JP 2001333802 A JP2001333802 A JP 2001333802A JP 2001333802 A JP2001333802 A JP 2001333802A JP 2003138235 A JP2003138235 A JP 2003138235A
Authority
JP
Japan
Prior art keywords
sensitive adhesive
pressure
sheet
adhesive sheet
parts
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2001333802A
Other languages
Japanese (ja)
Inventor
Takeshi Nagakura
毅 長倉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Saiden Chemical Industry Co Ltd
Original Assignee
Saiden Chemical Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Saiden Chemical Industry Co Ltd filed Critical Saiden Chemical Industry Co Ltd
Priority to JP2001333802A priority Critical patent/JP2003138235A/en
Publication of JP2003138235A publication Critical patent/JP2003138235A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To provide a pressure-sensitive adhesive composition which exhibits an excellent opacifying capability without detriment to pressure-sensitive adhesive properties of an acrylic pressure-sensitive adhesive even when a substrate sheet is transparent or even when the pressure-sensitive adhesive layer is thin; and a pressure-sensitive adhesive sheet using the same. SOLUTION: This pressure-sensitive adhesive composition contains a copolymer consisting mainly of structural units derived from an alkyl (meth)acrylate monomer, a particle-surface-treated aluminum powder having an average particle size of 5-50 μm and an aspect ratio of 50-200, and titanium oxide. The pressure- sensitive adhesive sheet is prepared by using the composition.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明の属する技術分野】本発明は、屋内外の装飾、マ
ーキングフィルム、ネームラベル等に使用される隠蔽性
を有する粘着剤組成物及びそれを用いた粘着シートに関
し、更に詳しくは、優れた粘着特性を有し、且つ貼り付
けた部分に対して被着体の下地の色や文字等を遮蔽す
る、優れた隠蔽性を有する粘着剤組成物及びそれを用い
た粘着シートに関するものである。なお、粘着シートと
は、テープ、ラベル、シート等を含めて表現する。
TECHNICAL FIELD The present invention relates to a pressure-sensitive adhesive composition having a concealing property, which is used for indoor and outdoor decorations, marking films, name labels and the like, and more particularly to a pressure-sensitive adhesive sheet using the same. The present invention relates to a pressure-sensitive adhesive composition that has characteristics and has an excellent concealing property that shields the underlying color and characters of an adherend from the adhered portion, and a pressure-sensitive adhesive sheet using the same. The adhesive sheet is expressed by including tapes, labels, sheets and the like.

【0002】[0002]

【従来の技術】従来、マーキングフィルム及びネームラ
ベルは、一般に、書類や整理棚等に見出しや表示用とし
て使用されている。特に、ネームラベルを書類に重ね貼
りした場合あるいは色の濃い被着体に貼り付ける場合、
下の文字あるいは下地の色が透けて、文字や色が不鮮明
になるという問題がある。この問題を解決するために、
粘着シートの隠蔽性を高めることが求められている。
2. Description of the Related Art Conventionally, marking films and name labels have been generally used as headings and displays on documents and shelves. Especially when the name label is overlaid on a document or when it is attached on a dark-colored adherend,
There is a problem that the letters and colors underneath become transparent and the letters and colors become unclear. to solve this problem,
It is required to improve the hiding power of the pressure-sensitive adhesive sheet.

【0003】粘着シートの隠蔽性を高めるために種々の
方法が考えられている。 例えば、基材シートに充填剤を
多量に添加する方法があるが、シートの強度が低下し、
破れ易く使用に耐え難い問題がある。更に、基材シート
を厚くする方法や粘着剤層を厚くする方法がある。基材
シートを厚くするとシートの腰が強過ぎるため、屈曲面
への接着が悪くなり剥がれ易い問題がある。粘着剤層を
厚くすると再剥離用に使用されるラベル等において、被
着体に糊残りを起す問題があり、コスト的にも問題があ
る。
Various methods have been considered to enhance the concealing property of the pressure-sensitive adhesive sheet. For example, there is a method of adding a large amount of filler to the base sheet, but the strength of the sheet decreases,
There is a problem that it breaks easily and cannot be used. Furthermore, there are a method of thickening the base material sheet and a method of thickening the pressure-sensitive adhesive layer. If the base sheet is made thick, the sheet becomes too stiff, and there is a problem in that the adhesion to the bent surface is poor and the base sheet is easily peeled off. If the pressure-sensitive adhesive layer is made thick, there is a problem in that a label or the like used for re-peeling causes adhesive residue on an adherend, which is also a cost problem.

