DE1917744C3 - Process for making photographic images - Google Patents

Process for making photographic images

Info

Publication number
DE1917744C3
DE1917744C3 DE19691917744 DE1917744A DE1917744C3 DE 1917744 C3 DE1917744 C3 DE 1917744C3 DE 19691917744 DE19691917744 DE 19691917744 DE 1917744 A DE1917744 A DE 1917744A DE 1917744 C3 DE1917744 C3 DE 1917744C3
Authority
DE
Germany
Prior art keywords
silver
image
layer
photographic
solution
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
DE19691917744
Other languages
German (de)
Other versions
DE1917744A1 (en
DE1917744B2 (en
Inventor
Rudolf Dr Ranz Erwin Dr Konig Anita von Dr 5090 Lever kusen Weyde Edith Dr 5073 Kurten Rintelen Harald von Dr 5090 Leverkusen Meyer
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Agfa Gevaert AG
Original Assignee
Agfa Gevaert AG
Filing date
Publication date
Application filed by Agfa Gevaert AG filed Critical Agfa Gevaert AG
Priority to DE19691917744 priority Critical patent/DE1917744C3/en
Priority to CA078816A priority patent/CA929400A/en
Priority to BE748354D priority patent/BE748354A/en
Priority to CH486570A priority patent/CH527443A/en
Priority to GB1594770A priority patent/GB1278403A/en
Priority to FR7012214A priority patent/FR2042929A5/fr
Publication of DE1917744A1 publication Critical patent/DE1917744A1/en
Publication of DE1917744B2 publication Critical patent/DE1917744B2/en
Application granted granted Critical
Publication of DE1917744C3 publication Critical patent/DE1917744C3/en
Expired legal-status Critical Current

Description

Die Erfindung betrifft ein Verfahren zur Herstellung photographischer Bilder, die aus einem Silberbild und einem dem Silberbild überlagerten Bläschenbild bestehen, unter Verwendung von lichtempfindlichen photographischen Materialien, die in einer Schicht eine Entwicklersubstanz enthalten.The invention relates to a method for producing photographic images from a silver image and consist of a bubble image superimposed on the silver image, using light-sensitive photographic materials which contain a developer substance in a layer.

Es ist bekannt, zur Herstellung von Bläschenbildern ein photographisches Material zu verwenden, das eine Schicht aus einem Bindemittel besitzt, in der lichtzersetzliche Verbindungen, beispielsweise Diazoniumsalze, dispergiert sind. Wird dieses Material bildmäßig belichtet, so wird die lichtzersetzliche Verbindung entsprechend dem aufbelichteten Bild zersetzt, wobei ein Gas in Freiheit gesetzt wird. Die anschließende Erwärmung des Materials bewirkt, daß das in Freiheit gesetzte Gas sich ausdehnt und ein Bild in Form von Bläschen entsteht. Das so erhaltene Bläschenbild ruft eine Lichtstreuung an den Bildstellen hervor, während die unbelichteten Teile der Schicht das auffallende Licht im wesentlichen durchlassen. Ein Bläschenbild erscheint daher im durchfallenden Licht dunkel, bei Betrachtung im reflektierten Licht dagegen hell.It is known to use a photographic material for the production of vesicle images, the one Has a layer of a binder in which light-decomposing compounds, for example diazonium salts, are dispersed. If this material is exposed imagewise, the light-decomposing compound becomes decomposed according to the exposed image, releasing a gas. The subsequent Heating the material causes the released gas to expand and create an image in the form of Vesicles appear. The bubble image obtained in this way causes light scattering at the image areas while the unexposed parts of the layer essentially let the incident light through. A picture of bubbles therefore appears dark in transmitted light, but bright when viewed in reflected light.

Aus der deutschen Patentschrift 15 97512 ist ein Verfahren zur Herstellung photographischer Bilder bekannt, bei dem man in an sich bekannter Weise in einem Bindemittel erzeugte Silberbilder mit einer Verbindung behandelt, die durch die Silberbilder unter Freisetzung von Gas zersetzt wird, und das Gas unter Bildung eines Bläschenbilds expandiert. Es werden auf diese Weise photographische Bilder erhalten, die in einer Schicht, z. B. einer Gelatineschicht, ein Silberbild und ein dem Silberbild überlagertes Bläschenbild enthalten.From the German patent specification 15 97512 is a Process for the production of photographic images is known, in which in a manner known per se in treated with a compound produced by the silver images under Release of gas is decomposed, and the gas expands to form a vesicle image. It will be on this Way to obtain photographic images which are in one layer, e.g. B. a gelatin layer, a silver image and contain a bubble image superimposed on the silver image.

Die Vorteile dieses Verfahrens bestehen darin, daß man zur Erzeugung der Bilder von Silbersalz-, insbesondere Silberhalogenidemulsionsschichten ausgehen kann, die verglichen mit den bekannten Materialien zur Herstellung von Bläschenbildern eine relativ hohe Lichtempfindlichkeit besitzen und für den ganzen Spektralbereich bis zum roten Licht sensibilisierbar sind.The advantages of this method are that you can generate the images of silver salt, in particular Silver halide emulsion layers can go out, which compared with the known materials for Production of vesicle images have a relatively high sensitivity to light and for the whole Spectral range up to red light can be sensitized.

