GB2134282A - Optical elements having interference layers of ZnS and Al2O3 - Google Patents

Optical elements having interference layers of ZnS and Al2O3 Download PDF

Info

Publication number
GB2134282A
GB2134282A GB08402075A GB8402075A GB2134282A GB 2134282 A GB2134282 A GB 2134282A GB 08402075 A GB08402075 A GB 08402075A GB 8402075 A GB8402075 A GB 8402075A GB 2134282 A GB2134282 A GB 2134282A
Authority
GB
United Kingdom
Prior art keywords
layer
zns
layers
filters
substrates
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
GB08402075A
Other versions
GB8402075D0 (en
GB2134282B (en
Inventor
Reinhard Born
Werner Herbert
Hans-Georg Lotz
Norbert Rocker
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Balzers und Leybold Deutschland Holding AG
Original Assignee
Leybold Heraeus GmbH
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Leybold Heraeus GmbH filed Critical Leybold Heraeus GmbH
Publication of GB8402075D0 publication Critical patent/GB8402075D0/en
Publication of GB2134282A publication Critical patent/GB2134282A/en
Application granted granted Critical
Publication of GB2134282B publication Critical patent/GB2134282B/en
Expired legal-status Critical Current

Abstract

Optical elements, in particular filters, with interference layers comprise alternately slightly refractive and highly refractive dielectric layers deposited on a substrate 2. The first layer 1 applied to the substrate is Al2O3, constituting a slightly refractive layer, after which further layers 2 to n of ZnS and Al2O3 are applied in an alternating sequence. The last layer n consists of Al2O3. Such layers can be applied, at low temperatures, on flat substrates and, in particular, on sharply curved substrates. <IMAGE>