【0004】次に、基材シートと粘着層の間に隠蔽性を
有する下塗り層を形成させる方法がある。例えば、特開
平7−11202号公報では、透明な延伸ポリプロピレ
ンフィルムの片面に印刷が施され、該印刷面に金属含有
白色インク層、粘着層が順次積層されてなる隠蔽性粘着
テープが開示されている。特開平8−104848号公
報では、フィルム基材の片面に、酸化チタンの顔料容積
濃度が50%以上である隠蔽層と粘着層とが順次形成し
てなる粘着テープが開示されている。隠蔽性は得られる
ものの、2工程のため作業性が悪く、経済性にも問題が
ある。
Next, there is a method of forming an undercoat layer having a hiding property between the base sheet and the adhesive layer. For example, Japanese Patent Laid-Open No. 7-11202 discloses a concealable pressure-sensitive adhesive tape in which a transparent stretched polypropylene film is printed on one side and a metal-containing white ink layer and an adhesive layer are sequentially laminated on the printed surface. There is. JP-A-8-104848 discloses a pressure-sensitive adhesive tape in which a concealing layer having a titanium oxide pigment volume concentration of 50% or more and a pressure-sensitive adhesive layer are sequentially formed on one surface of a film substrate. Although the concealing property is obtained, the workability is poor because of two steps, and there is a problem in economical efficiency.

【0005】更に、基材シートと粘着剤層を着色して隠
蔽性を付与する方法がある。例えば、特開平5−438
46号公報では着色された合成樹脂製テープもしくはシ
ートの片面に、ベージュ色に着色された粘着剤層が設け
られている粘着テープもしくはシートが開示されてい
る。特開平5−108011号公報では白色顔料が含有
するポリエチレンテレフタレート基材の裏面に、粘着剤
に白色顔料を含有する粘着剤層が積層されている粘着ラ
ベルが開示されている。特開平11−106713号公
報では合成樹脂シートの一面に、粘着ベースポリマーお
よびパール顔料からなる粘着剤が積層されている粘着シ
ートが開示されている。しかし、いずれも基材に顔料等
を添加して不透明にしているため隠蔽性は得られるもの
の、基材シートが透明な場合や粘着剤層が薄い場合には
隠蔽性が得られ難い問題がある。
Further, there is a method of coloring the base sheet and the pressure-sensitive adhesive layer to impart a hiding property. For example, JP-A-5-438
Japanese Patent Publication No. 46 discloses an adhesive tape or sheet in which a beige colored adhesive layer is provided on one surface of a colored synthetic resin tape or sheet. Japanese Unexamined Patent Publication (Kokai) No. 5-108011 discloses an adhesive label in which an adhesive layer containing a white pigment as an adhesive is laminated on the back surface of a polyethylene terephthalate substrate containing a white pigment. Japanese Patent Laid-Open No. 11-106713 discloses a pressure-sensitive adhesive sheet in which a pressure-sensitive adhesive comprising a pressure-sensitive adhesive base polymer and a pearl pigment is laminated on one surface of a synthetic resin sheet. However, in both cases, the hiding property is obtained because the substrate is made opaque by adding a pigment or the like, but there is a problem that the hiding property is difficult to obtain when the substrate sheet is transparent or the pressure-sensitive adhesive layer is thin. .

【0006】[0006]

【発明が解決しようとする課題】本発明の目的は、粘着
剤の粘着特性を損なうことなく、基材シートが透明な場
合でもあるいは粘着剤層が薄い場合でも、優れた隠蔽性
を有する粘着剤組成物及びそれを用いた粘着シートを提
供することである。
An object of the present invention is to provide a pressure-sensitive adhesive having excellent concealing properties, even if the base sheet is transparent or the pressure-sensitive adhesive layer is thin, without impairing the pressure-sensitive adhesive properties of the pressure-sensitive adhesive. To provide a composition and a pressure-sensitive adhesive sheet using the same.

【0007】[0007]

【課題を解決するための手段】本発明者らは、上記の問
題点を解決するために鋭意検討した結果、(メタ)アクリ
ル酸アルキルエステル単量体を主成分とする共重合体
に、特定物性を有する粒子表面が処理された微細な鱗片
状粒子であるアルミニウム粉と酸化チタンとを併用する
ことで、粘着特性を低下させることなく隠蔽性が向上す
ることを見出し、本発明を完成するに至った。
Means for Solving the Problems As a result of intensive studies to solve the above problems, the present inventors have identified a copolymer containing an alkyl (meth) acrylate ester as a main component as a main component. By using a combination of aluminum powder and titanium oxide, which are fine scale-like particles having a particle surface having physical properties treated, it is found that the hiding property is improved without lowering the adhesive property, and the present invention is completed. I arrived.

【0008】即ち、本発明は、(a)アルキル基の炭素
数が1〜12の(メタ)アクリル酸アルキルエステル単量
体を主成分とする共重合体の樹脂成分100重量部に対
して、(b)平均粒径が5〜50μm、アスペクト比が
50〜200である粒子表面が処理されたアルミニウム
粉0.1〜5重量部、及び(c)酸化チタン5〜60重
量部を含有してなる隠蔽性を有する粘着剤組成物であ
り、それを用いた粘着シートである。
That is, according to the present invention, (a) 100 parts by weight of a resin component of a copolymer whose main component is a (meth) acrylic acid alkyl ester monomer having an alkyl group having 1 to 12 carbon atoms, (B) 0.1 to 5 parts by weight of aluminum powder having an average particle size of 5 to 50 μm and an aspect ratio of 50 to 200, the surface of which has been treated, and (c) 5 to 60 parts by weight of titanium oxide. And a pressure-sensitive adhesive sheet using the same.

