CN214205965U - Composite metal foil and circuit board - Google Patents

Composite metal foil and circuit board Download PDF

Info

Publication number
CN214205965U
CN214205965U CN202022693989.2U CN202022693989U CN214205965U CN 214205965 U CN214205965 U CN 214205965U CN 202022693989 U CN202022693989 U CN 202022693989U CN 214205965 U CN214205965 U CN 214205965U
Authority
CN
China
Prior art keywords
layer
resistance
resistance layer
conductive layer
composite metal
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN202022693989.2U
Other languages
Chinese (zh)
Inventor
苏陟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangzhou Fangbang Electronics Co Ltd
Original Assignee
Guangzhou Fangbang Electronics Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangzhou Fangbang Electronics Co Ltd filed Critical Guangzhou Fangbang Electronics Co Ltd
Priority to CN202022693989.2U priority Critical patent/CN214205965U/en
Application granted granted Critical
Publication of CN214205965U publication Critical patent/CN214205965U/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The utility model discloses a composite metal paper tinsel and circuit board, composite metal paper tinsel include first conducting layer and first resistance layer, first resistance layer sets up one side of first conducting layer, first resistance layer is kept away from the at least subregion of one side of first conducting layer is provided with protruding structure. Due to the existence of the protruding structure, the sectional area of the first resistance layer is increased, the current-carrying capacity of the first resistance layer is improved, the ESD resistance of the first resistance layer is further improved, and the antistatic breakdown performance of the embedded resistor is further improved.

Description

Composite metal foil and circuit board
Technical Field
The utility model relates to a composite metal paper tinsel technical field especially relates to a composite metal paper tinsel and circuit board.
Background
With the rapid development of wireless communication and electronic devices, electronic devices have evolved toward miniaturization, and lightness, and therefore, the size of components inside the electronic devices is required to be as miniaturized and as light as possible.
The resistance element inside the electronic device gradually develops from the previous plug-in resistor with pins, to the chip resistor, and then to the embedded resistor, to be light and thin. The preparation process of the embedded resistor is roughly as follows: and attaching the composite metal foil to the circuit board, and etching the embedded resistor by an etching process.
The embedded resistors are integrated on a circuit board inside an application terminal electronic product, the circuit is sensitive to high static voltage, when people or objects with static electricity contact the embedded resistors, static electricity can be released, and after the static voltage impacts the circuit, the embedded resistors are easily broken down by the high static voltage, so that the embedded resistors fail to function.
SUMMERY OF THE UTILITY MODEL
An object of the utility model is to provide a composite metal foil can improve the current-carrying capacity of first resistance layer, and then has improved the resistant ESD (Electro-Static Discharge, electrostatic Discharge) performance of first resistance layer, and then has improved and has buryed electrical impedance electrostatic breakdown ability.
Another object of the present invention is to provide a circuit board, including the embodiment of the present invention provides a composite metal foil.
In a first aspect, an embodiment of the present invention provides a composite metal foil, including: a first conductive layer and a first resistive layer;
the first resistance layer is arranged on one side of the first conducting layer;
at least partial region of one side of the first resistance layer, which is far away from the first conducting layer, is provided with a convex structure.
Optionally, the roughness Rz of the side of the first resistance layer away from the first conductive layer ranges from 0.1 μm to 30 μm.
Optionally, the roughness Sdr of the side of the first resistance layer away from the first conductive layer ranges from 0.5% or more.
Optionally, all areas of one side of the first resistance layer, which is far away from the first conductive layer, are provided with protruding structures.
Optionally, at least a partial region of a side of the first resistance layer away from the first conductive layer is provided with a plurality of continuous protruding structures.
Optionally, all areas of one side of the first resistance layer, which is far away from the first conductive layer, are provided with a plurality of continuous protruding structures.
Optionally, the roughness Rz of the side of the first resistance layer away from the first conductive layer ranges from 0.1 μm to 10 μm, and the roughness Sdr of the side of the first resistance layer away from the first conductive layer ranges from greater than or equal to 20%.
Optionally, the roughness Rz of the side of the first resistance layer away from the first conductive layer ranges from 0.1 μm to 10 μm, and the roughness Sdr of the side of the first resistance layer away from the first conductive layer ranges from greater than or equal to 50%.
Optionally, the roughness Rz of the side of the first resistance layer away from the first conductive layer ranges from 0.1 μm to 10 μm, and the roughness Sdr of the side of the first resistance layer away from the first conductive layer ranges from greater than or equal to 200%.
Optionally, the composite metal foil further includes at least one dielectric layer, and the dielectric layer is disposed on a side of the first resistance layer away from the first conductive layer and covers the protrusion structure.
Optionally, a second resistance layer and a second conductive layer are disposed on one side of the dielectric layer away from the first resistance layer, and the second resistance layer is located between the dielectric layer and the second conductive layer.
Optionally, the material of the first resistance layer includes at least one simple substance metal of nickel, chromium, platinum, palladium, and titanium, and/or a nickel-chromium alloy, a nickel-phosphorus alloy, or a chromium-silicon alloy.
Optionally, the first resistive layer is a single-layer structure or at least a two-layer structure.
In a second aspect, the embodiment of the present invention further provides a circuit board, including the utility model discloses the first aspect provides a composite metal foil.
The embodiment of the utility model provides a composite metal foil, including first conducting layer and first resistance layer, first resistance layer sets up in one side of first conducting layer, and the at least partial region of one side that first conducting layer was kept away from to first resistance layer is provided with protruding structure. Due to the existence of the protruding structure, the sectional area of the first resistance layer is increased, the current-carrying capacity of the first resistance layer is improved, the ESD resistance of the first resistance layer is further improved, and the anti-static breakdown capability of the embedded resistance device is further improved.
Drawings
The present invention will be described in further detail with reference to the accompanying drawings and examples.