Description

SPECIFICATION Method of producing optical elements having interference layers The invention concerns a method of producing optical elements comprising interference layers of alternately slightly refractive and highly refractive dielectric materials on organic and inorganic substrates.
The production of interference layers has been known for a long time. Depending upon the requirements imposed on the end product, the thicknesses of the various layers generally lie between A/4 and A/8 of what is called the reference wavelength for which the system is designed. Examples of end products are optical elements such as subtractive and additive colour-separation filters, cold-light mirrors; heat-reflection filters, colour-temperature conversion filters, colour-temperature conversion reflectors, dielectric narrow-band filters and beam dividers.
The substrates used for these purposes consist of transparent or translucent materials such as glass, sapphire and plastics materials, as well as metals. A preferred plastics material is a product known as CR 39.
Optical elements of this kind have to meet specific requirements particularly as regards their optical properties, such as freedom from absorption, stability of the edge deposition etc., and as regards their mechanical and chemical properties such as galling resistance, adhesive strength, resistance to boiling, heat-resistance, as well as resistance to acids etc.
The requirements regarding the above-mentioned properties have increased in the course of time, so that the use of "soft" substances such as ZnS and cryolite which can be thermally vaporized, has been abandoned and "hard" oxide layers such as TiO2 and SiO2 for the vaporization of which electron-beam guns are used, have been introduced.
The layer materials previously used for interference layer systems were generally oxides of titanium, providing a highly refractive layer, and oxides of silicon, providing a slightly refractive layer. The vapour deposition operation was usually begun at < 1.3 X 10-2 Pa and at a substrate temperature of between 200 and 350"C. The period required for reaching the stated pressure and a temperature above 250"C could be as much as 90 minutes. Typical vapour deposition rates were approximately 1 5 A/sec for SiO2 and approximately 3 A/sec for TiO2. The vapour deposition time for the production of 1 5 layers in the case of a reference wavelength Ao of 400 nm could consequently be as much as 50 minutes in all.Furthermore, the highly heated substrates required a considerable cooling time which could be as much as 1 50 minutes. The known layer system could not be used either for heat-sensitive substrates such as plastics materials. In the case of flat substrate surfaces, resistance to boiling was in accordance with DIN 58196, Part 2 C 60, and in the case of sharply curved substrates, with DIN 58196 Part 2 C 1 5. In the case of sharply curved substrates and following treatment as called for in DIN 58196 Part 2 C 15, no adhesive strength at all, as specified in MIL C 675 C, is achieved.
The expressions "C60" and "cm 5" used in the details regarding resistance to boiling in DIN 58196 Part 2 mean than the layer could not automatically become detached during the boiling time of 60 minutes and 1 5 minutes respectively. Thus, TiO2/SiO2 coatings on flat substrates withstood the boiling tests for about 20 hours, but on sharply curved substrates (hemispherical surfaces) for only approximately 1 5 minutes. This does not, however, mean that the layer in question also resists the adhesion strength test in accordance with MIL C 675 C.
In particular, the last-mentioned adhesive strength test indicates specifically that the known layer system, applied to sharply curved substrates such as occur in particular in the case of optical lenses and cold-light mirrors exhibited no adhesive strength at all after a boiling time of only 1 5 minutes.
The object of the invention is, therefore, to provide a method of producing optical elements which is more economical to operate, enables boiling-resistant and adhesive coatings to be provided even on sharply curved substrate surfaces, and is furthermore suitable for the coating of plastics materials.
According to the invention this object is achieved by a method of producing optical elements, comprising interference layers of alternately slightly refractive and highly refractive dielectric materials on organic and inorganic substrates, the method including the steps of applying to the substrate a first and slightly refractive layer in Al203, applying subsequent layers of ZnS and Awl203 in an alternating sequence, and applying a final layer of Al203.
Whereas the application of an Awl203 layer as a covering or protective layer is known per se, novelty resides in the subjacent combination of layers including the feature that an Awl203 layer is applied to the substrate as a first layer. Surprisingly, it has been found that Al203 is very cleariy an advantageous adhesion-inducing medium which also develops it effect when vapour deposition is carried out at a very sharp angle as is the case, for example, at the edge of hemispherical glass cups. The reverse sequence wherein ZnS is applied as a first layer in no case leads to the advantageous adhesive strength as achieved with the procedure in accordance with the invention.The high adhesive strength and resistance to boiling are quite obviously achieved by the first Awl203 layer which acts as an adhesion-promoting medium and which may have a thickness of between 10 nm and 300 nm without resulting in any appreciable fluctuations in the values for adhesive strength and resistance to boiling. The remaining mechanical and chemical properties depend mainly upon the outer At203 layer which may have a thickness many times greater than the reference wavelength.