【0009】[0009]

【発明の実施の形態】以下、本発明の構成を詳細に説明
する。本発明に使用する(a)アルキル基の炭素数が1
〜12の(メタ)アクリル酸アルキルエステル単量体とし
ては、具体的にメチル(メタ)アクリレート、エチル(メ
タ)アクリレート、プロピル(メタ)アクリレート、ブチ
ル(メタ)アクリレート、イソブチル(メタ)アクリレー
ト、2−エチルヘキシル(メタ)アクリレート、オクチル
(メタ)アクリレート、イソオクチル(メタ)アクリレー
ト、イソノニル(メタ)アクリレート、ラウリル(メタ)ア
クリレート等が挙げられる。これらの群より選ばれる少
なくとも1種以上使用することができる。さらにその他
の共重合可能な不飽和基含有単量体を使用することがで
きる。その他の共重合可能な不飽和基含有単量体として
は、具体的に(メタ)アクリル酸、マレイン酸、クロト
ン酸、無水マレイン酸、ヒドロキシエチル(メタ)アクリ
レート、4−ヒドロキシブチルアクリレート、(メタ)ア
クリロニトリル、酢酸ビニル、プロピオン酸ビニル、バ
ーサチック酸ビニル、アルキル基の炭素数が13〜20
の(メタ)アクリル酸アルキルエステル等が挙げられ
る。これらの群より選ばれる少なくても1種以上使用す
ることができる。(メタ)アクリル酸アルキルエステル単
量体の使用量が80〜99.5重量%、その他の共重合
可能な不飽和基含有単量体が0.5〜20重量%からな
る共重合体が好ましい。
DETAILED DESCRIPTION OF THE INVENTION The constitution of the present invention will be described in detail below. The number of carbon atoms of the (a) alkyl group used in the present invention is 1
Specific examples of the (meth) acrylic acid alkyl ester monomer of 1 to 12 include methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, butyl (meth) acrylate, isobutyl (meth) acrylate, and 2 -Ethylhexyl (meth) acrylate, octyl
Examples thereof include (meth) acrylate, isooctyl (meth) acrylate, isononyl (meth) acrylate, and lauryl (meth) acrylate. At least one selected from these groups can be used. Furthermore, other copolymerizable unsaturated group-containing monomers can be used. Specific examples of the other copolymerizable unsaturated group-containing monomer include (meth) acrylic acid, maleic acid, crotonic acid, maleic anhydride, hydroxyethyl (meth) acrylate, 4-hydroxybutyl acrylate and (meth ) Acrylonitrile, vinyl acetate, vinyl propionate, vinyl versatate, alkyl group having 13 to 20 carbon atoms
(Meth) acrylic acid alkyl ester and the like. At least one selected from these groups can be used. A copolymer in which the amount of the (meth) acrylic acid alkyl ester monomer used is 80 to 99.5% by weight and the other copolymerizable unsaturated group-containing monomer is 0.5 to 20% by weight is preferable. .

【0010】本発明の共重合体は、通常、塊状重合反応
や溶液重合反応から得ることができる、好ましくは溶液
重合反応から得られたものである。溶液重合反応に使用
する溶剤としては、酢酸エチル、トルエン、ヘキサン、
アセトン等の有機溶剤が挙げられる。また溶液重合反応
に使用する重合開始剤としてはペンゾイルパーオキサイ
ド、ラウリルパーオキサイド等の過酸化物、アゾビスイ
ソブチロニトリル、アゾビスバレロニトリル等のアゾビ
ス化合物である油溶性の重合開始剤を使用することがで
きる。
The copolymer of the present invention can be usually obtained by a bulk polymerization reaction or a solution polymerization reaction, preferably a solution polymerization reaction. The solvent used in the solution polymerization reaction, ethyl acetate, toluene, hexane,
An organic solvent such as acetone can be used. Further, as the polymerization initiator used in the solution polymerization reaction, an oil-soluble polymerization initiator which is an azobis compound such as penzoyl peroxide and lauryl peroxide, and azobisisobutyronitrile and azobisvaleronitrile is used. can do.

