CN1743600A - Method for manufacturing bamboo lock-latch floor - Google Patents
Method for manufacturing bamboo lock-latch floor Download PDFInfo
- Publication number
- CN1743600A CN1743600A CN 200410054239 CN200410054239A CN1743600A CN 1743600 A CN1743600 A CN 1743600A CN 200410054239 CN200410054239 CN 200410054239 CN 200410054239 A CN200410054239 A CN 200410054239A CN 1743600 A CN1743600 A CN 1743600A
- Authority
- CN
- China
- Prior art keywords
- bamboo
- assembly group
- thin slice
- filament
- powder
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
This invention relates to a manufacturing method for bamboo made floors including boiling, steaming thin bamboo plates, thin threads and powder and processing them with mildewproof then baking, drying and matching them in many groups to be mixed evenly and spread for hot pressing under 130-150deg.C with 200-500kg/sqcm pressure for 25-35min to become blocks to be cut into floor bases of necessary diameters, then to be processed to a necessary lock catch tongue at one end face and a side face and a corresponding lock slot is processed on the other end face and side face to be ground and painted to get the bamboo lock catch floor.
Description
Technical field:
The present invention relates to a kind of manufacture method of Bamboo floor, particularly have the manufacture method of the Bamboo floor of snap close.
Background technology:
In existing technology, make the bamboo product and produce a large amount of leftover bits and pieces, for example bamboo thin slice, bamboo filament, bamboo powder, the way of handling mainly is to burn now, has both caused atmosphere pollution, wastes bamboo timber resource again, the structure of Bamboo floor is a bamboo chip tiling composite construction in addition, its tenon tongue-and-groove adopts rectangle or semicircular arc, and its main cause is that bamboo material fragility is bigger, adopts the structure of snap close to make the tongue-and-groove cracking cause the product waste when laying easily.The deficiency of the Bamboo floor of existing tenon tenon groove structure is expanding with heat and contract with cold through weather behind the floor covering layers, cause easily to produce the slit between the floor, and have the possibility of slippage, fix so the way of common employing is a nailing, take a lot of work, take material, increase and lay cost.
Summary of the invention:
The object of the present invention is to provide a kind of minimizing atmosphere pollution, make full use of bamboo timber resource, avoid tongue-and-groove cracking when laying, generation slit, floor effectively prevents to expand with heat and contract with cold, stop the possibility of slippage, lay simply, reduce the Bamboo floor of laying cost with snap close.
The technical scheme of the manufacture method of bamboo matter latch floor of the present invention comprises the following steps: 1. bamboo thin slice, bamboo filament, bamboo powder boiling mildew-resistant to be handled; 2. the bamboo thin slice after mildew-resistant being handled, bamboo filament, the baking of bamboo powder is dry handles, and makes water content reach 5%~10%, and preferably 7%; 3. according to the market demand situation, by weight percentage bamboo thin slice, bamboo filament, bamboo powder are done following multiple assembly:
Assembly group A: bamboo thin slice 25%~35%, preferably 30%, bamboo filament 25%~35%, preferably 30%, bamboo powder 30%~50%, preferably 40%;
Assembly group B: bamboo thin slice 35%~45%, preferably 40%, bamboo powder 55%~65%, preferably 60%;
Assembly group C: bamboo filament 35%~45%, preferably 40%, bamboo powder 55%~65%, preferably 60%;
Assembly group D: bamboo thin slice 45%~55%, preferably 50%, bamboo filament 45%~55%, preferably 50%;
Assembly group E: bamboo thin slice 100%;
Assembly group F: bamboo filament 100%;
Assembly group G: bamboo powder 100%.
4. with in the assembly group any one group stir after, impregnation reaches the glue saturation state; 5. the assembly group material behind the impregnation is paved enforcement hot pressing at the press platform, temperature is 130 ℃~150 ℃, preferably 140 ℃, pressure is every square centimeter 200 kilograms~500 kilograms, preferably 300 kilograms, insulation, pressurize 25 minutes~35 minutes preferably 30 minutes, are pressed into long 3.6 meters, wide 1.6 meters, thick 0.01~0.025 meter plate; 6. sawing becomes the floor blank of required size, processes the snap close tongue of required form in an end face and side, processes the lock buckling groove of relative shape in other end and another side; 7. sanding, paint promptly are bamboo matter latch floors.
1), the leftover bits and pieces that produces when utilizing the bamboo production beneficial effect of bamboo matter latch floor manufacture method of the present invention is:, avoid the burning of bamboo matter leftover bits and pieces, both reduced the pollution to environment, made full use of bamboo timber resource again; 2), adopt the method for impregnation hot pressing, the hardness and the toughness of ground slab integral greatly increase, and make Bamboo floor application lock buckle structure be achieved, and have avoided the slit that produces because of the variation of weather and the possibility of slippage, need not nailing during laying and fix, reduced the laying cost.
Description of drawings:
Fig. 1 is first kind of floor lock button structure that the manufacture method of bamboo matter latch floor of the present invention can realize;
Fig. 2 is second kind of floor lock button structure that the manufacture method of bamboo matter latch floor of the present invention can realize;
Fig. 3 is the third floor lock button structure that the manufacture method of bamboo matter latch floor of the present invention can realize;
Fig. 4 is the 4th kind of floor lock button structure that the manufacture method of bamboo matter latch floor of the present invention can realize.