Fig. 1A is a schematic structural diagram of a composite metal foil according to an embodiment of the present invention;
fig. 1B is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention;
fig. 2A is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention;
fig. 2B is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention;
fig. 3 is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention;
fig. 4A is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention;
fig. 4B is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention;
fig. 5A is a flowchart of a method for manufacturing a composite metal foil according to an embodiment of the present invention;
fig. 5B is a schematic diagram of a first conductive layer according to an embodiment of the present invention;
fig. 5C is a schematic diagram of forming a first resistance layer on a first conductive layer according to an embodiment of the present invention;
fig. 5D is a schematic diagram of forming a protruding structure on a side of the first resistance layer away from the first conductive layer according to an embodiment of the present invention;
fig. 6A is a flowchart of another method for manufacturing a composite metal foil according to an embodiment of the present invention;
fig. 6B is a schematic diagram of forming a first resistive layer on a carrier layer according to an embodiment of the present invention;
fig. 6C is a schematic diagram of forming a protruding structure on a side of the first resistance layer away from the first conductive layer according to an embodiment of the present invention;
fig. 6D is a schematic diagram of forming a dielectric layer on a first resistive layer according to an embodiment of the present invention;
fig. 6E is a schematic diagram of the carrier layer being peeled off according to an embodiment of the present invention;
fig. 6F is a schematic diagram of forming a first conductive layer on a first resistive layer according to an embodiment of the present invention.
Detailed Description
In order to make the technical problems, technical solutions and technical effects achieved by the present invention more clear, the embodiments of the present invention will be described in further detail with reference to the accompanying drawings, and obviously, the described embodiments are only some embodiments, not all embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative efforts belong to the protection scope of the present invention.
In the description of the present invention, unless expressly stated or limited otherwise, the terms "connected," "connected," and "fixed" are to be construed broadly, e.g., as meaning permanently connected, detachably connected, or integral to one another; can be mechanically or electrically connected; either directly or indirectly through intervening media, either internally or in any other relationship. The specific meaning of the above terms in the present invention can be understood in specific cases to those skilled in the art.
In the present disclosure, unless expressly stated or limited otherwise, the first feature "on" or "under" the second feature may comprise direct contact between the first and second features, or may comprise contact between the first and second features not directly. Also, the first feature being "on," "above" and "over" the second feature includes the first feature being directly on and obliquely above the second feature, or merely indicating that the first feature is at a higher level than the second feature. A first feature being "under," "below," and "beneath" a second feature includes the first feature being directly under and obliquely below the second feature, or simply meaning that the first feature is at a lesser elevation than the second feature. Furthermore, the terms "first" and "second" are used merely for descriptive purposes and are not intended to have any special meaning.
Fig. 1A is a schematic structural diagram of a composite metal foil provided by an embodiment of the present invention, and fig. 1B is a schematic structural diagram of another composite metal foil provided by an embodiment of the present invention, as shown in fig. 1A and fig. 1B, in an embodiment of the present invention, the composite metal foil includes a first conductive layer 110 and a first resistance layer 120.
Specifically, the first conductive layer 110 may have good conductive performance, and the material of the metal layer may be gold, silver, copper, or aluminum, or an alloy of at least two of them. The utility model discloses in other embodiments, first conducting layer 110 also can be other non-metal layers that have good electric conductivity, and the material on non-metal layer can be graphite alkene etc. the embodiment of the utility model provides a do not limit to the material of first conducting layer, as long as have good electric conductivity can.
First resistive layer 120 is a key functional layer of the composite metal foil, and is used to implement the resistive function of the embedded resistor. Generally, the resistor 120 may be made of different materials according to different functional requirements, and thus have different resistance characteristics. The material of first resistance layer 120 may include at least one elemental metal of nickel, chromium, platinum, palladium, and titanium, and/or an alloy including at least two combinations of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus, and aluminum. For example, the metal material may be nickel-chromium alloy (NiCr) or nickel-phosphorus alloy (NiP) with low resistivity, or may also be chromium-silicon alloy (CrSi) with high resistivity, and the embodiments of the present invention are not limited herein. The first resistance layer 120 serves as a precursor of a resistance layer in the embedded resistance device, in other words, the resistance layer in the embedded resistance device is obtained by removing a portion of the first resistance layer 120 through a process such as etching. It should be noted that the high resistivity and the low resistivity in the embodiments of the present invention are for the first resistance layer itself, and not for the first conductive layer.
In some embodiments of the present invention, first resistive layer 120 has a single-layer structure or at least a two-layer structure. Illustratively, the single-layer structure may be a single-layer structure composed of any one metal of nickel, chromium, platinum, palladium and titanium, or may be a single-layer structure composed of an alloy of at least two combinations of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum. Any layer in the at least two-layer structure can be a simple substance metal composed of any one of nickel, chromium, platinum, palladium and titanium, and can also be an alloy of at least two combinations of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum.
First resistive layer 120 is disposed on one side of first conductive layer 110, and in particular, first resistive layer 120 may be formed on one side of first conductive layer 110 by physical vapor deposition, chemical vapor deposition, evaporation plating, sputter plating, electroplating, hybrid plating, and the like. In other embodiments of the present invention, the first conductive layer 110 may be formed on one side of the first resistance layer 120 by physical vapor deposition, chemical vapor deposition, evaporation plating, sputtering plating, electroplating, and hybrid plating, and the order of forming the first conductive layer 110 and the first resistance layer 120 is not limited in the embodiments of the present invention.
The inventors have found that the cross-sectional area of the first resistance layer in the embedded resistance device affects the ESD resistance. When the sectional area of the first resistance layer is larger, the current-carrying capacity of the first resistance layer is larger, and the ESD resistance is better. In order to improve the ESD resistance of the embedded resistor device, the cross-sectional area of the first resistance layer may be increased.
The embodiment of the present invention provides the protrusion structure 121 on at least a partial region of the side of the first resistance layer 120 away from the first conductive layer 110, so that at least a partial region of the side of the first resistance layer 120 away from the first conductive layer 110 has a rough surface. The presence of protrusion structure 121 increases the cross-sectional area of first resistance layer 120, increases the current-carrying capacity of first resistance layer 120, and further increases the ESD resistance of first resistance layer 120, and further improves the anti-electrostatic breakdown capability of the embedded resistance film.