【0011】本発明において隠蔽性を上げるために、ア
ルミニウム粉と酸化チタンとを併用することが必要であ
る。酸化チタンを単独で使用しても隠蔽性は得られる
が、より高い隠蔽性、特に透明な基材シートを使用する
場合や粘着剤の塗布量を減少させても高い隠蔽性を得る
ためには、酸化チタンの使用量を多くしなければ得られ
ない。酸化チタンの使用量が多過ぎると、粘着剤特性の
低下、長期間貼り合せた後に剥す際、被着体への糊残り
等を起こしやすい。しかし、アルミニウム粉を少量併用
することで酸化チタンの使用量が少なくてもより高い隠
蔽性が得られるし、全体としての顔料の使用量を減らす
ことが可能である。
In the present invention, it is necessary to use aluminum powder and titanium oxide together in order to improve the hiding power. Although the hiding property can be obtained by using titanium oxide alone, higher hiding property, particularly when using a transparent base material sheet or in order to obtain high hiding property even when the coating amount of the adhesive is reduced. However, it cannot be obtained unless the amount of titanium oxide used is increased. If the amount of titanium oxide used is too large, the adhesive properties are likely to deteriorate, and adhesive residue on the adherend is liable to occur when peeling after bonding for a long time. However, by using a small amount of aluminum powder in combination, higher concealing property can be obtained even when the amount of titanium oxide used is small, and it is possible to reduce the amount of pigment used as a whole.

【0012】本発明に使用する(b)アルミニウム粉
は、粒子表面が処理されていることが必要である。アル
ミニウム粉は水、酸、アルカリと反応して水素ガスを発
生することがあるため、アルミ粒子表面がカップリング
剤で表面処理加工されていることあるいはアルミ粒子表
面が高分子化合物で均一に樹脂コーティングされている
ことが、共重合体に存在する酸との反応を防ぐために必
要である。好ましくは樹脂コーティングタイプである。
アルミニウム粉の好ましい態様は、アルミペーストタイ
プである。該アルミペーストは、アルミニウムを微細な
鱗片状粒子に加工し、ミネラルスピリット、ソルベント
ナフサ、トルエン、キシレン等の有機溶剤でペースト状
にした金属顔料で、アルミ粒子が塗膜表層に浮かんで並
行に配列するリーフィングタイプと、アルミ粒子が塗膜
中 に一様に分散し平行に配列するノンリーフィングタ
イプとがあり、好ましくはノンリーフィングタイプのア
ルミペーストである。なお、アルミペーストは、市販さ
れている例えば旭化成(株)製のアルミペーストを使用
することができる。
The (b) aluminum powder used in the present invention is required to have its surface treated. Aluminum powder may react with water, acid and alkali to generate hydrogen gas, so the surface of aluminum particles should be surface treated with a coupling agent or the surface of aluminum particles should be uniformly coated with a polymer compound. Must be present to prevent reaction with the acids present in the copolymer. A resin coating type is preferred.
A preferred embodiment of the aluminum powder is an aluminum paste type. The aluminum paste is a metal pigment obtained by processing aluminum into fine scale-like particles and forming a paste with an organic solvent such as mineral spirit, solvent naphtha, toluene and xylene, and the aluminum particles float on the coating surface layer and are arranged in parallel. And a non-leafing type in which aluminum particles are uniformly dispersed in the coating film and arranged in parallel, and a non-leafing type aluminum paste is preferable. As the aluminum paste, a commercially available aluminum paste manufactured by Asahi Kasei Co., Ltd. can be used.

【0013】また、本発明に使用する(b)粒子表面が
処理されたアルミニウム粉は、隠蔽性を高めるために平
均粒径が5〜50μmであることが必要であり、好まし
くは、10〜30μmである。平均粒径5μmより小さ
い場合には十分な隠蔽性が得られなく、粒径が50μm
を超える場合は隠蔽性が低下する。更に隠蔽性を高める
ためにアスペクト比が50〜200であることが必要で
あり、好ましくは、60〜150である。アスペクト比
が50以下では十分な隠蔽性が得られなく、200を超
える場合は粘着剤に対する分散性が低下する。なお、平
均粒子径は、試料をミネラルスピリットに分散し、レー
ザー回折・散乱法を用いて求める。アスペクト比は、平
均粒子径/アルミ粒子の厚みから求める。
The (b) particle surface-treated aluminum powder used in the present invention is required to have an average particle size of 5 to 50 μm, and preferably 10 to 30 μm, in order to enhance the hiding property. Is. If the average particle size is smaller than 5 μm, sufficient hiding property cannot be obtained and the particle size is 50 μm.
When it exceeds, the concealing property is deteriorated. In order to further improve the hiding property, it is necessary that the aspect ratio is 50 to 200, preferably 60 to 150. When the aspect ratio is 50 or less, sufficient hiding property cannot be obtained, and when the aspect ratio exceeds 200, dispersibility in the pressure-sensitive adhesive decreases. The average particle size is obtained by dispersing the sample in mineral spirits and using the laser diffraction / scattering method. The aspect ratio is calculated from the average particle diameter / thickness of aluminum particles.

【0014】本発明に使用するアルミニウム粉の使用量
は、共重合体の樹脂成分100重量部に対して0.1〜
5重量部である。その使用量が0.1重量部よりも少な
い場合は隠蔽性の効果が低く、5重量部を超える場合は
隠蔽性は高くなるが、メタリック感が強くなり白色隠蔽
性が低下する。
The amount of aluminum powder used in the present invention is 0.1 to 100 parts by weight of the resin component of the copolymer.
5 parts by weight. If the amount used is less than 0.1 part by weight, the effect of the hiding property is low, and if it exceeds 5 parts by weight, the hiding property is high, but the metallic feeling becomes strong and the white hiding property is deteriorated.

