FI95238B - Anti - caking product, its use and method of handling it - Google Patents
Anti - caking product, its use and method of handling it Download PDFInfo
- Publication number
- FI95238B FI95238B FI891647A FI891647A FI95238B FI 95238 B FI95238 B FI 95238B FI 891647 A FI891647 A FI 891647A FI 891647 A FI891647 A FI 891647A FI 95238 B FI95238 B FI 95238B
- Authority
- FI
- Finland
- Prior art keywords
- weight
- product
- acid
- caking
- group
- Prior art date
Abstract
Description
9523895238
Paakkuuntumista estävä tuote, sen käyttö ja menetelmä sillä käsittelemiseksi Klumpmotverkande produkt, dess användning samt behandlingssätt med denna 5Anti-caking product, its use and method of handling it Product type, anti-caking product, use and method of treatment 5
Keksinnön kohteena on paakkuuntumista estävä tuote sekoitettavaksi 10 yhdisteiden kanssa, joita olennaisesti käytetään yksinkertaisena tai monimutkaisina lannoitteina, paakkuuntumisen estämiseksi.The invention relates to an anti-caking product for mixing with compounds which are essentially used as simple or complex fertilizers to prevent caking.
Keksinnön kohteena on myös tuotteen käyttö ja menetelmä tuotteiden käsittelemiseksi, joita olennaisesti käytetään yksinkertaisina tai 15 monimutkaisina lannoitteina, mainittujen tuotteiden paakkuuntumisen estämiseksi.The invention also relates to the use of the product and to a method for treating products which are essentially used as simple or complex fertilizers in order to prevent agglomeration of said products.
Keksintö kohdistuu paakkuuntumista estäviin tuotteisiin, sekä yksinkertaisten että monimutkaisten lannoitteiden kovettumisen estämisek-20 si.The invention relates to anti-caking products for preventing the hardening of both simple and complex fertilizers.
« • <«• <
Keksinnössä tarkastelluista yksinkertaisista lannoitteista voidaan mainita typen suolat kuten ammonium·, kalium- ja kalsiumnitraatit sekä monoammonium- ja diammoniumsulfaatit sekä ureaa sisältävät lan-25 noitteet.Among the simple fertilizers considered in the invention, mention may be made of nitrogen salts such as ammonium ·, potassium and calcium nitrates as well as monoammonium and diammonium sulphates and urea-containing lan-25 waxes.
* Monimutkaiset lannoitteet ovat typen, fosforin ja kaliumin joukosta valittujen alkuaineiden kaksi- tai kolmiosaisia seoksia. Nämä lannoitteet tunnistetaan tyyppiä NjPyKj olevilla kaavoilla, joissa 30 esiintyvät luvut x, y ja z tarkoittavat vastaavasti typen, fosfori (V)pentoksidin ja yhdisteen K20 prosentuaalisia osuuksia, joista monimutkainen lannoite koostuu.* Complex fertilizers are two- or three-part mixtures of elements selected from nitrogen, phosphorus and potassium. These fertilizers are identified by formulas of the type NjPyKj, in which the numbers x, y and z in each case denote the percentages of nitrogen, phosphorus (V) pentoxide and compound K20 of which the complex fertilizer consists.
• · >• ·>
Kaikki lannoitteet kovettuvat tai paakkuuntuvat yleensä varastoinnin 35 aikana.All fertilizers usually harden or agglomerate during storage.
Paakkuunturaistaipumus on voimakkaampaa tai heikompaa riippuen: 2 95238 rakeistusmenetelmästä, rakeiden voidessa esiintyä rakeina, jyväsinä, helminä, pieninä palloina, pieninä sylintereinä tai kappaleina; lannoite voidaan myös puristaa kokoon; raaka-aineiden, joista lannoite koostuu, alkuperästä; 5 - massaan ennen rakeistamista lisättyjen lisäaineiden luontees ta.The tendency to agglomerate is stronger or weaker depending on: 2 95238 granulation method, the granules may be in the form of granules, grains, beads, small spheres, small cylinders or pieces; the fertilizer can also be compressed; the origin of the raw materials of which the fertilizer is composed; 5 - the nature of the additives added to the pulp before granulation.
Lukuisista, paakkuuntumiseen vaikuttavista tekijöistä voidaan mainita: 10 - lannoitteen luontainen kosteus sekä ulkopuolinen kosteus, lämpötila, varastointiaika, varastointipaine, rakenteellinen polymorfismi, erityisesti ammoniumnitraatin 15 faasisiirtymät, rakeiden fysikaalinen muoto ja kemiallinen koostumus.Numerous factors influencing caking include: - the natural moisture of the fertilizer as well as the external moisture, temperature, storage time, storage pressure, structural polymorphism, in particular the phase transitions of ammonium nitrate 15, the physical form of the granules and the chemical composition.
Kovettuminen voi joskus saavuttaa sellaiset mittasuhteet, että lannoite muuttuu suurina möhkäleinä esiintyvään kovaan kiinteään muo-20 toon, joiden möhkäleiden rikkominen on erittäin vaikeata. Lannoitetta ei tällöin voida enää käyttää sellaisenaan. Siilovarastoinnin tapauksessa kovettumisen seurauksena muodostunut kuori on rikottava raskailla mekaanisilla laitteilla. Kovettuminen aiheuttaa huomattavia ja epäasianmukaisia ylimääräisiä kustannuksia, koska lannoitteen 25 varastointi, käsittely ja levitys vaikeutuvat.Curing can sometimes reach such proportions that the fertilizer changes to a hard solid form in the form of large clumps, the clumps of which are very difficult to break. In this case, the fertilizer can no longer be used as it is. In the case of silo storage, the shell formed as a result of hardening must be broken by heavy mechanical equipment. Curing imposes significant and inappropriate additional costs as storage, handling and application of fertilizer 25 becomes more difficult.
Kovettumisen estämiseksi ollaan ehdotettu orgaanisten aineiden kuten anionisten ja kationisten pinta-aktiivisten aineiden käyttöä, joista aineista on muodostettu öljymäisiä tai vahamaisia johdannaisia, ja 30 joita käytetään mahdollisesti yhdessä muiden aineiden kuten tiettyjen polymeerien tai ei-ionisten pinta-aktiivisten aineiden kanssa.In order to prevent curing, it has been proposed to use organic substances, such as anionic and cationic surfactants, which have been formed into oily or waxy derivatives, and which may be used in combination with other substances, such as certain polymers or nonionic surfactants.
Ehdotetuista kationisista pinta-aktiivisista aineista voidaan mainita aminoidut öljyt.Among the proposed cationic surfactants, mention may be made of aminated oils.
3535
Jo ehdotetuista anionisista pinta-aktiivisista aineista voidaan mainita 95238 3 amiini-alkyyliaryylisulfonaatit, joiden käyttö on kuvattu hakijalle kuuluvassa ranskalaisessa patenttijulkaisussa 2 460 706, happamien fosfaatti-estereiden aminosuolat, joiden käyttö yh-5 dessä mineraaliöljyn, mikrokiteisen vahan ja makrokiteisen vahan kanssa on kuvattu eurooppalaisessa patenttijulkaisussa 113 687, sekä happamien fosfaattiestereiden kaliumsuolat, joiden käyttö on kuvattu neuvostoliittolaisessa patenttijulkaisussa SU 10 1 131 859.Of the anionic surfactants already proposed, mention may be made of 95238 3 amine alkylarylsulfonates, the use of which is described in the applicant's French patent 2,460,706, amino salts of acid phosphate esters, the use of which in combination with a mineral oil, microcrystalline wax and in Patent Publication 113 687, and the potassium salts of acid phosphate esters, the use of which is described in Soviet Patent Publication SU 10 1 131 859.
Nämä tekniikan nykytason mukaiset tuotteet ovat yleensä tyydyttäviä, mutta käyttäjien jatkuvasti kasvavien vaatimusten seurauksena hakijat ovat jatkaneet niiden tutkimista yhä tehokkaampien tuotteiden 15 kehittämiseksi.These state-of-the-art products are generally satisfactory, but as a result of ever-increasing user demands, applicants have continued to research them to develop increasingly efficient products 15.
Keksinnön mukainen paakkuntumista estävä tuote on pääasiassa tunnettu siitä, että se on yhdistelmä, joka sisältää 15-85 % ainakin yhtä alkyyliaryylisulfonihapon amiinisuolaa ja 85-15 % ainakin yhtä hap-20 pofosfaattiesterin amiinisuolaa, jossa alkyyliaryylisulfonihappo on valittu ryhmästä, johon kuuluu mono-, di- tai trisulfonihapot, joissa alkyyliaryyliosa on valittu ryhmästä, johon kuuluu mono- ja poly-alkyylisubstituoitu bentseeni ja naftaleeni ja jossa happofosfaat-tiesterit vastaavat kaavaa, joka on valittu seuraavista kaavoista 25 • i oh <n O—P—O—(RjO)„j —R; 30 \ o—(RjO)n:—Rj 35 ja . 95238 4 oh an 5 /The anti-caking product according to the invention is mainly characterized in that it is a combination containing 15-85% of at least one amine salt of an alkylarylsulfonic acid and 85-15% of at least one amine salt of an acid phosphate ester, wherein the alkylarylsulfonic acid is selected from the group consisting of mono-, di - or trisulfonic acids in which the alkylaryl moiety is selected from the group consisting of mono- and polyalkyl-substituted benzene and naphthalene and in which the acid phosphate thiesters correspond to the formula selected from the following formulas: 25- i oh <n O-P-O- (RjO) „ j - R; 30 (o) (RjO) n: —Rj 35 and. 95238 4 oh an 5 /
0=P—OH0 = P-OH
\ O—fRiO),,:—R-« 10 jossa\ O — FRiO) ,,: - R- «10 where
Ri on alkyleeniryhmä, jossa on 2-4 hiiliatomia, 15 R2, R3 ja R*, on alkyyliryhmä, jossa on 8-20 hiiliatomia tai alkyy- liaryyliryhmä, jossa alkyloitu osuus sisältää 8-12 hiiliatomia ja n1( n2 ja n3 on luku 0-15.R 1 is an alkylene group having 2 to 4 carbon atoms, R 2, R 3 and R 1 are an alkyl group having 8 to 20 carbon atoms or an alkylaryl group in which the alkylated moiety contains 8 to 12 carbon atoms and n 1 (n 2 and n 3 is a number 0 -15.