Weiterhin wird durch dieses Verfahren eine wesentliche Steigerung der Deckkraft der in den photographischen Silbersalzschichten erzeugten Silberbilder durch die Überlagerung mit dem Bläschenbild erzielt. Es ist daher möglich, für die Durchführung des Verfahrens von relativ silberarmen Schichten auszugehen und die hierin erzeugten Silberbilder mit ungenügender Deckkraft durch Überlagerung mit dem Bläschenbild in Bilder normaler Deckkraft zu überführen.Furthermore, this procedure becomes an essential Increasing the opacity of the silver images produced in the silver salt photographic layers achieved by superimposing the image of the bubbles. It is therefore possible to carry out the procedure starting from relatively low-silver layers and the silver images produced therein with insufficient To convert opacity by overlaying the image of bubbles in images of normal opacity.

Bei dem in der deutschen Patentschrift 15 97 512 beschriebenen Verfahren wird ausgegangen von Süberbildern, die in bekannter Weise durch Behandlung der belichteten Silbersalzemulsionsschicht mit einem Entwicklerbad erhalten werden.The method described in German patent specification 15 97 512 is based on Süberbildern, in a known manner by treating the exposed silver salt emulsion layer with a developer bath can be obtained.

Der Erfindung liegt die Aufgabe zugrunde, das Verfahren zur Herstellung der kombinierten Bläschen- und Silberbilder zu vereinfachen, so daß die Anwendung von wäßrigen Verarbeitungsbädern ganz oder teilweise vermieden wird.The invention is based on the object of the method for producing the combined vesicle and to simplify silver images, so that the application of aqueous processing baths entirely or is partially avoided.

Gegenstand der vorliegenden Zusatzerfindung ist ein Verfahren zur Herstellung von photographischen Bildern, die aus einem Silberbild und einem dem Silberbild überlagerten Bläschenbild bestehen, durch bildmäßige Belichtung einer auf einem Schichtträger befindlichen lichtempfindlichen, wasserdurchlässigen Silbersalzemulsionsschicht, anschließende photographische Verarbeitung und Behandlung des in der Schicht erzeugten Silberbilds mit einer Verbindung, die durch das Silberbild unter Bildung eines Bläschenbilds zersetzt wird (gemäß deutsche Patentschrift 15 97512) dadurch gekennzeichnet, daß ein photographisches Material mit einer auf einem Schichtträger befindlichen lichtempfindlichen Silbersalzemulsionsschicht verwendet wird, das in der Emulsionsschicht oder einer Hilfsschicht eine photographische Entwicklersubstanz enthält.The present additional invention is a process for the production of photographic Images that consist of a silver image and a vesicle image superimposed on the silver image imagewise exposure of a light-sensitive, water-permeable material located on a layer support Silver salt emulsion layer, subsequent photographic processing and treatment of the in der Layer produced a silver image with a compound that caused the silver image to form a vesicle image is decomposed (according to German Patent 15 97512) characterized in that a photographic Material having a photosensitive silver salt emulsion layer on a support is used, the in the emulsion layer or an auxiliary layer a photographic developer substance contains.

Die im Rahmen des erfindungsgemäßen Verfahrens verwendeten lichtempfindlichen photographischen Materialien enthalten auf einem Schichtträger angeordnet mindestens eine Emulsionsschicht mit einem lichtempfindlichen Silbersalz, vorzugsweise eine Silberhalogenidemulsionsschicht. Die Entwicklersubstanz kann entweder in dieser Emulsionsschicht oder in einer Hilfsschicht, z. B. einer Schicht, die zwischen Schichtträger und Emulsionsschicht angeordnet ist, enthalten sein.The photographic light-sensitive materials used in the process of the present invention contain at least one emulsion layer with a light-sensitive emulsion layer arranged on a layer support Silver salt, preferably a silver halide emulsion layer. The developer substance can either in this emulsion layer or in an auxiliary layer, e.g. B. a layer between the substrate and emulsion layer is arranged.

Die Einlagerung von photographischen Entwicklersubstanzen in Silbersalzemulsionsschichten oder benachbarte Schichten ist an sich bekannt. Verwiesen sei z. B. auf die deutschen Patentschriften 8 88 045 oder 10 03 578, sowie die deutsche Auslegeschrift 11 23 203.The incorporation of photographic developer substances in silver salt emulsion layers or adjacent layers Layers is known per se. Reference is z. B. on the German patents 8 88 045 or 10 03 578, as well as the German Auslegeschrift 11 23 203.