【0015】本発明に使用する(c)酸化チタンとして
好ましい態様は、酸化チタンペーストタイプである。該
酸化チタンペーストは、アクリル系重合体を分散剤とし
て、酸化チタンをミネラルスピリット、ソルベントナフ
サ、トルエン、キシレン、アセトン、イソプロピールア
ルコール等の有機溶剤でペースト状にしたタイプであ
る。酸化チタンの使用量は、共重合体の樹脂成分100
重量部に対し5〜60重量部であり、好ましくは10〜
40重量部である。その使用量が5重量部よりも少ない
場合は隠蔽性の効果が低く、60重量部を超える場合は
隠蔽性は高くなるが、粘着特性が低下し、基材に対する
密着性も低下する。
A preferred embodiment of the (c) titanium oxide used in the present invention is a titanium oxide paste type. The titanium oxide paste is a type in which an acrylic polymer is used as a dispersant and titanium oxide is made into a paste with an organic solvent such as mineral spirit, solvent naphtha, toluene, xylene, acetone, and isopropyl alcohol. The amount of titanium oxide used is 100% of the resin component of the copolymer.
It is 5 to 60 parts by weight, preferably 10 to 10 parts by weight.
40 parts by weight. When the amount used is less than 5 parts by weight, the effect of the hiding property is low, and when it exceeds 60 parts by weight, the hiding property is high, but the adhesive property is deteriorated and the adhesion to the substrate is also decreased.

【0016】本発明に使用する粘着シートの基材は、各
種フィルム基材を使用することができる。具体的にはポ
リエチレンフィルム、ポリエステルフィルム、ポリプロ
ピレンフィルム、ポリ塩化ビニルフィルム、ポリカーボ
ネートフィルム、ポリアクリル系フィルム等が挙げられ
る。本発明の粘着シートは、屋内外の装飾テープ、マー
キングシート、ネームラベル等に使用することができ
る。
As the base material of the pressure-sensitive adhesive sheet used in the present invention, various film base materials can be used. Specific examples include polyethylene film, polyester film, polypropylene film, polyvinyl chloride film, polycarbonate film, polyacrylic film and the like. The pressure-sensitive adhesive sheet of the present invention can be used for indoor and outdoor decorative tapes, marking sheets, name labels and the like.

【0017】本発明の粘着剤組成物は、必要に応じて粘
着性や凝集力を調整する目的で、テルペン系、テルペン
−フェノール系、クマロンインデン系、スチレン系、ロ
ジン系、キシレン系、フェノール系、石油系等の粘着付
与樹脂、メラミン樹脂、架橋剤等を添加することができ
る。
The pressure-sensitive adhesive composition of the present invention is a terpene-based, terpene-phenol-based, coumarone-indene-based, styrene-based, rosin-based, xylene-based, phenol for the purpose of adjusting the tackiness and cohesive force as necessary. System, petroleum-based tackifying resins, melamine resins, cross-linking agents and the like can be added.

【0018】[0018]

【実施例】以下、本発明を実施例において詳しく説明す
るが、本発明はこれによって制限される物ではない。な
お、実施例および比較例における部もしくは%とあるも
のは特にことわりのない限り、重量部または重量%を示
す。
EXAMPLES The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, parts or% means parts by weight or% by weight, unless otherwise specified.

【0019】製造例1(共重合体A−1) 攪拌機、温度計、還流冷却器、窒素導入管を備えた反応
装置に、窒素ガスを封入後、酢酸エチル100部、ブチ
ルアクリレート98部、アクリル酸2部、重合開始剤ア
ゾビスイソブチロニトリル0.2部仕込む。攪拌しなが
ら窒素ガス気流中酢酸エチルの還流温度で8時間反応す
る。反応終了後、トルエン85部を添加して室温まで冷
却する。粘度2000mPa・s、固形分濃度35%な
る共重合体A−1を得た。
Production Example 1 (Copolymer A-1) After nitrogen gas was charged into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, 100 parts of ethyl acetate, 98 parts of butyl acrylate, and acryl. Charge 2 parts of acid and 0.2 part of polymerization initiator azobisisobutyronitrile. The mixture is reacted for 8 hours at the reflux temperature of ethyl acetate in a nitrogen gas stream with stirring. After completion of the reaction, 85 parts of toluene is added and cooled to room temperature. A copolymer A-1 having a viscosity of 2000 mPa · s and a solid content concentration of 35% was obtained.

【0020】製造例2(共重合体A−2)及び製造例3
(共重合体A−3) 共重合体A−2及びA−3は、表1に示すように共重合
体A−1の単量体の種類と量を変える以外は全く同様に
して得た。
Production Example 2 (Copolymer A-2) and Production Example 3
(Copolymer A-3) Copolymers A-2 and A-3 were obtained in exactly the same manner as shown in Table 1, except that the type and amount of the monomer of copolymer A-1 were changed. .