20 Keksinnön mukaista tuotetta käytetään paakkuuntumista estävän tuotteen materiaalissa, jota olennaisesti käytetään lannoitteena, jolloin patenttivaatimuksen 1 mukaista paakkuuntumista estävää ainetta käytetään määrässä 0,03 - 0,4 paino-% mainitun materiaalin määrän suhteen.The product according to the invention is used in an anti-caking product material which is essentially used as a fertilizer, wherein the anti-caking agent according to claim 1 is used in an amount of 0.03 to 0.4% by weight relative to the amount of said material.
2525
Keksinnön mukainen menetelmä tuotteiden käsittelemiseksi on tunnettu siitä, että menetelmä käsittää seuraavat vaiheet: a) valmistetaan tuote käytettäväksi olennaisesti lannoitteena, 30 johon kuuluu tuotteen erottaminen valmistusvyöhykkeestä, kun tuote on olennaisesti saanut lopulliset mekaaniset ominaisuu-tensa ja b) olennaisesti erottamisen ajan hetkellä sisällytetään tuottee- 35 seen koostumus, joka käsittää ainakin yhtä alkyyliaryylisul- fonihapon amiinisuolaa ja ainakin yhtä happofosfaattiesterin amiinisuolaa 95238 5 ja jossa sisällyttämisvaihe suoritetaan ruiskuttamalla tuotteeseen 0,03-0,4 paino-% koostumusta tuotteeseen nähden ja jossa koostumus käsittää: 5 a) 5-35 paino-% yhdistelmää, joka sisältää 15-85 paino-% ainakin yhtä alkyyliaryylisulfonihapon amiinisuolaa ja 85-15 % ainakin yhtä happofosfaattiesterin amiinisuolaa, jossa alkyy-liaryylisulfonihappo valitaan ryhmästä, johon kuuluu mono-, di- tai trisulfonihapot, jossa alkyyliaryyliosa on valittu 10 ryhmästä, johon kuuluu mono- tai polyalkyylisubstituoitu bentseeni ja naftaleeni ja jossa happofosfaattiesterit vas-taavaat kaavaa, joka on valittu ryhmästä, johon kuuluu 15 0=p—o—(R|0)„1 — R-2 —CRlO)«2 R-3 20 ja OH al) /The method for treating products according to the invention is characterized in that the method comprises the steps of: a) preparing the product for use essentially as a fertilizer, comprising separating the product from the manufacturing zone when the product has substantially acquired its final mechanical properties; A composition comprising at least one amine salt of an alkylarylsulfonic acid and at least one amine salt of an acid phosphate ester 95238 5 and wherein the incorporation step is performed by injecting 0.03-0.4% by weight of the composition relative to the product and wherein the composition comprises: 5 a) 5-35% by weight -% of a combination containing 15-85% by weight of at least one amine salt of an alkylarylsulphonic acid and 85-15% by weight of at least one amine salt of an acid phosphate ester, wherein the alkylarylsulphonic acid is selected from the group consisting of mono-, di- or trisulphonic acids with an alkylaryl moiety is selected from the group consisting of mono- or polyalkyl-substituted benzene and naphthalene and wherein the acid phosphate esters correspond to the formula selected from the group consisting of 15 O = p-o- (R | 0) „1 - R-2 -CR10) «2 R-3 20 and OH al) /
25 0=P—OH25 0 = P-OH
\ O— CRlO)a3“^ jossa 30 • · » i\ O— CR10) a3 “^ where 30 • ·» i
Rj on alkyleeniryhmä, jossa on 2-4 hiiliatomia, R2, R3 ja R, on alkyyliryhmä, jossa on 8-20 hiiliatomia tai alkyy-35 liaryyliryhmä, jossa alkyloitu osuus sisältää 8-12 hiiliatomia ja n1( n2 ja n3 on 0-15; 6 95238 b) 0-10 % rasvahappoa tai yhtä sen suolaa; c) 20-90 paino-% mineraaliöljyä; ja 5 d) 0-50 paino-% makrokiteistä vahaa.R 1 is an alkylene group having 2 to 4 carbon atoms, R 2, R 3 and R 1 are an alkyl group having 8 to 20 carbon atoms or an alkylaryl group in which the alkylated moiety contains 8 to 12 carbon atoms and n 1 (n 2 and n 3 is 0 to 15 6 95238 b) 0-10% fatty acid or one of its salts; c) 20-90% by weight of mineral oil; and 5 d) 0-50% by weight of macrocrystalline wax.
Keksinnön puitteissa ollaan todettu yllättäen ja odottamattomasti, että kahden erilaisen paakkuuntumista estävän aineen, eli alkyyli-aryyli-sulfonihappojen aminosuolojen ja happamien fosfaattiesterei-10 den aminosuolojen, samanaikainen käyttö tehostaa molempien aineiden paakkuuntumista estäviä ominaisuuksia siten, että käytettäessä niitä keksinnön mukaisesti samanaikaisesti aktiivista materiaalia tarvitaan vähemmän saman paakkuuntumista estävän vaikutuksen saamiseksi kuin käytettäessä jompaa kumpaa ainetta yksinään. Tämän lisäksi mai-15 nittu samanaikainen käyttö tekee mahdolliseksi yleensä välttämättömien pinnoittavien ainepanosten pienentämisen tai jopa jättämisen kokonaan pois, tällöin kuitenkin sama paakkuuntumista estävä vaikutus saavuttaen.In the context of the invention, it has been surprisingly and unexpectedly found that the simultaneous use of two different anti-caking agents, i.e. amino salts of alkylarylsulfonic acids and amino salts of acidic phosphate esters, enhances the anti-caking properties of both substances. to obtain the same anti-caking effect as when either substance is used alone. In addition to this, the said simultaneous use makes it possible to reduce or even omit the generally necessary coatings in the coating material, in which case the same anti-caking effect is achieved.
20 Keksinnön avulla saadaan ratkaistuksi hyvin herkästi paakkuuntuvien lannoitteiden kuten sulfaatteja massassaan sisältävien ammoniumnit-raattien tai monimutkaisten lannoitteiden kovettumisongelma.The invention solves the problem of curing of very easily agglomerated fertilizers, such as ammonium nitrates containing sulphates in their mass or complex fertilizers.
Näin ollen keksinnön mukainen paakkuuntumista estävä aine yksinker-25 talsia ja monimutkaisia lannoitteita varten koostuu olennaisesti alkyyliaryyli-sulfonihappojen yhden tai useamman aminosuolan sekä happamien fosfaattiestereiden yhden tai useamman aminosuolan yhdistelmästä, jossa on tarvittaessa läsnä ylimäärä amiinia, ja joka yhdistelmä voidaan tuottaa neutraloimalla tai "ylineutraloimalla" yh-30 den tai useamman alkyyliaryylisulfonihapon sekä yhden tai useamman happaman fosfaattiesterin seos yhdellä tai useammalla amiinilla.Thus, the anti-caking agent according to the invention for simple and complex fertilizers consists essentially of a combination of one or more amino salts of alkylarylsulphonic acids and one or more amino salts of acidic phosphate esters, optionally with an excess of amine, and which combination can be produced by "neutralizing" a mixture of one or more alkylarylsulfonic acids and one or more acidic phosphate esters with one or more amines.
« Käsitteellä "alkyyliaryyli-sulfonihapot" tarkoitetaan mono-, di- tai trisulfonihappojen seoksia, joiden happojen aromaattinen osa, edul-35 lisesti bentseeni- tai naftaleeniosa, edullisemmin naftaleeniosa, on substituoitunut yhdellä tai useammalla alkyylillä, substitutioasteen ollessa synteesissä käytettyjä alkyylin ja aryylin moolisuhteita 95238 7 vastaava keskimääräinen aste. On selvää, että kunkin tarkastellun substitutioasteen, joka on tavallisesti 1-4, tapauksessa sulfonihap-pojen isomeerien monimutkaiset seokset ovat mahdollisia. Hiiliatomien kokonaislukumäärä alkyyliosassa ei ole suurempi kuin 16 tarkas-5 tellussa seoksessa.The term "alkylarylsulfonic acids" means mixtures of mono-, di- or trisulfonic acids in which the aromatic moiety of the acids, preferably the benzene or naphthalene moiety, more preferably the naphthalene moiety, is substituted with one or more alkyls, the degree of substitution being 95 alkyls used in the synthesis. 7 corresponding average degree. It will be appreciated that for each degree of substitution considered, which is usually 1 to 4, complex mixtures of sulfonic acid isomers are possible. The total number of carbon atoms in the alkyl moiety does not exceed 16 in the mixture examined.
Mainittakoon esimerkiksi, että 1,3-isopropyyli-naftaleeni-sulfoni-hapon tapauksessa isopropyylin ja naftaleenin keskimääräinen moolisuhde on 1,3.For example, in the case of 1,3-isopropyl-naphthalenesulfonic acid, the average molar ratio of isopropyl to naphthalene is 1.3.