Brauchbar sind dabei die üblichen Entwicklersubstanzen, z. B. aromatische Phenole, insbesondere solche der Di-hydroxybenzolreihe, ferner Aminophenol- bzw. Aminonaphthol-Verbindungen oder Entwickler des Phenylendiamintyps. Als besonders geeignet haben sich Entwickler der 3-Pyrazolidon-Gruppe, insbesondere solche der l-Phenyl-3-Pyrazolidonreihe erwiesen. Gute Wirkung haben auch die in der deutschen Patentschrift 9 46 606 beschriebenen l-Aryl-3-aminopyrazoline, insbesondere die Verbindung, die an dem Arylrest eine Aminogruppe enthält. Verwiesen sei ferner auf die in der deutschen Patentschrift 9 55 025 beschriebenen 4-Aminopyrazolone.The usual developer substances can be used, e.g. B. aromatic phenols, especially those the di-hydroxybenzene series, aminophenol or aminonaphthol compounds or developers of the phenylenediamine type. Developers of the 3-pyrazolidone group, in particular, have proven to be particularly suitable those of the l-phenyl-3-pyrazolidone series have been found. The l-aryl-3-aminopyrazolines described in German patent specification 9 46 606 also have a good effect, in particular the compound which contains an amino group on the aryl radical. Be referred also to the 4-aminopyrazolones described in German Patent 9 55 025.

Von besonderer Brauchbarkeit sind sogenannte verkappte photographische Entwickler. Bei diesen Entwicklern sind photographisch aktive Gruppen durch Substituenten, die vor der Entwicklung wieder abge-So-called masked photographic developers are of particular utility. With these developers are photographically active groups through substituents that are removed again before development

ItIt

spalten werden, unwirksam gemacht, so daß diese Bads, das gegebenenfalls die üblichen Zusätze enthält, lichtempfindlichen Schichten weitgehend lagerstabil durchgeführt werden. Man kann aber auch durch sjnd. Derartige Entwickler sind in den deutschen einfache Erwärmung des belichteten Materials ohne Patentschriften 10 25 264, 10 38 913, 10 56 472, Anwendung wäßriger Verarbeitungsbäder entwickeln. 1159 785, 1200679, 1203 129 oder 1203605 bzw. 5 In diesem Falle empfiehlt es sich, in an sich bekannter der britischen Patentschrift 8 12 673 beschrieben. Weise für einen gewissen Feuchtigkeitsgehalt derare made ineffective, so that these baths, which may contain the usual additives, light-sensitive layers are carried out largely stable in storage. But one can also use s j n d. Such developers are developed in the German simple heating of the exposed material without patents 10 25 264, 10 38 913, 10 56 472, application of aqueous processing baths. 1159 785, 1200679, 1203 129 or 1203605 or 5 In this case, it is advisable to use the British patent 8 12 673, which is known per se. Way for a certain moisture content of the

Da das dem Silberbild überlagerte Bläschenbild eine Schicht Sorge zu tragen, z. B. durch Zusatz Feuchtighohe Deckkraft besitzt, kann man lichtempfindliche keit abgebender Substanzen, wie wasserhaltiges Na-Silbersalzemulsionsschiclhten mit einem relativ gerin- triumacetat oder durch Anfeuchtung der belichteten gen Gehalt an Silbersalzen, z. B. Silberhalogeniden, i.o Schicht vor der Erwärmung.Since the vesicle image superimposed on the silver image has to take care of a layer, e.g. B. has high coverage by adding moisture, you can light-sensitive speed-releasing substances, such as water-containing Na silver salt emulsion layers with a relatively gerin- trium acetate or by moistening the exposed gene content of silver salts, z. B. silver halides, i. o Layer before heating.

verwenden. Brauchbare Konzentrationen liegen etwa Besonders gut kann das Silberbild entwickelt werdenuse. Usable concentrations are around. The silver image can be developed particularly well

zwischen 0,1 bis 0,3 g Silber in Form des !Silbersalzes durch Wasserdampf von etwa 50 bis 900C, wobei pro m2. Man erhält bei der photographs ichen Ent- Wärme und Feuchtigkeit gleichzeitig zur Anwendung wicklung zwar Silberbilder unzureichender Dichte, die gelangen.between 0.1 to 0.3 g of silver in the form of the silver salt by means of steam at from about 50 to 90 ° C., with per m 2 . In the case of the photographic development, heat and moisture are obtained at the same time as the application of silver images of insufficient density, which get there.

normalerweise nicht brauchbar wären, durch die nach- 15 Die so erhaltenen Silbcrbtlder werden mit einer Verfolgende Erzeugung des Bläschenbilds entsteht jedoch bindung behandelt, die am Silberbild unter Bildung ein kombiniertes Bild mit ausgezeichneter Deckung. gasförmiger Produkte zersetzt wird. Bevorzugt geeignet Bei Verwendung solcher silberarmer Schichten kann ist Wasserstoffperoxid (H2O2).Normally it would not be useful because of the subsequent bonding, which is treated with a subsequent generation of the vesicle image, but the bond is formed on the silver image with the formation of a combined image with excellent coverage. of gaseous products is decomposed. Preferred suitability When using such low-silver layers, hydrogen peroxide (H 2 O 2 ) can be used.

