DE2938905A1 - METHOD AND DEVICE FOR PRODUCING MOLDINGS FROM THERMOPLASTIC PLASTIC, WHICH READS TO BE SET IN ITS PART CRYSTALLINE CONDITION BY MEANS OF PHYSICAL INFLUENCES, IN PARTICULAR TEMPERATURE INFLUENCES - Google Patents

METHOD AND DEVICE FOR PRODUCING MOLDINGS FROM THERMOPLASTIC PLASTIC, WHICH READS TO BE SET IN ITS PART CRYSTALLINE CONDITION BY MEANS OF PHYSICAL INFLUENCES, IN PARTICULAR TEMPERATURE INFLUENCES

Info

Publication number
DE2938905A1
DE2938905A1 DE19792938905 DE2938905A DE2938905A1 DE 2938905 A1 DE2938905 A1 DE 2938905A1 DE 19792938905 DE19792938905 DE 19792938905 DE 2938905 A DE2938905 A DE 2938905A DE 2938905 A1 DE2938905 A1 DE 2938905A1
Authority
DE
Germany
Prior art keywords
temperature
semi
finished product
plastic
conditioning
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
DE19792938905
Other languages
German (de)
Inventor
geb. Wiegand Barbara 6200 Wiesbaden Geppert
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Bellaplast GmbH
Original Assignee
Bellaplast GmbH
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Bellaplast GmbH filed Critical Bellaplast GmbH
Priority to DE19792938905 priority Critical patent/DE2938905A1/en
Priority to NO802566A priority patent/NO802566L/en
Priority to DK371180A priority patent/DK371180A/en
Priority to NL8005039A priority patent/NL8005039A/en
Priority to FI802843A priority patent/FI802843A/en
Priority to GB8029403A priority patent/GB2059328B/en
Priority to ES494962A priority patent/ES494962A0/en
Priority to ZA00805677A priority patent/ZA805677B/en
Priority to SE8006558A priority patent/SE8006558L/en
Priority to FR8020494A priority patent/FR2465586A1/en
Priority to BE0/202262A priority patent/BE885436A/en
Priority to YU02461/80A priority patent/YU246180A/en
Priority to JP13308280A priority patent/JPS56106845A/en
Priority to ES495803A priority patent/ES8106436A1/en
Publication of DE2938905A1 publication Critical patent/DE2938905A1/en
Priority to YU00324/83A priority patent/YU32483A/en
Ceased legal-status Critical Current

Description

PATENTANWALT DIPL.-PHYS. HEINRICH SEIDSPATENT ADVOCATE DIPL.-PHYS. HEINRICH SEIDS

62 Wiesbaden · Bierstadtcr Höhe 15 ■ rostfach 12068 ■ Telefon (0 61 21) 56 53 82 Postscheck Frankfurt/Main 1810 08 - 602 · Bank Deutsche Bank 395 63 72 ■ Nass. Sparkasse 108 00 30 6562 Wiesbaden · Bierstadtcr Höhe 15 ■ rostfach 12068 ■ Telephone (0 61 21) 56 53 82 Postscheck Frankfurt / Main 1810 08 - 602 · Bank Deutsche Bank 395 63 72 ■ Nass. Sparkasse 108 00 30 65

Wiesbaden, den 25. Sept. 1979 X 222 S/weWiesbaden, September 25, 1979 X 222 S / we

Bellaplast GmbH
Karl-Bosch-Strasse 10 6200 Wiesbaden
Bellaplast GmbH
Karl-Bosch-Strasse 10 6200 Wiesbaden

Verfahren und Vorrichtung zum Herstellen von Formungen aus thermoplastischem Kunststoff, der sich mittels physikalischer Einflüsse, insbesondere Temperatureinflüsse, wahlweise in seinem teilkristallinen Zustand einstellen läßtMethod and apparatus for making molds made of thermoplastic material, which by means of physical influences, in particular temperature influences, can optionally be set in its partially crystalline state

Die Erfindung bezieht sich auf ein Verfahren und eine Vorrichtung zum Herstellen von Formungen aus thermoplastischem Kunststoff, der sich mittels physikalischer Einflüsse, insbesondere Temperatureinflüsse, wahlweise in seinem teilkristallinen Zustand einstellen läßt, durch:The invention relates to a method and an apparatus for producing moldings from thermoplastic Plastic, which by means of physical influences, in particular temperature influences, optionally in its semi-crystalline Can be set by:

Bilden eines Halbzeugs, insbesondere fortlaufendes Extrudieren eines Bandes oder Schlauches, aus dem plastifizierten Kunststoff,Forming a semi-finished product, in particular continuous extrusion of a tape or tube from the plasticized plastic,

Stabilisieren des Halbzeugs durch Abkühlen zumindest an einer Oberfläche,Stabilizing the semi-finished product by cooling at least on one surface,

Thermo-Konditionieren des stabilisierten Halbzeugs zu Thermoverformbarkeit undThermal conditioning of the stabilized semi-finished product Thermoformability and

- Thermoverformen zum Bilden formstabiler endgültiger Formlinge aus dem Halbzeug.- Thermoforming to form dimensionally stable final molded articles from the semi-finished product.

130 0 16/0098130 0 16/0098

Dipl.-Phy». Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Pottfach 5105 · ^(o 61 21) 56 53 8aDipl.-Phy ». Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Pottfach 5105 · ^ (o 61 21) 56 53 8a

-Vf--Vf-

Aus DE-OS 28 30 740 und DE-OS 28 30 788 sind Verfahren zum Herstellen dünnwandiger Artikel aus kristallinem thermoplastischem Material bekannt. Das in diesen Verfahren zu verarbeitenden thermoplastische Material, insbesondere Polyolefin, ist in jedem Fall nur kristalliner Art und bietet somit nur die Möglichkeit, den teil-, kristallinen Zustand in der Formlingwand mehr oder weniger stark kristallin einzustellen und durch Temperatur· führung und Benutzung physikalischer Einflüsse die im Kunststoff der Formlingwand enthaltenen Kristalle zu beeinflussen. Dementsprechend sind diese bekannten Verfahren auch darauf abgestellt, die Kristallinität des Kunststoffes und die physikalische Beeinflussung der Kristalle im Kunststoff bei dem Herstellungsverfahren der Formlinge derart zu steuern, daß optimale Annäherung an die gewünschten Eigenschaften der Formlingwand und zugleich brauchbare Voraussetzungen für das Thermoverformen erzielbar sind.From DE-OS 28 30 740 and DE-OS 28 30 788 are processes known for making thin-walled articles from crystalline thermoplastic material. That in these proceedings The thermoplastic material to be processed, in particular polyolefin, is only more crystalline in any case Type and thus only offers the possibility of the partial, crystalline state in the molding wall more or less strongly crystalline and through temperature control and use of physical influences the im To influence the plastic of the molding wall contained crystals. Accordingly, these are known methods also aimed at the crystallinity of the plastic and the physical influence of the To control crystals in the plastic in the manufacturing process of the moldings in such a way that optimal approximation on the desired properties of the molding wall and at the same time useful requirements for thermoforming are achievable.

Aus GB-PS 1 514 277 ist auch bereits die Herstellung von Formungen, insbesondere Flaschen, aus Polyestermaterial durch kombiniertes Spritzgießen und Blasverformen bekannt. Danach soll zunächst ein Vorformling durch Spritzformen hergestellt und durch Abkühlen an der Außenfläche stabilisiert werden. Es soll dann ein erstes Aufweiten unter Recken der gekühlten Wandbereiche und dann das vollständige Ausformen durch Blasformen erfolgen. DiesesFrom GB-PS 1 514 277 the production of Formings, in particular bottles, made of polyester material by combined injection molding and blow molding are known. According to this, a preform should first be produced by injection molding and stabilized on the outer surface by cooling will. There should then be a first widening with stretching of the cooled wall areas and then the complete one Molding done by blow molding. This

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Palentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 - <[?(o 61 21) 56 53 82 ! Dipl.-Phys. Heinrich Seids · Palentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 - <[? (O 61 21) 56 53 82 !

bekannte Verfahren ist relativ kompliziert, nimmt erhebliche Zeit in Anspruch und läßt sich nicht im fortlaufenden Verfahren unter Bilden eines Halbzeugs durchführen. known method is relatively complicated, takes a considerable amount of time and cannot be continuous Carry out the process while forming a semi-finished product.

Demgegenüber ist es Aufgabe der Erfindung, ein Verfahren und eine Vorrichtung zu schaffen, die es dem Benutzer ermöglichen, beim Verarbeiten von Kunststoffen die sich mittels physikalischer Einflüsse, insbesondere Temperatureinflüsse wahlweise amorph oder teilkristallin einstellen lassen nach Wunsch den Kunststoff in der Formlingwand amorph oder in einem gewünschten Kristallinitätszustand und Kristallinitätsgrad einzustellen und dabei gewünschte physikalische Eigenschaften, beispielswei se gewünschte Elastizität, Festigkeit und bzw. oder Temperaturformbeständigkeit des Formlinge zu erreichen.In contrast, it is the object of the invention to provide a method and a device that the user enable when processing plastics which are affected by physical influences, in particular temperature influences The plastic in the molding wall can be set to either amorphous or partially crystalline as required amorphous or set in a desired crystallinity state and degree of crystallinity and thereby desired physical properties, e.g. desired ones To achieve elasticity, strength and / or temperature resistance of the molded article.

Erfindungsgemäß wird diese Aufgabe durch die Benutzung der folgenden Verfahrensmerkmale gelöst:According to the invention, this object is achieved by using the following method features:

für die Herstellung von Formungen aus solchem Kunststoff, dessen Kristallinitätszustand wahlweise zwischen amorph und teilkristallin einstellbar ist, wird das Einstellen des gewünschten Kristallinitätszustandes in der Formlingwand durch ein erstes, am Halbzeug auszuführendes Thermo-Konditionieren und ein zweites, am Formling auszuführendes Thermo-Konditionieren vorgenommen; for the production of moldings from such plastic, the crystallinity of which can be set between amorphous and partially crystalline Adjustment of the desired crystallinity state in the molding wall by means of a first, on the semi-finished product thermal conditioning to be carried out and a second thermal conditioning to be carried out on the molding;

Dipl.-Phys. Heinrich Seids ■ Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 ■ ξ?(ο 61 2ΐ) 5ό 53 ε* ;Dipl.-Phys. Heinrich Seids ■ Patent attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · PO Box 51 05 ■ ξ? (Ο 61 2ΐ) 5ό 53 ε *;

die bei dem zwischen Stabilisieren und Thermo verformen-, j auszuführenden ersten Thermo-Konditionieren auf das Vi Halbzeug auszuübenden physikalischen Einflüsse werden in vorher zu bestimmender Weise auf Erzielung eines ι gewünschten vorbereitenden Kristallinitätszustandes ' sowie Thermoverformbeirkeit des Kunststoffs des Halb- :the deforming between stabilizing and thermo, j first thermal conditioning to be carried out on the Vi Physical influences to be exerted on semifinished products are to be determined in advance in order to achieve a ι desired preparatory crystallinity state 'as well as thermoformability of the plastic of the semi-finished:

zeugs abgestimmt und modifiziert, wobei über dem Halb- ιstuff matched and modified, with over the half-ι

• Γ zeug-Querschnitt ein auf den anschließenden Thermo- !• Γ tool cross-section on the subsequent thermal!

Verformungsvorgang abgestimmtes und den gewünschten ! endgültigen Kristallinitätszustand im Kunststoff der ' Formlingwand vorbereitendes Temperaturprofil eingestellt wird; und : Deformation process coordinated and the desired! final crystallinity state in the plastic of the ' molding wall preparatory temperature profile is set; and :

das zweite Thermo-Konditionieren während des Thermo- jthe second thermo-conditioning during the thermo j

verformungsvorganges und wahlweise noch daran an- ' schließend wird mit Temperaturführung zu Erzeugung j bzw. Erhaltung des gewünschten endgültigen Kristallini-deformation process and optionally still attached to it ' then, with temperature control, production j or preservation of the desired final crystalline

tätszustandes im Kunststoff der Formlingwand in Verbindung mit Herbeiführen der Formbeständigkeit des Formlings ausgeführt.ity state in the plastic of the molding wall in connection with bringing about the dimensional stability of the Formlings executed.

Das erfindungsgemäße Verfahren bietet einerseits eine Vielzahl von wahlweise modifizierbaren und einstellbaren Verfahrensparametern, die reproduzierbar und genau vorher festlegbar den endgültigen Kristallinitätszustand des Kunststoffes in der Formlingwand und die für den Gebrauch des Formlings wesentlichen physikalischen Eigenschaften beeinflussen., Das wirksame Einsetzen und _______The method according to the invention offers, on the one hand, a large number of options that can be modified and set as desired Process parameters that are reproducible and precisely determinable in advance, the final crystallinity state of the plastic in the molding wall and the physical properties essential for the use of the molding affect., Effective onset and _______

aoao

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadler Hohe 15 · Postfach 51 05 · Q?(o 61 23) 56 53 82 jDipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadler Hohe 15 · Postfach 51 05 · Q? (O 61 23) 56 53 82 j

gegenseitiges Kombinieren der benutzten Verfahrensparametern, insbesondere der Wärmebehandlung während des Verfahrens, wird besonders günstig durch die Benutzung zweier .Thermo-Konditioniergänge. Ferner bietet das erfindungsgemäße Verfahren auch die Möglichkeit der Einbeziehung zusätzlicher, physikalischer Behandlungsschritte wie Strecken, Walzen, Kalandrieren, Verdichten, Bestrahlen, elektrostatische Behandlung, elektromagnetische Behandlung u.dgl. mehr ohne die Stabilität des Herstellungsganges und die gewünschte stabile Einstellung des Kristallinitätszustandes im Kunststoff der Formlingwand zu beeinträchtigen. Auch für diese zusätzlichen physikalischen Behandlungsschritte bieten die beiden Thermo-Konditionierungsgänge günstige Einsatz- und Kombinationsmöglichkeiten.mutual combination of the process parameters used, in particular the heat treatment during the process, is particularly cheap through the use of two .Thermo-conditioning courses. Furthermore, the invention offers Procedure also the possibility of including additional, physical treatment steps such as stretching, rolling, calendering, compaction, irradiation, electrostatic treatment, electromagnetic Treatment and the like more without the stability of the manufacturing process and the desired stable setting to impair the crystallinity state in the plastic of the molding wall. Even for these additional ones physical treatment steps, the two thermo-conditioning courses offer favorable application and Possible combinations.

Eine im Rahmen der Erfindung gegebene grundsätzliche Verfahrensmöglichkeit cjöit vor, daßA basic method possibility given within the scope of the invention cjöit before that

das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren über seinen gesamten Querschnitt unter Einstellen des gewünschten endgültigen Kristallinitätszustandes bis zu einer Temperatur abgekühlt wird, bei der keine erhebliche Veränderung des Kristallinitätszustandes im Kunststoff mehr stattfindet, und zwar auch beim Einrichten des Temperaturprofils für die Erfordernisse beim Thermoverformen in allen Halbzeug-Bereichen solche Temperaturen eingehalten werden, beithe semi-finished product during stabilization and initial thermal conditioning over its entire cross-section while setting the desired final crystallinity state is cooled to a temperature at which no significant change in the crystallinity state takes place more in the plastic, including when setting up the temperature profile for the Requirements for thermoforming in all areas of semi-finished products such temperatures are maintained at

130016/0098130016/0098

Dipl.-Phys. Heinrich Seide ■ Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · ^"(o 61 21) 56 53 8iDipl.-Phys. Heinrich Silk ■ Patent Attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · ^ "(o 61 21) 56 53 8i

welchen keine wesentliche Veränderung des Kristallinitätszustandes eintritt, undwhich no significant change in the crystallinity state occurs, and

beim Thermoverformen ein Tiefziehen und zweites
Thermo-Konditionieren zum fixieren des Kristallinitäts·■ zustandes im Kunststoff und der dabei geformten und
verfestigten Formlingwand erfolgen.
thermoforming, a deep drawing and a second
Thermo-conditioning to fix the crystallinity · ■ state in the plastic and the formed and
solidified molding wall.