10 Käsitteen "happamien fosfaattien esterit" mukaiset yhdisteet voidaan valmistaa saattamalla hydroksyyliryhmän käsittävä yhdiste kuten alkoholi, alkyylifenoli tai alkyylinaftoli reagoimaan suoraan esimerkiksi fosforipentoksidin kanssa, ja edullisimpia tämän käsitteen 15 mukaisia yhdisteitä ovat ne, joilla on seuraavat yleiset kaavat:Compounds of the term "esters of acid phosphates" may be prepared by reacting a compound having a hydroxyl group such as alcohol, alkylphenol or alkylnaphthol directly with, for example, phosphorus pentoxide, and the most preferred compounds of this concept are those having the following general formulas:
^°H .OH^ ° H .OH
° " “ (Rl°)nl " r2 ja O - P-OH° "" (R10) nl "r2 and O - P-OH
20 ° " <Rl0)n2 - r3 - (RX0)n3 - R420 ° "<R10) n2 - r3 - (RX0) n3 - R4
(I) (ID(I) (ID
joissa 25 R·! tarkoittaa 2-4 hiiliatomia käsittävää alkyleeniryhmää;where 25 R ·! represents an alkylene group having 2 to 4 carbon atoms;
Ra, F-3 ja Ra tarkoittavat 8-20 hiiliatomia käsittävää alkyyliryhmää tai alkyyliaryyliryhmää, jonka alkyloidussa osassa on 8-12 hiiliato-30 mia, ; ja ni>n2 Ja n3 tarkoittavat lukua 0-15, edullisesti 0-5.Ra, F-3 and Ra represent an alkyl group having 8 to 20 carbon atoms or an alkylaryl group having 8 to 12 carbon atoms in the alkylated moiety; and n1> n2 and n3 are 0-15, preferably 0-5.
Edellä mainittu reaktio näiden estereiden valmistamiseksi johtaa 35 yleensä mono- ja diestereiden seoksiin.The above reaction to prepare these esters generally results in mixtures of mono- and diesters.
8 952388 95238
Taloudellisista syistä valitaan usein hydroksyyliryhmän käsittävien yhdisteiden seos, esimerkiksi rasva-alkoholien seos.For economic reasons, a mixture of compounds having a hydroxyl group, for example a mixture of fatty alcohols, is often chosen.
Keksinnön mukaisen paakkuuntumista estävän tuotteen valmistamiseksi 5 muodostetaan alkyyliaryyli-sulfonihappojen ja happamien fosfaatti -estereiden seos, joka tämän jälkeen neutraloidaan tai jopa "ylineut-raloidaan" yhdellä tai useammalla amiinilla.To prepare the anti-caking product according to the invention, a mixture of alkylarylsulfonic acids and acidic phosphate esters is formed, which is then neutralized or even "over-neutralized" with one or more amines.
Amiinina käytetään edullisesti alkyyliamiineja, sykloalkyyliamiineja 10 tai aromaattisia amiineja ja mahdollisesti alkanoliamiineja; mainitut amiinit voivat olla primäärisiä, sekundäärisiä tai tertiäärisiä.Preferred amines are alkylamines, cycloalkylamines or aromatic amines and optionally alkanolamines; said amines may be primary, secondary or tertiary.
Amiini voi olla oksialkylenoituja.The amine may be oxyalkylenated.
15 Valmistukseen käytetään edullisesti rasva-alkyyliamiineja ja edullisesti alkyyliamiineja tai tällaisten amiinien seoksia, jotka amiinit käsittävät 12-20 hiiliatomia. Hyviin tuloksiin päästään teknisellä stearyyliamiinilla ja hydratun talin amiinilla.Fatty alkylamines and preferably alkylamines or mixtures of such amines comprising 12 to 20 carbon atoms are preferably used in the preparation. Good results are obtained with technical stearylamine and hydrogenated tallow amine.
20 Ylineutraloinnin tapauksessa amiinin molaarinen ylimäärä on korkeintaan 25 %, ja se rajoitetaan edullisesti 10 %:ksi.In the case of over-neutralization, the molar excess of amine is at most 25% and is preferably limited to 10%.
Keksintö kohdistuu samoin paakkuuntumista estäviin valmisteisiin, jotka käsittävät edellä mainittujen, keksinnön mukaisten paakkuun-• 25 tumista estävien tuotteiden lisäksi vähintään yhtä muuta paakkuun tumista estävää tuotetta, joka valitaan edullisesti rasvahappojen ja niiden suolojen sekä vähintään yhden sekoittamista helpottavan aineen joukosta. Tämä sekoittamista helpottava aine valitaan edullisesti joukosta, joka koostuu mineraaliöljyistä sekä niiden seoksista 30 makrokiteisten vahojen kanssa.The invention likewise relates to anti-caking preparations which, in addition to the above-mentioned anti-caking products according to the invention, comprise at least one other anti-caking product, preferably selected from fatty acids and their salts and at least one mixing aid. This mixing aid is preferably selected from the group consisting of mineral oils and mixtures thereof with macrocrystalline waxes.
Rasvahappoina käytetään edullisesti 12-20 hiiliatomia käsittäviä rasvahappoja, edullisesti steariinihappoa.As the fatty acids, fatty acids having 12 to 20 carbon atoms, preferably stearic acid, are preferably used.
35 Rasvahappojen suoloina käytetään edullisesti kalsium- tai magnesium-suoloja, mielellään alumiinisuoloja. Erityisen edullisia ovat alu- 95258 9 miinisuolat, joissa alumiinin ja steariinihapon moolisuhde on arvon 2 läheisyydessä.Calcium or magnesium salts, preferably aluminum salts, are preferably used as salts of fatty acids. Particularly preferred are the aluminum salts of aluminum, in which the molar ratio of aluminum to stearic acid is close to 2.
Yleensä käytetään öljyjä, jotka ovat luonteeltaan paraffiinisia tai 5 nafteenisia, esimerkiksi nafteeniöljyä, jota yhtiö NYNAS Company myy tavaramerkkinä NYTEX, ja jolla on seuraavat ominaisuudet: ‘ tiheys : 0,894 kinemaattinen viskositeetti : 23 cSt 10 hiilivetykoostumus aromaatit : 10 % nafteenit : 46 % paraffiinit : 44 %, tai 15 - paraffiiniöljyä, jota yhtiö BP France markkinoi tavaramerkkinä ENERPAR, ja jolla on seuraavat ominaisuudet: tiheys : 0,925 kinemaattinen viskositeetti 40 °C:ssa : 620 cSt hiilivetykoostumus : 20 aromaatit : 12 % nafteenit : 22 % paraffiinit : 66 %.Generally, oils are used which are paraffinic or naphthenic in nature, for example naphthenic oil sold by NYNAS Company under the trademark NYTEX and having the following characteristics: density: 0.894 kinematic viscosity: 23 cSt 10 hydrocarbon composition aromatics: 10% naphthenes: 46% paraffins: 44%, or 15 - paraffin oil marketed by BP France under the trademark ENERPAR and having the following characteristics: density: 0,925 kinematic viscosity at 40 ° C: 620 cSt hydrocarbon composition: 20 aromatics: 12% naphthenes: 22% paraffins: 66% .
25 Kun valmiste muodostetaan makrokiteisen vahan avulla, niin tällöin käytetään edullisesti paraffiinivahaa, jolla on seuraavat ominaisuudet:When the preparation is formed by means of a macrocrystalline wax, paraffin wax having the following properties is preferably used:
sulamispiste : 58-60 eCmelting point: 58-60 eC
kinemaattinen viskositeetti 100 °C:ssa : 9 cSt 30 tunkeutuma 25 °C:ssa : 16 '' tarttumislämpötila : 40.kinematic viscosity at 100 ° C: 9 cSt 30 penetration at 25 ° C: 16 '' adhesion temperature: 40.
Edellä mainitut keksinnön mukaiset paakkuuntumista estävät valmisteet ovat tavallisesti alla olevassa taulukossa A määriteltyä tyyp-35 piä I tai II, jotka eroavat toisistaan aineosien osuuksien suhteen.The above-mentioned anti-caking preparations according to the invention are usually type I or II as defined in Table A below, which differ in the proportions of the ingredients.
TAULUKKO ATABLE A
10 95238 ————————— ^——_H——)10 95238 ————————— ^ ——_ H——)
Aineosa, paino-% Tyypin I Tyypin IIIngredient,% by weight Type I Type II
I koostumus koostumusI composition composition
Paakkuuntumista estävä tuote 5-35 60 - 100 (keksinnön mukainen)Anti-caking product 5-35 60 - 100 (according to the invention)
Rasvahappo tai sen jokin suola 0-10 0-10Fatty acid or a salt thereof 0-10 0-10
Mineraaliöljy 20-90 0-30Mineral oil 20-90 0-30
Makrokiteinen vaha 0 - 50 0 -15 10Macrocrystalline wax 0 - 50 0 -15 10
Tyypeissä I ja II keksinnön mukainen paakkuuntumista estävä tuote käsittää: - 15-85 % alkyyliaryylisulfonihappoja, 15 - 85-15 % happamia fosfaattiestereitä, ja edullisesti - 30-70 % alkyyliaryylisulfonihappoja, - 70-30 % happamia fosfaattiestereitä.In types I and II, the anti-caking product according to the invention comprises: - 15-85% of alkylarylsulfonic acids, 15-85-15% of acidic phosphate esters, and preferably - 30-70% of alkylarylsulfonic acids, - 70-30% of acidic phosphate esters.