auch die Konzentration des Entwicklers in der Emul- Die Behandlung mit der gasbläschenbildenden Versionsschicht oder einer benachbarten Schicht relativ «0 bindung, insbesondere mit Wasserstoffperoxid kann in gering gewählt werden. Während man üblicherweise der verschiedensten Weise erfolgen. Man kann z. B. Konzentrationen von etwa 0,5 bis 5 g Entwickler/m2 die das entwickelte Silberbild enthaltende Schicht mit Schicht anwendet, genügen bei solchen silberaimen einer Wasserstoffperoxid enthaltenden neuen Schicht Schichten Mengen von 0,01 bis 0,5 g/m2. überziehen, z. B. mit einer Lösung von Polyvinyl-also the concentration of the developer in the emulsion, in particular with hydrogen peroxide, can be chosen to be low. While one is usually done in a variety of ways. You can z. B. Concentrations of about 0.5 to 5 g developer / m 2 the layer containing the developed silver image with layer applies, amounts of 0.01 to 0.5 g / m 2 are sufficient for such silver-bound layers of a new layer containing hydrogen peroxide. overlay, e.g. B. with a solution of polyvinyl

Da für das erfindungsgemäße Verfahren Silber- ns chlorid in Bi'tarton-(2), die Wasserstoffperoxid enthält, halogenidschichten verwendet werden können mit Nach dem Beschichten wird getrocknet und durch einem sehr geringen Silberhalogenidgehalt, erübrigt Erwärmen die Bläschen erzeugt. Die entwickelte photosich in diesen Fällen das ansonsten anzuwendende graphische Schicht kann ferner mit einer Wasserstoff-Fixierbad, peroxidlösung, z. B. einer alkoholischen Lösung be-Since for the process according to the invention silver ns chloride in Bi'tarton- (2), which contains hydrogen peroxide, Halide layers can be used with After coating is dried and through a very low silver halide content, eliminating the need for heating which creates bubbles. The developed photosich in these cases the otherwise applicable graphic layer can also be treated with a hydrogen fixer, peroxide solution, e.g. B. an alcoholic solution

Die erfindungsgemäßen Materialien können zur 30 handelt werden.The materials according to the invention can be traded.

Verbesserung der Lagerstabilität an sich bekannte Am günstigsten ist die Behandlung der photogra-Improvement of the storage stability known per se The most favorable is the treatment of the photographic

Antioxydantien, wie Alkalisulfit, Bisulfitadditionspro- phischen Schicht mit dampfförmigem Wasserstoffdukte von Aldehyden oder Ketonen, vorzugsweise von peroxid. Nach einer Zeit von etwa 30 see mit einem Cycloalkylketonen, insbesondere Cyclohexanonbisulfit gesättigten Wasserstoffperoxiddampf hat die Schicht enthalten. 35 genügend Wasserstoffperoxid aufgenommen. Selbst-Antioxidants such as alkali sulfite, bisulfite addition-prophetic layer with vaporous hydrogen products of aldehydes or ketones, preferably of peroxide. After a period of about 30 seconds with a Cycloalkyl ketones, especially cyclohexanone bisulfite saturated hydrogen peroxide vapor, has the layer contain. 35 absorbed enough hydrogen peroxide. Self-

Ais Filmbildner für die Silbersalzemulsionsschicht verständlich hängt die Einwirkungszeit von der Em- oder die Entwickler enthaltenden Schichten sind die Wirkungstemperatur und der Konzentration des Wasüblichen wasserdurchlässigen und hydrophilen Film- serstoffperoxiddampfs ab. Geeignet sind z. B. Tempebildner geeignet, z. B. natürliche Bindemittel wie raturen von 50 bis 90° C.As a film-forming agent for the silver salt emulsion layer, the exposure time depends on the em- or the developer-containing layers are the working temperature and the concentration of the usual water-permeable and hydrophilic film hydrogen peroxide vapor. Suitable are e.g. B. Tempebuilders suitable e.g. B. natural binders such as temperatures from 50 to 90 ° C.

Proteine, insbesondere Gelatine, Cellulose und deren 40 Nach einer bevorzugten Ausführungsform wird die Derivate, wie Celluloseester oder -äther, z. B. Carboxy- entwickelte Silberhalogenidemulsionsschicht nach der methylcellulose oder /5-Hydroxyäthylcellulose, Algin- Behandlung mit dem Wasserstoffperoxiddampf tür säure oder Derivate davon, wie Ester, Salze oder etwa 0,5 bis 5 see einer Wasserdampfattnosphare von Amide, Stärke oder Stärkederivate, Caraghenate und etwa 50 bis 900C ausgesetzt. Dabei tritt der bei der ähnliche. Die natürlichen Filmbildner können dabei 45 Behandlung mit Wasserstoffperoxid allein nur relativ ganz oder teilweise ersetzt werden durch synthetische langsam zu erreichende Verstärkungseffekt sehr Polymere, wie Polyvinylalkohol, partiell verseifte; schnell ein.Proteins, especially gelatin, cellulose and their 40. In a preferred embodiment, the derivatives, such as cellulose esters or ethers, e.g. B. Carboxy-developed silver halide emulsion layer after the methyl cellulose or / 5-hydroxyethyl cellulose, algin treatment with the hydrogen peroxide vapor for acid or derivatives thereof, such as esters, salts or about 0.5 to 5 see a water vapor atnosphere of amides, starch or starch derivatives, caraghenates and exposed to about 50 to 90 ° C. Thereby the similar one occurs. The natural film-forming agents can only be relatively completely or partially replaced by synthetic reinforcement effects that can be achieved slowly, very polymers such as polyvinyl alcohol, partially saponified; quickly one.