Bei diesem, im Rahmen der Erfindung möglichen, grundsätzlichen Verfahrensablauf wird der im Kunststoff der
Formlingwand gewünschte endgültige Kristallinitätszu-
In this, possible within the scope of the invention, the basic process sequence in the plastic is the
Molding wall desired final crystallinity

stand weitgehend schon frühzeitig, nämlich beim Stabili- j sieren und ersten Thermo-Konditionieren des Halbzeugswas largely at an early stage, namely when the semi-finished product was stabilized and thermo-conditioned for the first time

j eingestellt und bis zur Fertigstellung der Formlinge jj set and until the moldings are finished j

weitestgehend beibehalten. ■;largely retained. ■;

Man kann diese grundsätzliche Verfahrensweise dazu benutzen, um im Halbzeug beim Stabilisieren und anschließenden ersten Thermo-Konditionieren einen weitgehend amorphen Zustand im Kunststoff einzustellen und
diesen weitgehend amorphen Zustand beim weiten Thermo-Konditionieren einschließlich Thermoverformen möglichst
This basic procedure can be used to set a largely amorphous state in the plastic in the semi-finished product during stabilization and subsequent first thermal conditioning
this largely amorphous state during extensive thermo-conditioning including thermoforming, if possible

weitgehend zu erhalten. Die auf diese Weise hergestellten!largely to be preserved. The ones made this way!

I Formlinge haben im Kunststoff ihrer Wandung praktisch ■I moldings have practically ■ in the plastic of their wall

amorphen Zustand und zeichnen sich durch relativ hohe !amorphous state and are characterized by relatively high!

i Elastizität und Nachgiebigkeit aus. Sie haben dafüri elasticity and resilience. You have for it

aber nur verhältnismäßig geringe Temperaturformbeständig-but only relatively low temperature resistance

i__L· i__L

Dipl.-Phys. Heinrich Seids · Patentanwalt ■ 6200 Wiesbaden 1 · Bierstadter"HoKe 15 · Postfach 51 05 ■ iSf(o 6i 21) 56 53Dipl.-Phys. Heinrich Seids · Patent Attorney ■ 6200 Wiesbaden 1 · Bierstadter "HoKe 15 · Postfach 51 05 ■ iSf (o 6i 21) 56 53

Eine andere, im Rahmen der Erfindung mögliche, grundsätzliche Verfahrensführung besteht darin, daß das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren über seinen gesamten Querschnitt rasch abgekühlt und auf ein Temperaturprofil eingestellt wird, das das Thermoverformen zuläßt, aber in allen Halbzeug-Bereichen Temperaturen einhält, bei denen keine wesentliche Veränderung des Kristallinitätszustandes in dem jeweiligen Kunststoff eintritt; .. das Thermoverformen auf mindestens eine Formoberfläche erfolgt, die auf eine Temperatur erwärmt ist, bei der Kristallwachsturn im jeweiligen Kunststoff eintritt undAnother basic method that is possible within the scope of the invention is that the semifinished product is rapidly cooled over its entire cross-section during stabilization and initial thermo-conditioning and is set to a temperature profile that allows thermoforming but maintains temperatures in all semifinished product areas in which there is no significant change in the crystallinity state in the respective plastic; A mold surface is carried out .. d as thermoforming at least, which is heated to a temperature which occurs in the crystal growth turn in the respective plastic and

das in Berührung der Formlingwand mit der erwärmten Formoberfläche erfolgende oder einsetzende zweite Thermo-Konditionieren in Temperatur und Zeitdauer auf Einstellung einer gewünschten Teilkristallinität des Kunststoffs der Fomflingwand abgestimmt wird.the second that takes place or begins in contact of the molding wall with the heated mold surface Thermal conditioning in terms of temperature and duration to achieve a desired partial crystallinity of the plastic of the Fomfling wall is matched.

Bei dieser Verfahrensweise wird ein Kristallinitätszustand im Kunststoff des Halbzeugs vorbereitend eingestellt und ausgehend von diesem Kristallinitätszustand beim Thermoverformen der gewünschte endgültige Kristallini tätszustand in der Formlingwand erzeugt. Man kann dabei den Kunststoff des Halbzeugs beim ersten Thermo-Konditionieren im wesentlichen in amorphen Zustand halten. Es ist jaber auch möglich^ den Kunststoff__de^s Halbzeugs Jbeim_In this procedure, a crystallinity state is set in the plastic of the semifinished product in preparation and starting from this crystallinity state during thermoforming the desired final crystalline ity state generated in the molding wall. The plastic of the semi-finished product can be thermo-conditioned for the first time keep in an essentially amorphous state. But it is also possible ^ the plastic__de ^ s semi-finished product Jbeim_

TiO 016/13 09 6TiO 016/13 09 6

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden χ · Bicrstadter Höhe 15 · Postfach 51 05 · Q?(o 61 21) 56 53 82 1Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden χ · Bicrstadter Höhe 15 · Postfach 51 05 · Q? (O 61 21) 56 53 82 1

ersten Thermo-Konditionieren einem ersten geringen j Kristallwachstum zu unterziehen. Die Wahl der einen jfirst thermal conditioning a first low j To undergo crystal growth. Choosing the one j

■ I oder anderen Möglichkeit richtet sich unter anderem \ ■ I or another possibility is directed, among other things, \

i nach dem gewünschten endgültigen Kristallinitätszustand ji according to the desired final crystallinity state j

1 im Kunststoff der Formlingwand und dem während des ι1 in the plastic of the molding wall and during the ι

Thermoverformens gewünschten Grad des Kristallwachstums, jThermoforming desired degree of crystal growth, j

Um das Kristallwachstum während des Thermoverformens in gewünschtem Maß hervorzurufen, kann die Formoberfläche auf einer Temperatur im Bereich unterhalb bis oberhalb der Temperatur für optimales Kristallwachstum im jeweiligen Kunststoff gehalten werden. Will man einen möglichst hohen Grad von Kristallwachstuin während des Thermoverformens bei angemessen kurzer Thermoverformzeit erreichen, so wird man die Formoberfläche auf einer Temperatur im Bereich der Temperatur für optimales Kristallwachstum im jeweiligen Kunststoff halten,ggf» im oberen Teil dieses Temperaturbereiches um möglichst schnell in dem Kunststoff die für optimales Kristallwachstum geeignete Temperatur einzustellen.In order to bring about the crystal growth during the thermoforming to the desired extent, the mold surface at a temperature in the range below to above the temperature for optimal crystal growth in the respective Plastic are held. If one wants the highest possible degree of crystal growth during the Thermoforming with an appropriately short thermoforming time reach, the mold surface will be at a temperature in the range of the temperature for optimum Keep crystal growth in the respective plastic, if necessary »in the upper part of this temperature range by as much as possible quickly in the plastic for optimal crystal growth set suitable temperature.

Wenn man im erfindungsgemäßen Verfahren beim Stabilisieren und ersten Thermo-Konditionieren des HalbzeugsIf one in the process according to the invention when stabilizing and first thermal conditioning of the semi-finished product

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 ■ Postfach 51 05 · (&(o 61 21) 56 53Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 ■ Postfach 51 05 · (& (o 61 21) 56 53

solche Temperaturverhältnisse einstellt, bei denen praktisch keine oder nur noch sehr geringe Veränderungen des Kristallinitätszustandes eintreten, dann kann man das Halbzeug während des ersten Thermo-Konditionierens und bzw. oder zwischen dem ersten Thermo-Konditionieren und dem Thermoverformen unter praktischem Beibehalten des Kristallinitätszustandes seines Kunststoffes einem Recken, beispielsweise biaxialen Recken als zusätzliche physikalische Bearbeitung unterwerfen. Dieses Recken kann in praktisch amorphen Zustand des Kunststoffs oder auch bei mehr oder weniger teilkristallinem Zustand des Kunststoffes erfolgen. Dieses Recken hat im Rahmen des erfindungsgemäßen Verfahrens die überraschende Wirkung, daß die unter diesem zusätzlichen, physikalischen Einfluß hergestellten Formlinge hohe Festigkeit, hohe Elastizität und hohe Temperaturformbeotändigkeit miteinander vereint aufweisen.sets such temperature conditions at which practically no or only very slight changes the state of crystallinity occur, then the semifinished product can be used during the first thermo-conditioning and / or between the first thermo-conditioning and thermoforming while practically maintaining it the crystallinity state of its plastic to stretching, for example biaxial stretching as additional subject to physical processing. This stretching can result in the plastic or in a practically amorphous state even if the plastic is in a more or less partially crystalline state. This stretching has in the context of Process according to the invention the surprising effect that under this additional, physical influence produced moldings high strength, high elasticity and high temperature resistance to each other show united.

Eine weitere Möglichkeit für die Durchführung des erfindungsgemäßen Verfahrens besteht darin, daß - das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren an seinen Oberflächenbereichen auf Temperaturen für zum Handhaben des Halbzeugs geeignete Verfestigung und im Inneren auf Temperaturen für optimales Kristallwachstum im jeweiligen Kunststoff eingestellt wird, undAnother possibility for carrying out the invention The method consists in that - the semi-finished product during stabilization and initial thermo-conditioning on its surface areas to temperatures suitable for handling the semi-finished product Solidification and inside at temperatures for optimal crystal growth in the respective plastic is set, and

das Thermoverformen auf mindestens eine Formoberflächethermoforming on at least one mold surface

Dipl.-Phys. Heinrich Scids · Patentanwalt · 6200 Wiesbaden t · Bierstadter Hohe 15 · Postfach 51 05 · ζ5?(ο 6i 21) 56 53 8iDipl.-Phys. Heinrich Scids Patent Attorney 6200 Wiesbaden t Bierstadter Hohe 15 Postfach 51 05 ζ5? (Ο 6i 21) 56 53 8i

erfolgt, die auf eine Temperatur erwärmt ist, bei der Kristallwachstum in dem jeweiligen Kunststoff eintritt.takes place, which is heated to a temperature at which crystal growth in the respective plastic entry.

Diese Ausführungsvariante des erfindungsgemäßen Verfahrens eignet sich besonders für solche Fälle, in denen möglichst weitgehendes Auskristallisieren des Kunststoffes in der Formlingwand erwünscht ist. Nach dieser Ausführungsvariante des Verfahrens hergestellte Formlinge zeichnen sich durch besonders hohe Temperaturformbeständigkeit aus. Bei dieser Durchführungsvarianten des erfindungsgemäßen Verfahrens ist es jedoch zweckmäßig, daß der Kunststoff im Inneren des Halbzeugs durch den Einfluß der eingestellten Temperatur und die zeitliche Dauer des ersten Thermo-Konditionierens zur Bildung eines solchen Kristallinitätszustandes eingestellt werden, bei dem der jeweilige Kunststoff noch thermoverformbar ist. Man kann jedoch auch - wenn erwünscht - den Kunststoff im Inneren des Halbzeugs durch den Einfluß der eingestellten Temperatur und die zeit- !This variant embodiment of the method according to the invention is particularly suitable for those cases in which the most extensive possible crystallization of the Plastic in the molding wall is desired. Manufactured according to this variant of the process Moldings are characterized by a particularly high temperature resistance the end. In this implementation variant of the method according to the invention, however, it is expedient to that the plastic inside the semi-finished product due to the influence of the set temperature and the time Set the duration of the first thermal conditioning to form such a crystallinity state in which the respective plastic is still thermoformable. You can, however, if you wish - The plastic inside the semi-finished product due to the influence of the set temperature and the time!

liehe Dauer des ersten Thermo-Konditionierens in einen \ jenseits der Grenze der eigentlichen Thermoverformbar- !lent duration of the first thermo-conditioning into a \ beyond the limit of the actual thermoformable!

keit des jeweiligen Kunststoffs liegenden Kristallinitäts-jability of the respective plastic lying crystallinity j

zustand überführen. In solchem Fall bilden die Oberflächen-state. In such a case, the surface

bereiche des Halbzeugs, die mehr oder weniger in amorphem j oder nur geringer teilkristallinem Zustand gehalten werden],areas of the semi-finished product that are kept more or less in an amorphous or only slightly partially crystalline state],

während des Thermoverformens ausreichend haltbare Schalen,!trays that are sufficiently durable during thermoforming!

130016/0096130016/0096

DipL-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadtcr Höhe 15 Pos'fac!. 51 o; · fl?(j 61 21) ,6 53 82 jDiploma Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadtcr Höhe 15 Pos'fac !. 51 o; Fl? (J 61 21), 6 53 82 j

zwischen denen sich der schon außerhalb der eigentlichen Thermoverformbarkeit kristallisierte Kunststoff im Inneren des Halbzeugs noch sicher verformen läßt. Bei dieser letzteren Ausführungsmöglichkeit des erfindungsgemäßen Verfahrens ist es besonders vorteilhaft, die Formoberflächen auf eine Temperatur für optimales Kristallwachstum in dem jeweiligen Kunststoff zu erwärmen. Es erfolgt dadurch ein letztes Durchwärmen des gesamten Kunststoffes der gebildeten Formlingwand und dadurch ein gleichmäßiges Auskristallisieren.between which the plastic, which has already crystallized outside of the actual thermoformability, is located in the Can still be safely deformed inside the semi-finished product. In this latter embodiment of the invention In the process, it is particularly advantageous to bring the mold surfaces to a temperature for optimal crystal growth to be heated in the respective plastic. This results in a final warming through of the whole Plastic of the molded wall formed and thereby a uniform crystallization.

Eine weitere Möglichkeit für die Durchführung des erfindungsgemäßen Verfahrens sieht vor, daß das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren an den Oberflächenbereichen seines Querschnitts auf Temperaturen für zum Handhaben des Halbzeugs geeignete Verfestigung eingestellt und im Inneren im wesentlichen auf der beim Extrudieren des Materialbandes benutzten Plastifiziertemperatur belassen wird;Another possibility for carrying out the invention The method provides that the semi-finished product is stabilized and initially thermo-conditioned at the surface areas of its cross-section to temperatures for handling the Set suitable solidification of the semi-finished product and essentially on the inside during the extrusion of the Material band used plasticizing temperature is left;

- das Thermoverformen auf mindestens eine Formoberfläche erfolgt, die auf eine Temperatur erwärmt ist, bei der Kristallwachstum in dem jeweiligen Kunststoff eintritt und
die Formlingwand zum zweiten Thermo-Konditionieren über eine auf den gewünschten endgültigen Kristallini-
- The thermoforming takes place on at least one mold surface which is heated to a temperature at which crystal growth occurs in the respective plastic and
the molding wall for the second thermo-conditioning via a final crystalline

der Formlingwand abgestimmte Zeitdauer auf. the molding wall on carefully prepared mth time period.

130016/0098130016/0098

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden ι ■ Uierstadtcr I'il.e ij · Postf^Ui 51 c^ · &"(.. 61 2.) 56 53 Sz Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden ι ■ Uierstadtcr I'il.e ij · Postf ^ Ui 51 c ^ · &"(.. 61 2.) 56 53 Sz

einer Temperatur gehalten wird, bei der Kristallwachs-ia temperature is maintained at which crystal wax-i

turn im Kunststoff der Formlingwand erfolgt. jturn takes place in the plastic of the molding wall. j

Bei dieser, im Rahmen der Erfindung möglichen, Verfahrens-In this, possible within the scope of the invention, process

i führung wird der Kunststoff im Inneren des Halbzeugs auf Ji guide, the plastic inside the semi-finished product is placed on J

einer Temperatur gehalten, die oberhalb desjenigen ;maintained at a temperature above that;

Temperaturbereiches liegt, in welchem Kristallwachstum jTemperature range in which crystal growth j

im jeweiligen Kunststoff eintritt. Die Oberflächenbe- joccurs in the respective plastic. The surface j

reiche des Halbzeugs werden dagegen so weitgehend abge- ] On the other hand, some of the semi-finished products are largely depleted ]

kühlt, daß in ihnen der jeweilige kristalline Zustand, |cools that in them the respective crystalline state, |

beispielsweise amorpher Zustand oder gering teil- I kristalliner Zustand eingefroren wird. Im Gegensatz zu ! den herkömmlichen Inline-Thermoformverfahren erfolgt '.'for example, amorphous state or low partial I crystalline state is frozen. In contrast to ! conventional inline thermoforming processes '.'

im eigentlichen Thermoverformvorgang jetzt ein voll- ! ständiges Durchwärmen der gesamten gebildeten Formling-in the actual thermoforming process now a fully! constant heating of the entire formed molding

wand und mit diesem Durchwärmen während des Thermo- |wall and with this warming up during the thermo- |

verformens und zweiten Thermo-Konditionierens die Ein- ■deforming and second thermo-conditioning the input ■

stellung des jeweils gewünschten mehr oder weniger ■position of the more or less desired in each case ■

stark teilkristallinen Zustandes. Da bei dieser Art ι der Verfahrensführung der Kunststoff im Inneren decstrongly partially crystalline state. Since with this type ι the process control of the plastic inside dec

Halbzeugs beträchtliche Wärmemengen in das erste Therrno- ίSemifinished considerable amounts of heat in the first thermal ί

Konditionieren und bis hin in das Thermoverformen und ;Conditioning and up to thermoforming and;

zweite Thermo-Konditionieren mitbringt, wird man vor- !brings a second thermo-conditioning with you, you will advance!

teilhafter Weise die Temperatur an den Formoberflächen
etwas unterhalb der Temperatur für optimales Kristall- . wachstum einstellen, um dadurch ein schnelleres Abkühlen j
part way the temperature on the mold surfaces
slightly below temperature for optimal crystal . set growth to allow faster cooling j

l__ _de_s Kunststoffs im Inneren der gebildeten Formlingwand ; l___de_s plastic in the interior of the molded wall formed;

130016/0098130016/0098

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · BierstaJter Höhe 15 · Postfach 51 05 · ζ?(ο 6ι 21) 56 53Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · BierstaJter Höhe 15 · P.O. Box 51 05 · ζ? (Ο 6ι 21) 56 53

in denjenigen Temperaturbereich hervorzurufen, in welchem optimales Kristallwachstum eintritt.cause in that temperature range in which optimal crystal growth occurs.