The specific embodiment:
Below in conjunction with embodiment the present invention is further described:
Embodiment 1 selects assembly group A:
Bamboo thin slice, bamboo filament, bamboo powder boiling mildew-resistant are handled; Bamboo thin slice after the mildew-resistant processing, bamboo filament, the dry processing of bamboo powder baking are made water content reach at 5%~10% o'clock and can take out, and best water content is 7%; By weight percentage with bamboo thin slice 25%~35% preferably 30%, bamboo filament 25%~35% preferably 30%, bamboo powder 30%~50% preferably the 40% back impregnation that stirs reach the glue saturation state; Pave hot pressing at the press platform, temperature is 130 ℃~150 ℃ preferably 140 ℃, pressure is every square centimeter 200 kilograms~500 kilograms preferably 300 kilograms, insulation, pressurize 25 minutes~35 minutes preferably 30 minutes, be pressed into long 3.6 meters, wide 1.6 meters, thickness and can be 0.01~0.025 meter plate as required, sawing becomes the floor blank of required size then, process the snap close tongue of required form in an end face and side, process the lock buckling groove of relative shape in other end and another side; Sanding then, paint promptly are bamboo matter latch floors.
Embodiment 2 selects assembly group C:
Bamboo filament, bamboo powder boiling mildew-resistant are handled; With the bamboo filament after the mildew-resistant processing, the dry processing of bamboo powder baking, making water content reach at 5%~10% o'clock can take out, and optimum moisture content is 7%; By weight percentage with bamboo filament 35%~45% preferably 40%, bamboo powder 55%~65% preferably the 60% back impregnation that stirs reach the glue saturation state; Pave hot pressing at the press platform, temperature is 130 ℃~150 ℃ preferably 140 ℃, pressure is every square centimeter 200 kilograms~500 kilograms preferably 300 kilograms, insulation, pressurize 25 minutes~35 minutes preferably 30 minutes, be pressed into long 3.6 meters, wide 1.6 meters, thickness as required can be from 0.01~0.025 meter plate, sawing becomes the floor blank of required size then, process the snap close tongue of required form in an end face and side, process the lock buckling groove of relative shape in other end and another side; Sanding then, paint promptly are bamboo matter latch floors.
Embodiment 3 selects assembly group E:
Bamboo thin slice boiling mildew-resistant is handled; With dry processing of bamboo thin slice baking after the mildew-resistant processing, making water content reach 5%~10% can take out, and optimum moisture content is 7%; Bamboo thin slice impregnation is reached the glue saturation state; Pave hot pressing at the press platform, temperature is 130 ℃~150 ℃ preferably 140 ℃, pressure is every square centimeter 200 kilograms~500 kilograms preferably 300 kilograms, insulation, pressurize 25 minutes~35 minutes preferably 30 minutes, be pressed into long 3.6 meters, wide 1.6 meters, thickness as required can be from 0.01~0.025 meter plate, sawing becomes the floor blank of required size then, process the snap close tongue of required form in an end face and side, process the lock buckling groove of relative shape in other end and another side; Sanding then, paint promptly are bamboo matter latch floors.
Certainly as required, the manufacture method of bamboo matter latch floor of the present invention produce the thickness of bamboo matter latch floor can reach 0.06 meter, length can be selected in 0.6 meter~3.5 meters, width can be selected in 0.09 meter~0.3 meter.
Claims (7)
1. the manufacture method of a bamboo matter latch floor is characterized in that, it comprises the following steps: 1. bamboo thin slice, bamboo filament, bamboo powder boiling mildew-resistant to be handled; 2. the bamboo thin slice after mildew-resistant being handled, bamboo filament, the dry processing of bamboo powder baking make water content reach 5%~10%; 3. by weight percentage bamboo thin slice, bamboo filament, bamboo powder can be made following multiple assembly group as required:
Assembly group A: bamboo thin slice 25%~35%, bamboo filament 25%~35%, bamboo powder 30%~50%;
Assembly group B: bamboo thin slice 35%~45%, bamboo powder 55%~65%;
Assembly group C: bamboo filament 35%~45%, bamboo powder 55%~65%;
Assembly group D: bamboo thin slice 45%~55%, bamboo filament 45%~55%;
Assembly group E: bamboo thin slice 100%;
Assembly group F: bamboo filament 100%;
Assembly group G: bamboo powder 100%; 4. the back impregnation that any assembly group in the assembly stirred reaches the glue saturation state; 5. the assembly group material behind the impregnation is paved enforcement hot pressing at the press platform, temperature is 130 ℃~150 ℃, pressure is every square centimeter 200 kilograms~500 kilograms, and insulation, pressurize 25 minutes~35 minutes are pressed into long 3.6 meters, wide 1.6 meters, thick 0.01~0.025 meter plate; 6. sawing becomes the floor blank of required size, processes the snap close tongue of required form in an end face and side, processes the lock buckling groove of relative shape in other end and another side; 7. sanding, paint promptly are bamboo matter latch floors.
2. bamboo matter latch floor according to claim 1 is characterized in that: the water content after described bamboo thin slice, bamboo filament, the bamboo powder for drying is 7%.
3. bamboo matter latch floor according to claim 1 is characterized in that: described assembly group A is bamboo thin slice 30%, bamboo filament 30%, bamboo powder 40%.
4. bamboo matter latch floor according to claim 1 is characterized in that: described assembly group B is bamboo thin slice 40%, bamboo powder 60%.
5. bamboo matter latch floor according to claim 1 is characterized in that: described assembly group C is bamboo filament 40%, bamboo powder 60%.
6. bamboo matter latch floor according to claim 1 is characterized in that: described assembly group D is bamboo thin slice 50%, bamboo filament 50%.
7. bamboo matter latch floor according to claim 1 is characterized in that: described hot pressing temperature is 140 ℃, and pressure is 300 kilograms every square centimeter, insulation, pressurize 30 minutes.