Polyvinylester, z. B. teilweise verseiftes Polyvinylacetat., Als noch günstiger hat es sich erwiesen, die mitPolyvinyl ester, e.g. B. partially saponified polyvinyl acetate., It has proven to be even cheaper to use with

Polyvinylpyrrolidon, oder Copolymerisate von Acryl- Wasserstoffperoxid behandelte entwickelte photogravure oder Methacrylsäure, die auch Einheiten von. 5° phische Schicht einer alkalischen Wasserdampfatmo-Acryl- oder Methacrylsäureester oder Nitrile oder Sphäre auszusetzen, dabei sind pH-Werte zwiscnen Amide dieser Säuren enthalten können. 8 und 12 geeignet. Dies kann leicht dadurch erreichtPolyvinylpyrrolidone, or copolymers of acrylic hydrogen peroxide treated, developed photogravure or methacrylic acid, which also have units of. 5 ° phic layer of an alkaline water vapor atmosphere acrylic or methacrylic acid esters or nitriles or spheres, with pH values between Amides of these acids may contain. 8 and 12 suitable. This can easily be achieved by doing this

Die Herstellung des photographischen Bildes erfolgte werden, daß dem Wasserdampf geringe Mengen in der in der deutschen Patentschrift 15 97512 Ammoniak oder Dämpfe flüchtiger Amine zugesetzt beschriebenen Weise 55 werden. Die Konzentration der alkalisch wirkendenThe production of the photographic image was carried out using small amounts of water vapor in the German patent 15 97512 ammonia or vapors of volatile amines are added 55 described way. The concentration of the alkaline acting

Dabei geht man von lichtempfindlichen Silbersalz·· Zusätze ist nicht kritisch, im allgemeinen haben sich schichten, insbesondere Silberhalogenidemulsion*· Mengen zwischen 0,1 bis 5 Volumprozent, vo«ugsschichten aus. Es sind sowohl Silberchlorid- als auch weise etwa 0,3 bis 1 Volumprozent als ausreichend Silberbromidemulsionen oder Gemische davon, die erwiesen.This is based on photosensitive silver salt ·· additives are not critical, in general they have to be layers, in particular silver halide emulsion * amounts between 0.1 to 5 percent by volume, top layers out. Both silver chloride and about 0.3 to 1 percent by volume are sufficient Silver bromide emulsions or mixtures thereof which have been demonstrated.

gegebenenfalls Silberjodid bis zu etwa 10 Molprozent 6° Die Bildung der sichtbaren Bläschen erfolgt durch enthalten können, geeignet. Die Emulsionen können Ausdehnung der primär gebildeten gasförmigen Reakdas Silberhalogenid in feinkörniger oder grobkörniger tionsprodukte. Dies wird erreicht durch Erwarmen 1uf Form wie z. B. im Falle von Ammoniakemulsionett Temperaturen zwischen 60 und 100 C. Die Bildung enthalten der Bläschen wird unterstützt durch schwaches Erwei-optionally silver iodide up to about 10 mol percent 6 ° The formation of the visible vesicles takes place by being able to contain, suitable. The emulsions can expand the primarily formed gaseous reaction of the silver halide into fine-grained or coarse-grained ionic products. This is achieved by heating on a mold such as B. in the case of Ammoniakemulsionett temperatures between 60 and 100 C. The formation of the bubbles contained is supported by weak expanded

* h d Shiht B durch Befeuchten D^ Effekt* h d Shiht B by moistening D ^ effect

thalten der Bläs keep the blower

Die Herstellung des Silberbilds im Rahmen des *5 chen der Schicht z. B. durch Befeuchten erfindungsgemäßen Verfahrens kann durch eine Naß- wird durch die weiter ob en *s?hr«*™ ? entwicklung, d. h. eine Behandlung des belichteten, mit Wasserdampf erreicht. Dabei:stell sich eine beson entwicklerhältigen Materials mittels eines alkalischen ders günstige Bläschenform ein. Die Bläschen sind sehrThe production of the silver image in the context of the * 5 chen the layer z. B. by moistening the method according to the invention can be carried out by a wet through the further ob en * s ? hr «* ™? development, ie a treatment of the exposed, achieved with water vapor. In doing so, a particularly developer-containing material is created by means of an alkaline or favorable bubble shape. The vesicles are very

klein und die daraus gebildeten Bilder besitzen daher eine besonders hohe Dichte,small and the resulting images therefore have a particularly high density,

Da das endgültige Bild, das aus dem Silberbild und dem diesem überlagerten Bläschenbild besteht, eine gewisse Empfindlichkeit gegenüber der Luftfeuchtigkeit oder wäßrigen Bädern besitzt, empfiehlt es sich, geeignete Maßnahmen zur Stabilisierung gegenüber Feuchtigkeit zu treffen. Verwiesen sei hierbei auf die deutschen Offenlegungsschi iftcn 18 15 143, 19 00 540 und 19 00 864.Since the final image, which consists of the silver image and the vesicle image superimposed on it, is a some sensitivity to humidity or aqueous baths, it is advisable to take suitable measures for stabilization To meet moisture. Reference is made to the German Offenlegungsschi iftcn 18 15 143, 19 00 540 and 19 00 864.