< 20 Keksinnön mukainen paakkuuntumista estävä käsittely on tunnettu siitä, että yksinkertaiseen tai monimutkaiseen lannoitteeseen lisätään edullisesti rummun tai leijupetin ulostulossa, jossa käsiteltävä tuote on jo saavuttanut lähes kaikki lopulliset mekaaniset ominai-suutensa, tehokas määrä keksinnön mukaista paakkuuntumista estävää 25 tuotetta, jota käytetään edullisesti keksinnön mukaisena paakkuuntumista estävänä valmisteena.The anti-caking treatment according to the invention is characterized in that an effective amount of the anti-caking product according to the invention is preferably added to a simple or complex fertilizer at the outlet of a drum or fluidized bed where the product to be treated has already reached almost all final mechanical properties. as an anti-caking agent in accordance with
Edellä mainittu tehokas määrä keksinnön mukaista tuotetta on 0,03-0,4 % yksinkertaisen tai monimutkaisen lannoitteen painosta 30 laskien.The above-mentioned effective amount of the product according to the invention is 0.03 to 0.4% based on the weight of the simple or complex fertilizer.
Erityisemmin, yksinkertaiseen tai monimutkaiseen lannoitteeseen voidaan sisällyttää sumuttamalla joko tyyppiä I olevaa paakkuuntumista estävää 35 valmistetta määränä, joka on 0,03-0,4 % käsiteltävän tuotteen painosta laskien. Ennen tätä sumuttamista tai sen jälkeen voi- 95258 11 daan toteuttaa pinnoittaminen liidun, piimään, talkin, savien ja muiden vastaavien joukosta valitulla aineella; tai niinkutsuttu seostettu aine-erä, joka on saatu käsittelemällä liidun, piimään, talkin ja savien joukosta valittua mate-5 riaalia tyyppiä 11 olevalla paakkuuntumista estävällä valmis teella, tyyppiä 11 olevan valmisteen osuuden kyseisen materiaalin suhteen ollessa 1-10 paino-%, edullisesti 1-6 paino-%, jota seostettua aine-erää käytetään pinnoitteena suhteessa 0,1-1 %, edullisesti 0,2-0,6 % käsiteltävän tuotteen painosta las-10 kien.More specifically, a simple or complex fertilizer can be incorporated by spraying either a type I anti-caking agent in an amount of 0.03 to 0.4% by weight of the product to be treated. Before or after this spraying, 95258 11 may be coated with a substance selected from chalk, diatomaceous earth, talc, clays and the like; or a so-called doped batch obtained by treating a material selected from chalk, diatomaceous earth, talc and clays with an anti-caking agent of type 11, the proportion of the type 11 preparation being 1-10% by weight, preferably 1 -6% by weight of the doped batch used as a coating in a ratio of 0.1-1%, preferably 0.2-0.6% by weight of the product to be treated.
On selvää, että kummassakin tapauksessa yksinkertaiseen tai monimutkaiseen lannoitteeseen sisällytetyn, keksinnön mukaisen paakkuuntumista estävän tuotteen osuus on 0,03-0,4 % käsiteltävän yksinkertai-15 sen tai monimutkaisen lannoitteen painosta laskien.It is clear that in either case the proportion of the anti-caking product according to the invention incorporated in a simple or complex fertilizer is 0.03 to 0.4%, based on the weight of the simple or complex fertilizer to be treated.
Tunnetusti ei ole toivottavaa valmistaa seostettua aine-erää käyttäen aineita, jotka sisältävät liikaa öljyä.It is known that it is not desirable to prepare a batch of substances using substances that contain too much oil.
20 Yksinkertaisen tai monimutkaisen lannoitteen pinnoittamista seostetulla aine-erällä seuraa yleensä öljyn, vaseliinin tai vahamaisten tuotteiden sumuttaminen. Myös raskasta polttoöljyä käytetään runsaasti. Näiden aineiden tehtävänä on tarttua aine-erän pintaan ja estää pölyäminen.20 Coating a simple or complex fertilizer with a compound batch is usually followed by spraying oil, petrolatum or waxy products. Heavy fuel oil is also widely used. The function of these substances is to adhere to the surface of the substance batch and prevent dusting.
25 Jäähdytysrummun tai leijupetin ulostulossa käsitellyn tuotteen lämpötila on yleensä alle 40 “C ja usein alle 32 eC, joka lämpötila vastaa ammoniumnitraatin tapauksessa siirtymälämpötilaa faasista IV faasiin III, mikä on hyvin valmistajien tiedossa. Kosteus on yleensä 30 tässä vaiheessa vähemmän kuin 1 %.25 The temperature of the product treated at the outlet of the cooling drum or fluidized bed is generally below 40 ° C and often below 32 ° C, which in the case of ammonium nitrate corresponds to the transition temperature from phase IV to phase III, which is well known to manufacturers. The humidity is usually less than 1% at this stage.
> · *> · *
Eräissä tietyissä tapauksissa paakkuuntumista estävä käsittely voidaan toteuttaa lannoitteella, joka on jäähdytetty osittain alueella 80- 40 °C olevaan lämpötilaan. Jäähdyttämistä jatketaan sitten paak-35 kuunturaista estävän aineen sisällyttämisen jälkeen.In certain cases, the anti-caking treatment may be carried out with a fertilizer partially cooled to a temperature in the range of 80-40 ° C. Cooling is then continued after the addition of the anti-pharyngeal agent.
12 9525812 95258
Siinä tapauksessa, että käytetään tyyppiä I olevaa paakkuuntumista estävää ainetta, tätä ainetta voidaan sumuttaa noin 80 eC:n lämpötilassa sopivalla järjestelmällä, joka tekee mahdolliseksi sen homogeenisen jakautumisen lannoitteen pinnalle. Pinnoitteen, jota mah-5 dollisesti levitetään ennen tyyppiä I olevan paakkuuntumista estävän aineen levittämistä tai sen jälkeen, määrä voi olla korkeintaan 2 % käsitellyn tuotteen painosta, mutta tavallisesti tämä määrä ei ylitä 0,5 painoprosenttia.In the case of the use of an anti-caking agent of type I, this agent can be sprayed at a temperature of about 80 ° C with a suitable system which allows it to be homogeneously distributed on the surface of the fertilizer. The amount of coating which may be applied before or after the application of the type I anti-caking agent may not exceed 2% by weight of the treated product, but will normally not exceed 0.5% by weight.
10 Keksinnön mukaisten paakkuuntumista estävien aineiden avulla voidaan edullisesti välttyä mineraalipinnoitteiden käytöltä, joiden pinnoitteiden vaikutus pölyämiseen on hyvin tunnettu.The anti-caking agents according to the invention can advantageously avoid the use of mineral coatings, the effect of which coatings on dusting is well known.
Tietty määrä vertailevia kokeita toteutettiin keksinnön mukaisten 15 tuotteiden paakkuuntumista estävien ominaisuuksien havainnollistamiseksi .A number of comparative experiments were performed to illustrate the anti-caking properties of the products of the invention.
Näissä kokeissa käytettiin betonimyllyä, jossa 20 kg lannoitetta alistettiin keksinnön mukaiseen paakkuuntumista estävään käsitte-20 lyyn.A concrete mixer was used in these experiments, in which 20 kg of fertilizer was subjected to the anti-caking treatment according to the invention.
Tämän jälkeen lannoite pakattiin polyetyleenisäkkeihin ja pinottiin ainoassa kuviossa esitetyn kaltaiseen paakkuunnuttamistelineeeseen.The fertilizer was then packed in polyethylene bags and stacked in a caking rack as shown in the sole figure.
Tämä paakkuunnuttamisteline käsittää metallirungon, joka koostuu 25 pystysuorista osista 1, lastaustasanteesta 2, jäykistimistä 3 ja kiinteästä tasanteesta 4.This caking rack comprises a metal body consisting of 25 vertical parts 1, a loading platform 2, stiffeners 3 and a fixed platform 4.
Testattavalla tuotteella täytetyt polyetyleenisäkit 5 pinottiin tasanteelle 2 kuviossa esitetyllä tavalla. Nostavaa tyynyä 7 kantava 30 tasanne 6 sijoitettiin säkkipinon päälle. Säkkipinoon kohdistettiin painetta täyttämällä tyyny paineilmalla liikkuvan tasanteen 6 ja kiinteän tasanteen 4 välissä. Säkkipinoon kohdistuvaa painetta voitiin muutella ja sen avulla voitiin jäljitellä 12 metrin korkuista säkkipinoa.Polyethylene bags 5 filled with the product to be tested were stacked on the platform 2 as shown in the figure. The platform 6 carrying the lifting pad 7 was placed on top of the stack of sacks. Pressure was applied to the stack of sacks by filling the cushion with compressed air between the moving platform 6 and the fixed platform 4. The pressure on the sack stack could be varied and used to mimic a sack stack 12 meters high.
Lannoitetta pidettiin paineen alaisuudessa eripituisten ajanjaksojen ajan, yleensä 10-45 vuorokautta, joskus useita kuukausia. Kokeen 35 13 95238 päätyttyä säkit avattiin, paakut punnittiin ja paakkujen kovuus mitattiin dynamometrillä.The fertilizer was kept under pressure for periods of varying lengths, usually 10 to 45 days, sometimes several months. At the end of experiment 35 13 95238, the sacks were opened, the lumps were weighed and the hardness of the lumps was measured with a dynamometer.
Paakkuuntuminen esitetään paakkujen prosentuaalisena osuutena (arvot 5 alueella 0-100). Paakkujen kovuus on yleensä 0-100 N, mutta kovuus voi saavuttaa jopa arvon 200 N käsittelemättömien vertailujen tapauksessa,Caking is expressed as a percentage of clumps (values 5 in the range 0-100). The hardness of the lumps is usually 0-100 N, but the hardness can reach up to 200 N in the case of untreated comparisons,
Paakkuuntumisindeksi määritellään lukuna, joka saadaan kertomalla 10 paakkujen prosentuaalinen osuus paakkujen kovuudella.The clumping index is defined as the number obtained by multiplying the percentage of 10 clumps by the hardness of the clumps.