The embodiment of the utility model provides a composite metal foil, including first conducting layer and first resistance layer, first resistance layer sets up in one side of first conducting layer, and the at least partial region of one side that first conducting layer was kept away from to first resistance layer is provided with protruding structure. Due to the existence of the protruding structure, the cross section profile of the first resistance layer is more complex, the sectional area of the first resistance layer is increased, the current-carrying capacity of the first resistance layer is improved, the ESD resistance of the first resistance layer is further improved, and the anti-static breakdown capability of the embedded resistor is further improved.
Further, at least a partial region (region provided with the convex structure) of first resistance layer 120 on the side away from first conductive layer 110 has a roughness Rz in a range of 0.1 μm or more and a roughness Sdr in a range of 0.5% or more. Roughness Rz and roughness Sdr are used to characterize the microscopic unevenness of the surface of first resistive layer 120. Specifically, the roughness Rz is generally taken as the sum of the average of the five largest profile peak heights and the average of the five largest profile valley depths within the sampling length; the roughness Sdr is an extended area (surface area) of the defined region indicates how much an increase is made with respect to the area of the defined region, wherein the roughness Sdr of the completely flat surface is zero. In this and subsequent examples, the roughness test standard is ISO25178 standard.
Further, in some embodiments of the present invention, in order to further improve the ESD resistance of the first resistance layer, the roughness Rz of at least a partial region (region provided with protruding structures) of the side of the first resistance layer 120 away from the first conductive layer 110 is in a range of 0.1 μm to 30 μm, including 0.1 μm and 30 μm, and the roughness Rz of at least a partial region (region provided with protruding structures) of the side of the first resistance layer 120 away from the first conductive layer 110 may also take on a value of 1 μm, 5 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, and the like. The roughness Sdr may range from 0.5% to 8000%, including 0.5% and 8000%, and may also take on values of 1%, 5%, 12%, 20%, 50%, 80%, 100%, 200%, 500%, 800%, 1500%, 2000%, 2500%, 3000%, 3500%, 4000%, 4500%, 5000%, 5500%, 6000%, 6500%, 7000%, 7500%, and the like.
Table 1 shows the ESD resistance test on the first resistance layers with different roughness Rz, and the test method is as follows: under other conditions, a test electrostatic positive voltage (electrostatic discharge resistance voltage in table 1) was applied to the first resistance layer having a certain roughness three times with an interval of 10 seconds, and then a test electrostatic negative voltage (electrostatic discharge resistance voltage in table 1) was applied to the first resistance layer three times with an interval of 10 seconds. And gradually increasing the testing electrostatic voltage, and taking the testing electrostatic voltage which breaks through the first resistance layer as the electrostatic discharge resistant voltage of the first resistance layer.
TABLE 1
Rz(μm) Resisting electrostatic discharge voltage (KV)
0.1 0.51
1 1.22
2 1.57
4 2.25
6 3.15
10 3.49
30 4.1
As shown in table 1, the different roughness Rz has different esd voltages, that is, the roughness Rz of the first resistance layer is adjusted by providing a protrusion structure on at least a partial region of the first resistance layer on the side away from the first conductive layer, so that the esd voltage of the first resistance layer can be increased.
Table 2 shows the ESD resistance test performed on the first resistance layers with different roughness Sdr, and the test method is the same as the above.
TABLE 2
Figure BDA0002787470610000081
Figure BDA0002787470610000091
As shown in table 2, different roughness Sdr have different electrostatic discharge voltage resistances, that is, by providing a protruding structure on at least a partial region of the first resistance layer on the side away from the first conductive layer, the roughness Sdr of the first resistance layer is adjusted, so that the electrostatic discharge voltage resistance of the first resistance layer can be improved.
In the embodiment of the present invention, the shape of the protruding structure 121 may have diversity according to actual needs, and may be a regular or irregular solid geometry, for example, the shape of the protruding structure 121 may be one or more of a sharp corner shape, an inverted cone shape, a granular shape, a dendritic shape, a columnar shape, a block shape, and an arc shape, and the embodiment of the present invention is not limited herein.
Further, in order to further improve ESD resistance (i.e., electrostatic discharge voltage resistance) of first resistance layer 120, protruding structures 121 are continuously disposed on at least a partial region of first resistance layer 120 on a side away from first conductive layer 110. Illustratively, as shown in fig. 1A, the shape of the protruding structures 121 is dendritic, and the protruding structures 121 are continuously distributed on at least a partial region of the first resistive layer 120; as shown in fig. 1B, the protruding structures 121 are arc-shaped, and the protruding structures 121 are continuously distributed on at least a partial area of the first resistive layer 120 to form a structure similar to a "sine line" shape on the side of the first resistive layer 120 away from the first conductive layer 110. In addition, in other embodiments of the present invention, the protruding structure may include a continuous undulating surface formed on the first resistance layer side, and a plurality of protruding portions formed on the undulating surface, and the embodiments of the present invention are not limited herein. In addition, in other embodiments of the present invention, at least a partial region of the protrusion structures 121 on the side of the first resistive layer 120 away from the first conductive layer 110 may also be discontinuously distributed, and the embodiments of the present invention are not limited herein.
Fig. 2A is a schematic structural diagram of another composite metal foil provided in an embodiment of the present invention, and fig. 2B is a schematic structural diagram of another composite metal foil provided in an embodiment of the present invention, as shown in fig. 2A and fig. 2B, in this embodiment, the composite metal foil includes a first conductive layer 210 and a first resistance layer 220.
Specifically, the first conductive layer 210 may have good conductive performance, and the material of the metal layer may be gold, silver, copper, or aluminum, or an alloy of at least two of them. The first resistive layer 220 is a key functional layer of the composite metal foil, and is used for realizing the resistive function of the composite metal foil. The material of the first resistance layer 220 may include at least one elemental metal of nickel, chromium, platinum, palladium, titanium, and/or an alloy including at least two combinations of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus, and aluminum. Exemplary, for example, a nickel-chromium alloy (NiCr) or a nickel-phosphorus alloy (NiP) having a low resistivity, and may also be a chromium-silicon alloy (CrSi) having a high resistivity. In some embodiments of the present invention, the first resistance layer 220 may have a single-layer structure or at least a two-layer structure. Any layer can be made of any metal of nickel, chromium, platinum, palladium and titanium, or can be made of an alloy of at least two of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum.