Bei allen erfindungsgemäßen Verfahrensvarianten, bei denen Kristallwachstum während des eigentlichen Thermoverformens zugelassen wird, kann man die Formlingwand so lange in Berührung mit der Formoberfläche halten, bis der Kunststoff den gewünschten Kristallinitätsgrad erreicht hat ο Man kann aber auch das Kristallwachstum auf der Formoberfläche nur einleiten und den Formling bei Erreichen ausreichender Formstabilität von der Formoberfläche abnehmen und das zweite Thermo-Konditionieren in einer sich an den Ausgang der Thermoverformvorrichtung anschliessenden Warmebehandlungsvorrichtung durchführen. Diese zweite Thermo-Konditionierung - beginnend auf der Formoberfläche - kann mit gleichbleibender Temperatur durchgeführt werden„ Man kann jedoch auch die Temperatur während des zweiten Thermo-Konditionierens verändern, beispielsweise mit zeitlich absinkender Temperatur temperieren. Bei der !letzteren Art der Temperaturführung kann man von einer Temperatur an der Formoberfläche aus- j gehen, die für optimales Kristallwachstum im jeweiligen Kunststoff geeignet ist und die Formlingwand zeitlich abkühlen.In all process variants according to the invention in which crystal growth occurs during the actual thermoforming is allowed, you can keep the molding wall in contact with the mold surface until the plastic has reached the desired degree of crystallinity ο but you can also increase the crystal growth only introduce the mold surface and remove the molding from the mold surface when sufficient dimensional stability has been achieved remove and the second thermo-conditioning in one at the output of the thermoforming device perform subsequent heat treatment device. This second thermal conditioning - starting on the mold surface - can take place at a constant temperature be carried out “You can also change the temperature change during the second thermal conditioning, for example with the temperature falling over time temper. In the case of the latter type of temperature control, a temperature at the mold surface can be used as a basis which is suitable for optimal crystal growth in the respective plastic and the molding wall in terms of time cooling down.

Das Thermoverformen kann im erfindungsgernäßen Verfahren unter Ausüben von Formdruck auf den Kunststoff der Form-The thermoforming can in the process according to the invention while exerting mold pressure on the plastic of the mold

130016/0098130016/0098

Dipl.-Phys. Heinrich Scids · I'atcnljnwalt · 6200 Wiesbaden t · Uicrst.idler Hohe 15 · l'oslfach 51 05 ■ φζ'(ο6ι .·ι) ;;ι. y·, Λι Dipl.-Phys. Heinrich Scids · I'atcnljnwalt · 6200 Wiesbaden t · Uicrst.idler Hohe 15 · l'oslfach 51 05 ■ φζ '(ο6ι. Ι) ;; ι. y ·, Λι

lingwand ausgeführt werden. Dieser Formdruck kann ggf„ ; zu einer gewissen Verdichtung des Kunststoffs geeignet ' gewählt werden. ' jlingwand are executed. This form pressure can possibly "; suitable for a certain compression of the plastic 'can be selected. 'j

Das erfindungsgemäße Verfahren läßt auch zu, daß Halb- :The inventive method also allows that half:

1 zeug zwischen dem Extrudieren und dem Thermoverformen ;1 tool between extrusion and thermoforming;

einem Kalandrier- und bzw. oder Walzvorgang unter , Dickenreduzierung zur zusätzlichen physikalischen Be- : einflussung des Kristallinitätszustandes zu unterwerfen. '\ Dieses Kalandrieren bzw. Walzen kann in das Stabilisieren ιa calendering and / or rolling process under, thickness reduction for additional physical: influencing the crystallinity state. '\ This calendering or rolling can be incorporated into the stabilization ι

des Halbzeugs einbezogen werden. jof the semi-finished product are included. j

Das erfindungsgemäße Verfahren läßt sich bevorzugt für i die Herstellung von Formungen aus Polyäthylen-Terephthalat einsetzen. Es kommt jedoch auch ebensogut ■ die Herstellung von Formungen aus modifizierten Poly-The inventive method can preferably be used for i use the manufacture of moldings from polyethylene terephthalate. However, it also happens just as well the production of moldings from modified poly-

äthylen-Terephthalat beispielsweise 1,4 - Cyclohexyl- ; dimethylenterephthalat / Isophthalat - Copolymerisat .
in Betracht. Denkbar ist auch die Herstellung von
Formungen aus Polybutylenterephthalat im erfindungsgemäßen Verfahren. Im letzteren Fall ist jedoch zu
ethylene terephthalate, for example 1,4 - cyclohexyl; dimethylene terephthalate / isophthalate copolymer.
into consideration. The production of
Moldings from polybutylene terephthalate in the process according to the invention. In the latter case, however, is closed

beachten, daß der Temperaturbereich, innerhalb dessen
Kristallwachstum in Polybutylenterephthalat eintritt,
weit herunter d.ho bis etwa 300C reicht.
note that the temperature range within which
Crystal growth occurs in polybutylene terephthalate,
far down that o extends to about 30 0C.

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Palentanwalt · 6200 Wiesbaden 1 · Bicrstadter Höhe 15 · Postfach 51 05 · ®(o 61 21) 56 53Dipl.-Phys. Heinrich Seids · Palentanwalt · 6200 Wiesbaden 1 · Bicrstadter Höhe 15 · Postfach 51 05 · ® (o 61 21) 56 53

Für die Durchführung des erfindungsgemäßen Verfahrens eignet sich insbesondere eine Vorrichtung mit einer Extrudiervorrichtung zur kontinuierlichen Herstellung des Halbzeugs, einer Stabilisiervorrichtung für das Halbzeug und einer Thermoverformungsvorrichtung undA device with a is particularly suitable for carrying out the method according to the invention Extrusion device for the continuous production of the semi-finished product, a stabilizing device for the Semi-finished product and a thermoforming device and

einer Thermo-Konditionierungsvorrichtung für das Halbzeug, sowie ggf. eine Vorrichtung zum Heraustrennen der Formlinge aus den umgebenden Teilen des Halbzeugs. Eine solche Vorrichtung sollte sich erfindungsgemäß kenn- *Ό zeichnen durch die folgenden Merkmale: - Zwischen der Stabilisierungsvorrichtung und der Thermo-a thermo-conditioning device for the semi-finished product, and possibly a device for separating out the Moldings from the surrounding parts of the semi-finished product. Such a device should be known according to the invention * Ό have the following features: - Between the stabilization device and the thermal

Verformungsvorrichtung ist eine erste Thermo-Konditionierstation angeordnet; Die Thermoverformungsvorrichtung liegt in einer zweitenA first thermo-conditioning station is arranged in the deforming device; The thermoforming device lies in a second

Thermo-Konditionierstation; jThermal conditioning station; j

Die Stabilisierungsvorrichtung und die Thermoverformungsvorrichtung sind mit Steuereinrichtung zu vorher festgelegter ggf. programmierbarer Regelung der in der Stabilisierungsvorrichtung und der Thermo-Verformungsvorrichtung erfolgenden physikalischen, insbesondere thermischen Einwirkungen auf den Kunststoff des Halbzeugs ausgestattet und den Thermo-Konditionierstationen sind Einrichtungen zu physikalischem, insbesondere thermischem Einwirken auf den Kunststoff des Halbzeugs bzw. Form-The stabilization device and the thermoforming device are with the control device to previously defined, possibly programmable regulation the physical in the stabilization device and the thermoforming device, in particular equipped with thermal effects on the plastic of the semi-finished product and the thermo-conditioning stations are facilities for physical, in particular thermal, action on the plastic of the semi-finished product or molded

lings und Steuereinrichtungen zu vorher festgelegter, ggf. programmierbarer Regelung der Einwirkungsein-130018/0096 ~~ lings and control devices to previously defined, possibly programmable regulation of the impacts 130018/0096 ~~

ORIGINALORIGINAL

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden t ■ Bierstadter Höhe 15 · Postfach 51 05 ■ ί?(ο οι 2j) 56 53 82Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden t ■ Bierstadter Höhe 15 · Postfach 51 05 ■ ί? (Ο οι 2j) 56 53 82

richtung zugeordnet. \ assigned direction. \

Eine solche Vorrichtung bietet den Vorteil, daß sie ohne jSuch a device has the advantage that it can be used without j

j nennenswerte Umrüstungsmaßnahmen praktisch alle ge- \ j significant retooling measures to virtually all \

wünschten Varianten des erfindungsgemäßen Verfahrens j durchführen läßt. Sie bietet auch den Vorteil, daß Ein- , richtungen für gewünschte spezielle, physikalische Ein- |desired variants of the method according to the invention can be carried out j. It also offers the advantage that input, directions for required special, physical equipment

wirkung wie Recken, Walzen, Bestrahlen usw. ohne | Schwierigkeit an gewünschter Stelle in die Vorrichtung j eingefügt werden können» ιeffects such as stretching, rolling, irradiating, etc. without | Difficulty at the desired point in the device j can be inserted »ι

Die erfindungsgemäße Vorrichtung kann in ihren Thermo- j Konditionierungsstationen vornehmlich in der ersten !The device according to the invention can be used in its thermo-conditioning stations primarily in the first!

Thermo-Konditionierstation für das Halbzeug mit Heiz- ίThermal conditioning station for the semi-finished product with heating ί

und Kühleinrichtungen für das Halbzeug bzwo die Form- \ and cooling devices for the semi-finished product or o the form \

linge mit Regelmöglichkeit für Temperatur und Heiz- , bzw. Kühlzeit ausgerüstet sein. Mit dieser Ausrüstung ] ist das Thermo-Konditionieren in der erfindungsgemäßen \ be equipped with control options for temperature and heating or cooling time. With this equipment], the thermal conditioning is in the \

Vorrichtung in allen denkbaren Verfahrensvarianten mit ' voller Sicherheit und optimaler Wirksamkeit durchführ- j bar. j Device in all conceivable variants of the process with 'full safety and optimum efficiency feasibility j bar. j

ι Der ersten Thermo-Konditionierstation, nämlich derjenigen : ι The first thermal conditioning station, namely the one:

für das Halbzeug, kann auch eine Reckvorrichtung für das jfor the semi-finished product, a stretching device for the j

Halbzeug mit Regelmöglichkeit für Recktemperatur, Reckungs|Semi-finished product with control option for stretching temperature, stretching |

grad und ggf. Reckgeschwindigkeit zugeordnet sein. Dasdegree and, if necessary, the stretching speed. That

130016/009Θ130016 / 009Θ

Dipl.-Phys. Heinrich Seids · Palentanwalt ■ 6200 Wiesbaden ι · Bierstadtor Höhe 15 · Postfach 51 05 · ®(o 61 21) 56 53Dipl.-Phys. Heinrich Seids · Palentanwalt ■ 6200 Wiesbaden ι · Bierstadtor Höhe 15 · Postfach 51 05 · ® (o 61 21) 56 53

Zuordnen der Reckvorrichtung zur ersten Thermo-Konditionierstation hat seinen besonderen Vorteil darin, daß der Reckvorgang in einem Stadium des Halbzeugs vorgenommen wird, bei dem optimale Bedingungen für das Recken selbst und auch optimale Bedingungen für die Einwirkung des Reckens auf den Kristallinitätszustand des Kunststoffes einstellbar sind und auch bis zum Thermoverformen erhalten bleiben können.Assignment of the stretching device to the first thermal conditioning station has its particular advantage that the stretching process is carried out in one stage of the semi-finished product is where optimal conditions for the stretching itself and also optimal conditions for the Effect of stretching on the crystallinity state of the plastic are adjustable and also up to Thermoforming can be retained.

Will man in der erfindungsgemäßen Vorrichtung zusätzliehe Einrichtungen zum Kalandrieren und bzw. oderIf one wants additional devices for calendering and / or or in the device according to the invention

! Walzen eines bandförmigen Halbzeugs unter Dicken-! Rolling a strip-shaped semi-finished product under thickness

j reduzierung vorsehen, so könnte diese der Stabilisierung^j provide for a reduction, so this could stabilize ^

vorrichtung zugeordnet werden.device can be assigned.

In der erfindungsgemäßen Vorrichtung können die in der Stabilisierungsvorrichtung vorgesehenen Kühleinrichtungen mit Einrichtungen zum Erzeugen einer in zeitlicher Folge auf den Kunststoff des Halbzeugs wirksamen, regelbaren Temperaturführung ausgestattet sein. Dies bedeutet, daß bei Hintereinanderanordnung mehrerer Kühleinrichtungen diese mit verschiedenen Temperaturen betrieben werden können.The cooling devices provided in the stabilizing device can be used in the device according to the invention with devices for generating a controllable one that is effective in chronological order on the plastic of the semi-finished product Be equipped with temperature control. This means that when several cooling devices are arranged one behind the other these can be operated at different temperatures.

In der erfindungsgemäßen Vorrichtung sollte die Thermoverformvorrichtung zweckmäßig mit mindestens einem Formwerkzeug ausgestattet sein^d In the device according to the invention, the thermoforming device should expediently be equipped with at least one molding tool

130016/0098130016/0098

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 ■ ^"(o 61 21) 56 53 82Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · P.O. Box 51 05 ■ ^ "(o 61 21) 56 53 82

kühlbare Formoberfläche aufweist. Zweckmäßig kann die
Thermoverformvorrichtung mindestens ein Formwerkzeug
enthalten, das mit einer Steuereinrichtung zum Erzeugen j einer vorher festlegbaren ggf. programmierbaren zeit- , liehen Temperaturänderung bzw. Temperaturführung während ,
Has coolable mold surface. The
Thermoforming device at least one molding tool
contain, which with a control device for generating j a previously definable, possibly programmable time, borrowed temperature change or temperature control during,

f des Thermoverformvorganges an mindestens einer Formober- | fläche ausgerüstet ist. Die Thermoverformvorrichtung kann j auch mindestens ein Formwerkzeug enthalten, das mit Ein- ■ richtungen zum Erzeugen eines vorher festlegbaren, regelbaren Formdruckes ausgestattet ist. Diese Einrichtungen f of the thermoforming process on at least one upper mold | area is equipped. The thermoforming device can also contain at least one molding tool which is equipped with devices for generating a pre-determinable, controllable molding pressure. These bodies

zum Erzeugen des Formdruckes können mit Steuereinrichtungen zum regelbaren ggf. programmierbaren zeitlichen Variieren ■ des Formdruckes während des Thermoverformvorganges aus- ' gerüstet sein. ito generate the form pressure, control devices for controllable, possibly programmable, temporal variation can be used the molding pressure during the thermoforming process' be equipped. i

i In der erfindungsgemäßen Vorrichtung kann bevorzugt die j zweite Thermo-Konditionierungsstation in ihrem Eingangs- I bereich die Thermoverformungsvorrichtung enthalten und j sich über den Ausgang der Thermoverformungsvorrichtung jIn the device according to the invention, the j second thermal conditioning station can preferably be located in its entrance I area contain the thermoforming device and j is on the output of the thermoforming device j

hinaus erstrecken. Dabei kann die zweite Thermo-Kondition-' ierungsstation eines sich an den Ausgang der Thermover- \ formungsvorrichtung anschliessenden Wärmebehandlungsvor- I richtung für die Formlinge enthalten.extend beyond. Here, the second thermal-Kondition- 'ierungsstation one at the output of the thermoformable \ molding apparatus subsequent Wärmebehandlungsvor- I device for the moldings contain.