The method of the invention is suitable for the production of optical elements which are optically effective at wavelengths of between 0.39 m and Gium. It is known per se that ZnS can be used for optical elements that are optically effective between 0.2 m (commencement of intrinsic absorption) and 14 item. At203 can be used between 0.2pm (commencement of intrinsic absorption) and 7 ym. However, since Al203 tends to form cracks, the range is narrower for practical reasons. Surprisingly, the tendency to form cracks is so much reduced by the use of "soft" ZnS intermediate layers, that the range can be extended to approximately 6 ym.
When the method in accordance with the invention is being carried out, the pressure at the commencement of the vapour deposition process may be above 1.3 X 10-2 Pa, for example, in the range between this vaiue and 1.05 Pa. Furthermore, the coating process can be commenced with cold substrates, i.e. substrates at room temperature, so that a pre-heating period is not necessary. Consequently, the time preceding the commencement of vapour deposition is reduced to below 30 minutes; this is one-third of the prior art time mentioned above, assuming the details of the vapour deposition equipment to be identical.Because of the extremely high possible vapour deposition rate of ZnS which typically is approximately 20 A/Sec as compared with approximately 3 A/sec in the case of TiO2, the deposition time for fifteen layers can be reduced to below approximately 1 5 minutes. This is again less than one third of the corresponding prior art time mentioned above. Furthermore, as a result of the extremely low substrate temperature, no cooling time is required.
Therefore, given a comparable size of vapour deposition equipment, the number of charges increases roughly three-foid per unit of time, so that very much lower production costs are involved The method in accordance with the invention is carried out in a particularly advantageously manner at substrate temperatures of between 20"C and 180"C, and is expediently used at the lower end of the temperature range. In contrast to the prior art, this creates the possibility of also applying vapour deposits to plastics materials, for example, the material CR 39.
Due to the short pump-off time because of the lower vacuum, and because of the absence of a heating and cooling time and as a result of the higher deposition rates, a considerably shorter operating timecompared with that invoived in producing the previous oxide layers is achieved as previously mentioned.
Although it is known to produce interference layers by applying vapour deposits to substrate surfaces at extremely sharp angles, MgF2 or cryolite, in addition to ZnS, were applied, in a gas dispersion, as the coating material in the earlier systems, and ZnS could also be produced by separately depositing Zn and S vapours. However, the interference layer systems produced in this way have mechanical-chemical and thermal properties which fall well below those of the coatings produced in accordance with the present invention. On the other hand, in the producing of layer systems of exclusively "hard" oxide materials, it is found that when the materials are deposited at a sharp angle, the adhesive strength and resistance to boiling gradually drop to zero.
Using the method of the invention, the resistance to boiling on flat substrates as well as on sharply curved substrates (for example hemispherical substrates) were tested in accordance with DIN 58196 Part 2 C 60. In neither case was it found, even after a 60-hour continuous boiling test, that any loosening of the layers or diminution of the galling resistance and adhesive strength takes place, each of these properties being determined in accordance with MIL C675 C.
The low substrate temperature renders it possible, for the first time, to produce all optical elements with thin layers which permit absorption of approximately 1 % and may also be made of temperature-sensitive plastics materials, these layers having properties hitherto unknown except in the case of oxide materials. The only exceptions are temperature stability, which is limited by the plastics substrate, and performance in the boiling test.
A system of layers formed in accordance with the invention is illustrated in Fig. 1 of the accompanying drawings, in which a substrate, consisting of glass, is designated by the letter S.
The number of the layers corresponds to the sequence in which they are applied, n designating the top or covering layer which is made of Al2O3. The layers 1, 3. . ,n-2 and n are of Awl203, whereas layers 2, 4. ., n-1 consist of ZnS.
Example 1: Yellow Filters on Glass A vapour deposition installation, Type 1100 Q (produced by Messrs. Leybold-Heraeus GmbH of Hanau, Federal Republic of Germany), was fitted with disc-like glass substrates and was pumped off to a pressure of approximately 10 Pa in six minutes. The substrates were then cleaned in the known manner by means of a glow discharge. The equipment was then brought to a pressure of 5 x 10-3 Pa in a further 14 minutes, whereafter, a dispersing gas consisting of oxygen was introduced to establish a pressure of up to 2 x 10-2 Pa. Thereafter, Awl203 was degassed with an electron-beam gun for a period of two minutes until the pressure remained stable.Then A12O2 was applied as a first layer or adhesion promoting medium at a deposition rate of 1 3 /sec. Adjustment of the rate and control of the screens (for covering the vaporizing means) was carried out by the crystal oscillator method. Following the Awl203 layer, the first ZnS layer was deposited at a rate of 10 A/sec, while the AI2O3 was held at a raised temperature level by applying a small amount of energy. After the screen for the ZnS vaporizing means (thermal vaporizer) had been closed, the vaporizer means was likewise held at a raised temperature level by the application of a small amount of energy, and the electron-beam gun was again raised to vaporizing capacity.By repeating this coating procedure, a total of 1 7 separate layers of the condition and thickness indicated below were deposited.