【0021】[0021]

【表1】 [Table 1]

【0022】表1中の単量体を下記の略号にて記載。 BA :ブチルアクリレート 2EHA:2エチルヘキシルアクリレート VAc :酢酸ビニル AAc :アクリル酸The monomers in Table 1 are described by the following abbreviations. BA: Butyl acrylate 2EHA: 2 ethylhexyl acrylate VAc: Vinyl acetate AAc: acrylic acid

【0023】実施例1 製造例1で得られた共重合体A−1を286部(樹脂分
で100部)、チタンペーストZC−300(酸化チタ
ン分濃度60%、御国色素(株)製)を25部(酸化チ
タン分で15部)、アルミペーストHR−7000(ポ
リマー被覆タイプ、平均粒径15μ、アスペクト比 1
00、蒸発残分 50%、旭化成(株)製)を0.6部
(アルミニウム分で0.3部)、硬化剤としてコロネー
トL−45(日本ポリウレタン(株)製)を1.0部配
合し、十分に混合して隠蔽性粘着剤を得た。該粘着剤を
塗膜厚さが20μm(dry)になるように離型紙に塗
工し、100℃の乾燥機で60秒間乾燥させた後、厚さ
50μmの透明ポリエステルフィルムに転写して粘着シ
ートを作製した。該粘着シートについて、隠蔽性、粘着
力、保持力、糊残り性、全光線透過率を試験した結果い
ずれも良好であった。結果は表2に示す。
Example 1 286 parts (100 parts by resin content) of the copolymer A-1 obtained in Production Example 1 and titanium paste ZC-300 (60% titanium oxide content concentration, manufactured by Mikuni Pigment Co., Ltd.) 25 parts (15 parts by titanium oxide content), aluminum paste HR-7000 (polymer coating type, average particle size 15 μ, aspect ratio 1
00, evaporation residue 50%, Asahi Kasei Co., Ltd. 0.6 part (aluminum 0.3 part), Coronate L-45 (Nippon Polyurethane Co., Ltd.) 1.0 part as a curing agent Then, the mixture was thoroughly mixed to obtain a concealing pressure-sensitive adhesive. The pressure-sensitive adhesive is applied to release paper so that the coating film thickness is 20 μm (dry), dried for 60 seconds in a dryer at 100 ° C., and then transferred to a transparent polyester film having a thickness of 50 μm to give a pressure-sensitive adhesive sheet. Was produced. The adhesive sheet was tested for hiding power, adhesive strength, holding power, adhesive residue, and total light transmittance, and all were good. The results are shown in Table 2.

【0024】実施例2〜4 実施例2〜4は表2に示す材料を用いて実施例1と同様
にして粘着シートを作製し、同様に試験をした。試験結
果はすべて良好であった。結果は表2に示す。
Examples 2 to 4 In Examples 2 to 4, pressure-sensitive adhesive sheets were prepared in the same manner as in Example 1 using the materials shown in Table 2 and tested in the same manner. All test results were good. The results are shown in Table 2.

【0025】実施例5 実施例5は実施例2のアルミペーストHR−7000を
アルミペーストCR−300(ポリマー被覆タイプ、平
均粒径20μ、アスペクト比60、旭化成(株))に変
える以外は実施例2と同様にして粘着シートを作製し、
同様に試験した。結果は良好であった。結果は表2に示
す。
Example 5 Example 5 is an example except that the aluminum paste HR-7000 of Example 2 was changed to aluminum paste CR-300 (polymer coating type, average particle size 20 μ, aspect ratio 60, Asahi Kasei Co., Ltd.). Prepare an adhesive sheet in the same manner as in 2,
It tested similarly. The results were good. The results are shown in Table 2.

【0026】比較例1 比較例1は実施例2のアルミペーストを除いた例であ
り、実施例1と同様にして粘着シートを作製し、試験し
た。結果は隠蔽性と全光線透過率が悪かった。結果は表
2に示す。
Comparative Example 1 Comparative Example 1 is an example excluding the aluminum paste of Example 2, and an adhesive sheet was prepared and tested in the same manner as in Example 1. As a result, the hiding property and the total light transmittance were poor. The results are shown in Table 2.