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids ■ Patentanwalt ■ 6100 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · <3?(o 61 21) 56 53 82 jDipl.-Phys. Heinrich Seids ■ Patent attorney ■ 6100 Wiesbaden 1 · Bierstadter Höhe 15 · PO Box 51 05 · <3? (O 61 21) 56 53 82 j

Ausführungsbeispiele der Erfindung v/erden im folgenden anhand der Zeichnung näher erläutert. Es zeigen:Embodiments of the invention are explained in more detail below with reference to the drawing. Show it:

Fig. 1 ein Schema für den grundsätzlichen Ablauf des erfindungsgemäßen Verfahrens bzw. den1 shows a scheme for the basic sequence of the method according to the invention or the

grundsätzlichen Aufbau einer erfindungsgemäßen Vorrichtung;basic structure of a device according to the invention;

Fig. 2 die Abhängigkeit der Kristallwachstumsgeschwindigkeit V von der Temperatur T bei2 shows the dependence of the crystal growth rate V on the temperature T at

Polyäthylenterephthalat; IPolyethylene terephthalate; I.

Fig. 3 eine Gruppe von Temperaturprofilen für ι eine erste Ausführungsmöglichkeit des erfindungsgemäßen Verfahrens mit Polyäthylenterephthalat ;Fig. 3 shows a group of temperature profiles for ι a first possible embodiment of the method according to the invention with polyethylene terephthalate ;

Fig. 4 eine Gruppe von Temperaturprofilen für4 shows a group of temperature profiles for

eine zweite Ausführungsmöglichkeit des erfindungsgemäßen Verfahrens mit Polyäthylenterephthalat ;a second embodiment of the method according to the invention with polyethylene terephthalate ;

Fig. 5 eine Gruppe von Temperaturprofilen für eine dritte Ausführungsmöglichice it des5 shows a group of temperature profiles for a third embodiment of the

erfindungsgemäßen Verfahrens mit Polyäthylenterephthalat ;
Fig. 6 eine Gruppe von Temperaturprofilen für
process according to the invention with polyethylene terephthalate;
6 shows a group of temperature profiles for

j eine vierte Ausführungsmöglichkeit desj a fourth option for the

erfindungsgemäßen Verfahrens mit Polymethod according to the invention with poly

äthylenterephthalat ;ethylene terephthalate;

130016/0096130016/0096

3?3?

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden ι · Bierstadter Hohe 15 · Postfach 51 05 · ^(o 61 21) 56 53 82Dipl.-Phys. Heinrich Seids Patent Attorney 6200 Wiesbaden ι Bierstadter Hohe 15 Postfach 51 05 ^ (o 61 21) 56 53 82

Fig. 7 eine Gruppe von Temperaturprofilen für eine fünfte Ausführungsmöglichkeit des erfindungngemäßen Verfahrens mit Polyathylenterephthalat ;7 shows a group of temperature profiles for a fifth embodiment of the process according to the invention with polyethylene terephthalate ;

Fig. 8 eine Gruppe von Temperaturprofilen für8 shows a group of temperature profiles for

eine sechste Ausführungsmöglichkeit des erfindungsgernäßen Verfahrens mit Polyathylenterephthalat unda sixth embodiment of the process according to the invention with polyethylene terephthalate and

Fig. 9 eine Gruppe von Temperaturprofilen für eine siebte Ausführungsmöglichkeit des9 shows a group of temperature profiles for a seventh embodiment of the

erfindungsgemäßen Verfahrens mit Polyathylenterephthalat .Process according to the invention with polyethylene terephthalate .

Figur 1 illustriert die Folge von Arbeitsgängen in einer ! Figure 1 illustrates the sequence of operations in one !

bevorzugten Ausführungsform des Verfahrens zum Herstellen ι dünnwandiger Artikel aus thermoplastischem Kunststoff, |Preferred embodiment of the method for producing ι thin-walled articles made of thermoplastic material, |

der wahlweise amorph oder mehr oder weniger teilkristallin;the optionally amorphous or more or less partially crystalline;

! eingestellt werden kann. Im dargestellten Beispiel ist! can be adjusted. In the example shown is

eine Extruderpresse 11 vorgesehen, die dazu geeignet ist, |an extruder press 11 is provided which is suitable for |

den granulierten thermoplastischen Kunststoff, beispiels- ; weise Polyathylenterephthalat, aufzunehmen und kontinuier-i lieh zu komprimieren und zu heizen, bis er geschmolzenthe granulated thermoplastic material, for example; wise polyethylene terephthalate, to include and continuous-i lent to compress and heat until melted

wird und mit einer Temperatur TE (Figuren 3 bis 8) ober- jis and with a temperature T E (Figures 3 to 8) above j

halb des Kristall-Schmelzpunktes dem Extrudierwerkzeug, \ half of the crystal melting point to the extrusion tool, \

beispielsweise einer Breitschlitzdüse 12, zuzuführen. !for example a slot nozzle 12 to be supplied. !

Diese Breitschlitzdüse 12 ergibt im vorliegenden Beispiel ;This slot nozzle 12 results in the present example;

i ein bandförmiges Halbzeug 10, das aus der BreitschlitzdüseI i a strip-shaped semi-finished product 10, which is produced from the slot die I.

130016/009B130016 / 009B

Dipl.-Phys. Heinrich Seids ■ Patentanwalt · 6200 Wiesbaden 1 ■ Bierstadtcr Höhe 15 · Postfacfi '51 05 · S?(o 61 21) 56 53 82Dipl.-Phys. Heinrich Seids ■ Patent Attorney · 6200 Wiesbaden 1 ■ Bierstadtcr Höhe 15 · Postfacfi '51 05 · S? (O 61 21) 56 53 82

12 kommend in die Stabilisierungsvorrichtung 13 eingeführt wird. In der Stabilisierungsvorrichtung 13 wird in erster Linie das Halbzeug 10 durch Abkühlen mindestens einer Oberfläche für das weitere Verfahren handhabbar gemacht. Aus der Stabilisierungsvorrichtung 13 läuft das bandförmige Halbzeug 10 in eine erste Konditionierstation 14. Diese Halbzeug-Konditionierntation 14 hat in erster Linie den Zweck, in dem Halbzeug 10 vorbereitende Temperaturprofile einzustellenο Es ist aber auch Zweck der Halbzeug-1q Konditionierstation 14, an dem Halbzeug 10 zusätzliche gewünschte physikalische Einflüsse auszuüben oder vorher in dem Halbzeug 10 ausgeübte zusätzliche physikalische Einflüsse zu fixieren.12 is introduced into the stabilization device 13 as it comes will. In the stabilization device 13, the semifinished product 10 is primarily at least one by cooling Surface made manageable for the further process. The ribbon-shaped runs out of the stabilizing device 13 Semifinished product 10 in a first conditioning station 14. This semifinished product conditioning station 14 has primarily the purpose of setting preparatory temperature profiles in the semi-finished product 10 o But it is also the purpose of the semi-finished product 1q Conditioning station 14 to exert additional desired physical influences on the semi-finished product 10 or beforehand to fix additional physical influences exerted in the semi-finished product 10.

j Zu diesen Zwecken ist die Halbzeug-Konditionierstation 14 mit Heizeinrichtungen und Kühleinrichtungen ausgestattet, die Regeleinrichtungen aufweisen, die nach Wunsch steuerbar und ggf. programmierbar sind. Außerdem können der Halbzeug-Konditionierstation 14 Einrichtungen für physikalische Beeinflussung des Halbzeugs 10 zugeordnet sein. Dazu gehören Reckvorrichtungen, Bestrahlungsvorrichtungen, eventuell Walz- und Verdichtungsvorrichtungen.j For these purposes, the semi-finished product conditioning station 14 is equipped with heating devices and cooling devices, which have control devices that can be controlled and, if necessary, programmed as desired. In addition, the Semifinished product conditioning station 14 assigned to devices for physically influencing the semifinished product 10 be. This includes stretching devices, irradiation devices, possibly rolling and compacting devices.

I Die letzteren Vorrichtungen können jedoch auch bereits inI The latter devices can, however, already be used in

die Stabilisierungsvorrichtung 13 einbezogen werden.the stabilization device 13 are included.

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Biersta»1»-?- Höh» 15 · j^-trac1» 51 05 · '2"(O .;i n) 56 53 82 IDipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Biersta » 1 » -? - Höh »15 · j ^ -trac 1 » 51 05 · '2 "(O .; I n) 56 53 82 I.

Im dargestellten Beispiel ist die Halbzeug-Konditionier- |In the example shown, the semi-finished product conditioning |

i station 14 zweistufig ausgebildet, nämlich mit einer erstenj Stufe 14a, die zur Behandlung d.h. zum Thermo-Konditionieren des kontinuierlich hindurchgeführten Halbzeugs 10
ausgebildet ist, und mit einer zweiten Stufe 14b, die für
Behandlung und Thermo-Konditionieren des schrittweise
hindurchgeführten Halbzeugs 10 ausgebildet ist0 Zv/ischen
i station 14 is designed in two stages, namely with a first stage 14a, which is used for treatment, ie for thermal conditioning of the semi-finished product 10 that is continuously passed through
is formed, and with a second stage 14b, which for
Treatment and thermo-conditioning of the gradual
semifinished product 10 passed through is formed 0 Zv / ischen

beiden Stufen 14a und 14b der Halbzeug-Konditionierstation jtwo stages 14a and 14b of the semi-finished product conditioning station j

14 - in die Halbzeug-Konditionierstation 14 einbezogen - j ist eine Vorrichtung 15 zum Steuern und Umsetzen der Be- !14 - included in the semi-finished product conditioning station 14 - j is a device 15 for controlling and converting the loading!

wegung des Halbzeugs 10 von kontinuierlichem Vorschub auf ' schrittweisen Vorschub vorgesehen. Mit dieser Vorrichtung ιmovement of the semi-finished product 10 from continuous feed to ' gradual feed provided. With this device ι

15 wird die Vorschubbewegung des Halbzeugs 10 auf den i Arbeitstakt der schrittweise des Halbzeug 10 aufnehmenden '15 is the feed movement of the semi-finished product 10 on the i Work cycle of the gradually picking up the semi-finished product 10 '

Fertigteil-Konditionierstation 17 mit Thermoverformvor-Finished part conditioning station 17 with thermoforming

richtung 16 abgestimmt. jdirection 16 coordinated. j

Diese Fertigteil-Konditionierstation 17 bzw, zweite \ Thermo-Konditionierstation 17 enthält in ihrem ersten j Teil die Thermoverformvorrichtung 16, die im dargestellten!This pre-fabricated conditioning station 17 or second \ thermo-conditioning station 17 contains in its first part the thermoforming device 16, which is shown in the!

Beispiel mit Tiefziehwerkzeugen ausgestattet ist, deren ' Formflächen nach Wahl heizbar oder kühlbar sind und auch j zum Verändern der Temperatur während jedes Arbeitsablaufes j ausgebildet sein können. Nach der Darstellung der Figur 1 ! schließt sich an die Thermoverformungsvorrichtung 16 noch J ein Abschnitt der Fertigteil-Konditionierstation 17 an,Example is equipped with deep-drawing tools whose ' Mold surfaces can be heated or cooled as desired and also j to change the temperature during each work cycle j can be formed. According to the representation of Figure 1! the thermoforming device 16 is followed by J a section of the precast conditioning station 17,

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfacn 51 05 · ξ?(ο 6ι 21) 56 53Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfacn 51 05 · ξ? (Ο 6ι 21) 56 53

der im dargestellten Beispiel von dem aus der Thermoverformungsvorrichtung 16 kommenden bandförmigen Halbzeug mit eingeformten Formungen 16 schrittweise durchlaufen wirrt. In diesem zweiten Abschnitt der Fertigteil-Konditionierstation 17 sind Heiz-"und Kühleinrichtungen angebracht. Außerdem könen dort auch noch Einrichtungen zur physikalischen Behandlung der Formlinge 18 beispielsweise zum Bestrahlen oder Beschallen und dergleichen mehr angeordnet sein.that in the example shown from the one from the thermoforming device 16 coming band-shaped semi-finished product with molded-in formations 16 gradually go through confuses. In this second section of the precast conditioning station 17 are heating and cooling devices appropriate. In addition, there can also be devices for the physical treatment of the molded articles 18, for example be arranged for irradiation or sonication and the like.

Aus der zweiten Thermo-Konditionierstation 17 gelangt das j bandförmige Halbzeug mit eingeformten Formungen 18 in ■From the second thermo-conditioning station 17, the j band-shaped semi-finished product with molded-in formations 18 in ■

j eine Stanzvorrichtung 19, mit der die Formlinge 18 aus- j geschnitten und die Halbzeugreste 20 zur Materialrückgewinnung ggf. direkten Rückführung des zerkleinerten Materials zur Extruderpresse 11 abgeführt werden.j a punching device 19 with which the moldings 18 are cut out and the semi-finished product residues 20 for material recovery if necessary, direct return of the comminuted material to the extruder press 11 can be discharged.

Das oben beispielshalber als Kunststoffband angesprochene Halbzeug 10 kann bei Verarbeitung von Polyäthylenterephthalat eine Dicke von etwa 2 mm aufweisen.The semifinished product 10 mentioned above as a plastic tape by way of example can be used when processing polyethylene terephthalate have a thickness of about 2 mm.

Anstelle von bandförmigen Halbzeug kommen auch jegliche anderen denkbaren und kontinuierlich herstellbare Halbzeuge in Betracht, beispielsweise Schläuche, Profilstränge u.dgl β mehr.Instead of strip-shaped semi-finished products, any other conceivable and continuously producible semi-finished products are also used into consideration, for example hoses, profile strands and the like β more.

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · ®"(o 6x 21) 56 53 82Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · ® "(o 6x 21) 56 53 82

Das Halbzeug kann auch Schichtmaterial aus verschiedenen
Kunststoffen sein, von denen allerdings ein wesentlicher \ Teil solche Kunststoffe sein sollen, die durch physikalische Beeinflussung insbesondere durch Temperaturführung wahl- \ weise amorph oder in gewünschtem Ausmaß teilkristallin ein-j
The semi-finished product can also consist of different layer material
Be plastics, of which however a substantial \ part should be such plastics obtained by physical interference especially by temperature control \ election as amorphous or desired extent partially crystalline a-j

stellbar sind. jare adjustable. j

Eine Druckbehandlung des Kunststoffes kann am Halbzeug \ beispielsweise durch Walzen oder Kalandrieren in der i Stabilisierstation 13 oder auch im ersten Teil 14a der
Halbzeug-Konditionierstation 14 vorgenommen werden. Es \ ist aber auch denkbar, eine Druckbehandlung des Kunststoffes durch schrittweises Flächenpressen beim schritt- ; weisen Durchführen durch den zweiten Teil 14b der Halb- i zeug-Konditionierstation 14 durchzuführenο Die Erfindung j ermöglicht ferner, Druckbehandlung am Formling bzw. j Fertigteil d.h. innerhalb der zweiten Thermo-Konditionier- \ station 17. Bevorzugt wird man diese Druckbehandlung am | Fertigteil durch Ausüben eines vorher bestimmten Form- ; druckes in der Thermoverformungsvorrichtung 16 ausführen. ,
A pressure treatment of the plastic can at the half-finished \ for example by rolling or calendering in the i stabilizing station 13 or in the first part 14a of the
Semi-finished conditioning station 14 are made. It is also conceivable \, a pressure treatment of the plastic surface by gradually pressing the gradual; comprise performing i through the second part 14b of the semi-finished-conditioning station 14 durchzuführenο j The invention further enables, pressure treatment at the molding or j finished part that is inside the second thermal conditionable \ station 17. Preferably, it will be this pressure treatment at | Finished part by exercising a predetermined shape; pressure in the thermoforming device 16 run. ,

Anstelle der Druckbehandlung, sei es am Halbzeug oder arnInstead of the pressure treatment, be it on the semi-finished product or arn

ι Fertigteil, oder zusätzlich dazu, kann ach eine Ultraschall-;ι prefabricated part, or in addition to it, can also be an ultrasonic;

behandlung vorgenommen werden. Die Druckbehandlung bzw. \ die Ultraschallbehandlung führt neben der Beeinflussung
des Kristallinitätszustandes auch zu wesentlich erhöhter
treatment can be carried out. The pressure treatment or \ ultrasound treatment results in addition to the influence
the crystallinity state is also significantly increased

130016/0096130016/0096

Dipl.-Phys. Heinrich Scids ■ Patentanwalt ■ 6200 Wiesbaden 1 · Bicrstaditr iIOl>e 15 · Po< >>faclv>i 05 · C?(o 6. zi) 56 57Dipl.-Phys. Heinrich Scids ■ Patent attorney ■ 6200 Wiesbaden 1 · Bicrstaditr iIOl> e 15 · Po < >> faclv> i 05 C? (o 6. zi) 56 57

Steifigkeit und damit verbesserter Kalt-Formbeständigkeit der hergestellten Formlinge.Rigidity and thus improved cold dimensional stability of the moldings produced.