1 sot layer Al203 1 X A/4 for 450 nm (reference wavelength) 2nd layer ZnS 0.45 x A/4 for 450 nm 3rd layer Al2O3 0.9 X A/4 for 450 nm 4th layer ZnS 0.95 X A/4 for 450 nm 5th layer AI2O3 1 x A/4 for 450 nm 6th layer ZnS 1 X A/4 for 450 nm 7th layer Al203 1 A/4 for 450 nm 8th layer ZnS 1 x X/4 for 450 nm 9th layer Al2O3 1 x A/4 for 450 nm 10th layer ZnS 1 X A/4 for 450 nm 11th layer Awl203 1 x A/4 for 450 nm 12th layer ZnS 1 X K/4 for 450 nm 1 3th layer AI2O3 1 x A/4 for 450 nm 14th layer ZnS 1 x A/4 for 450 nm 15th layer Awl203 1 x A/4 for 450 nm 16th layer ZnS 1 x A/4 for 450 nm 17th layer AT203 2.1 X A/4 for 450 nm The substrate assumed an average temperature of approximately 50"C.
Pressure was kept constant during the entire process. After the last (1 7th) layer had been deposited, the vaporizing means was switched off, and the equipment was flushed for a minute after the vaporizing means had cooled.
On all of the substrates, interference layers were obtained which passed the above-described tests as regards galling resistance, adhesive strength and resistance to boiling. Also achieved were an absorption of below 1% and a long-term stability of the edge deposit (sharp drop in the curve for the transmission measurement) of 10 nm from the start-up of the installation to its stoppage.
Example 2: Yellow Filters on CR 39: The procedure used in Example 1 was repeated with the single difference that use was made of substrates of the plastics material CR 39 instead of glass substrates. The plastics substrates became heated up from room temperature to approximately 50"C during the coating procedure.
The end product met the optical and mechanical requirements perfectly; it failed only in the boiling test. In particular, excellent resistance to galling and adhesive strength in accordance with MIL C 675 C were achieved.
Example 3: Cold-light Mirrors on Hemispherical Surface: The vapour deposition equipment used in Example 1 was provided with substrates for coldlight mirrors made of glass. The hemispherical bodies had a diameter of 32 and 54 mm and a central opening and were of the kind such as is used for projector lamps, for example.
The parameters for evacuation, cleaning by glow discharge and working pressure including the introduction of oxygen as a dispersing gas, as well as the deposition rates for the various layers correspond to those used in Example 1. The "raised temperature level" was such as to permit initiation of the spontaneous vaporization, but without the substances concerned being able to develop a vapour pressure sufficient for marked vaporization. By repetition of the various coating procedures, a total of 35 separate layers was deposited to give the condition and thicknesses indicated in the Table reproduced below.
The substrate temperature established itself at approximately 50"C on average. Pressure was kept constant during the entire process. After the last (35th) layer had been deposited, the vaporizing means was switched off and the equipment was flushed a minute after the vaporizing means had cooled.
On all of the substrates, interference layers were obtained which met the above-described tests as regards resistance to galling, adhesive strength and resistance to boiling. This was the case particularly as regards the cold-light mirrors having a diameter of 32 mm, which are particularly critical as regards resistance to boiling in view of their small radius of curvature. In addition, an absorption of below 1% was obtained as well as long-term stability of the edge deposit of 10 nm from the start-up to the stoppage of the equipment.
1st layer Al2O3 2.27 X A/4 for 400 nm 2nd layer ZnS 1.80 x A/4 for 400 nm 3rd layer AT203 1.67 X A/4 for 400 nm 4th layer ZnS 1.21 x A/4 for 400 nm 5th layer Al203 1.85 X A/4 for 400 nm 6th layer ZnS 1.63 x A/4 for 400 nm 7th layer Al2O3 1.81 x A/4 for 400 nm 8th layer ZnS 1.62 x X/4 for 400 nm 9th layer AI2O3 1.60 X A/4 for 400 nm 1 0th layer ZnS 1.78 x A/4 for 400 nm 11th layer AI2O3 1.65 X A/4 for 400 nm 12th layer ZnS 1.59 x A/4 for 400 nm 1 3th layer Al2O3 1.44 x A/4 for 400 nm 14th layer ZnS 1.63 x A/4 for 400 nm 15th layer Al2O2 1.52 x A/4 for 400 nm 16th layer ZnS 1.43 x A/4 for 400 nm 1 7th layer Al2O3 1.40 X A/4 for 400 nm 18th layer ZnS 1.34 X A/4 for 400 nm 1 9th layer AI2O3 1.40 X A/4 for 400 nm 20th layer ZnS 1.32 X X/4 for 400 nm 21st layer Al2O3 1.40 X A/4 for 400 nm 22nd layer ZnS 1.46 X A/4 for 400 nm 23rd layer A12O3 1.28 X A/4 for 400 nm 24th layer ZnS 1.12 x A/4 for 400 nm 25th layer Al2O3 1.13 X A/4 for 400 nm 26th layer ZnS 1.14 x A/4 for 400 nm 27th layer AI2O3 1.14 x A/4 for 400 nm 28th layer ZnS 1.08 X A/4 for 400 nm 29th layer Al203 1 O6 1.06 X A/4 for 400 nm 30th layer ZnS 0.91 x A/4 for 400 nm 31st layer AI2O3 1.08 X A/4 for 400 nm 32nd layer ZnS 1.26 x A/4 for 400 nm 33rd layer Al2O3 1.05 X A/4 for 400 nm 34th layer ZnS 0.55 x A/4 for 400 nm 35th layer Al2O3 1.06 X A/4 for 400 nm Example 4: Antireflex Layers The vapour deposition equipment used in Example 1 was provided with various sheet-like substrates having the dimensions 50 mm X 50 mm X 2 mm and consisting of the following materials: Glass (BK7) Polycarbonate ("Makrolon" (R.T.M.) produced by Bayer) CR 39.
The process parameters were the same as those of Example 1, with the exception that no oxygen was introduced and that the screens were controlled by photometric measurements.
A total of seven layers, as listed in the following Table, were formed by vapour deposition, and it was regarded as surprising that although two components had refractive indices greater than that of the substrate, perfect dereflection layers could be produced which also posses advantageous mechanical and chemical properties.
istlayerAI2O3 1 X A/4 for 913 nm 2nd layer ZnS 1 X h/4 for 127 nm 3rd layer Al203 1 X A/4 for 556 nm 4th layer ZnS 1 X A/4 for 264 nm 5th Awl203 1 X A/4 for 242 nm 6th layer ZnS 1 X A/4 for 619 nm 7thAl202 1 X A/4 for 616 nm The reflection properties are illustrated in the graph in Fig. 2 of the accompanying drawings, the reflection values being shown as percentages on the ordinate axis. There is a good wideband dereflection roughly in the zone 460 to 640 nm, and this can be regarded as very good for plastics substrates.