The first resistance layer is arranged on one side of the first conducting layer, and at least partial area of one side, far away from the first conducting layer, of the first resistance layer is provided with a protruding structure. Exemplarily, as shown in fig. 2A and 2B, in this embodiment, all areas of the side of the first resistance layer 220 away from the first conductive layer 210 are provided with the protrusion structures 221, so that the whole surface of the side of the first resistance layer 220 away from the first conductive layer 210 forms a rough surface. Since the whole surface of the first resistance layer 220 away from the first conductive layer 210 is provided with the protrusion structure 221, compared with the protrusion structure 221 provided in a partial region, the sectional area of the first resistance layer 220 is further increased, and the anti-electrostatic breakdown capability of the embedded resistor is improved.
Specifically, the roughness Rz of the first resistance layer 220 on the side away from the first conductive layer 210 ranges from 0.1 μm or more, and the roughness Sdr ranges from 0.5% or more. Preferably, the roughness Rz of the side of the first resistance layer 220 away from the first conductive layer 210 ranges from 0.1 μm to 30 μm, including 0.1 μm and 30 μm, and the roughness Rz of the side of the first resistance layer 220 away from the first conductive layer 210 can also take on the values of 1 μm, 5 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, and the like. The roughness Sdr may range from 0.5% to 8000%, including 0.5% and 8000%, and may also take on values of 1%, 5%, 12%, 20%, 50%, 80%, 100%, 200%, 500%, 800%, 1500%, 2000%, 2500%, 3000%, 3500%, 4000%, 4500%, 5000%, 5500%, 6000%, 6500%, 7000%, 7500%, and the like. The embodiment of the utility model provides an in, the shape of protruding structure can have the variety according to actual need, can be regular or anomalous solid geometry, the embodiment of the utility model provides a do not limit here. In some examples, the shape of the protruding structures is one or more of a cusp shape, an inverted cone shape, a granular shape, a dendritic shape, a columnar shape, a block shape, and an arc shape.
In the embodiment of the present invention, as shown in fig. 2B, in order to further improve the ESD resistance of the first resistance layer 220, the protrusion structures 221 disposed in all the regions of the first resistance layer 220 away from the first conductive layer 210 are disposed continuously, that is, the protrusion structures 221 are disposed continuously on the whole side of the first resistance layer 220, so as to further improve the sectional area of the first resistance layer 220, improve the ESD resistance of the first resistance layer 220, and further improve the anti-electrostatic breakdown capability of the embedded resistor.
Further, if the roughness height parameter Rz of the protruding structure 221 is set too high, the protruding structure 221 is easily broken by an external force during application, and the ESD resistance of the first resistance layer 220 is further affected, so the roughness Rz of the first resistance layer 220 is set to be in a range of 0.1 μm to 10 μm, and the roughness Sdr of the first resistance layer 220 is set to be greater than or equal to 20%. By defining the roughness height parameter Rz of the first resistance layer 220 to be 0.1 μm-10 μm and the range of the increase parameter Sdr of the surface area relative to the area of the defined area to be more than or equal to 20%, the continuous and tightly arranged protrusion structures 221 (the continuous and tightly arranged protrusion structures of the whole area are similar to a "fluff" structure) are obtained in the whole area of the first resistance layer 220 on the side far away from the first conductive layer 210 within a certain height range of the protrusion structures 221, so that the first resistance layer 220 with a larger cross section is obtained under the condition that the height parameter Rz of the roughness is certain, that is, the protrusion structures 221 are not broken due to the external force, the ESD resistance of the first resistance layer 220 is further improved, and the embedded resistance has a stronger anti-static breakdown capability.
Preferably, the roughness Rz of the first resistance layer 220 ranges from 0.1 μm to 10 μm, and the roughness Sdr of the first resistance layer 220 ranges from 50% or more. By defining the roughness height parameter Rz of the first resistance layer 220 to be 0.1 μm-10 μm and the range of the increase parameter Sdr of the surface area relative to the area of the defined area to be more than or equal to 50%, the continuous and more closely arranged protrusion structures 221 are obtained in the whole area of the side of the first resistance layer 220 far away from the first conductive layer 210 within a certain height range of the protrusion structures 221, that is, the protrusion structures which are more closely arranged than the range of the roughness Sdr to be more than or equal to 20% are obtained, so that the cross section of the first resistance layer is further increased, the ESD resistance of the first resistance layer is further improved, and the embedded resistance is effectively ensured to have stronger anti-static breakdown capability.
More preferably, the roughness Rz of the first resistance layer 220 ranges from 0.1 μm to 10 μm, and the roughness Sdr of the first resistance layer 220 ranges from 200% or more, so as to further increase the cross section of the first resistance layer, further improve the ESD resistance of the first resistance layer, and effectively ensure that the embedded resistor has excellent anti-electrostatic breakdown capability.
Fig. 3 is a schematic structural diagram of another composite metal foil according to an embodiment of the present invention, as shown in fig. 3, in this embodiment, the composite metal foil includes a first conductive layer 310, a first resistive layer 320, and a dielectric layer 330.
Specifically, the first conductive layer 310 may have good conductive performance, and the material of the metal layer may be gold, silver, copper, or aluminum, or an alloy of at least two of them. The first resistance layer 320 is a key functional layer of the composite metal foil, and is used for realizing the resistance function of the composite metal foil. The material of the first resistance layer 320 may include at least one elemental metal of nickel, chromium, platinum, palladium, titanium, and/or an alloy including at least two combinations of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus, and aluminum. For example, a nickel-chromium alloy (NiCr) or a nickel-phosphorus alloy (NiP) having a low resistivity, and may also be a chromium-silicon alloy (CrSi) having a high resistivity. In some embodiments of the present invention, the first resistance layer 320 may have a single-layer structure or at least a two-layer structure. Any layer can be made of any metal of nickel, chromium, platinum, palladium and titanium, or can be made of an alloy of at least two of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum.