Kunkin mittauksen tulos on lukuisilla säkeillä (yleensä 4 säkkiä) saatu keskiarvo.The result of each measurement is the average obtained with numerous sacks (usually 4 sacks).
15 Esimerkki 115 Example 1
Rakeistettu monimutkainen, kaavan 15.12.24 mukainen NPK-lannoite alistettiin paakkuuntumista estävään käsittelyyn, jossa käytettiin: keksinnön mukaista paakkuuntumista estävää valmistetta A tai 20 - paakkuuntumista estävää valmistetta B, joka käsittää jompaa kumpaa koostumuksen A mukaisen paakkuuntumista estävän tuotteen valmistamiseen käytettyä ainetta tai valmistetta C, joka käsittää jäljellä olevaa toista koostumuksen A mukaisen paakkuuntumista estävän tuotteen valmistamiseen 25 käytettyä ainetta tai tekniikan nykytason mukaista paakkuuntumista estävää ainetta.The granulated complex NPK fertilizer of formula 15.12.24 was subjected to an anti-caking treatment using: an anti-caking preparation A according to the invention or an anti-caking preparation B comprising either the anti-caking agent C used in the preparation of the anti-caking product of composition A, comprising the remaining second anti-caking agent used in the preparation of the anti-caking product according to composition A or the anti-caking agent according to the prior art.
Paakkuuntumista estävä aine A muodostui 15 painoprosentista tuotetta, jota saadaan neutraloimalla 66 30 paino-% 1,3-isopropyyli-naftaleenisulfonihappoa ja 37 paino-% '* hapanta lauryylifosfaattia sisältävä seos 3 moolilla etyleeni- oksidia ja stearyyliamiinia, 60 painoprosentista mineraaliöljyä, 25 painoprosentista makrokiteistä vahaa.Anti-caking agent A consisted of 15% by weight of product obtained by neutralizing a mixture of 66% by weight of 1,3-isopropylnaphthalenesulfonic acid and 37% by weight of acidic lauryl phosphate with 3 moles of ethylene oxide and stearylamine, 60% by weight of mineral crystal oil, 60% by weight of mineral oil. wax.
Paakkuuntumista estävä valmiste B muodostui 35 14 95238 15 painoprosentista tuotetta, joka saadan neutraloimalla 1,3-isopropyyli-naftaleenisulfonihappo stearyyliamiinilla, 60 painoprosentista mineraaliöljyä, 25 painoprosentista makrokiteistä vahaa.Anti-caking preparation B consisted of 35 14 95238 15% by weight of product obtained by neutralizing 1,3-isopropyl-naphthalenesulfonic acid with stearylamine, 60% by weight of mineral oil, 25% by weight of macrocrystalline wax.
5 Paakkuuntumista estävä valmiste C muodostui 15 painoprosentista tuotetta, joka saadaan neutraloimalla hapan lauryylifosfaatti 3 moolilla etyleenioksidia (mono- ja dieste-reiden 50/50 molaarinen seos) ja stearyyliamiinia, 60 painoprosentista mineraaliöljyä, 10 - 25 painoprosentista makrokiteistä vahaa.Anti-caking preparation C consisted of 15% by weight of product obtained by neutralizing acidic lauryl phosphate with 3 moles of ethylene oxide (50/50 molar mixture of mono- and diesters) and stearylamine, 60% by weight of mineral oil, 10 to 25% by weight of macrocrystalline.
Paakkuuntumista estäviä valmisteita A, B ja C levitetään sumuttamal-la 80 °C:n lämpötilassa määränä, joka on 0,15 % lannoitteen painosta. Tätä levitystä edeltää inertin saven levitys määränä, joka on 15 0,3 % lannoitteen painosta.Anti-caking preparations A, B and C are applied by spraying at 80 ° C in an amount of 0.15% by weight of the fertilizer. This application is preceded by the application of inert clay in an amount of 0.3% by weight of the fertilizer.
Tekniikan nykytilan mukainen paakkuuntumista estävä valmiste muodostui seostetusta savesta, joka sisälsi 3 paino-% stearyyliamiinia.According to the state of the art, the anti-caking preparation consisted of a mixed clay containing 3% by weight of stearylamine.
Sitä levitettiin määränä, joka on 0,6 % lannoitteen painosta, minkä 20 jälkeen vaseliinia levitettiin sumuttamalla 0,2 % lannoitteen painosta .It was applied in an amount of 0.6% by weight of the fertilizer, after which Vaseline was applied by spraying 0.2% by weight of the fertilizer.
Käsitelty lannoite pakattiin polyetyleenisäkkeihin ja se testattiin paakkuuntumiskokeella käyttäen edellä kuvattua paakkuunnuttamisteli-25 nettä. Varastoinnin pituus oli 20 vuorokautta paineen ollessa 1,5 kg/cm2.The treated fertilizer was packed in polyethylene bags and tested in an agglomeration test using the agglomeration scaffold described above. The storage length was 20 days at a pressure of 1.5 kg / cm2.
Tämän kokeen päätyttyä säkit avattiin huolellisesti. Paakut punnittiin ja paakkujen kovuus mitattiin dynamometrillä.At the end of this experiment, the bags were carefully opened. The lumps were weighed and the hardness of the lumps was measured with a dynamometer.
30 Näistä mittauksista saadut tulokset on koottu taulukkoon B.30 The results of these measurements are summarized in Table B.
Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deks iHandling Agglomeration- Agglomeration of agglomerates, hardness%
TAULUKKO BTABLE B
15 9523815 95238
Savi, johon on sekoi- 5 tettu 3 % amiinia 0,6 % 88 62 5500Clay mixed with 3% amine 0.6% 88 62 5500
Mineraaliöljy 0,2 % (tekniikan nykytasoMineral oil 0.2% (state of the art
Savi 0,3 % 35 46,5 1630 10Clay 0.3% 35 46.5 1630 10
Valmiste A 0,15 % (keksinnön mukainen)Preparation A 0.15% (according to the invention)
Savi 0,3 % 71 59 4200 15 Valmiste B 0,15 %Clay 0.3% 71 59 4200 15 Preparation B 0.15%
Savi 0,3 % 50 47 2400Clay 0.3% 50 47 2400
Valmiste C 0,15 % Käsittelemätön vertailu 100 160 16000 20Preparation C 0.15% Untreated comparison 100 160 16000 20
Taulukkoon B kootuista tuloksista nähdään, että pinnoittavan aineen annosta voidaan pienentää puoleen kaupallisesta seostetusta aine-erästä muodostuvaan, paakkuuntumista estävään aineeseen nähden, ja että keksinnön mukaisten paakkuuntumista estävien aineiden yhdistel-25 mä tehostaa tässä yhdistelmässä komponentteina läsnäolevien aktii-. . visten materiaalien paakkuuntumista estäviä ominaisuuksia.From the results summarized in Table B, it can be seen that the dose of the coating agent can be reduced by half with respect to the anti-caking agent formed from a commercial batch of agent, and that the combination of anti-caking agents of the invention enhances the active ingredients present in the combination. . anti-caking properties of materials.
Esimerkki 2 30 Ammoniumnitraatti, joka sisältää 33,5 paino-% typpeä ja 3 paino-% ammoniumsulfaattia, alistettiin paakkuuntumista estävään käsitte- ; lyyn. Lannoite käsiteltiin 30 °C:n lämpötilassa.Example 2 Ammonium nitrate containing 33.5% by weight of nitrogen and 3% by weight of ammonium sulfate was subjected to an anti-caking concept; lyyn. The fertilizer was treated at 30 ° C.
• «• «
Esimerkissä toteutettiin neljä koetta, joissa paakkuuntumista estä-35 väksi käsittelemiseksi lannoitteeseen sumutettiin 80 “C:n lämpötilassa 0,1 % lannoitteen painosta jäljempänä kuvattuja, paakkuuntumista estäviä valmisteita D, E ja F sekä tekniikan nykytason mukaista paakkuuntumista estävää ainetta, joka koostui kaupallisesta, 15 % 16 95238 stearyyliamiinia sisältävästä aminoidusta öljystä, ja joka sumutet-tiin samoissa olosuhteissa.In the example, four experiments were performed in which the anti-caking agent D, E and F described below and the prior art anti-caking agent consisting of a commercial anti-caking agent were sprayed at a temperature of 80 ° C to treat the anti-caking agent at 80 ° C. % 16 95238 of an aminated oil containing stearylamine, and which was sprayed under the same conditions.
Valmiste D koostui: 5 - 19 painoprosentista tuotetta, joka saadaan neutraloimalla 66 paino-% 1,3-isopropyylinaftaleenisulfonihappoa ja 37 paino-% hapanta lauryylifosfaattia (mono- ja diestereiden 50/50 molaa-rinen seos) sisältävä seos stearyyliamiinilla, 6 painoprosentista steariinihappoa, 10 - 50 painoprosentista mineraaliöljyä, 25 painoprosentista makrokiteistä vahaa.Preparation D consisted of: 5 to 19% by weight of product obtained by neutralizing a mixture of 66% by weight of 1,3-isopropylnaphthalenesulphonic acid and 37% by weight of acidic lauryl phosphate (50/50 molar mixture of mono- and diesters) with stearylamine, 6% by weight of stearic acid, 10 to 50% by weight of mineral oil, 25% by weight of macrocrystalline wax.