Die in Figur 2 gezeigte Kurve, zeigt die Abhängigkeit der Kristallwachstumsgeschwindigkeit V in Polyäthylenterephthalat in Abhängigkeit von der in Grad Celsius aufgetragenen Temperatur T. Wie Figur 2 zeigt, weist Polyäthylenterephthalat zwischen 10O0C und dem Kristallinschmelzpunkt (250 bis 260°C) einen Kristallwachstums-Temperaturbereich innerhalb dessen optimales Kristallwachstum bei etwa 1700C bis 1750C eintritt. Oberhalb vom Kristallinschmelzpunkt geht Polyäthylenterephthalat in plastifizierten Zustand über. Unterhalb 600C liegt Polyäthylenterephthalat in festem Zustand vor, ohne das in dem Material noch Kristallwachstum in nennenswerten Maß vonstatten geht. Dies bedeutet, daß sich durch Abkühlen des Polyathylenterephthalats unter 6O0C der jeweilige Kristallinitätszustand des Materials einfrieren läßt.The curve shown in Figure 2, showing the dependency of the crystal growth rate V in polyethylene terephthalate as a function of the applied in degrees Celsius temperature T. As Figure 2 shows, polyethylene terephthalate has, between 10O 0 C and the crystalline melting point (250 to 260 ° C) a crystal growth Temperature range within which optimal crystal growth occurs at around 170 ° C. to 175 ° C. Above the crystalline melting point, polyethylene terephthalate changes to a plasticized state. Below 60 0 C is polyethylene terephthalate before solid state, without the crystal growth is still in the material in significant measure vonstatten. This means that it is possible to freeze the material by cooling the Polyathylenterephthalats below 6O 0 C, the respective state of crystallinity.

Zur Vereinfachung der Erläuterungen sei im Rahmen dieser Anmeldung auch der amorphe Zustand als ein Kristallinitäts-j zustand, nämlich ein Zustand mit "Kristallinität Null" anzusehen.To simplify the explanations, the amorphous state should also be used as a crystallinity j in the context of this application state, namely to consider a state with "crystallinity zero".

130018/0096130018/0096

Dipl.-Phys. Heinrich Scids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Hüne 15 · Postfacn 51 05 · *5?(o 01 21) 56 53 82Dipl.-Phys. Heinrich Scids Patent Attorney 6200 Wiesbaden 1 Bierstadter Hüne 15 Postfacn 51 05 * 5? (O 01 21) 56 53 82

i. Mit dem erfindungsgemäßen Verfahren sollen wirtschaft- J lieh günstige Herstellungsmö'glichkeiten für Formlinge j aus Kunststoff mit den oben beschriebenen Eigenschaften
zur Verfügung gestellt werden, wobei das Verfahren Wahl-
i. The method according to the invention is intended to provide economically favorable manufacturing options for molded articles made of plastic with the properties described above
are made available, whereby the procedure elective

möglichkeit für den endgültigen Kristallinitätszustandpossibility for the final crystallinity state

des Kunststoffes in der Formlingwand bieten soll. Grund- jof the plastic in the molding wall should provide. Reason j

sätzlich wird dies mit der Erfindung dadurch bewerkstelligt, daß man unter Ausnutzung der oben in Ver-In addition, this is achieved with the invention in that one takes advantage of the above in

1 bindung mit Figur 2 erläuterten Verhaltungsweise der '1 binding with Figure 2 explained behavior of the '

hier in Betracht gezogenen Kunststoffe ein HalbzeugThe plastics considered here are a semi-finished product

durch fortlaufendes Extrudieren bei einer Temperatur ;by continuously extruding at one temperature;

TE (vergleiche Figuren 3 bis 8) herstellt, die oberhalb '*■ T E (compare FIGS. 3 to 8) produces the above '* ■

des Kristallinschmelzpunktes in einem Temperaturbereich ' liegt, in welchem das Material plastifiziert vorliegt.of the crystalline melting point in a temperature range ' lies in which the material is plasticized.

Aus diesem plastifizierten Zustand ist das MaterialThe material is in this plasticized state

den jeweiligen Wünschen und Anforderungen an den Formling;the respective wishes and requirements of the molding;

entsprechend durch den in Figur 2 wiedergegebenen icorrespondingly by the i shown in FIG

Kristallwachstums-Temperaturbereich hindurch so abzu- IThrough the crystal growth temperature range

kühlen und thermisch zu konditionieren, daß es bei Er- jto cool and to condition thermally that it is at Er- j

j reichen des Temperaturbereiches, in welchem es als fester!j range of the temperature range in which it is considered to be more solid!

Stoff vorliegt (bei Polyäthylenterephthalat unterhalb \ 600C), einen gewünschten Kristallinitätszustand, ver- ! bunden mit gewünschten physikalischen Eigenschaften, \ Substance is present (with polyethylene terephthalate below \ 60 0 C), a desired crystallinity state, ver! bound with desired physical properties, \

aufweist. ■:having. ■:

130016/0096130016/0096

Dipl.-Phys. Heinrich Selds · Patentanwalt · 6200 Wiesbaden 1 · Bierstadte·- Hön» 15 ■ Poetfach 51 05 · v?(o 61 2\) 56 53 82 !Dipl.-Phys. Heinrich Selds · Patent Attorney · 6200 Wiesbaden 1 · Bierstadte · - Hön »15 ■ Poetfach 51 05 · v? (O 61 2 \) 56 53 82!

Einige Beispiele mit erfindungsgemäßem Thermo-Konditionieren erzielbare Möglichkeiten ergeben sich aus der folgenden Erläuterung der Figuren 3 bis 8.A few examples show the possibilities that can be achieved with thermal conditioning according to the invention can be derived from the following explanation of FIGS. 3 to 8.

Im Beispiel der Figur 3 v/ird bei der Herstellung von Formungen aus Polyäthylenterephthalat das Halbzeug beim Stabilisieren stark abgekühlt und beim Thermo-Konditionieren auf ein Temperaturprofil über die Halbzeugdicke eingestellt, das im Bereich von 55 bis 1000C liegt, in welchem praktisch kein Kristallwachstum bzw. keine Kristallbildung eintritt. Die Aussenbereiche bzw. Oberflächenbereiche des Halbzeugs können dabei bis unterhalb dieses Temperaturbereiches abgekühlt, während der Kunststoff im Inneren des Halbzeugs bis etwa 1000C warm sein kann, zumindest nicht nennens-i wert diese Temperatur überschreiten sollte. Beim Stabilisieren kann - wie im oberen Teil der Figur 3 angedeutet - ausgehend von einem beim Extrudieren j herschenden, bei der Extrudiertemperatur T-g liegenden Temperaturprofil durch schnelles Abkühlen zu dem links im oberen Teil der Figur 3 gezeigten Temperatur der amorphe Zustand im Kunststoff im wesentlichen gehalten bzw. eingefroren werden. Beim nachfolgenden Thermo-Konditionieren (mittlere Teil der Figur 3) und dem das Thermoverformen einschließenden zweitenIn the example in FIG. 3, the semifinished product is strongly cooled during stabilization during the production of moldings from polyethylene terephthalate and, during thermal conditioning, set to a temperature profile over the semifinished product thickness that is in the range from 55 to 100 ° C., in which there is practically no crystal growth or no crystal formation occurs. The outer regions or surface regions of the semi-finished product can thereby cooled to below this temperature range, while the plastic in the interior of the semifinished product may be up to about 100 0 C warm, at least not should nennens-i value exceed this temperature. During stabilization - as indicated in the upper part of FIG be frozen. During the subsequent thermo-conditioning (middle part of FIG. 3) and the second including thermoforming

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids - Patentanwalt · 6200 Wiesbadi-n 1 · Bicrstat!.. ι Hol·r 15 · Pri'tach -χ oj · *-?(o 6- -.1) 56 53 82Dipl.-Phys. Heinrich Seids - Patent Attorney · 6200 Wiesbadi-n 1 · Bicrstat! .. ι Hol · r 15 · Pri'tach -χ oj · * -? (O 6- -.1) 56 53 82

Thermo-Konditionieren (Figur 3 unterer Teil) können
solche Temperaturvarhältnisse am und im inneren des
Halbzeugs 10 und dem Formling 18 eingehalten v/erden,
daß auch dann nicht wesentliches Kristallwachstum
Thermo-conditioning (Figure 3, lower part) can
such temperature conditions on and inside the
The semi-finished product 10 and the molding 18 are adhered to,
that even then there is no essential crystal growth

bzw. wesentliche Kristallbildung eintreten. Der soor substantial crystal formation occur. The so

hergestellte Formling ist - wenn aus pigmentfreiem j Kunststoff bestellend - klar durchsichtig, was bedeutet, ;The molded product is - if ordered from pigment-free plastic - clearly transparent, which means;

daß der Kunststoff in der Formlingwand praktisch in | amorphen Zustand ist. Die Temperaturformbeständigkeit !that the plastic in the molding wall is practically in | is amorphous state. The temperature resistance!

des Formlings liegt bei etwa 700C. [ of the molded article is about 70 0 C. [

Will man bei dieser Verfahrensweise einen gewissen Grad· von Teilkristallinität im Kunststoff der Forihlingwand
zulassen oder ausbilden, 3D kann dies beim Stabilisieren · und ersten Thermo-Konditionieren dadurch geschehen, daß
man die Abkühlung des Halbzeugs 10 langsamer vornimmt
und dabei schon Teilkristallinität in einem gewünschten j
With this procedure, one wants a certain degree of partial crystallinity in the plastic of the mold wall
allow or train, 3D this can happen during stabilization · and first thermo-conditioning that
the cooling of the semifinished product 10 is carried out more slowly
and even partial crystallinity in a desired j

Grad eintreten läßt« Diese Teilkristallinität kann man j dann beim Thermoverformen und zweiten Thermo-Konditio- i nieren durch entsprechende Temperaturführung (vergleiche < untere Teil der Figur 3) im Kunststoff des Formlings Can enter degrees "This partial crystallinity can then j during thermoforming and second thermal conditionality i kidney by appropriate temperature control (see <lower part of Figure 3) in the plastic of the molding

bzw. Fertigteils im wesentlichen beibehalten. |or the finished part is essentially retained. |

Figur 4 illustriert eine Möglichkeit für die Führung
des erfindungsgemäßen Verfahrens, bei der man das
Halbzeug 10 zwar rasch abkühlt, um es an seinen Außenbereichen Jbzw. Oberflächenbereichen zu verfestigen und
130016/0096
Figure 4 illustrates one possibility for guidance
of the method according to the invention, in which the
Semi-finished product 10 cools down quickly to make it Jbzw on its outer areas. To solidify surface areas and
130016/0096

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden t · Bierstadler Höhe 15 · Postfach 51 05 · &?{o 61 21) 5O 53 82Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden t · Bierstadler Höhe 15 · P.O. Box 51 05 · &? {O 61 21) 5O 53 82

handhabbar zu machen. Der Kunststoff im Inneren des Halbzeugs} bleibt aber auf einer Temperatur, die merklich oberhalb 1000C liegt. Dieser Übergang von dem bei der Extrudiertemperatur T-, liegenden Temperaturprofile zu dem durch ■> Stabilisieren eingestellten Temperaturprofil ist aus dem oberen Teil der Figur 4 ersichtlich. Bei dem sich an das Stabilisieren anschließende Thermo-Konditionieren am Halbzeug kann man dann ein Temperaturprofil einstellen, bei dem die Aussenbereiche des Halbzeugs auf Temperaturen bei bis h0 knapp oberhalb 500C und der Kern des Halbzeugs auf Temperatüren oberhalb 1000C liegen. Bei dieser Temperaturführungto make manageable. But the plastic in the interior of the semifinished} remains at a temperature which is appreciably above 100 0 C. This transition from the temperature profile at the extrusion temperature T 1 to the temperature profile set by stabilizing can be seen from the upper part of FIG. During the thermo-conditioning of the semifinished product following the stabilization, a temperature profile can then be set in which the outer areas of the semifinished product are at temperatures of up to h0 just above 50 ° C. and the core of the semifinished product is at temperatures above 100 ° C. With this temperature control

j während des Stabilisierens und ersten Thermo-Konditionierensj during stabilization and initial thermal conditioning

j treten in dem Polyäthylenterephthalat im Inneren des HaIbi j occur in the polyethylene terephthalate inside the Halbi

zeugs 10 merkliche Kristallbildung und merkliches Kristall-stuff 10 noticeable crystal formation and noticeable crystal

wachstum ein, was sich durch Trübung des Materials äußert. Da die Zeitspanne zwischen dem Halbzeug-Konditionieren (mittlerer Teil der Figur 4) und dem Thermoverformen mit Fertigteil-Konditionieren (unterer Teil der Figur 4) im erfindungsgemäßen Verfahren festgelegt ist, läßt sich durch das im mittleren Teil der Figur 4 gezeigte Temperaturprofil und das Maß, um das die Temperatur im Inneren des Halbzeugs 10 oberhalb 1000C liegt, vorher festlegen, wie groß der Kristallisationsgrad des Halbzeugs bei Beginn des Fertigteil-Konditionierens ist.growth, which manifests itself in the opacity of the material. Since the period of time between conditioning of semifinished products (middle part of FIG. 4) and thermoforming with conditioning of finished parts (lower part of FIG , by which the temperature inside the semi-finished product 10 is above 100 ° C., determine beforehand how great the degree of crystallization of the semi-finished product is at the start of the conditioning of the finished part.

130016/009B130016 / 009B

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadler Höhv'.x? Poitfacli 51 05 · <£j?(o 6j 21) 5η ·,$ Sz Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadler Höhv'.x? Poitfacli 51 05 <£ j? (O 6j 21) 5η , $ Sz

Das Thermoverformen erfolgt in diesem Beispiel durch ziehen des Werkstoffes auf eine heiße Formoberfläche, deren Temperatur bei 120 bis 1800C liegen soll. Im dargestellten Beispiel wird eine Temperatur an der Formoberfläche bei 1800C angenommen» Bei dem während des Thermoverformens einsetzenden und ggf. über das Thermoverformen hinaus noch stattfindende Fertigteil-Konditionierens tritt somit ein weitgehendes Auskristallisieren des Polyäthylenterephthalats ein» Der Formling erhält eine Opakewandung (wenn von pigmentfreiem Material1 The thermoforming is carried out in this example by pulling out the material on a hot mold surface whose temperature is to lie at 120 to 180 0 C. In the illustrated example, a temperature is assumed at the mold surface at 180 0 C "With the onset during thermal forming and possibly over the thermoforming addition, still held precast conditioning process thus occurs a far-reaching crystallization of the polyethylene terephthalate an" The molding receives a Opakewandung (if of pigment-free material 1

ausgegangen wird). Die Temperaturformbeständigkeit des jis assumed). The temperature resistance of the j

Formlings liegt oberhalb 2000C. iMolding is above 200 0 C. i

Ein ähnlicher Verfahrensablauf wäre gemäß Figur 5 erziel-j bar, wenn man beim Stabilisieren und bzw. oder Halbzeug- · Konditionieren unter Druck ein Temperaturprofil einstellt ,j wie es in den oberen und mittleren Teilen der Figuren 3 und 5 gezeigt ist. Will man in solchem Fall beim Fertigteil-Konditionieren ein weitgehendes Auskristallisieren im Kunststoff hervorrufen, so müßte ausgehend von dem nahezu amorphen Zustand des Polyäthylenterephthalats entweder längere Zeit zum Auskristallisieren zur Verfügung gestellt werden, oder es würde kein so hoher Kristallinitätsgrad erreicht, wie mit den Ausgangsbedingungen gemäß Figur 4. Wie im unteren Temperaturprofil der Figur 5 angedeutet, kann man in solchem Fall auchA similar process sequence would be achieved according to FIG bar, if a temperature profile is set during stabilization and / or conditioning of semi-finished products under pressure, j as shown in the upper and middle parts of Figs. In such a case you want to Conditioning of the finished part would cause extensive crystallization in the plastic, based on The almost amorphous state of the polyethylene terephthalate is either available for a longer period of time to crystallize out or the degree of crystallinity would not be as high as with the starting conditions in accordance with FIG. 4. As indicated in the lower temperature profile of FIG. 5, it is also possible in such a case

130016/0096130016/0096

Dipl.-Phys. Heinrich Sclds ■ Patentanwalt · 6200 Wiesbaden ι · Bicrsladter Hohe *5 · Γ ostfach >i 05 · &(o 61 21) 515-53Dipl.-Phys. Heinrich Sclds ■ Patent attorney · 6200 Wiesbaden ι · Bicrsladter Hohe * 5 · Γ ostfach> i 05 · & (o 61 21) 515-53

eventuell mit etwas höherer Temperatur an der Formoberfläche, beispielsweise bis 2000C arbeiten. Man kann aber vor allem auch das Fertigteil-Konditionieren entsprechend langer nach dem Thermoverformen zeitlich ausdehnen, wie dies in Figur 1 mit der zweiten Thermo-Konditionierstation 17 angedeutet ist. Die nach dieser Weise hergestellten Formlinge haben (wenn von pigmentfreiem Material ausgegangen wird) durchsichtige Wandung. Die Temperatur-Formbeständigkeit der so hergestellten Formlinge liegt bei etwa 1500C bis 2000C.may work with a somewhat higher temperature at the mold surface, for example, to 200 0 C. Above all, however, the conditioning of the finished part can also be extended in time correspondingly longer after the thermoforming, as is indicated in FIG. 1 with the second thermo-conditioning station 17. The moldings produced in this way have transparent walls (if pigment-free material is assumed). The temperature dimensional stability of the moldings thus produced is about 150 0 C to 200 0 C.