The first resistance layer is arranged on one side of the first conducting layer, and at least partial area of one side, far away from the first conducting layer, of the first resistance layer is provided with a protruding structure. For example, as shown in fig. 3, in this embodiment, all areas of the side of the first resistance layer 320 far from the first conductive layer 310 are provided with the protruding structures 321, so that the side of the first resistance layer 320 far from the first conductive layer 310 has a rough surface.
Specifically, the surface roughness Rz of the first resistance layer 320 on the side away from the first conductive layer 310 ranges from 0.1 μm or more, and the roughness Sdr ranges from 0.5% or more. Preferably, the roughness Rz of the side of the first resistance layer 320 far away from the first conductive layer 310 ranges from 0.1 μm to 30 μm, including 0.1 μm and 30 μm, and the roughness Rz of the side of the first resistance layer 320 far away from the first conductive layer 310 can also take on the values of 1 μm, 5 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, and the like. The roughness Sdr may range from 0.5% to 8000%, including 0.5% and 8000%, and may also take on values of 1%, 5%, 12%, 20%, 50%, 80%, 100%, 200%, 500%, 800%, 1500%, 2000%, 2500%, 3000%, 3500%, 4000%, 4500%, 5000%, 5500%, 6000%, 6500%, 7000%, 7500%, and the like.
At least one dielectric layer 330 is disposed on a side of the first resistive layer 320 away from the first conductive layer 310 and covers the protruding structure 321. The dielectric layer 330 may be made of resin adhesive, Polyimide (PI), modified polyimide, fiberglass cloth composite material, paper substrate, composite substrate, HDI plate, modified epoxy resin, modified acrylic resin, polyethylene terephthalate, glycol ester, polybutylene terephthalate, polyethylene, or the like, and is used to protect the first resistance layer 320 and prevent the first resistance layer 320 from being damaged by external force. Specifically, the dielectric layer 330 may be a single-layer structure or at least two-layer structure, and when the structure is at least two-layer structure, the material of each layer may be the same or different.
The utility model discloses a specific embodiment, dielectric layer 330 is two-layer structure, and the two-layer structure of dielectric layer 330 all can be prepared by same kind of material, for example polyimide, also can be prepared by two kinds of different materials, for example one deck resin glue, one deck polyimide, but, no matter which structure, in order to accord with some specific requirements, all the choice is set up the filler in the dielectric layer that is close to first resistance layer 320, thereby improve the cohesion of dielectric layer rather than adjacent layer, or some functional fillers, for example, the thermal conductivity filler, in order to lead away the heat that produces on the resistance layer through the thermal conductivity filler, effectively guarantee can derive fast because of the heat that electrostatic impact produced, improve the resistant ESD performance of first resistance layer, and then effectively improve the antistatic breakdown ability of buryying formula resistance device.
In some embodiments of the present invention, a side of the dielectric layer away from the first resistive layer is provided with a second resistive layer and a second conductive layer, the second resistive layer being located between the dielectric layer and the second conductive layer. The materials and purposes of the second resistance layer and the first resistance layer can be the same or different, and the materials and purposes of the second conductive layer and the first conductive layer can be the same or different. In addition, the structure and parameters of the second resistance layer may be the same as those of the first resistance layer, and the structure and parameters of the second conductive layer may also be the same as those of the first conductive layer, which is not repeated herein.
Fig. 4A is a schematic structural diagram of another composite metal foil provided in an embodiment of the present invention, and fig. 4B is a schematic structural diagram of another composite metal foil provided in an embodiment of the present invention, as shown in fig. 4A and fig. 4B, the composite metal foil includes a first conductive layer 410, a first resistance layer 420, a dielectric layer 430, a second resistance layer 440, and a second conductive layer 450. The first resistance layer 420 is disposed on one side of the first conductive layer 410, and the whole area of the side of the first resistance layer 420 away from the first conductive layer 410 is provided with the protruding structure 421, so that the whole surface of the side of the first resistance layer 420 away from the first conductive layer 410 forms a rough surface. The dielectric layer 430 is disposed on a side of the first resistive layer 420 away from the first conductive layer 410 and covers the protrusion 421. The materials of the first conductive layer, the first resistance layer and the dielectric layer, the shape of the protruding structure and the roughness of the side of the first resistance layer away from the first conductive layer have been described in detail in the foregoing embodiments, which are not repeated herein.
Second resistive layer 440 is disposed on a side of dielectric layer 430 distal from first resistive layer 420, and second conductive layer 450 is disposed on a side of second resistive layer 440 distal from dielectric layer 430. In an embodiment of the present invention, the material and purpose of the second resistance layer 420 and the first resistance layer 440 are the same, and the material and purpose of the second conductive layer 450 and the first conductive layer 410 are the same.
The side of the second resistance layer 440 away from the second conductive layer 450 may be a flat surface, or at least a portion of the area may be provided with a protruding structure, like the first resistance layer 420. For example, as shown in fig. 4A, a side of the second resistance layer 440 away from the second conductive layer 450 is a flat surface; as shown in fig. 4B, the whole area of the side of the second resistance layer 440 away from the second conductive layer 450 is provided with the protruding structure 451, and the protruding structure 451 may refer to the protruding structure on the first resistance layer 420 described in the foregoing embodiments of the present invention, which is not repeated herein.
Fig. 5A is a flowchart of a method for manufacturing a composite metal foil according to an embodiment of the present invention, and as shown in fig. 5A, the method includes:
s501, providing a first conducting layer.
Specifically, the first conductive layer may have good conductive performance, and the material of the metal layer may be any one of gold, silver, copper, or aluminum, or an alloy including a combination of at least two of copper, gold, silver, or aluminum. The first conductive layer may be independent or formed on the carrier, and the embodiment of the present invention is not limited herein. Fig. 5B is a schematic diagram of a first conductive layer according to an embodiment of the present invention, as shown in fig. 5B, for example, in this embodiment, the first conductive layer 510 is independent.
And S502, forming a first resistance layer on one side of the first conductive layer.