【0027】比較例2〜4 比較例2は、実施例1の酸化チタンペーストを除いた例
である。実施例1と同様にして粘着シートを作製し、試
験した。隠蔽性と全光線透過率が悪かった。比較例3
は、実施例2の酸化チタンペーストが本発明の範囲外で
ある例である。実施例1と同様にして粘着シートを作製
し、試験した。隠蔽性は得られたが、粘着力、糊残り性
が悪かった。比較例4は、実施例1のアルミペーストが
本発明の範囲外である例である。実施例1と同様にして
粘着シートを作製し、試験した。隠蔽性は得られたがア
ルミペーストの添加量が多くメタリック感が出てしま
い、白色隠蔽性が得られなかった。結果は表2に示す。
Comparative Examples 2 to 4 Comparative Example 2 is an example excluding the titanium oxide paste of Example 1. A pressure-sensitive adhesive sheet was prepared and tested in the same manner as in Example 1. The hiding power and total light transmittance were poor. Comparative Example 3
Is an example in which the titanium oxide paste of Example 2 is outside the scope of the present invention. A pressure-sensitive adhesive sheet was prepared and tested in the same manner as in Example 1. Although hiding power was obtained, the adhesive strength and adhesive residue were poor. Comparative Example 4 is an example in which the aluminum paste of Example 1 is outside the scope of the present invention. A pressure-sensitive adhesive sheet was prepared and tested in the same manner as in Example 1. Although the hiding property was obtained, a large amount of aluminum paste was added to give a metallic feeling, and the white hiding property was not obtained. The results are shown in Table 2.

【0028】比較例5 比較例5は実施例2のアルミペーストHR−7000を
アスペクト比が本発明の範囲外にあるアルミペーストC
R−50FM(ポリマー被覆タイプ、平均粒径20μ、
アスペクト比40、旭化成(株)製)に変更する以外は
実施例2と同様にして粘着シートを作製した。結果は隠
蔽性と全光線透過率が得られなかった。結果は表2に示
す。
Comparative Example 5 In Comparative Example 5, the aluminum paste HR-7000 of Example 2 was used as the aluminum paste C having an aspect ratio outside the range of the present invention.
R-50FM (polymer coating type, average particle size 20μ,
An adhesive sheet was produced in the same manner as in Example 2 except that the aspect ratio was changed to 40 and the product was changed to Asahi Kasei. As a result, hiding power and total light transmittance were not obtained. The results are shown in Table 2.

【0029】[0029]

【表2】 [Table 2]

【0030】表2中の略号は、下記の材料を示す。 L−45 :架橋剤、日本ポリウレタン(株)製、
商品名コロネートL−45 HR−7000:旭化成(株)製、商品名アルミペース
トHR−7000、ポリマー被覆タイプ、平均粒径15
μ、アスペクト比 100、蒸発残分 50% CR−300 :旭化成(株)、商品名アルミペースト
CR−300、ポリマー被覆タイプ、平均粒径20μ、
アスペクト比60 CR−50FM:旭化成(株)製、商品名アルミペース
トCR−50FM、ポリマー被覆タイプ、平均粒径20
μ、アスペクト比40 ZC−300 :御国色素(株)製、商品名チタンペー
ストZC−300、酸化チタン分濃度60%、
The abbreviations in Table 2 indicate the following materials. L-45: Crosslinking agent, manufactured by Nippon Polyurethane Industry Co., Ltd.
Product name Coronate L-45 HR-7000: Asahi Kasei Corporation, product name Aluminum Paste HR-7000, polymer coating type, average particle size 15
μ, aspect ratio 100, evaporation residue 50% CR-300: Asahi Kasei Co., Ltd., trade name Aluminum Paste CR-300, polymer coating type, average particle size 20 μ,
Aspect ratio 60 CR-50FM: Asahi Kasei Corporation, trade name Aluminum paste CR-50FM, polymer coating type, average particle size 20
μ, aspect ratio 40 ZC-300: manufactured by Mikuni Pigment Co., Ltd., trade name titanium paste ZC-300, titanium oxide concentration 60%,

【0031】試験方法 隠蔽性 表2及び3で示す粘着剤組成物を塗膜厚さが20μm
(dry)になるように離型紙に塗工し、100℃の乾
燥機で60秒間乾燥させた後、厚さ50μmの透明ポリ
エステルフィルムに転写して粘着シート試料を作製し
た。該試料を黒の文字が印字された白色台紙に貼り付
け、目視により隠蔽性を判断する。 ○:文字がほとんど見えない。 ▲:文字がほとんど見えないがシートにメタリック感が
ある。 △:文字がやや見える。 ×:文字がほとんど全部見える。
Test Method Concealment Property The pressure-sensitive adhesive compositions shown in Tables 2 and 3 were used to form coating films having a thickness of 20 μm.
The release paper was coated so as to be (dry), dried for 60 seconds in a dryer at 100 ° C., and then transferred to a transparent polyester film having a thickness of 50 μm to prepare an adhesive sheet sample. The sample is affixed to a white mount on which black characters are printed, and the hiding property is visually determined. ○: Almost no characters are visible. ▲: Almost no letters are visible, but the sheet has a metallic feel. Δ: Characters are slightly visible. X: Almost all characters are visible.