Valmiste E koostui: 19 painoprosentista tuotetta, joka saadaan neutraloimalla 1,3-15 isopropyylinaftaleenisulfonihappo stearyyliamiinilla, 6 painoprosentista steariinihappoa, 50 painoprosentista mineraaliöljyä ja 25 painoprosentista makrokiteistä vahaa.Preparation E consisted of: 19% by weight of product obtained by neutralizing 1.3-15% of isopropylnaphthalenesulfonic acid with stearylamine, 6% by weight of stearic acid, 50% by weight of mineral oil and 25% by weight of macrocrystalline wax.
20 Valmiste F koostui: 19 paino-% tuotetta, joka saadaan neutraloimalla hapan lauryy-lifosfaatti (mono- ja diestereiden 50/50-seos) stearyyliamiinilla, 6 painoprosentista steariinihappoa, 25-50 painoprosentista mineraaliöljyä ja 25 painoprosentista makrokiteistä vahaa.Preparation F consisted of: 19% by weight of product obtained by neutralizing acidic lauryl phosphate (50/50 mixture of mono- and diesters) with stearylamine, 6% by weight of stearic acid, 25-50% by weight of mineral oil and 25% by weight of macrocrystalline wax.
Valmisteita D, E ja F lisättiin määränä, joka oli 0,1 % lannoitteen painosta.Preparations D, E and F were added in an amount of 0.1% by weight of the fertilizer.
30 • Käsitelty lannoite alistettiin esimerkissä 1 kuvattuun kokeeseen ja samat mittaukset toteutettiin. Näistä mittauksista saadut tulokset on koottu taulukkoon C.30 • The treated fertilizer was subjected to the experiment described in Example 1 and the same measurements were performed. The results of these measurements are summarized in Table C.
3535
TAULUKKO CTABLE C
Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deksi 17 95258Handling Agglomeration - Agglomeration of agglomerates, hardness% agglomeration index 17 95258
Koostumus DComposition D
5 (keksinnön mukainen) 6 20 1205 (according to the invention) 6 20 120
Koostumus E 50 55 2750Composition E 50 55 2750
Koostumus F 27 45 1200Composition F 27 45 1200
Kaupallinen aminoitu öljy 25 39 1000 (tekniikan nykytason mukai-10 nen) Käsittelemätön vertailu 100 200 20000Commercial Aminated Oil 25 39 1000 (Prior Art 10) Crude Comparison 100 200 20000
Taulukkoon C kootuista tuloksista nähdään, että keksinnön mukainen 15 yhdistelmä tehostaa paakkuuntumista estäviä ominaisuuksia verrattuna kummankin yhdistelmässä komponenttina läsnäolevan aineen paakkuuntumista estäviin ominaisuuksiin toisistaan erillään käytettynä ja samanlaiseksi valmisteeksi muodostettuna.It can be seen from the results summarized in Table C that the combination of the invention enhances the anti-caking properties of the anti-caking properties of the two substances present in the combination as a component when used separately and formulated as a similar preparation.
20 Esimerkki 320 Example 3
Kaavan 16.10.5 mukainen monimutkainen NPK-lannoite, jonka paakkuun-tumisen estäminen tiedetään vaikeaksi, ja jonka lämpötila oli 35 °C, alistettiin paakkuuntumista estävään käsittelyyn. Käsittelyssä käy-25 tettiin keksinnön mukaista valmistetta G, joka koostui: 10 painoprosentista tuotetta, joka saadaan neutraloimalla 75 paino-% 1,3-isopropyylinaftaleenisulfonihappoa ja 25 paino-% hapanta alkyylifosfaattia (mono- ja diestereiden 50/50 molaa-rinen seos), jonka alkyyliosa koostui olennaisesti C16:n ja 30 C18:n seoksen käsittävästä ketjusta, sisältävä seos stearyyli- amiinilla, 90 painoprosentista mineraaliöljyä.A complex NPK fertilizer of formula 16.10.5, which is known to be difficult to prevent caking and had a temperature of 35 ° C, was subjected to an anti-caking treatment. The treatment used preparation G according to the invention, consisting of: 10% by weight of product obtained by neutralizing 75% by weight of 1,3-isopropylnaphthalenesulfonic acid and 25% by weight of acidic alkyl phosphate (50/50 molar mixture of mono- and diesters), the alkyl moiety of which consisted essentially of a chain of a mixture of C16 and 30 C18, containing a mixture of stearylamine, 90% by weight of mineral oil.
Lannoitteeseen lisättiin ensin 0,3 % lannoitteen painosta savea ja 35 sitten siihen sumutettiin 80 °C:ssa valmistetta G 0,2 % lannoitteen painosta.0.3% by weight of fertilizer was first added to the fertilizer and then at 80 ° C, preparation G was sprayed with 0.2% by weight of fertilizer.
18 9523818 95238
Kaksi vertailukoetta toteutettiin kahdella tekniikan nykytason mukaisella valmisteella, joista käytettiin nimityksiä "vertailu 1" ja "vertailu 2".Two comparative experiments were performed with two prior art preparations, referred to as "Comparison 1" and "Comparison 2".
5 Vertailu 1 oli alkyyliaryylisulfonaatti, jota yhtiö Compagnie5 Comparison 1 was an alkylaryl sulfonate manufactured by Compagnie
FranQaise de Produits Industriels markkinoi tavaramerkkinä "GALORYL ATH 24". Sitä käytettiin lannoitteen käsittelyssä, jossa lannoitteen pinnoittamiseen käytettiin savea 0,7 % lannoitteen painosta, minkä jälkeen lannoitteeseen sumutettiin 80 °C:n lämpötilassa 0,2 % lan-10 noitteen painosta seosta, joka sisälsi 15 paino-% vertailua 1 raskaassa polttoöljyssä.FranQaise de Produits Industriels markets it under the trademark "GALORYL ATH 24". It was used in the treatment of a fertilizer in which 0.7% by weight of the fertilizer was used to coat the fertilizer, followed by spraying at 80 ° C of a mixture containing 0.2% by weight of the lan-10 weft containing 15% by weight of comparison 1 in heavy fuel oil.
Vertailu 2 oli vaseliinia. Sitä käytettiin lannoitteen käsittelyssä, jossa lannoitteen pinnoittamiseen käytettiin 0,5 % lannoitteen pai-15 nosta savea, johon oli seostettu 3 paino-% stearyyliamiiniin perustuvaa koostumusta, minkä jälkeen lannoitteeseen sumutettiin 80 °C:n lämpötilassa 0,2 % lannoitteen painosta mainittua vertailua.Comparison 2 was Vaseline. It was used in the treatment of a fertilizer in which 0.5% by weight of a fertilizer clay mixed with 3% by weight of a composition based on stearylamine was used to coat the fertilizer, followed by spraying the fertilizer at 80 ° C with 0.2% by weight of the fertilizer.
Käsitelty lannoite allistettiin esimerkissä 1 kuvattuun kokeeseen ja 20 samat mittaukset toteutettiin. Näistä mittauksista saadut tulokset on koottu taulukkoon D.The treated fertilizer was subjected to the experiment described in Example 1 and the same measurements were performed. The results of these measurements are summarized in Table D.
TAULUKKO DTABLE D
25 Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deksi25 Handling Agglomeration - Agglomeration of agglomerates, hardness in%
Vertailu: 74 96 7100 0,7 % savea 0,03 % GALORYL ATH 24 0,17 % raskasta polttoöljyä 30____Comparison: 74 96 7100 0.7% clay 0.03% GALORYL ATH 24 0.17% heavy fuel oil 30____
Vertailu 2: 95 85 8070 0,5 % seostettua savea 0,2 % vaseliiniaComparison 2: 95 85 8070 0.5% alloyed clay 0.2% Vaseline
Valmiste G: 50 43 2150 35 0,3 % saveaPreparation G: 50 43 2150 35 0.3% clay
0,2 % valmistetta G0.2% of preparation G
Käsittelemätön vertailu 100 20 20000 95238 19Unprocessed comparison 100 20 20000 95238 19
Taulukkoon D kootuista tuloksista nähdään, että lannoitteiden, joiden paakkuuntumisen estäminen on hyvin vaikeata, tapauksessa keksinnön avulla mineraaliöljypinnoitteiden määriä voidaan pienentää, jolloin pölyäminen vähenee merkittävästi paakkuuntumista estävän suori-5 tuskyvyn parantuessa.From the results summarized in Table D, it can be seen that in the case of fertilizers which are very difficult to prevent caking, the invention can reduce the amounts of mineral oil coatings, thereby significantly reducing dusting as the anti-caking performance is improved.
Paakkuuntumista estävä valmiste G ei sisällä mikrokiteistä vahaa. Esimerkki 4 10Anti-caking preparation G does not contain microcrystalline wax. Example 4 10
Kaavan 15.12.24 mukainen rakeistettu monimutkainen NPK-lannoite käsitellään paakkuuntumisen estämiseksi käyttäen: keksinnön mukaisia valmisteita H ja I, esimerkin 1 mukaista, paakkuuntumista estävää valmistetta B, 15 - paakkuuntumista estävää valmistetta J, joka käsittää jäljellä olevaa ainetta niistä kahdesta aineesta, joita on läsnä komponentteina koostumuksen H ja I mukaisissa paakkuuntumista estävissä tuotteissa, tekniikan nykytason mukaista paakkuuntumista estävää ainetta.The granulated complex NPK fertilizer of formula 15.12.24 is treated to prevent caking using: preparations H and I according to the invention, anti-caking preparation B according to Example 1, 15 - anti-caking preparation J comprising the remaining substance of the two substances present as components in the anti-caking products according to compositions H and I, an anti-caking agent according to the prior art.