Figur 6 gibt eine Möglichkeit für die Führung des erfindungsgemäßen Verfahrens wieder, die sich gegenüber derjenigen gemäß Figur 3 bzw. derjenigen gemäß Figur 5 dadurch unterscheidet, daß während des Halbzeug-Konditionierens (vergleiche mittlerer Teil der Figur 6), d.h. zwischen dem Stabilisieren und dem Thermoverforraen ein Recken des Halbzeugs 10 vorgenommen wird. Bei diesem Recken tritt - wie das mittlere Temperaturprofil in Figur 6 andeutet - noch eine zusätzliche Kühlung am Halbzeug 10 ein. Das gereckte, vorzugsweise biaxialgereckte Halbzeug 10 wird dann beim Thermoverformen auf die heiße Formoberfläche tiefgezogen, die eine Temperatur von beispielsweise 150 bis 2000C aufweisen kann. Im Beispiel der Figur 6 wird von einer Temperatur von etwa 2000C an der Formoberfläche des Thermoverformungswerkzeugs ausgegangen. Die in VerfahrensführungFIG. 6 shows a possibility for the implementation of the method according to the invention, which differs from that according to FIG. 3 or that according to FIG Thermoverforraen stretching of the semifinished product 10 is carried out. During this stretching, as the mean temperature profile in FIG. 6 indicates, additional cooling takes place on the semifinished product 10. The stretched, preferably biaxialgereckte semi-finished product 10 is then deep-drawn during thermoforming to the hot mold surface, which may have a temperature of for example 150 to 200 0 C. In the example of Figure 6 is assumed a temperature of about 200 0 C at the shaping surface of the thermoforming tool. The one in conduct of the proceedings

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Patenlanwalt · 62ου Wiesbaden t · Bierstadtcr Hiü'u? 35" * T\»stfacH jio; ς'?(o c : 2i) ,( y$ 82 ;Dipl.-Phys. Heinrich Seids · Patenlanwalt · 62ου Wiesbaden t · Bierstadtcr Hiü'u? 35 "* T \» stfacH jio; ς '? (Oc: 2i), ( y $ 82;

j gemäß Figur 6 hergestellten Formlinge haben wiederum j durchsichtige Wandung (wenn von pigmentfreiem Material ausgegangen), aber noch eine wesentlich verbesserte Temperatur-Formbeständigkeit, nämlich bis zu Temperaturen von 20O0C bis 2500C. Außerdem zeichnen sich die so hergestellten Formlinge durch erhöhte Festigkeit und Elastizität aus. j moldings produced according to Figure 6 have again j transparent wall (when starting from pigment-free material), but yet a significantly improved temperature resistance, namely up to temperatures of 20O 0 C to 250 0 C. In addition, the moldings thus produced by increased draw Strength and elasticity.

Im Beispiel nach Figur 7, wird beim Stabilisieren und anschließend beim Thermo-Konditionieren am Halbzeug 10 ein Temperaturprofil eingestellt, bei dem relativ starke Oberflächenbereiche 10a auf eine Temperatur unterhalb 1000C gekühlt und in praktisch amorphen Zustand des Polyathylenterephalats gehalten werden. Im Inneren des Halbzeugs 10 wird eine Temperatur von maximal etwa 150 C eingestellt. Ausgehend von diesem, im mittleren Teil von Figur 7 dargestellten Temperaturprofil erfolgen das Thermoverformen und Fertigteil-Konditionieren an Formoberflächen, die auf etwa 150 bis 1800C erwärmt sind. Im dargestellten Beispiel beträgt die Temperatur beider Formoberflächen, zwischen denen die Formlingwand 18 gebildet wird, 18O0C0 Der Kunststoff der Formlingwand 18 wird zwischen beiden auf 1800C gehaltenen Formoberiläche weitgehend auskristallisiert. Der so hergestellte Form- f ling hat eine Temperatur-Formbeständigkeit von etwa j 20O0C.In the example of Figure 7, in stabilizing and then set a temperature profile in the thermal conditioning of the semifinished product 10 can be cooled at the relatively high surface areas 10a to a temperature below 100 0 C and maintained in substantially amorphous state of the Polyathylenterephalats. A maximum temperature of approximately 150 ° C. is set inside the semi-finished product 10. Proceeding from this, shown in the middle part of Figure 7, the temperature profile thermoforming and precast-conditioning occur at mold surfaces are heated to about 150 to 180 0 C. In the illustrated example, the temperature of both mold surfaces between which the blank wall 18 is formed, 18O 0 C 0 The plastic of the preform wall 18 is substantially crystallized out between the two to 180 0 C held Formoberiläche. The molding produced in this way has a temperature resistance of about 20O 0 C.

130016/0096130016/0096

Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadtcr Hone"15 · Postfach 51 05 · ®(o 61 21) 36 53 82 iDipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadtcr Hone "15 · Postfach 51 05 · ® (o 61 21) 36 53 82 i

Im Beispiel der Figur 8 wird beim Stabilisieren ein.In the example in FIG. 8, a.

I rasches Abschrecken beider Oberflächen des Halbzeugs 10 j vorgenommen. Beim Halbzeug-Konditionieren wird dann an den Oberflächen des Halbzeugs 10 eine Temperatur zwischen etwa 50 und 1000C eingestellt, während das Polyethylenterephthalat im Kern bzw. Inneren des Halbzeugs noch weitgehend die Extrudiertemperatur behält, also auf einer Temperatur bei etwa 2700C liegt. Das mit diesen (im mittleren Teil der Figur 8 gezeigten) Temperaturprofil ausgestattete Halbzeug wird zwischen zwei heißen Formoberflächen thermoverformt. Die Formoberflächen können dabei eine Temperatur von 150 bis 16O°C aufweisen. Zwischen den Formoberflächen tritt - wie der untere Teil der Figur 8 erkennen läßt - ein wesentlicher Ausgleich im Temperaturprofil ein. Dadurch wird in den Oberflächenbereichen der gebildeten Formlingwand 18 das Polyäthylenterephthalat bei etwa 16O°C und im Innenbereich der Formlingwand 18 bei etwa 190°C weitgehend Auskristallisiert, also in den Außenbereichen etwas unterhalb und im Innenbereich etwas oberhalb der optimalen Kristallisationstemperatur von etwa 1700C. Die auf diese Weise hergestellten Formlinge haben Opakeformlingwände (wenn von pigmentfreiem Material ausgegangen wird). Die Temperatur-Formbeständigkeit liegt" bei ca. 2000C. I carried out rapid quenching of both surfaces of the semi-finished product 10 j. During conditioning of the semifinished product, a temperature between about 50 and 100 ° C. is then set on the surfaces of the semifinished product, while the polyethylene terephthalate in the core or interior of the semifinished product still largely retains the extrusion temperature, i.e. at a temperature of about 270 ° C. The semifinished product equipped with this temperature profile (shown in the middle part of FIG. 8) is thermoformed between two hot mold surfaces. The mold surfaces can have a temperature of 150 to 160 ° C. As can be seen in the lower part of FIG. 8, an essential equalization in the temperature profile occurs between the mold surfaces. Characterized the molding wall formed 18 is largely crystallized polyethyleneterephthalate at about 16O ° C and in the inner region of the blank wall 18 at about 190 ° C in the surface regions, so in the outer regions slightly below and in the inner region somewhat above the optimal crystallization temperature of about 170 0 C. The moldings produced in this way have opaque molding walls (if pigment-free material is assumed). The temperature resistance is "about 200 0 C.

130016/0096130016/0096

Dipl.-Phys. Helnridi Scids ratcnt.uiw.ili · 6200 WicsbaJ.-u ι · Bicrstadu-r H-Im- -5 · "o:.lf.ul ,ι o;, «-,^(o ι,. ;·ι) ■,< v; H,Dipl.-Phys. Helnridi Scids ratcnt.uiw.ili · 6200 WicsbaJ.-u ι · Bicrstadu-r H-Im- -5 · "o: .lf.ul, ι o ;,« -, ^ (o ι ,. ; · ι) ■, <v; H ,

Figur 9 gibt eine abgewandelte Arbeitsweise wieder, in der beim Stabilisieren durch rasches Abschrecken beider Oberflächen das Halbzeug handhabbar gemacht wird. Beim Halbzeug-Konditionieren wird ein Temperaturprofil eingestellt, das - wie der mittlere Teil der Figur zeigt zwischen Extrudiertemperatur (26O°C bis 2900C) und ca. 1700C liegt. Beim Thermoverformen und Fertigteil-Konditionieren wird an der Formlingwand ein Temperaturprofil zwischen 12O0C und 1700C eingestellt. Die nach dieser abgewandelten Weise hergestellten Formlinge haben ebenfalls opake Formlingwände (wenn von pigmentfreiem Material ausgegangen wird) und eine Temperaturformbeständigkeit bei ca. 200 bis 220°C.FIG. 9 shows a modified mode of operation in which, during stabilization, the semi-finished product is made manageable by rapidly quenching both surfaces. When semi-conditioning a temperature profile is set, which - as the central part of the figure shows between extrusion temperature (26O ° C to 290 0 C) and about 170 0 C. When thermoforming and precast-conditioning a temperature profile between 12O 0 C and 170 0 C is set at the molding wall. The moldings produced in this modified way also have opaque molding walls (if pigment-free material is assumed) and a temperature resistance of approx. 200 to 220.degree.

Ergänzend zu den obigen Darlegungen können außer dem erwähnten Recken auch noch andere mechanische und I physikalische Behandlungen beim Halbzeug-Konditionieren j und sinngemäß auch beim Fertigteil-Konditionieren aus- ;In addition to the above-mentioned stretching, other mechanical and I physical treatments during conditioning of semifinished products j and correspondingly also during conditioning of finished parts;

j geübt werden, beispielsweise Verdichten und Dicken- :j are practiced, for example compaction and thickness-:

reduzierung durch Walzen oder Formdruck, Bestrahlen : mit Strahlung verschiedenster Art, UltraschallbehandlungReduction by rolling or molding pressure, irradiation: with various types of radiation, ultrasound treatment

u.dgl. mehr. Die oben beschriebenen Ausführungsweisen des erfindungsgemäßen Verfahrens lassen sich bei Halbzeug verschiedenster Art beispielsweise Schlauch, Profilleisten u.dgl. mehr ausführen.and the like more. The modes of execution described above of the method according to the invention can be used for various types of semi-finished products, for example hose, Run profile strips and the like more.

130016/0096130016/0096

-so--so-

e e r s ee e r s e

iteite

Claims (1)