Claims (6)

1. A method of producing optical elements, comprising interference layers of alternately slightly refractive and highly refractive dielectric materials on organic and inorganic substrates, the method including the steps of applying to the substrate a first and slightly refractive layer of Al203, applying subsequent layers of ZnS and Awl203 in an alternating sequence, and applying a final layer of AI2O3.
2. A method according to Claim 1, wherein the first layer is applied at a substrate temperature of 20 to 180"C.
3. A method according to Claim 1, wherein the application of the layers is carried out by a vapour deposition process at pressures of between 1.3 X 10-3 and 1.05 Pa.
4. A method according to Claim 3, wherein Awl203 is applied at a vapour deposition rate of between 10 and 1 5 A/sec, and ZnS at a vapour deposition rate of between 10 and 30 A/sec.
5. The use of the method according to Claims 1 to 4 in the production of filters in the group comprising subtractive and additive colour-separation filters, cold-light mirrors, heat-reflection filters, colour-temperature conversion filters, colour-temperature conversion reflectors, dielectric narrow-band filters and light-beam dividers, in combination with substrates contained in the group comprising glass, sapphire and plastics materials.
6. A method according to Claim 1 for the production of optical elements and substantially as hereinbefore described.
GB08402075A 1983-01-28 1984-01-26 Optical elements having interference layers of zns and al2o3 Expired GB2134282B (en)