Specifically, the first resistance layer may be formed on one side of the first conductive layer by physical vapor deposition, chemical vapor deposition, evaporation plating, sputter plating, electroplating, hybrid plating, or the like. The first resistance layer is a key functional layer of the composite metal foil and is used for realizing the resistance function of the composite metal foil. Generally, the resistor can be made of different materials according to the requirements of different functions, and further has different resistance characteristics. For example, the material of the first resistance layer may include at least one elemental metal of nickel, chromium, platinum, palladium, titanium, and/or an alloy including a combination of at least two of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus, and aluminum. For example, the metal material may be nickel-chromium alloy (NiCr) or nickel-phosphorus alloy (NiP) with low resistivity, or may also be chromium-silicon alloy (CrSi) with high resistivity, and the embodiments of the present invention are not limited herein. In some embodiments of the present invention, the first resistance layer may have a single-layer structure or at least a two-layer structure. Any layer can be made of any metal of nickel, chromium, platinum, palladium and titanium, or can be made of an alloy of at least two of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum.
Fig. 5C is a schematic diagram of forming a first resistance layer on a first conductive layer according to an embodiment of the present invention, and as shown in fig. 5C, the first resistance layer 520 is formed on one side of the first conductive layer 510.
And S503, forming a protruding structure on at least a partial region of one side of the first resistance layer far away from the first conductive layer.
Specifically, at least a partial region of the first resistance layer on the side away from the first conductive layer may be roughened. After the roughening treatment, a raised structure is formed on at least a partial region of one side of the first resistance layer, which is far away from the first conductive layer, so that at least a partial region of one side of the first resistance layer, which is far away from the first conductive layer, has a rough surface. The process for roughening at least a partial region of the side of the first resistance layer away from the first conductive layer includes, but is not limited to, one or more processes of electroless plating, physical vapor deposition, chemical vapor deposition, evaporation plating, sputtering plating, electroplating and hybrid plating.
Fig. 5D is a schematic diagram of forming a protruding structure on a side of the first resistance layer away from the first conductive layer according to an embodiment of the present invention, as shown in fig. 5D, exemplarily, a protruding structure 521 is formed on the whole area of a side of the first resistance layer 520 away from the first conductive layer 510, so that a side of the first resistance layer 520 away from the first conductive layer 510 has a rough surface. The embodiment of the utility model provides an in, protruding structure 521's shape can have the variety according to actual need, can be regular or anomalous solid geometry, the embodiment of the utility model provides a do not limit here. In some examples, the shape of the raised structures 521 is one or more of a cusp, an inverted cone, a particle, a dendrite, a pillar, a block.
Specifically, the roughness Rz of the first resistance layer 520 on the side away from the first conductive layer 510 ranges from 0.1 μm or more, and the roughness Sdr ranges from 0.5% or more. Preferably, the roughness Rz of the side of the first resistance layer 520 away from the first conductive layer 510 ranges from 0.1 μm to 30 μm, including 0.1 μm and 30 μm, and the roughness Rz of the side of the first resistance layer 520 away from the first conductive layer 510 can also take on the values of 1 μm, 5 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, and the like. The roughness Sdr may range from 0.5% to 8000%, including 0.5% and 8000%, and may also take on values of 1%, 5%, 12%, 20%, 50%, 80%, 100%, 200%, 500%, 800%, 1500%, 2000%, 2500%, 3000%, 3500%, 4000%, 4500%, 5000%, 5500%, 6000%, 6500%, 7000%, 7500%, and the like.
The embodiment of the utility model provides a preparation method of composite metal foil, include: providing a first conductive layer, forming a first resistance layer on one side of the first conductive layer, and forming a convex structure on at least partial region of one side of the first resistance layer far away from the first conductive layer. The bulge structure is formed in at least part of the area of one side, far away from the first conducting layer, of the first resistance layer, so that the sectional area of the first resistance layer is increased, the current-carrying capacity of the first resistance layer is improved, the ESD resistance of the first resistance layer is further improved, and the antistatic breakdown capacity of the embedded resistor is further improved.
In another specific embodiment of the present invention, after step S503, the method may further include: and forming at least one dielectric layer on one side of the first resistance layer, which is far away from the first conductive layer, wherein the dielectric layer covers the protruding structure. The dielectric layer can be made of resin adhesive, Polyimide (PI), modified polyimide, fiberglass cloth composite material, a paper substrate, a composite substrate, an HDI plate, modified epoxy resin, modified acrylic resin, polyethylene terephthalate, glycol ester, polybutylene terephthalate, polyethylene and the like, and is used for protecting the first resistance layer and preventing the first resistance layer from being damaged by external force. Specifically, the precursor solution of the dielectric layer may be formed on the side of the first resistance layer away from the first conductive layer by spraying or coating, so as to obtain the dielectric layer, or directly attach the dielectric layer to the first resistance layer.
Further, the dielectric layer may be a single-layer structure or at least a two-layer structure. For example, the dielectric layer has a two-layer structure, and the two-layer structure of the dielectric layer may be made of the same material, such as polyimide, or may be made of two different materials, such as a layer of resin adhesive and a layer of polyimide, however, in any structure, in order to meet some specific requirements, it may be selected to set a filler in the layer of the dielectric layer close to the first resistance layer so as to improve the bonding force between the dielectric layer and its adjacent layers, or some functional fillers, such as thermal conductive fillers, so as to conduct away heat generated on the resistance layer through the thermal conductive filler, thereby effectively ensuring that heat generated due to electrostatic impact can be quickly conducted away, improving the ESD resistance of the first resistance layer, and further effectively improving the anti-static breakdown capability of the embedded resistor device.
Furthermore, a second resistance layer and a second conductive layer are arranged on one side of the dielectric layer far away from the first resistance layer, and the second resistance layer is located between the dielectric layer and the second conductive layer. The materials and purposes of the second resistance layer and the first resistance layer can be the same or different, and the materials and purposes of the second conductive layer and the first conductive layer can be the same or different.
Fig. 6A is a flowchart of another method for manufacturing a composite metal foil according to an embodiment of the present invention, and as shown in fig. 6A, the method includes:
s601, providing a carrier layer.