Beispiel 1example 1

Auf einen Schichtträger aus Polyethylenterephthalat wird eine Silberhalogenidemulsionsschicht aus folgender Gießlösung aufgetragen:A silver halide emulsion layer composed of the following is formed on a support made of polyethylene terephthalate Casting solution applied:

15,0 ml einer Silberchloridgelatineemulsion15.0 ml of a silver chloride gelatin emulsion

(Silberchloridgehalt 3 Gewichtsprozent, Geiatinegehalt 6 Gewichtsprozent);
285,0 ml einer 6%igen wäßrigen Lösung einer
(Silver chloride content 3 percent by weight, gelatin content 6 percent by weight);
285.0 ml of a 6% aqueous solution of a

photographisch inerten Gelatine; ao photographically inert gelatin; ao

3,0 ml einer 5%igen methanolischen Lösung von 1 -Phenylpyrazolidon-3;3.0 ml of a 5% strength methanolic solution of 1-phenylpyrazolidone-3;

5,0 ml einer 7,5%igen wäßrigen Lösung von Saponin;5.0 ml of a 7.5% aqueous solution of Saponin;

1,5 ml einer 30%igen wäßrigen Formalinlösung.1.5 ml of a 30% strength aqueous formalin solution.

Die Schicht enthält 0,15 g Silber (in Form von Silberhalogenid) und 0,1 g l-Phenylpyrazolidon-3/m2. Die belichtete Probe wird 20 see lang in Wasserdampf von 75°C gebracht. Es wird ein negatives Bild der Vorlage erhalten, das jedoch nur schwach gedeckt und nach üblichen Methoden nicht kopierfähig ist. Fixieren und Wässern entfallen, da der niedrige Gehalt an Silberhalogenid nicht stört.The layer contains 0.15 g of silver (in the form of silver halide) and 0.1 g of 1-phenylpyrazolidone-3 / m 2 . The exposed sample is placed in steam at 75 ° C. for 20 seconds. A negative image of the original is obtained, but it is only weakly covered and cannot be copied using conventional methods. There is no need for fixing or washing, as the low content of silver halide does not interfere.

Nach kurzer Trocknung der nur schwach gequollenen Schicht wird wie folgt weiterverarbeitet:After the slightly swollen layer has dried briefly, it is processed further as follows:

1. 30 see Behandlung mit gesättigtem Wasserstoffperoxiddampf von 70° C.1. 30 see treatment with saturated hydrogen peroxide vapor from 70 ° C.

2. 0,5 see Aussetzen einer Wasserdampfatmosphäre von 750C.2. 0.5 seconds exposure to a water vapor atmosphere of 75 ° C.

Es tritt sofort durch Bläschenbildung ein außerordentlich großer Verstärkungseffekt auf, wobei z. B. eine Stelle mit einer Dichte von 0,04 des Silberbilds im gerichteten Licht auf 1,9 gesteigert wird. «5It occurs immediately through the formation of bubbles on an extraordinarily large reinforcing effect, with z. B. a spot with a density of 0.04 of the silver image in the directed light is increased to 1.9. «5

Beispiel 2Example 2

Auf einen Schichtträger aus Cellulosetriacetat wird folgende Lösung aufgetragen: sOn a cellulose triacetate film base following solution is applied: s "

285,0 ml einer 6%igen wäßrigen Gelatinelösung;
15,0 ml einer 2,5%igen wäßrigen Lösung von
285.0 ml of a 6% aqueous gelatin solution;
15.0 ml of a 2.5% strength aqueous solution of

p-Methylaminophenol;
5,0 ml einer 3%igen wäßrigen Lösung von
p-methylaminophenol;
5.0 ml of a 3% aqueous solution of

Natriumsulfit; 5SSodium sulfite; 5S

5,0 ml einer 7,5%igen wäßrigen Lösung von5.0 ml of a 7.5% aqueous solution of

Saponin;Saponin;

1,5 ml einer 30%igen wäßrigen Formaldehydlösung. 1.5 ml of a 30% strength aqueous formaldehyde solution.

6060

Nach dem Erstarren dieser Schicht wurde darauf eine Silberhalogenidemulsionsschicht aus der folgenden Gießlösung aufgetragen:After this layer was solidified, a silver halide emulsion layer composed of the following was formed thereon Casting solution applied:

15,0 ml einer Silberchloridgelatineemulsion (Silberchloridgehalt 3 Gewichtsprozent, Gelatinegehalt 6 Gewichtsprozent);
285,0 ml einer 6%igcn wäßrigen Lösung einer photographisch inerten Gelatine;
15.0 ml of a silver chloride gelatin emulsion (silver chloride content 3 percent by weight, gelatin content 6 percent by weight);
285.0 ml of a 6% strength aqueous solution of a photographically inert gelatin;

5,0 ml einer 7,5%igen wäßrigen Lösung von5.0 ml of a 7.5% aqueous solution of

Saponin;
1,5 ml einer 30%igen wäßrigen Formaldeliyd-
Saponin;
1.5 ml of a 30% aqueous formaldehyde

lösung.solution.