【0032】粘着力 隠蔽性試験で得られた粘着シート試料をJIS Z02
37に準じて23℃、65%HRの雰囲気中で、貼り、
貼り付け20分後にその温度内で、テンシロン万能引張
り試験機((株)オリエンテック製)にて180°引き
剥がし粘着力を測定する。粘着力は、7.5N/25m
m以上であることが好ましい。
The pressure-sensitive adhesive sheet sample obtained in the adhesive power hiding test was JIS Z02.
According to 37, paste in an atmosphere of 23 ° C, 65% HR,
Twenty minutes after application, 180 ° peeling adhesion is measured with a Tensilon universal tensile tester (manufactured by Orientec Co., Ltd.) within that temperature. Adhesive strength is 7.5N / 25m
It is preferably m or more.

【0033】保持力 隠蔽性試験で得られた粘着シート試料をJIS Z02
37に準じて、40℃の恒温槽中で1kg荷重を懸け落
下するまでの秒数を計る。5時間で落下しない場合は、
接着面のズレ具合を測定し、NCはズレ無しを表す。
The pressure-sensitive adhesive sheet sample obtained in the holding power hiding test was JIS Z02.
According to 37, measure the number of seconds until a load of 1 kg is dropped in a constant temperature bath at 40 ° C. If it does not fall in 5 hours,
The degree of deviation of the adhesive surface was measured, and NC represents no deviation.

【0034】糊残り性 隠蔽性試験で得られた粘着シート試料を23℃、65%
HRの雰囲気中で、予め表面を研磨し清浄にしたステン
レス板に貼り付け、室温に3日間放置した後、JIS
Z0237に準じてテンシロン万能引張り試験機
((株)オリエンテック製)にて180°引き剥がし、
糊残り具合を観察する。 ◎:糊残り無し ○:0〜5%糊残り △:6〜50% 糊残り ▲:51〜90%糊残り ×:91〜100%糊残り
The pressure-sensitive adhesive sheet sample obtained in the adhesive residue hiding test was tested at 23 ° C. and 65%.
In a HR atmosphere, attach it to a stainless steel plate whose surface has been polished and cleaned beforehand, and leave it at room temperature for 3 days, then JIS
According to Z0237, peeled by 180 ° with Tensilon universal tensile tester (manufactured by Orientec Co., Ltd.),
Observe the amount of glue left. ⊚: No glue residue ○: 0 to 5% glue residue △: 6 to 50% glue residue ▲: 51 to 90% glue residue ×: 91 to 100% glue residue

【0035】全光線透過率(%) 隠蔽性試験で得られた粘着シート試料を23℃、65%
RH中で、NDH2000 ヘーズメーター(日本電色
工業(株)製)を用いて全光線透過率(%)を測定す
る。20%以下であることが好ましい。
Total light transmittance (%) The pressure-sensitive adhesive sheet sample obtained in the hiding test was tested at 23 ° C. and 65%.
The total light transmittance (%) is measured in RH using an NDH2000 haze meter (manufactured by Nippon Denshoku Industries Co., Ltd.). It is preferably 20% or less.

【0036】[0036]

【発明の効果】本発明の隠蔽性を有する粘着剤組成物及
びそれを用いた粘着シートは、基材シートが透明な場合
でもあるいは粘着剤層が薄い場合でも優れた隠蔽性を有
するので隠蔽性シート、隠蔽性テープ、隠蔽性ラベルに
好適に使用することができる。
EFFECTS OF THE INVENTION The pressure-sensitive adhesive composition of the present invention and the pressure-sensitive adhesive sheet using the same have excellent masking ability even when the base sheet is transparent or when the pressure-sensitive adhesive layer is thin. It can be suitably used for a sheet, a masking tape, and a masking label.

Claims (2)

【特許請求の範囲】[Claims] 【請求項1】 (a)アルキル基の炭素数が1〜12の
(メタ)アクリル酸アルキルエステル単量体を主成分とす
る共重合体の樹脂成分100重量部に対して、(b)平
均粒径が5〜50μm、アスペクト比が50〜200で
ある粒子表面が処理されたアルミニウム粉0.1〜5重
量部、及び(c)酸化チタン5〜60重量部を含有して
なる隠蔽性を有する粘着剤組成物。
1. The (a) alkyl group having 1 to 12 carbon atoms
With respect to 100 parts by weight of the resin component of the copolymer mainly composed of the (meth) acrylic acid alkyl ester monomer, (b) the particle surface having an average particle diameter of 5 to 50 μm and an aspect ratio of 50 to 200 is A pressure-sensitive adhesive composition comprising 0.1 to 5 parts by weight of treated aluminum powder and (c) 5 to 60 parts by weight of titanium oxide.
【請求項2】 請求項1に記載の隠蔽性を有する粘着剤
組成物を基材シート上に、塗布、乾燥してなる粘着シー
ト。
2. A pressure-sensitive adhesive sheet obtained by applying and drying the pressure-sensitive adhesive composition having the concealing property according to claim 1 on a substrate sheet.
JP2001333802A 2001-10-31 2001-10-31 Pressure-sensitive adhesive composition having opacifying capability and pressure-sensitive adhesive sheet using the same Pending JP2003138235A (en)