Specifically, the support layer may be a polyimide substrate or a resin substrate or a metal layer.
S602, forming a first resistive layer on one side of the carrier layer.
Specifically, the first resistance layer may be formed on one side of the carrier layer by physical vapor deposition, chemical vapor deposition, evaporation plating, sputter plating, electroplating, hybrid plating, and the like. The first resistance layer is a key functional layer of the composite metal foil and is used for realizing the resistance function of the composite metal foil. The material of the first resistance layer may include at least one elemental metal of nickel, chromium, platinum, palladium, and titanium, and/or an alloy including at least two combinations of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus, and aluminum, for example, a nickel-chromium alloy (NiCr) or a nickel-phosphorus alloy (NiP) with low resistivity, and may also be a chromium-silicon alloy (CrSi) with high resistivity, which is not limited herein. In some embodiments of the present invention, the first resistance layer may have a single-layer structure or at least a two-layer structure. Any layer can be made of any metal of nickel, chromium, platinum, palladium and titanium, or can be made of an alloy of at least two of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum.
Fig. 6B is a schematic diagram of forming a first resistance layer on a carrier layer according to an embodiment of the present invention, and as shown in fig. 6B, a first resistance layer 620 is formed on one side of the carrier layer 640.
And S603, forming a convex structure on at least partial region of the side, away from the carrier layer, of the first resistance layer.
Specifically, the side of the first resistance layer away from the first conductive layer may be roughened. After the roughening treatment, a raised structure is formed on at least a partial region of one side of the first resistance layer, which is far away from the first conductive layer, so that at least a partial region of one side of the first resistance layer, which is far away from the first conductive layer, has a rough surface. The process for roughening at least a partial region of the side of the first resistance layer away from the first conductive layer includes, but is not limited to, one or more processes of electroless plating, physical vapor deposition, chemical vapor deposition, evaporation plating, sputtering plating, electroplating and hybrid plating.
Fig. 6C is a schematic diagram of forming a protruding structure on a side of the first resistance layer away from the first conductive layer according to an embodiment of the present invention, as shown in fig. 6C, exemplarily, a protruding structure 621 is formed on the whole area of the side of the first resistance layer 620 away from the first conductive layer 610, so that the side of the first resistance layer 620 away from the carrier layer 640 has a rough surface. In the embodiment of the present invention, the shape of the protruding structure 621 may have diversity according to actual needs, and may be a regular or irregular solid geometry, and the embodiment of the present invention is not limited herein. In some examples, the shape of the protruding structures 621 is one or more of a pointed shape, an inverted cone shape, a granular shape, a dendritic shape, a columnar shape, and a block shape.
Specifically, the roughness Rz of the first resistance layer 620 on the side away from the first conductive layer 610 ranges from 0.1 μm or more, and the roughness Sdr ranges from 0.5% or more. Preferably, the roughness Rz of the side of the first resistance layer 620 away from the first conductive layer 610 ranges from 0.1 μm to 30 μm, including 0.1 μm and 30 μm, and the roughness Rz of the side of the first resistance layer 620 away from the first conductive layer 610 can also take on the values of 1 μm, 5 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, and the like. The roughness Sdr may range from 0.5% to 8000%, including 0.5% and 8000%, and may also take on values of 1%, 5%, 12%, 20%, 50%, 80%, 100%, 200%, 500%, 800%, 1500%, 2000%, 2500%, 3000%, 3500%, 4000%, 4500%, 5000%, 5500%, 6000%, 6500%, 7000%, 7500%, and the like.
And S604, forming at least one dielectric layer on the side, far away from the carrier layer, of the first resistance layer, wherein the dielectric layer covers the protruding structure.
Specifically, at least one dielectric layer is formed on one side of the first resistance layer, which is far away from the first conductive layer, and the dielectric layer covers the protruding structure. The dielectric layer may be made of resin adhesive, Polyimide (PI), or the like, and is used to protect the first resistance layer and prevent the first resistance layer from being damaged by external force. Specifically, the precursor solution of the dielectric layer may be formed on the side of the first resistance layer away from the first conductive layer by spraying or coating, to obtain the dielectric layer, or directly attach the dielectric layer to the first resistance layer.
Fig. 6D is a schematic diagram of forming a dielectric layer on the first resistance layer according to an embodiment of the present invention, and exemplarily, as shown in fig. 6D, the dielectric layer 630 is formed on a side of the first resistance layer 620 away from the carrier layer 640, and the dielectric layer 630 covers the protrusion structure 621.
Further, the dielectric layer may be a single-layer structure or at least a two-layer structure. For example, the dielectric layer has a two-layer structure, and the two-layer structure of the dielectric layer may be made of the same material, such as polyimide, or may be made of two different materials, such as a layer of resin adhesive and a layer of polyimide, however, in any structure, in order to meet some specific requirements, it may be selected to set a filler in the layer of the dielectric layer close to the first resistance layer so as to improve the bonding force between the dielectric layer and its adjacent layers, or some functional fillers, such as thermal conductive fillers, so as to conduct away heat generated on the resistance layer through the thermal conductive filler, thereby effectively ensuring that heat generated due to electrostatic impact can be quickly conducted away, improving the ESD resistance of the first resistance layer, and further effectively improving the anti-static breakdown capability of the embedded resistor device.
Furthermore, a second resistance layer and a second conductive layer are arranged on one side of the dielectric layer far away from the first resistance layer, and the second resistance layer is located between the dielectric layer and the second conductive layer. The materials and purposes of the second resistance layer and the first resistance layer can be the same or different, and the materials and purposes of the second conductive layer and the first conductive layer can be the same or different.
S605, peeling the carrier layer.
In particular, the carrier layer and the first resistive layer should have a suitable peel strength such that the carrier layer can be peeled off from the first resistive layer.
Fig. 6E is a schematic diagram of the carrier layer being peeled off according to an embodiment of the present invention, as shown in fig. 6E, after the carrier layer 640 is peeled off, the remaining laminated structure includes the first resistance layer 620 and the dielectric layer 630, and the entire area of the side of the first resistance layer 620 close to the dielectric layer 630 is provided with the protruding structure 621.