2938905 PATENTANWALT DIPL.-PHYS. HEINRICH SEIDS Wiesbaden · Bierstadter Höhe 15 ■ Postfach 12068 · Telefon (0 61 21J 5o 53 82 Postscheck Frankfurt/Main 181008-602 · Bank Deutsch«· Bank 39563 72 · Nass. Sparkasse Ιϋβ 00X165 2938905 PATENT Attorney DIPL.-PHYS. HEINRICH SEIDS Wiesbaden · Bierstadter Höhe 15 ■ Postfach 12068 · Telephone (0 61 21J 5o 53 82 Postscheck Frankfurt / Main 181008-602 · Bank Deutsch «· Bank 39563 72 · Nass. Sparkasse Ιϋβ 00X165 Bellaplast GmbH Wiesbaden, den 25. Sept. 1979Bellaplast GmbH Wiesbaden, September 25, 1979 X 222 S/weX 222 S / wh PatentansprücheClaims 1.) Verfahren zum Herstellen von Formungen aus thermoplastischem Kunststoff, der sich mittels physikalischer Einflüsse, insbesondere Temperatureinflüsse, wahlweise in seinem teilkristallinen Zustand einstellen läßt, durch:1.) Process for making moldings from thermoplastic Plastic, which by means of physical influences, in particular temperature influences, can optionally be set in its partially crystalline state by: - Bilden eines Halbzeugs, insbesondere fortlaufendes Extrudieren eines Bandes oder Schlauches, aus dem plastifizierten Kunststoff,- Forming a semi-finished product, in particular a continuous one Extrusion of a tape or hose from the plasticized plastic, - Stabilisieren des Halbzeugs durch Abkühlen zumindest an einer Oberfläche, '- Stabilizing the semi-finished product by cooling at least on one surface, ' - Thermo-Konditionieren des stabilisierten Halbzeugs zu Thermoverformbarkeit und- Thermal conditioning of the stabilized semi-finished product to thermoformability and - Thermoverformen zum .Bilden formstabiler end- ι gültiger Formlinge aus dem Halbzeug, dadurch gekennzeichnet, daß- Thermoforming for forming dimensionally stable end ι valid briquettes from the semi-finished product, characterized in that - für Herstellung von Formungen aus solchem Kunststoff, dessen Kristallinitätszustand wahl v/eise zwischen amorph und teilkristallin einstellbar ist, das Einstellen des gewünschten Kristallini- :- for the production of moldings from such plastic, the crystallinity state of which can be set between amorphous and partially crystalline, the setting of the desired crystalline-: tätszustandes in der Formlingwand durch ein !state of affairs in the molding wall by a! erstes, am Halbzeug auszuführendes Thermo- ;first thermal to be performed on the semi-finished product; 13001 6/009S13001 6 / 009S ORIGINAL INSPECTEDORIGINAL INSPECTED Dipl.-Phys. Heinrich Seide ■ Patentanwalt · 6200 Wiesbaden ι · Bierstadter Höhe 15 · Postfach 51 05 ■ ®(o 61 21) 56 53 82Dipl.-Phys. Heinrich Silk ■ Patent Attorney · 6200 Wiesbaden ι · Bierstadter Höhe 15 · Postfach 51 05 ■ ® (o 61 21) 56 53 82 Konditionieren und ein zweites, am Formling auszuführendes Thermo-Konditionieren vorgenommen wird;Conditioning and a second to be carried out on the molding Thermal conditioning is done; - die bei dem zwischen Stabilisieren und Thermover- ' formen auszuführenden ersten Thermo-Konditionieren- The first thermo-conditioning to be carried out between stabilization and thermo-forming auf das Halbzeug auszuübenden physikalischen Einflüsse in vorher zu bestimmender Weise für Erzielung eines gewünschten vorbereitenden Kristallinitätszustandes sowie Thermoverformbarkeit des Kunststoffs des Halbzeugs abgestimmt und modifiziert werden und dabei über dem Halbzeugs-Querschnitt ein auf den anschliessenden Thermoverformungsvorgang abgestimmtes und den gewünschten endgültigen Kristallinitätszustand im Kunststoff der Fonnlingwand vorbereitendes Temperaturprofil eingestellt wird; undPhysical influences to be exerted on the semifinished product in a manner to be determined beforehand in order to achieve it a desired preparatory crystallinity state and thermoformability of the Plastic of the semi-finished product can be matched and modified and thereby over the semi-finished product cross-section one that is tailored to the subsequent thermoforming process and the one required final crystallinity state in the plastic of the molding wall preparatory temperature profile is set; and - das zweite Thermo-Konditionieren während des Thermoverfonnungsvorganges und wahlweise noch daran anschliessend mit Temperaturführung zu Erzeugung bzw. Erhaltung des gewünschten end- the second thermo-conditioning during the thermoforming process and optionally also then with temperature control to generate or maintain the desired end gültigen Kr.i ütallinitätszustandes im Kunststoff der Formlinp-wand in Verbindung mit Herbeiführen der Formbeständigkeit ausgeführt wird.valid crystallinity state in the plastic of the Formlinp-wall in connection with bringing about the dimensional stability is carried out. Y3ÜÜ16/0098Y3ÜÜ16 / 0098 Dipl.-Phys. Heinrich Scids · Patentanwalt ■ 6100 Wiesbaden ι · Bierstadtor lf.ihe 15 · Postfach 51 05 · <ξ?(ο 6i ii) 56 53 82Dipl.-Phys. Heinrich Scids · Patent Attorney ■ 6100 Wiesbaden ι · Bierstadtor lf.ihe 15 · Postfach 51 05 · <ξ? (Ο 6i ii) 56 53 82 2.) Verfahren nach Anspruch 1, dadurch gekennzeichnet, daß2.) The method according to claim 1, characterized in that - das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren über seinen gesamten Querschnitt unter Einstellen des gewünschten endgültigen Kristallinitatszustandes bis zu einer Temperatur abgekühlt wird, bei der keine erhebliche Veränderung des Kristallinitatszustandes im Kunststoff mehr stattfindet, und zwar auch beim Einrichten des Temperatur- the semi-finished product during the stabilization and first thermo-conditioning over its entire Cross-section with setting of the desired final crystallinity state up to is cooled to a temperature at which there is no significant change in the state of crystallinity takes place more in the plastic, even when setting up the temperature profils auf die Erfordernisse beim Thermoformen in allen Halbzeug-Bereichen solche Temperaturen eingehalten werden, bei welchenprofils to the requirements of thermoforming in all areas of semi-finished products Temperatures are maintained at which keine wesentliche Veränderung des Kristallini- I tätszustandes eintritt, und ;there is no significant change in the crystallinity state, and; - beim Thermoformen ein Tiefziehen und zweites j Thermo-Konditionieren zum Fixieren des ' Kristallin!tätszustandes im Kunststoff der ' dabei geformten und verfestigten Formlingwand !- with thermoforming a deep drawing and a second j thermo-conditioning to fix the ' Crystallinity in the plastic of the ' formed and solidified molded wall! erfolgen. < take place. < 3.) Verfahren nach Anspruch 2, dadurch gekennzeichnet, daß das Halbzeug beim Stabilisieren und ersten ' Thermo-Konditionieren unter weitgehender Beibe- :3.) The method according to claim 2, characterized in that the semi-finished product when stabilizing and first ' Thermal conditioning with extensive additional: haltung des amorphen Zustandes im Kunststoff jkeeping the amorphous state in the plastic j ! rasch bis zu einer Temperatur abgekühlt wird', bei '! is rapidly cooled to a temperature ', at' der keine wesentliche Veränderung des Kristallini-which does not significantly change the crystalline Dipl.-Phys. Heinrich Seide · Patent.inwalt · 6200 Wiesbaden 1 ■ DiersUdtor Hohe 15 · Postfach 51 05 · Q?(o 61 21) 56 53 82 Dipl.-Phys. Heinrich Silk · Patent.inwalt · 6200 Wiesbaden 1 ■ DiersUdtor Hohe 15 · Postfach 51 05 · Q? (O 61 21) 56 53 82 tätszustandes stattfindet.state of affairs takes place. 4.) Verfahren nach Anspruch 2 oder 3, dadurch gekennzeichnet, daß die Formlinge aus Polyäthylen-Terephthalat hergestellt und die Temperatur im Materialband beim Stabilisieren und ersten Thermo-Konditionieren in einen Bereich bei 50° bis 1000C eingestellt werden.4.) The method according to claim 2 or 3, characterized in that the moldings made of polyethylene terephthalate and the temperature in the material strip can be set in a range of 50 ° to 100 0 C during stabilization and first thermo-conditioning. 5.) Verfahren nach Anspruch 1, dadurch gekennzeichnet, daß5.) The method according to claim 1, characterized in that - das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren über seinen gesamten Querschnitt rasch abgekühlt und auf ein Temperaturprofil ein- j gestellt wird, das das Thermo^/erformen zuläi3t aber j in allen Halbzeug-Bereichen Temperaturen einhält, bei denen keine wesentliche Veränderung des- the semi-finished product during stabilization and initial thermal conditioning cooled rapidly over its entire cross-section and adjusted to a temperature profile that allows thermoforming but j maintains temperatures in all semi-finished product areas at which there is no significant change in the Kristallinitätszustandes in dem jeweiligen Kunst- {State of crystallinity in the respective art { stoff eintritt; jsubstance enters; j - das Therrnover formen auf mindestens eine Formober- ι- The Therrnover form on at least one Formober- ι fläche erfolgt, die auf eine Temperatur erwärmt ist|surface that is heated to a temperature | bei der Kristallwachstum im jeweiligen Kunststoffat the crystal growth in the respective plastic i eintritt und ji enter and j - das in Berührungen der Formlingwand mit der er- j wärmten Formoberfläche erfolgende oder einsetzende j zweite Thermo-Konditionieren in Temperaturen und- the j that takes place or begins when the molding wall comes into contact with the heated mold surface second thermo-conditioning in temperatures and 130016/0098130016/0098 Dipl.-Phy*. Heinrich Seids · Patentanwalt · 6200 Wiesbaden ι · Bierstadter Höhe 15 · Postfach 5105 · ζ?(ο 6i 21) 56 53 8aDipl.-Phy *. Heinrich Seids · Patent Attorney · 6200 Wiesbaden ι · Bierstadter Höhe 15 · Postfach 5105 · ζ? (Ο 6i 21) 56 53 8a Zeitdauer auf Einstellung einer gewünschten Teilkristallinität des Kunststoffs abgestimmt wird.Time to set a desired partial crystallinity of the plastic is matched. 6.) Verfahren nach Anspruch 5, dadurch gekennzeichnet, daß der Kunststoff des Halbzeugs beim Stabilisieren und ; ersten Thermo-Konditionieren weitgehend in amorphem ,6.) The method according to claim 5, characterized in that the plastic of the semi-finished product when stabilizing and; first thermal conditioning largely in amorphous, Zustand gehalten wird. jState is maintained. j 7.) Verfahren nach Anspruch 5, dadurch gekennzeichnet, daß der Kunststoff des Halbzeugs beim Stabilisieren und ; ersten Thermo-Kondjfcionieren bereits einem ersten
geringen Kristallwachstum unterzogen wird.
7.) The method according to claim 5, characterized in that the plastic of the semi-finished product when stabilizing and; first thermo-condensing already a first
undergoes little crystal growth.
8.) Verfahren nach einem der Ansprüche 5 bis 7» dadurch
gekennzeichnet, daß die Formoberfläche auf einer
Temperatur in Bereichen unterhalb bis oberhalb der
Temperatur für optimales Kristallwachstum im jeweiligen Kunststoff gehalten wird.
8.) Method according to one of claims 5 to 7 »thereby
characterized in that the mold surface on a
Temperature in areas below to above the
Temperature is maintained for optimal crystal growth in the respective plastic.
9.) Verfahren nach Anspruch 8, dadurch gekennzeichnet, daß j die Formoberfläche auf einer Temperatur im Bereich der Temperatur für optimales Kristallwachstum im jeweiligen!9.) The method according to claim 8, characterized in that j the mold surface at a temperature in the range of Temperature for optimal crystal growth in the respective! I Kunststoff gehalten wird.I held plastic. 10.) Verfahren nach einem der Ansprüche 1 bis 9, dadurch
gekennzeichnet, daß das Halbzeug während des ersten
10.) The method according to any one of claims 1 to 9, characterized
characterized in that the semi-finished product during the first
130016/0098130016/0098 11.) Verfahren nach einem der Ansprüche 5 bis 10, dadurch gekennzeichnet, daß bei Herstellen von Formungen a\:s Polyäthylen-Terephthalat11.) The method according to any one of claims 5 to 10, characterized in that when producing formations a \: s Polyethylene terephthalate - beim Stabilisieren und ersten Thermo-Konditionieren des Halbzeugs eine Temperatur im Bereich von 50° bis 1000C eingestellt wird und - an der Formoberfläche eine Temperatur im Bereich- in stabilizing and first thermal conditioning of the semifinished product to a temperature in the range of 50 ° is set to 100 0 C and - on the mold surface, a temperature in the range Dipl.-Phys. Heinrich Seide · Patentanwalt ■ 6200 Wiesbaden ί ■ Bierstadter Höhe 15 · Postfach 51 05 · fl?(o 61 21) 56 53 62Dipl.-Phys. Heinrich Silk · Patent Attorney ■ 6200 Wiesbaden ί ■ Bierstadter Höhe 15 · P.O. Box 51 05 · fl? (O 61 21) 56 53 62 Thermo-Konditionieren und bzw. oder zwischen dem ersten Thermo-Konditionieren und dem Thermoverformen unter im wesentlichen Beibehaltung des Kristallinitätszustandes seines Kunststoffs einem Recken, vorzugsweise biaxialen Recken, als zusätzlichemThermo conditioning and / or between the first thermo conditioning and thermoforming while substantially maintaining the crystallinity state of its plastic by stretching, preferably biaxial stretching, as an additional physikalischen Einfluß unterworfen sind. 'are subject to physical influence. ' von 120° bis 18O0C aufrechterhalten wird.is maintained from 120 ° to 18O 0 C. 12.) Verfahren nach Anspruch 1, dadurch gekennzeichnet, daß j12.) The method according to claim 1, characterized in that j - das Halbzeug beim Stabilisieren und ersten Thermo- j- the semi-finished product during stabilization and the first thermal j Konditionieren an seinen Oberflächenbereichen auf | Temperaturen für zum Handhaben des Halbzeugs geeignete Verfestigung und im Inneren auf TemperaturenConditioning on its surface areas on | Temperatures suitable for handling the semi-finished product Solidification and inside to temperatures für optimales Kristallwachstum im jeweiligen Kunst- ! stoff eingestellt wird und jfor optimal crystal growth in the respective art ! fabric is adjusted and j - das Thermoverformen auf mindestens eine Formoberflächje erfolgt, die auf eine Temperatur erwärmt ist, bei der! Kristallwachstum in dem jeweiligen Kunststoff eintritt.- The thermoforming takes place on at least one mold surface that is heated to a temperature at which! Crystal growth occurs in the respective plastic. 130016/009Θ130016 / 009Θ Dipl.-Phye. Heiniich Seids · Patentanwalt ■ 6200 Wiesbaden ι Eieriradter ΚΛιβ ι> · Postfach 51 ο j ■ ξ?(ο 6ι 2ΐ) 56 53 82 ιDipl.-Phye. Heiniich Seids · Patent attorney ■ 6200 Wiesbaden ι Eieriradter ΚΛιβ ι> · P.O. Box 51 ο j ■ ξ? (Ο 6ι 2ΐ) 56 53 82 ι ! 13.) Verfahren nach Anspruch 12, dadurch gekennzeichnet,! 13.) The method according to claim 12, characterized in that daß der Kunststoff im Inneren des Halbzeugs durch
den Einfluß der eingestellten Temperatur und die
zeitliche Dauer des ersten Thermo-Konditionierens
auf Bildung eines solchen Kristallinitatszustandes
that the plastic inside the semi-finished product through
the influence of the set temperature and the
duration of the first thermal conditioning
on the formation of such a crystalline state
eingestellt werden, bei dem der jeweilige Kunststoff noch thermoverformbar ist.can be set, in which the respective plastic is still thermoformable. 14.) Verfahren nach Anspruch 12, dadurch gekennzeichnet, j14.) The method according to claim 12, characterized in that j daß der Kunststoff im Inneren des Halbzeugs durch demthat the plastic inside the semi-finished product by the Einfluß der eingestellten Temperatur und die zeitliche Dauer des ersten Thermo-Konditionierens in einen · jenseits der Grenze der eigentlichen Thermoverformbarkeit des jeweiligen Kunststoffs liegenden ! Kristallinitätszustand übergeführt wird. ]Influence of the set temperature and the duration of the first thermal conditioning in a beyond the limit of the actual thermoformability of the respective plastic! State of crystallinity is transferred. ] 15.) Verfahren nach einem der Ansprüche 12 bis 14, dadurch gekennzeichnet, daß die Formoberfläche auf eine
Temperatur für optimales Kristallwachstum in dem
jeweiligen Kunststoff erwärmt ist.
15.) The method according to any one of claims 12 to 14, characterized in that the mold surface on a
Temperature for optimal crystal growth in that
respective plastic is heated.
16.) Verfahren nach einem der Ansprüche 12 bis 15, da- ι durch gekennzeichnet, daß bei Herstellen von Formungen aus Polyäthylen-Terephthalat
- beim Stabilisieren und ersten Thermo-Konditionieren . des Materialbandes die Oberflächenbereichstemperatur auf etwa 50° bis 10O0C und die Innen-
16.) The method according to any one of claims 12 to 15, da- ι characterized in that when producing moldings from polyethylene terephthalate
- during stabilization and initial thermal conditioning. of the material strip, the surface area temperature to about 50 ° to 10O 0 C and the interior