2020
Paakkuuntumista estävä valmiste H koostui: 15 painoprosentista tuotetta, joka saadaan neutraloimalla 65 paino-% 1,3-isopropyylinaftaleenisulfonihappoa ja 35 paino-% koostumusen J yhteydessä määriteltyä hapanta alkyylifosfaattia • 25 sisältävä seos stearyyliamiinilla, 60 painoprosentista mineraaliöljyä ja 25 painoprosentista makrokiteistä vahaa.Anti-caking preparation H consisted of: 15% by weight of a product obtained by neutralizing a mixture of 65% by weight of 1,3-isopropylnaphthalenesulfonic acid and 35% by weight of acidic alkyl phosphate as defined in composition J with stearylamine, 60% by weight of mineral oil and 25% by weight of macrocrystalline oil.
Paakkuuntumista estävän valmisteen I koostumus on koostumuksen H 30 kaltainen lukuunottamatta sitä pientä eroa, että 60 paino-% mineraa-·' liöljyä on korvattu 57 % mineraaliöljyä ja 3 % alumiinistearaattia sisältävällä seoksella.The composition of the anti-caking preparation I is similar to that of composition H 30, except that the small difference is that 60% by weight of mineral oil has been replaced by a mixture of 57% mineral oil and 3% aluminum stearate.
Paakkuuntumista estävä aine J koostuu: 35 - 15 painoprosentista tuotetta, joka saadaan neutraloimalla stea ryyliamiinilla hapan alkyylifosfaatti (mono- ja diestereiden 20 ΟΓ 07 0 ;ui.ou 50/50 molaarinen seos), jonka alkyyliosa muodostuu olennaisesti C8:n ja CIO:n seoksen käsittävästä ketjusta, 60 painoprosenttisesti mineraaliöljystä ja 25 painoprosenttisesti makrokiteisestä vahasta.The anti-caking agent J consists of: 35 to 15% by weight of a product obtained by neutralization with stearylamine of an acidic alkyl phosphate (a 20 to 07 molar mixture of mono- and diesters; uu.ou 50/50 molar mixture), the alkyl part of which consists essentially of C8 and C10 a mixture comprising a mixture, 60% by weight of mineral oil and 25% by weight of macrocrystalline wax.
55
Paakkuuntumista estävät valmisteet B, H, I ja J lisätään sumuttamal-la 80 eC:n lämpötilassa määränä, joka on 0,15 % lannoitteen painosta. Tätä lisäystä edeltää inertin saven lisääminen määränä, joka on 0,3 % lannoitteen painosta.Anti-caking preparations B, H, I and J are added by spraying at 80 ° C in an amount of 0.15% by weight of the fertilizer. This addition is preceded by the addition of inert clay in an amount of 0.3% by weight of the fertilizer.
1010
Tekniikan nykytason mukainen valmiste koostuu seostetusta savesta, joka sisältää 3 paino-% stearyyliamiinia. Sitä lisätään 0,6 % lannoitteen painosta, minkä jälkeen vaseliinia sumutetaan 0,2 % lannoitteen painosta.The prior art preparation consists of a mixed clay containing 3% by weight of stearylamine. It is added at 0.6% by weight of the fertilizer, after which Vaseline is sprayed at 0.2% by weight of the fertilizer.
15 Käsitelty lannoite pakataan polyetyleenisäkkeihin ja alistetaan edellä kuvattuun paakkuuntumiskokeeseen paakkuunnuttamistelineessä 1,5 kg/cmz:n suuruisen paineen alaisuudessa.The treated fertilizer is packed in polyethylene bags and subjected to the agglomeration test described above in a agglomeration rack under a pressure of 1.5 kg / cm 2.
20 Tämän kokeen päätyttyä polyetyleenisäkit avataan huolellisesti. Paakut punnitaan ja paakkujen kovuus mitataan dynamometrillä.20 At the end of this test, the polyethylene bags are carefully opened. The lumps are weighed and the hardness of the lumps is measured with a dynamometer.
Näistä mittauksista saadut tulokset on koottu taulukkoon E.The results of these measurements are summarized in Table E.
2525
TAULUKKO ETABLE E
21 Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deks i 9523821 Handling Agglomeration- Aggregation of agglomerates, hardness% agglomeration dex 95238
Seostettu savi, joka 5 sisältää 3 % amiinia 0,6 % 89 79 7030Alloyed clay containing 3% amine 0.6% 89 79 7030
Mineraaliöljy 0,2 % (tekniikan nykytasoMineral oil 0.2% (state of the art
Savi 0,3 % 62 52 3220 10Clay 0.3% 62 52 3220 10
Valmiste B 0,15 %Preparation B 0.15%
Savi 0,3 % 42 46 1930Clay 0.3% 42 46 1930
Valmiste H 0,15 % 15 (keksinnön mukainen)Preparation H 0.15% 15 (according to the invention)
Savi 0,3 % 31 51 15800Clay 0.3% 31 51 15800
Valmiste I 0,15 % (keksinnön mukainen) 20 Savi 0,3 % 48 52 2500Preparation I 0.15% (according to the invention) 20 Clay 0.3% 48 52 2500
Valmiste J 0,15 % 25 Tämä esimerkki havainnollistaa valmisteen muodostavan kahden aktiivisen materiaalin paakkuuntumista estävien ominaisuuksien tehostumista alumiinistearaattiin yhdistettynä.Preparation J 0.15% This example illustrates the enhancement of the anti-caking properties of the two active materials that make up the preparation when combined with aluminum stearate.
Esimerkki 5 30Example 5 30
Ammoniumnitraatti, jonka titrausarvo on 33,3 % ja joka sisältää 4 paino-% ammoniumsulfaattia, käsitellään paakkuuntumisen estämiseksi. Lannoite käsitellään 30 °C:n lämpötilassa.Ammonium nitrate with a titration value of 33.3% and containing 4% by weight of ammonium sulfate is treated to prevent caking. The fertilizer is treated at 30 ° C.
35 Esimerkissä toteutettiin neljä koetta, joiden mukaisissa käsittelyissä paakkuuntumisen estämiseksi lannoitteeseen sumutettiin 80 °C:n lämpötilassa 0,1 % lannoitteen painosta jäljempänä kuvattuja paakkuuntumista estäviä valmisteita K, L ja M sekä tekniikan nykytason mukaista paakkuuntumista estävää ainetta, joka käsitti kaupal- 22 95238 lista, 18 % stearyyliamiinia sisältävää aminoitua öljyä, ja jota sumutettiin samoissa olosuhteissa.35 In the example, four experiments were carried out in which, in order to prevent caking, the fertilizer was sprayed at a temperature of 80 ° C with 0.1% by weight of the fertilizer anti-caking preparations K, L and M described below and an anti-caking agent according to the prior art comprising 22 95238 , An aminated oil containing 18% stearylamine and sprayed under the same conditions.
Keksinnön mukainen koostumus K koostuu: 5 22 painoprosentista tuotetta, joka saadaan neutraloimalla 55 paino-% tributyyli-naftaleenisulfonihappoa ja 45 paino-% hapanta stearyylifosfaattia (mono- ja diestereiden 50/50-seos) sisältävä seos stearyyliamiinilla, 10 painoprosentista steariinihappoa, 10 - 45 painoprosentista paraffiiniöljyä, 23 painoprosentista makrokiteistä vahaa.Composition K according to the invention consists of: 22% by weight of product obtained by neutralizing a mixture of 55% by weight of tributylnaphthalenesulfonic acid and 45% by weight of acidic stearyl phosphate (50/50 mixture of mono- and diesters) with stearylamine, 10% by weight of stearic acid, weight percent paraffin oil, 23 weight percent macrocrystalline wax.
Valmiste L käsittää yhtä niistä kahdesta aineesta, jotka ovat läsnä komponentteina koostumuksen K mukaisessa paakkuuntumista estävässä 15 tuotteessa. Se koostuu: 22 painoprosentista tuotetta, joka saadaan neutraloimalla tri-butyyli-naftaleenisulfonihappoa stearyyliamiinilla, 10 painoprosentista steariinihappoa, 45 painoprosentista paraffiiniöljyä, 20 - 23 painoprosentista makrokiteistä vahaa.Preparation L comprises one of the two substances present as components in the anti-caking product of composition K. It consists of: 22% by weight of product obtained by neutralizing tri-butylnaphthalenesulphonic acid with stearylamine, 10% by weight of stearic acid, 45% by weight of paraffin oil, 20-23% by weight of macrocrystalline wax.
Valmiste M käsittää jäljelle jäävää toista niistä kahdesta aineesta, jottka ovat läsnä komponentteina koostumuksen K mukaisessa paakkuuntumista estävässä tuotteessa. Se koostuu: : 25-22 painoprosentista tuotetta, joka saadaan neutraloimalla hapan stearyylifosfaatti (mono- ja diestereiden 50/50-seos) stearyyliamiinilla, 10 painoprosentista steariinihappoa, 45 painoprosentista paraffiniöljyä, 30 - 23 painoprosentista makrokiteistä vahaa.Preparation M comprises the remaining one of the two substances present as components in the anti-caking product of composition K. It consists of:: 25 to 22% by weight of product obtained by neutralizing acidic stearyl phosphate (50/50 mixture of mono- and diesters) with stearylamine, 10% by weight of stearic acid, 45% by weight of paraffin oil, 30 to 23% by weight of macrocrystalline wax.
Käsitelty lannoite alistettiin esimerkissä 1 kuvattuun kokeeseen ja samat mittaukset toteutettiin. Varastointi pinottuna kesti tässä tapauksessa 45 vuorokautta 1 kg/cm2:n suuruisen paineen alaisuudessa.The treated fertilizer was subjected to the experiment described in Example 1 and the same measurements were performed. Stacked storage in this case lasted 45 days under a pressure of 1 kg / cm2.