And S606, forming a first conducting layer on one side, far away from the dielectric layer, of the first resistance layer.
Specifically, the first conductive layer may be formed on a side of the first resistance layer away from the dielectric layer by physical vapor deposition, chemical vapor deposition, evaporation plating, sputtering plating, electroplating, hybrid plating, or the like. The first conductive layer may have good conductive performance, and the material of the metal layer may be any one of gold, silver, copper, or aluminum, or an alloy including at least two of copper, gold, silver, or aluminum.
Fig. 6F is a schematic diagram of forming a first conductive layer on the first resistive layer according to an embodiment of the present invention, and as shown in fig. 6F, the first conductive layer 610 is formed on a side of the first resistive layer 620 away from the dielectric layer 630.
The embodiment of the utility model provides a preparation method of composite metal foil, include: providing a carrier layer, forming a first resistance layer on one side of the carrier layer, forming a protruding structure on at least a partial region of one side of the first resistance layer far away from the carrier layer, forming a dielectric layer on one side of the first resistance layer far away from the carrier layer, covering the protruding structure with the dielectric layer, stripping the carrier layer, and forming a first conducting layer on one side of the first resistance layer far away from the dielectric layer. At least part of the area of one side of the first resistance layer, which is far away from the first conducting layer, forms a plurality of protruding structures, so that the sectional area of the first resistance layer is increased, the current-carrying capacity of the first resistance layer is improved, the ESD resistance of the first resistance layer is further improved, and the antistatic breakdown performance of the embedded resistor is further improved. In addition, a dielectric layer is formed on the first resistance layer, so that the first resistance layer is prevented from being damaged by external force.
The embodiment of the utility model provides a still provides a circuit board, include the utility model discloses the compound metal forming that above-mentioned arbitrary embodiment provided.
The embodiment of the utility model provides a circuit board has with the embodiment of the utility model provides a corresponding function of composite metal paper tinsel and beneficial effect.
In the description herein, it is to be understood that the terms "upper," "lower," "left," "right," and the like are used in a descriptive sense and with reference to the illustrated orientation or positional relationship for purposes of descriptive convenience and simplicity of operation, and are not intended to indicate or imply that the referenced device or element must have a particular orientation, be constructed and operated in a particular orientation, and are not to be construed as limiting the present invention.
In the description herein, references to the description of "an embodiment," "an example" or the like are intended to mean that a particular feature, structure, material, or characteristic described in connection with the embodiment or example is included in at least one embodiment or example of the invention. In this specification, the schematic representations of the terms used above do not necessarily refer to the same embodiment or example.
Furthermore, it should be understood that although the present description refers to embodiments, not every embodiment may contain only a single embodiment, and such description is for clarity only, and those skilled in the art should integrate the description, and the embodiments may be appropriately combined to form other embodiments as will be appreciated by those skilled in the art.
The technical principle of the present invention is described above with reference to specific embodiments. The description is made for the purpose of illustrating the principles of the invention and should not be construed in any way as limiting the scope of the invention. Based on the explanations herein, those skilled in the art will be able to conceive of other embodiments of the present invention without any inventive effort, which would fall within the scope of the present invention.

Claims (14)

1. A composite metal foil, comprising: a first conductive layer and a first resistive layer;
the first resistance layer is arranged on one side of the first conducting layer;
at least partial region of one side of the first resistance layer, which is far away from the first conducting layer, is provided with a convex structure.
2. The composite metal foil according to claim 1, wherein the roughness Rz of the side of the first resistive layer facing away from the first conductive layer is in the range of 0.1 μ ι η to 30 μ ι η.
3. The composite metal foil according to claim 1, wherein a roughness Sdr of a side of the first resistive layer remote from the first conductive layer ranges from 0.5% or more.
4. The composite metal foil according to claim 1, wherein all areas of a side of the first resistive layer facing away from the first conductive layer are provided with raised structures.
5. The composite metal foil according to claim 1, wherein at least a partial area of a side of the first resistive layer facing away from the first electrically conductive layer is provided with a plurality of continuous raised structures.
6. The composite metal foil according to claim 5, wherein all areas of the side of the first resistive layer facing away from the first conductive layer are provided with a plurality of continuous raised structures.
7. The composite metal foil according to claim 1, 4, 5 or 6, wherein the roughness Rz of the side of the first resistance layer facing away from the first conductive layer ranges from 0.1 μm to 10 μm, and the roughness Sdr of the side of the first resistance layer facing away from the first conductive layer ranges from 20% or more.
8. The composite metal foil according to claim 1, 4, 5 or 6, wherein the roughness Rz of the side of the first resistance layer facing away from the first conductive layer ranges from 0.1 μm to 10 μm, and the roughness Sdr of the side of the first resistance layer facing away from the first conductive layer ranges from 50% or more.
9. The composite metal foil according to claim 1, 4, 5 or 6, wherein the roughness Rz of the side of the first resistance layer facing away from the first conductive layer ranges from 0.1 μm to 10 μm, and the roughness Sdr of the side of the first resistance layer facing away from the first conductive layer ranges from 200% or more.
10. The composite metal foil of any one of claims 1-6, further comprising at least one dielectric layer disposed on a side of said first resistive layer remote from said first conductive layer and covering said raised structures.
11. The composite metal foil of claim 10, wherein a side of the dielectric layer remote from the first resistive layer is provided with a second resistive layer and a second conductive layer, the second resistive layer being located between the dielectric layer and the second conductive layer.
12. The composite metal foil as claimed in any one of claims 1 to 6, wherein the first resistive layer is made of nickel, chromium, platinum, palladium, titanium, nichrome, nickel-phosphorous alloy or chromium-silicon alloy.
13. The composite metal foil according to claim 12, wherein the first resistive layer is a single layer structure or at least a two layer structure.
14. A wiring board comprising the composite metal foil as claimed in any one of claims 1 to 13.
CN202022693989.2U 2020-11-19 2020-11-19 Composite metal foil and circuit board Active CN214205965U (en)