130016/0098130016/0098 Dipl.-Phys. HeinriA Seids · Patentanwalt · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 · Postfach 51 05 · φ?(ο 6ι ιι) 56 53 Dipl.-Phys. HeinriA Seids · Patent Attorney · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 · Postfach 51 05 · φ? (Ο 6ι ιι) 56 53 bereichstemperatur auf etwa 140° bis 16O°C eingestellt werden undrange temperature set to around 140 ° to 160 ° C will and - die Formoberfläche beim Thermoverformen und zweiten Thermo-Konditionieren auf etwa 120° bis 1800C erwärmt ist.- the mold surface during the thermoforming and second thermal conditioning is heated to about 120 ° to 180 0 C. 17.) Verfahren nach Anspruch 1, dadurch gekennzeichnet, daß17.) The method according to claim 1, characterized in that - das Halbzeug beim Stabilisieren und ersten Thermo-Konditionieren an den Oberflächenbereichen seines Querschnitts auf Temperaturen für zum Hand- the semi-finished product during stabilization and initial thermal conditioning on the surface areas its cross-section on temperatures for at hand haben des Halbzeugs geeignete Verfestigung eingestellt und im Inneren im wesentlichen auf der beim Extrudieren des Materialbandes benutzten Plastifiziertemperatur belassen wird; - das Thermoverformen auf mindestens eine Formoberfläche erfolgt, die auf eine Temperatur erwärmt ist, bei der Kristallwachstum in dem jeweiligen Kunststoff eintritt undhave set suitable solidification of the semi-finished product and essentially on the inside Extruding the strip of material is left at the plasticizing temperature used; - the thermoforming on at least one mold surface takes place, which is heated to a temperature at which crystal growth in the respective Plastic enters and - die Formlingwand zum zweiten Thermo-Konditionieren über eine auf den gewünschten endgültigen- The molding wall for the second thermo-conditioning over one to the desired final Kristallinitätszustand der Formlingwand abgestimmteState of crystallinity of the molded wall matched I Zeitdauer auf eine Temperatur gehalten wird, bei jI period of time is held at a temperature at j der Kristallwachstum im Kunststoff der Formlingwand erfolgt.the crystal growth takes place in the plastic of the molding wall. 130016/0098130016/0098 Dlpl.-Phys. Heinrich Seide ■ Palentanwalt ■ 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · ®"(o 61 21) 56 53 82Dlpl.-Phys. Heinrich Silk ■ Palentanwalt ■ 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · ® "(o 61 21) 56 53 82 18.) Verfahren nach Anspruch 17, dadurch gekennzeichnet, j daß die Temperatur an der Formoberfläche etwas unterhalb der Temperatur für optimales Kristallwachstum eingestellt wird und der Formling während des zweiten Thermo-Konditionierens auf einer Temperatur im Temperaturbereich für optimales Kristallwachstum gehalten wird.18.) The method according to claim 17, characterized in that j that the temperature at the mold surface is slightly below the temperature is set for optimal crystal growth and the molding during the second Thermal conditioning at a temperature in the temperature range for optimal crystal growth is held. 19.) Verfahren nach Anspruch 17,oder 18, dadurch gekennzeichnet, daß der Kunststoff in den Oberflächenbereichen des Halbzeugs beim Stabilisieren und ersten Thermo-Konditionieren weitgehend in amorphem Zustand gehalten wird.19.) Method according to claim 17 or 18, characterized in that that the plastic in the surface areas of the semi-finished product when stabilizing and first Thermo-conditioning is kept largely in an amorphous state. 20.) Verfahren nach Anspruch 17 oder 18, dadurch gekennzeichnet, daß der Kunststoff in den Oberflächenbereichen des Halbzeugs beim Stabilisieren und ersten j Thermo-Konditionieren in vorher festgelegten gering20.) The method according to claim 17 or 18, characterized in that the plastic in the surface areas of the semi-finished product when stabilizing and first j thermo-conditioning in predetermined low teilkristallinen Zustand übergeführt wird,, jpartially crystalline state is transferred ,, j 21.) Verfahren nach einem der Ansprüche 17 bis 20, dadurch)21.) Method according to one of claims 17 to 20, characterized) gekennzeichnet, daß bei Herstellen von Formungen aus' Polyäthylen-Terephthalat jcharacterized that when producing moldings from ' Polyethylene terephthalate j - beim Stabilisieren und ersten Thermo-Konditionieren| des Materialbandes die Oberflächenbereichstemperatur auf etwa 80° bis 1000C eingestellt und die- during stabilization and first thermal conditioning | of the material strip, the surface area temperature set to about 80 ° to 100 0 C and the _25Q° bis_25Q ° to 13 0 016/009813 0 016/0098 Dlpl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 · Postfach 51 05 ■ 5?(o 61 21) 56 53 82Dlpl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 · P.O. Box 51 05 ■ 5? (O 61 21) 56 53 82 belassen wird undis left and - die Formoberfläche beim Thermoverformen und zweiter Thermo-Konditionieren auf etwa 140° bis 16O°C gehalten wird.- the mold surface during thermoforming and second thermo-conditioning to about 140 ° to 160 ° C is held. 22.) Verfahren nach einem der Ansprüche 5 bis 21, dadurch gekennzeichnet, daß die Formlingwand zum zweiten Thermo-Konditionieren in Berührung mit der Formoberflache gehalten wird»22.) The method according to any one of claims 5 to 21, characterized in that the molding wall to the second Thermal conditioning in contact with the mold surface is held » 23.) Verfahren nach einem der Ansprüche 5 bis 21, dadurch gekennzeichnet, daß der Formling beim zweiten Thermo-Konditionieren vor der Formoberfläche abgenommen und einer anschließenden Wärmebehandlung unterworfen wird.23.) Method according to one of claims 5 to 21, characterized in that the molding in the second Thermal conditioning removed from the mold surface and a subsequent heat treatment is subjected. 24.) Verfahren nach Anspruch 22 oder 23, dadurch gekennzeichnet, daß beim zweiten Thermo-Konditionieren der Kunststoff der Formlingwand weitgehend auskristallisiert wird.24.) The method according to claim 22 or 23, characterized in that the second thermo-conditioning Plastic of the molding wall is largely crystallized out. 25.) Verfahren nach Anspruch 22 bis 24, dadurch gekennzeichnet, daß die Formlingwand beim zweiten Thermo-Konditionieren auf im wesentlichen gleichbleibender Temperatur gehalten wird.25.) The method according to claim 22 to 24, characterized in that the molding wall during the second thermal conditioning is kept at a substantially constant temperature. 130016/0098130016/0098 Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 ·" bierstadter hohe 15 · Postfach 5X 05 ■ ®(o 61 21) 56 53 82 iDipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · "Bierstadter Hohe 15 · Postfach 5X 05 ■ ® (o 61 21) 56 53 82 i 26.) Verfahren nach einem der Ansprüche 22 bis 24, dadurch gekennzeichnet, daß die Formlingwand beim zweiten Thermo-Konditionieren zu zeitlich absinkender Temperatur temperiert wird.26.) The method according to any one of claims 22 to 24, characterized in that the molding wall at the second Thermo-conditioning is tempered to a temperature that falls over time. 27.) Verfahren nach Anspruch 26, dadurch gekennzeichnet, daß die Temperaturführung beim zweiten Thermo-Konditionieren im wesentlichen ausgehend von Temperatur für optimales Kristallwachstum in dem jeweiligen Kunststoff abkühlend erfolgt.27.) The method according to claim 26, characterized in that the temperature control during the second thermal conditioning essentially starting from temperature for optimal crystal growth in the respective Plastic takes place cooling. i j 10 28.) Verfahren nach einem der Ansprüche 1 bis 27, dadurch |i j 10 28.) The method according to any one of claims 1 to 27, characterized in | gekennzeichnet, daß das Thermoformen unter Ausüben j von Formdruck auf den Kunststoff der Formlingwand ausgeführt wird.characterized in that the thermoforming by exerting j molding pressure on the plastic of the molding wall is performed. 29.) Verfahren nach einem der Ansprüche 1 bis 28, dadurch gekennzeichnet, daß das Halbzeug zwischen dem Extrudieren und dem Thermoformen einem Kalandrier- und bzw. oder Walzvorgang unter Dickenreduzierung zur zusätzlichen physikalischen Beeinflussung des Kristallinitatszustandes unterworfen wird.29.) Method according to one of claims 1 to 28, characterized in that the semifinished product between the extrusion and thermoforming, a calendering and / or rolling process with a reduction in thickness is subjected to additional physical influencing of the crystallinity state. 30.) Verfahren nach Anspruch 29, dadurch gekennzeichnet, daß der Kalandrier- bzw. Walzvorgang in das Stabilisieren des Halbzeugs einbezogen ist.30.) The method according to claim 29, characterized in that that the calendering or rolling process is included in the stabilization of the semi-finished product. 130016/0096130016/0096 Dipl.-Phys. Heinrich Selds · Patentanwalt · 6200 Wiesbaden 1 ·' Biers'tadler Höhe 15 · Postfach 51 05 · $?(o 61 21) 56 53Dipl.-Phys. Heinrich Selds · Patent Attorney · 6200 Wiesbaden 1 · 'Biers'tadler Höhe 15 · Postfach 51 05 · $? (O 61 21) 56 53 31.) Verfahren nach einem der Ansprüche 1 bis 30, dadurch gekennzeichnet, daß glycolmodifiziertes Polyäthylen-Terephthalat als thermoplastisches Herstellungsmaterial verwendet wird, 31.) Method according to one of claims 1 to 30, characterized in that glycol-modified polyethylene terephthalate is used as a thermoplastic manufacturing material, 32.) Verfahren nach einem der Ansprüche 1 bis 30, dadurch gekennzeichnet, daß Polybutylenterephthalat als thermoplastisches Herstellungsmaterial verwendet wird.32.) The method according to any one of claims 1 to 30, characterized in that polybutylene terephthalate as thermoplastic manufacturing material is used. 33.) Vorrichtung zur Durchführung des Verfahrens nach einem der Ansprüche 1 bis 32, mit einer Extrudiervorrichtung zum kontinuierlichen Herstellen des Halbzeugs, einer Stabilisierungsvorrichtung für das Halbzeug und einer Thermoverformvorrichtung sowie ggf. einer Vorrichtung zum Heraustrennen der Formlinge aus den umgebenden Teilen des Halbzeugs, gekennzeichnet durch die Merkmale:33.) Device for performing the method according to one of claims 1 to 32, with an extrusion device for the continuous production of the semi-finished product, a stabilization device for the semi-finished product and a thermoforming device and, if necessary, a device for separating out the moldings from the surrounding parts of the semi-finished product, characterized by the following features: - zwischen der Stabilisierungsvorrichtung (13) und der Thermoverformungsvorrichtung (16) ist eine erste Thermo-Konditionierstation (14) angeordnet;- Between the stabilization device (13) and the thermoforming device (16) is a first thermal conditioning station (14) arranged; - die Thermoverformungsvorrichtung (16) liegt in einer zweiten Thermo-Konditionierstation (17);- The thermoforming device (16) is in a second thermal conditioning station (17); - die Stabilisierungsvorrichtung (13) und die Thermoverformungsvorrichtung (16) sind mit Steuereinrichtung zu vorher festgelegter, ggf. programmierbarer Regelung der in der Stabilisierungsvorrichtung (13) und der Thermoverformungsvorrichtung- the stabilizing device (13) and the thermoforming device (16) are with the control device for previously defined, possibly programmable regulation of the stabilization device (13) and the thermoforming device 130 016/0098130 016/0098 DipL-Phys. Heinrich Seids ■ Patentanwalt ■ 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach yi 05 · ®(o 61 21) 56 53 82Diploma Phys. Heinrich Seids ■ patent attorney ■ 6200 Wiesbaden 1 · Bierstadter Höhe 15 · P.O. Box yi 05 · ® (o 61 21) 56 53 82 (16) erfolgenden physikalischen, insbesondere thermischen Einwirkungen auf den Kunststoff des Halbzeugs (10) ausgestattet; und(16) occurring physical, in particular thermal effects on the plastic of the Semi-finished product (10) equipped; and - den Thermo-Konditionierstationen (14,17) sind Einrichtungen zu physikalischem,, insbesondere thermischem Einwirken auf den Kunststoff des Halbzeugs (10) bzw. Formlings (18) und Steuereinrichtung zu vorher festgelegter, ggf. programmierbarer Regelung der Einwirkungseinrichtung zugeordnet. j- The thermo-conditioning stations (14,17) are facilities to physical, especially thermal effects on the plastic of the semi-finished product (10) or moldings (18) and control device to previously defined, possibly programmable Control assigned to the action device. j 34.) Vorrichtung nach Anspruch 33, dadurch gekennzeichnet,. J34.) Device according to claim 33, characterized in that. J ι daß die Thermo-Konditionierstationen (14,17) Heiz- ι und Kühleinrichtungen für das Halbzeug (10) bzw. die Formlinge (18) mit Regelmöglichkeit für Temperatur und Heiz- bzw. Kühlzeit enthält.ι that the thermal conditioning stations (14, 17) heating ι and cooling devices for the semi-finished product (10) or the moldings (18) with the possibility of regulating the temperature and includes heating or cooling time. 35.) Vorrichtung nach Anspruch 33 oder 34, dadurch gekenn-35.) Device according to claim 33 or 34, characterized zeichnet, daß der ersten Thermo-Konditionierstation \ shows that the first thermal conditioning station \ (14) eine Reckvorrichtung für das Halbzeug (10) mit j(14) a stretching device for the semi-finished product (10) with j Regelmöglichkeit für Recktemperatur, Reckungsgrad IControl option for stretching temperature, degree of stretching I. I und ggf. Reckgeschwindigkeit zugeordnet ist. j I and, if applicable, the stretching speed is assigned. j 36.) Vorrichtung nach Anspruch 35, dadurch gekennzeichnet, J36.) Device according to claim 35, characterized in that J daß die Reckvorrichtung für biaxiales Recken von band-i förmigem oder schlauchförmigem Halbzeug (10) ausge- i bildet ist. !that the stretching device for biaxial stretching of band-i shaped or tubular semi-finished product (10) i forms is. ! 130016/0096130016/0096 Dipl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · Postfach 51 05 · <g"(o 61 21) 56 53Dipl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 · Bierstadter Höhe 15 · P.O. Box 51 05 · <g "(o 61 21) 56 53 37.) Vorrichtung nach einem der Ansprüche 33 bis 36, dadurch gekennzeichnet, daß der Stabilisierungsvorrichtung (13) Einrichtungen zum Kalandrieren und bzw. oder Walzen eines bandförmigen Halbzeugs unter Dickenreduzierung zugeordnet sind.37.) Device according to one of claims 33 to 36, characterized in that the stabilizing device (13) Devices for calendering and / or rolling a strip-shaped semi-finished product under Thickness reduction are assigned. 38.) Vorrichtung nach einem der Ansprüche 33 bis 37, dadurch gekennzeichnet, daß die in der Stabilisierungsvorrichtung (13) vorgesehenen Kühleinrichtungen mit Einrichtungen zur Erzeugung einer in zeitlicher Folge auf den Kunststoff des Halbzeugs (10) wirksamen, regelbaren Temperaturführung ausgestattet sind.38.) Device according to one of claims 33 to 37, characterized in that the cooling devices provided in the stabilizing device (13) with Devices for generating a sequential effect on the plastic of the semi-finished product (10), adjustable temperature control. 39.) Vorrichtung nach einem der Ansprüche 33 bis 38, dadurch gekennzeichnet, daß die Thermoverformvorrichtung (16) mindestens ein Formwerkzeug mit regelbar heiz- und Kühlbarer Formoberfläche enthält.39.) Device according to one of claims 33 to 38, characterized in that the thermoforming device (16) contains at least one molding tool with a mold surface that can be heated and cooled in an adjustable manner. 40.) Vorrichtung nach einem der Ansprüche 33 bis 391 da-40.) Device according to one of claims 33 to 391 there- durch gekennzeichnet, daß die Thermoverformvorrichtun& (16) mindestens ein Formwerkzeug enthält, das mit einer characterized in that the thermoforming device & (16) includes at least one molding tool with a Steuereinrichtung zum Erzeugen einer vorher festlegbaren, ggf. programmierbaren zeitlichen Temperaturänderung bzw. Temperaturführung während des Thermoverformvorganges an mindestens einer Formoberfläche ausgerüstet ist.Control device for generating a previously determinable, possibly programmable temperature change over time or temperature control during the thermoforming process is equipped on at least one mold surface. 130016/0096130016/0096 Dlpl.-Phys. Heinrich Seids · Patentanwalt · 6200 Wiesbaden 1 ■ Bierstadter höhe 15 · Postfach 51 05 · ξ?(ο 6ι 21) 56 53 82Dlpl.-Phys. Heinrich Seids · Patent Attorney · 6200 Wiesbaden 1 ■ Bierstadter Höhe 15 · Postfach 51 05 · ξ? (Ο 6ι 21) 56 53 82 41.) Vorrichtung nach einem der Ansprüche 33 bis 40, dadurch gekennzeichnet, daß die Thermoverformvorrichtung (16) mindestens ein Formwerkzeug enthält, das mit Einrichtungen zum Erzeugen eines vorher festlegbaren, regelbaren Formdruckes ausgestattet ist,41.) Device according to one of claims 33 to 40, characterized in that the thermoforming device (16) contains at least one molding tool with means for producing a previously is equipped with a definable, controllable form pressure, 42.) Vorrichtung nach Anspruch 41, dadurch gekennzeichnet, daß die Einrichtungen zum Erzeugen des Formdruckes mit einer Steuereinrichtung zum regelbaren, ggf. programmierbaren zeitlichen Variieren des Formdruckes42.) Device according to claim 41, characterized in that the devices for generating the molding pressure with a control device for the controllable, possibly programmable, temporal variation of the form pressure während des Thermoverformungsvorganges ausgerüstet j sind. ' jare equipped during the thermoforming process. 'j 43.) Vorrichtung nach einem der Ansprüche 33 bis 42, dadurch gekennzeichnet, daß die zweite Thermo-Konditionierungsstation (17) in ihrem Eingangsbereich die Thermoverformungsvorrichtung (16) enthält und sich über den Ausgang der Thermoverformungsvorrichtung (16) hinaus erstreckt.43.) Device according to one of claims 33 to 42, characterized in that the second thermal conditioning station (17) contains the thermoforming device (16) in its input area and extends beyond the exit of the thermoforming device (16). 44.) Vorrichtung nach Anspruch 43, dadurch gekennzeichnet,44.) Device according to claim 43, characterized in that ι daß die zweite Thermo-Konditionierungsstation (17)ι that the second thermal conditioning station (17) :20 eine sich an den Ausgang der Thermoverformungsvorrichtung (16) anschließende Wärmebehandlungsvor- ! richtung für die Formlinge enthält.: 20 one connected to the output of the thermoforming device (16) subsequent pre-heat treatment! contains direction for the briquettes. 130016/0098130016/0098
DE19792938905 1979-09-26 1979-09-26 METHOD AND DEVICE FOR PRODUCING MOLDINGS FROM THERMOPLASTIC PLASTIC, WHICH READS TO BE SET IN ITS PART CRYSTALLINE CONDITION BY MEANS OF PHYSICAL INFLUENCES, IN PARTICULAR TEMPERATURE INFLUENCES Ceased DE2938905A1 (en)