Die Schicht enthält 0,15 g Silber in Form von Silberhalogenid und 0,3 g p-Methylaminophenol/ma. Die weitere Verarbeitung erfolgt wie in Beispiel I. Man erhält eine außerordentlich große Verstärkung, wobei z. B. eine Stelle mit einer Dichte von 0,05 des Silberbilds im gerichteten Licht auf etwa 1,6 gesteigert wird.The layer contains 0.15 g of silver in the form of silver halide and 0.3 g of p-methylaminophenol / m a . The further processing is carried out as in Example I. An extremely large gain is obtained, with z. B. a point with a density of 0.05 of the silver image in the directed light is increased to about 1.6.

Beispiel 3Example 3

Auf einen Schichtträger aus Polyäthylenterephathalat wird eine Silberhalogenidemulsionsschicht aus der folgenden Gießlösung aufgetragen:On a support made of polyethylene terephthalate a silver halide emulsion layer is applied from the following coating solution:

20,0 ml einer Silberbromidgelatineemulsion, die 5 Molprozent Silberbromid bezogen auf das Gesamtsilberhalogenid enthält und deren Silberhalogenidgehalt 3 Gewichtsprozent und Gelatinegehalt 6 Gewichtsprozent beträgt.
280,0 ml einer 6%igen wäßrigen Lösung einer
20.0 ml of a silver bromide gelatin emulsion which contains 5 mol percent silver bromide based on the total silver halide and whose silver halide content is 3 percent by weight and gelatin content is 6 percent by weight.
280.0 ml of a 6% aqueous solution of a

photographisch inerten Gelatine;
5,0 ml einer 7,5%igen wäßrigen Lösung von
photographically inert gelatin;
5.0 ml of a 7.5% aqueous solution of

Saponin;
1,5 m! einer 30%igen wäßrigen Lösung von
Saponin;
1.5 m! a 30% aqueous solution of

Formaldehyd.Formaldehyde.

Nach dem Erstarren dieser Schicht wurde darauf eine entwicklerhaltige Gelatinelösung folgender Zusammensetzung aufgetragen:After this layer had solidified, a developer-containing gelatin solution of the following composition was applied applied:

280,0 ml einer 6%igen wäßrigen Gelatinelösung; 20,0 ml einer 5%igen wäßrigen Lösung von280.0 ml of a 6% strength aqueous gelatin solution; 20.0 ml of a 5% aqueous solution of

Brenzkatechin;
5,0 ml einer 7,5%igen wäßrigen Lösung von
Catechol;
5.0 ml of a 7.5% aqueous solution of

Saponin;Saponin;

1,5 ml einer 30%igen wäßrigen Formaldehydlösung. 1.5 ml of a 30% strength aqueous formaldehyde solution.

Die gesamte Schicht enthält 0,2 g Silber und 0,7 g Brenzkatechin/m2.The entire layer contains 0.2 g silver and 0.7 g pyrocatechol / m 2 .

Die belichtete Probe wird für 45 see in mit Ammoniak angereicherten Wasserdampf von 700C gebracht. Es wird ein negatives Bild der Vorlage erhalten, das jedoch nur schwach gedeckt und nach üblichen Methoden nicht kopierfähig ist. Fixieren und Wässern entfallen, da der niedrige Gehalt an Silberhalogenid nicht stört. Die Bläschenbildung erfolgt wie in Beispiel (. Es rusultiert ein großer Verstärkungseffekt, wobei eine Stelle mit einer Dichte von 0,04 des Silberbilds im gerichteten Licht auf 1,5 erhöht wird.The exposed sample is placed in ammonia-enriched water vapor at 70 ° C. for 45 seconds. A negative image of the original is obtained, but it is only weakly covered and cannot be copied using conventional methods. There is no need for fixing or washing, as the low content of silver halide does not interfere. The formation of bubbles takes place as in example (. A large amplification effect results, whereby a point with a density of 0.04 of the silver image in the directed light is increased to 1.5.

Beispiel 4Example 4

Auf einen Schichtträger aus Cellulosetriacetat wird folgende Lösung aufgetragen:The following solution is applied to a layer of cellulose triacetate:

285,0 ml einer 6%igen wäßrigen Gelatinelösung; 15,0 ml einer wäßrigen Lösung, die I %ig an Natriumsulfit und 2%ig an N,N-Diäthyl-pphenylendiamin-N'-methansulfonsaurem Natrium ist;
5,0 ml einer 7,5%igen wäßrigen Lösung von
285.0 ml of a 6% aqueous gelatin solution; 15.0 ml of an aqueous solution which is 1% sodium sulfite and 2% sodium N, N-diethyl-pphenylenediamine-N'-methanesulfonic acid;
5.0 ml of a 7.5% aqueous solution of

Saponin;Saponin;

1,5 ml einer 30%igen wäßrigen Formaldehydlösung. 1.5 ml of a 30% strength aqueous formaldehyde solution.

Nach dem Erstanen dieser Schicht wurde darauf eine Silberhalogenidemulsion wie in Beispiel 2 aufgetragen. After the first level this layer was applied a silver halide emulsion as in Example 2 was applied.