35 Näistä mittauksista saadut tulokset on koottu taulukkoon F.35 The results of these measurements are summarized in Table F.
I· Mllt MU 1:14« ; =I · Mllt MU 1:14 «; =
TAULUKKO FTABLE F
Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deksi 23 95238Handling Agglomeration- Agglomeration of agglomerates, hardness indexing index 23 95238
Valmiste KPreparation K
5 (keksinnön mukainen) 45 30 13505 (according to the invention) 45 30 1350
Valmiste L 95 80 7600Preparation L 95 80 7600
Valmiste M 95 72 6840Preparation M 95 72 6840
Kaupallinen aminoitu öljy 67 32 2140 (tekniikan nykytaso) 10 Käsittelemätön vertailu 100 200 20000Commercial Aminated Oil 67 32 2140 (Prior Art) 10 Crude Comparison 100 200 20000
Taulukkoon F kootut tulokset osoittavat, että keksinnön mukainen yhdistelmä aiheuttaa paakkuuntumista estävien ominaisuuksien ilmei-15 sen tehostumisen verrattuna kummankin tässä yhdistelmässä komponenttina läsnäolevan aineen vastaaviin ominaisuuksiin toisistaan erillään käytettynä ja samanlaisiksi valmisteiksi tehtyinä.The results summarized in Table F show that the combination of the invention causes an apparent enhancement of the anti-caking properties compared to the corresponding properties of the two components present in this combination when used separately and formulated as similar preparations.
Esimerkki 6 20Example 6 20
Kaavan 15.11.22 mukainen monimutkainen NPK-lannoite, jonka paakkuun-tumisen estäminen tiedetään vaikeaksi, ja jonka lämpötila oli 35 °C, käsiteltiin paakkuuntumisen estämiseksi sumuttamalla 0,1 % käsiteltävän lannoitteen painosta keksinnön mukaista paakkuuntumisen 25 estävää valmistetta N sekä tekniikan nykytason mukaista paakkuuntumisen estävää valmistetta, joka käsittää seostettua, 3 paino-% stea-ryyliamiinia sisältävää savea.A complex NPK fertilizer of the formula 15.11.22, which is known to be difficult to prevent caking and has a temperature of 35 ° C, was treated to prevent caking by spraying 0.1% by weight of the fertilizer to be treated with the anti-caking agent N according to the invention and the prior art anti-caking agent. a preparation comprising a doped clay containing 3% by weight of stearylamine.
; Valmiste N koostuu: * 30 - 15 painoprosentista tuotetta, joka saadaan neutraloimalla 50 % 1,3-isopropyyli-naftaleenisulfonihappoa ja 50 % hapanta lauryy-lifosfaattia (mono- ja diestereiden 50/50 molaarinen seos) sisältävä seos stearyyliamiinilla, 60 painoprosentista mineraaliöljyä ja 35 - 25 painoprosentista makrokiteistä vahaa.; Preparation N consists of: * 30 to 15% by weight of a product obtained by neutralizing a mixture of 50% 1,3-isopropyl-naphthalenesulphonic acid and 50% acid lauryl phosphate (50/50 molar mixture of mono- and diesters) with stearylamine, 60% by weight of mineral oil and 35% by weight - 25% by weight of macrocrystalline wax.
Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deks iHandling Agglomeration- Agglomeration of agglomerates, hardness%
TAULUKKO GTABLE G
24 9525824 95258
Valmiste NPreparation N
5 (keksinnön mukainen) 37 35 13005 (according to the invention) 37 35 1300
Vertailu 44 47 2070 0,6 % seostettua savea 0,2 % vaseliinia Käsittelemätön vertailu 100 160 16000 10 Tämä esimerkki havainnollistaa sitä tosiseikkaa, että keksinnön mukainen valmiste tekee mahdolliseksi mineraalipinnoitteesta luopumisen.Comparison 44 47 2070 0.6% alloyed clay 0.2% Vaseline Untreated Comparison 100 160 16000 10 This example illustrates the fact that the preparation according to the invention makes it possible to dispense with the mineral coating.
15 Tähän huomattavaan paakkuuntumista estävään suorituskykyyn liittyy edullisesti pölyyntymisen väheneminen.This significant anti-caking performance is preferably associated with a reduction in dusting.
Esimerkki 7 20Example 7 20
Ureapohjainen lannoite, joka oli rakeistettu aine-erän kanssa, käsiteltiin paakkuuntumisen estämiseksi käyttäen keksinnön mukaista paakkuuntumisen estävää valmistetta 0 sekä tekniikan nykytason mukaista paakkuuntumisen estävää valmistetta.The urea-based fertilizer granulated with the batch of material was treated to prevent caking using the anti-caking preparation 0 according to the invention and the anti-caking preparation according to the prior art.
2525
Paakkuuntumista estävä valmiste 0 koostuu: 19 painoprosentista tuotetta, joka saadaan neutraloimalla 75 % 1,3-isopropyylinaftaleenisulfonihappoa ja 25 % hapanta lauryy-lifosfaattia (mono- ja diestereiden 50/50 molaarinen seos) si-30 sältävä seos stearyyliamiinilla, 5 painoprosenttia steariinihappoa, 53 painoprosenttia mineraaliöljyä ja 23 painoprosenttia makrokiteistä vahaa.Anti-caking preparation 0 consists of: 19% by weight of product obtained by neutralizing a mixture of 75% 1,3-isopropylnaphthalenesulphonic acid and 25% acidic lauryl phosphate (50/50 molar mixture of mono- and diesters) with stearylamine, 53% by weight of stearic acid, 5% by weight of stea % by weight of mineral oil and 23% by weight of macrocrystalline wax.
95238 2595238 25
Tekniikan nykytilan mukainen paakkuuntumista estävä valmiste koostui kaupallisesta alkyylisulfaatin vesiliuoksesta yhdistettynä etyleeni-vinyyliasetaatin tyyppiseen liukoiseen polymeeriin.The prior art anti-caking preparation consisted of a commercial aqueous solution of alkyl sulfate combined with a soluble polymer of the ethylene-vinyl acetate type.
5 Paakkuuntumista estäviä valmisteita sumutettiin lannoitteeseen 0,1 % lannoitteen painosta.5 Anti-caking preparations were sprayed on the fertilizer at 0.1% by weight of the fertilizer.
Lannoitteet testattiin esimerkin 1 mukaisesti. Varastointi pinottuna kesti 20 vuorokautta 1 kg/cm2:n suuruisen paineen alaisuudessa.Fertilizers were tested according to Example 1. Stacked storage lasted for 20 days under a pressure of 1 kg / cm2.
1010
TAULUKKO HTABLE H
Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deksiHandling Clump- Clumping of clumps, hardness%
Tekniikan nykytason 15 mukainen liuos 100 47 4700Prior art solution 15 47 4700
Valmiste 0 30 22 660 (keksinnön mukainen) Käsittelemätön vertailu 100 60 6000 20 Tämä esimerkki havainnollistaa keksinnön mukaisen valmisteen paakkuuntumista estäviä ominaisuuksia.Preparation 0 30 22 660 (according to the invention) Untreated comparison 100 60 6000 20 This example illustrates the anti-caking properties of the preparation according to the invention.
• «• «
Esimerkki 8 25Example 8 25
Esimerkissä 5 kuvattu valmiste K ja patenttijulkaisussa EP 113 687 kuvatut valmisteet "pinnoiteseos A, B ja C" testattiin niiden vertaamiseksi toisiinsa. Kokeet toteutettiin 33,5 %:11a ammoniumnitraa-tilla, joka sisälsi 4 % ammoniumsulfaattia.Preparation K described in Example 5 and preparations "coating composition A, B and C" described in EP 113 687 were tested to compare them. The experiments were performed with 33.5% ammonium nitrate containing 4% ammonium sulfate.
- 30 Käsittelyssä lannoitteeseen sumutettiin 80 °C:n lämpötilassa 0,1 % lannoitteen painosta erilaisia paakkuuntumista estäviä valmisteita.During the treatment, at a temperature of 80 ° C, 0.1% by weight of the fertilizer was sprayed with various anti-caking preparations.
Käsitelty lannoite alistettiin esimerkissä 1 kuvattuun kokeeseen ja 35 samat mittaukset toteutettiin. Varastointi pinottuna kesti tässä 26 95238 tapauksessa 45 vuorokautta 1 kg/cm2:n suuruisen paineen alaisuudessa. Tulokset on koottu taulukkoon I.The treated fertilizer was subjected to the experiment described in Example 1 and the same measurements were performed. In this case, 26 95238 cases were stored stacked for 45 days under a pressure of 1 kg / cm2. The results are summarized in Table I.
TAULUKKO ) 5 Käsittely Paakkuun- Paakkujen Paakkuun- tuminen, kovuus tumisin- % deksiTABLE) 5 Handling Agglomeration - Agglomeration of agglomerates, hardness
Valmiste KPreparation K
(keksinnön mukainen) 45 50 1350(according to the invention) 45 50 1350
Pinnoiteseos A 100 100 10000 10 Pinnoiteseos B 100 100 10000Coating mixture A 100 100 10000 10 Coating mixture B 100 100 10000
Pinnoiteseos C 100 100 10000 Tämä esimerkki havainnollistaa keksinnön mukaisten paakkuuntumista 15 estävien valmisteiden ratkaisevaa paremmuutta verrattuna tekniikan nykytason mukaisiin valmisteisiin käytettynä lannoitteessa, jolla on voimakas taipumus kovettua.Coating Composition C 100 100 10000 This example illustrates the decisive superiority of the anti-caking preparations according to the invention compared to the prior art preparations used in a fertilizer with a strong tendency to harden.
tt
Claims (20)