Die Schicht enthält 0,15 g Silber in Form von Silberhalogenid und 0,25 g Ν,Ν-Diäthyl-p-phenylendiamin-N'-methansulfonsaures Natrium/m2. Die weitere Verarbeitung erfolgt wie in Beispiel 1. Man erhält eine große Verstärkung, wobei z. B. eine Stelle mit einer Dichte von 0,05 des Silberbilds im gerichteten Licht auf etwa 1,0 gesteigert wird.The layer contains 0.15 g of silver in the form of silver halide and 0.25 g of Ν, Ν-diethyl-p-phenylenediamine-N'-methanesulfonic acid sodium / m 2 . The further processing is carried out as in Example 1. A large reinforcement is obtained, with z. B. a point with a density of 0.05 of the silver image in the directed light is increased to about 1.0.

Beispiel 5Example 5

Es wird eine, photographische Schicht auf einen Schichtträger aus Polyäthylenterephthalat analog Beispiel 1 aufgetragen mit dem Unterschied, daß an Stelle des l-Phenylpyrazolidon-3 15 ml einer 2%igen wäßrigen Lösung von 4-Amino-o-kresol-N-methansulfonsaurem Natrium verwendet werden.It is a photographic layer on a support made of polyethylene terephthalate analogous to the example 1 applied with the difference that instead of the 1-phenylpyrazolidone-3 15 ml of a 2% aqueous Solution of 4-amino-o-cresol-N-methanesulfonic acid Sodium can be used.

Die Schicht enthält dann 0,15 g Silber (in Form von Silberhalogenid) und 0,2 g 4-Amino-o-kresol-N-me-The layer then contains 0.15 g of silver (in the form of silver halide) and 0.2 g of 4-amino-o-cresol-N-me-

thansulfonsaures Natrium/m2. Nach Belichtung und weiterer Verarbeitung wie in Beispiel 1 wird ein schwach gedecktes Silberbild enthalten, das durch Bläschenbildung entsprechend verstärkt wird.
5
sodium thanesulfonic acid / m 2 . After exposure and further processing as in Example 1, a weakly opaque silver image is obtained, which is correspondingly intensified by the formation of bubbles.
5

Beispiel 6Example 6

Entwicklung des Silberbilds durch Behandeln der Schicht in einer wäßrigen Lösung aus Natriumcarbonat und Natriumsulfit. Eine photographische Schicht mitDevelopment of the silver image by treating the layer in an aqueous solution of sodium carbonate and sodium sulfite. A photographic layer with

»ο geringem Silberauftrag und einem Gehalt an 1-Phenylpyrazolidon-3 gemäß Beispiel 1, wird belichtet und zur Entwicklung des Silberbilds 30 see lang in eine wäßrige Lösung von 13 g Natriumsulfit und 26 g Natriumcarbonat in 1 1 Wasser getaucht. Anschließend wird»Ο low silver application and a content of 1-phenylpyrazolidone-3 according to Example 1, is exposed and for 30 seconds to develop the silver image in an aqueous one Solution of 13 g of sodium sulfite and 26 g of sodium carbonate immersed in 1 l of water. Then will

»5 2 min gewässert und getrocknet. Man erhält ein schwach gedecktes Silberbild. Die Bläschenbildung erfolgt wie in Beispiel 1 mit dem gleichen Verstärkungsfaktor. »5 watered for 2 min and dried. A weakly opaque silver image is obtained. The blistering takes place as in example 1 with the same gain factor.

709631/101709631/101

Claims (2)

; Patentansprüche:; Patent claims: ί. Verfahren zur Herstellung von photographischen Bildern, die aus einem Silberbild und einem dem Silberbild überlagerten Bläschenbild bestehen, durch bildmäßige Belichtung einer auf einem Schichtträger befindlichen lichtempfindlichen, wasserdurchlässigen Silbersalzemulsionsschicht, anschließende photographische Verarbeitung und Behandlung des in der Schicht erzeugten Silberbilds mit einer Verbindung, die durch das Silberbild unter Bildung eines Bläschenbilds zersetzt wird, gemäß deutscher Patentschrift 15 97 512, dadurch gekennzeichnet, daß ein photpgraphisches Material mit einer auf einem Schichtträger befindlichen lichtempfindlichen Silbersalzemulsionsschicht verwendet wird, das in der Emulsionsschicht oder einer Hilfsschicht eine photographische Entwicklersubstanz enthält. aoί. Process for the production of photographic images, which consist of a silver image and a vesicular image superimposed on the silver image, by imagewise exposure of a light-sensitive, water-permeable silver salt emulsion layer located on a support, subsequent photographic processing and treatment of the silver image produced in the layer with a compound which is produced by the Silver image is decomposed to form a bubble image, according to German patent specification 15 97 512, characterized in that a photographic material is used with a photosensitive silver salt emulsion layer on a support which contains a photographic developer substance in the emulsion layer or an auxiliary layer. ao 2. Verfahren nach Anspruch 1, dadurch gekennzeichnet, daß das belichtete photographische Material durch Erwärmung auf Temperaturen zwischen 60 und 1500C entwickelt wird.2. The method according to claim 1, characterized in that the exposed photographic material is developed by heating to temperatures between 60 and 150 ° C. »5»5
DE19691917744 1969-04-05 1969-04-05 Process for making photographic images Expired DE1917744C3 (en)