CN1490152A - Preparing method for polyester sequin - Google Patents

Preparing method for polyester sequin Download PDF

Info

Publication number
CN1490152A
CN1490152A CNA031402267A CN03140226A CN1490152A CN 1490152 A CN1490152 A CN 1490152A CN A031402267 A CNA031402267 A CN A031402267A CN 03140226 A CN03140226 A CN 03140226A CN 1490152 A CN1490152 A CN 1490152A
Authority
CN
China
Prior art keywords
polyester film
vacuum
metallization processes
coating
polyester
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CNA031402267A
Other languages
Chinese (zh)
Inventor
李植来
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CNA031402267A priority Critical patent/CN1490152A/en
Publication of CN1490152A publication Critical patent/CN1490152A/en
Pending legal-status Critical Current

Abstract

A technology for preparing the nacreous square flaky particles of polyester includes such steps as pretreating raw material, vacuum plating, printing for coloring, high-temp fixing of color at 180-250 deg.C, longitudinal slitting, trasverse slicing, and sieving. Its advantages are simple technology, high productivity and quality of product and low cost.

Description

A kind of preparation method of polyester sequin
Technical field the present invention relates to be by division the plastic processing of the form of sheet, especially relates to a kind of preparation method of polyester sequin.
Background technology polyester sequin is to be formed through the precision cutting by the polyester film of the vacuum metallization processes of high-quality, its superficial layer coating is thermosetting paint, different color of all kinds can be provided, water and solvent there is anti-corrosion function, can resist 200 ℃ high temperature, has lasting glossiness, the polyester sequin has the size and shape of accurate control, pass silk screen and spray gun easily and do not produce choking phenomenon, therefore, the purposes of polyester sequin is quite extensive, comprise cosmetics, toy, red-letter day adornment, senior dress ornament, easy suit, embroidery, fringing, floriation and accessory etc., the polyester sequin can go out product miscellaneous and exhibit with the plastics type of mixing, and can also increase nail polish or powder, the color and luster of paste cosmetics and the attraction of toy.Screen painting merchant, advertiser and designer can consider to use the polyester sequin to gaze to attract the consumer.But the preparation method of existing polyester sequin still needs and further improves.
Summary of the invention is to remedy the defective that prior art exists, and the present invention proposes a kind of preparation method of polyester sequin.The technical scheme that adopts is as follows:
The preparation method of this polyester sequin is characterized in that pretreatment of raw material is arranged successively, vacuum coating, printing coating, high temperature fixation, rip cutting silk, transverse section and the operation of sieving:
The above-mentioned raw materials pretreatment process is, with the thickness of rolling be 15~75 microns polyester film to cut into width be 50~100 centimetres rolling polyester film, standby; Also paint composite is stirred and be mixed with oil-soluble chromium coating according to the percentage by weight of setting, standby.
Above-mentioned vacuum coating operation is, earlier the rolling polyester film inserted vacuum film coating chamber, and the limit is around film again, the limit evaporation, under vacuum condition with the even evaporation of metal set on polyester film, make the polyester film vacuum metallization processes.
The effect of this operation is can print color thereon after the polyester film vacuum metallization processes.
Above-mentioned printing painting process is the vacuum metallization processes polyester film to be delivered to printing machine, even coating 1~10 gram oil-soluble chromium coating every square metre vacuum metallization processes polyester film is two-sided.
Above-mentioned high temperature fixation operation is, with the vacuum metallization processes polyester film of dope dissolubility chromium coating, insert and carry out fixation treatment in the high temperature color-fixing device, high temperature color-fixing device temperature is 180~250 ℃, vacuum metallization processes polyester film fltting speed is 1~5 meter/minute, promptly the high temperature fixation treatment time of 1~5 meter vacuum metallization processes polyester film is 1 minute, the whole volume of last harvest.
This operation effect is, can make the coating that is coated on the vacuum metallization processes polyester film fit tightly top layer at aluminized mylar, acidproof, alkaline-resisting, sun-proof.
Above-mentioned rip cutting wire process is, to put in order the vacuum metallization processes polyester film of volume earlier repairs around film on membrane coiler, lie in a horizontal plane in again that pressurization makes it closely knit on the platform that is provided with the cutter sweep of the vertical lift pressing plate of cylinder interlock and accurate knife rest feeding Control Component, then, adjusting rip cutting silk width is the micron number magnitude, carry out the rip cutting silk, the whole vacuum metallization processes polyester film of rolling up is cut into thread vacuum metallization processes polyester film.
Above-mentioned transverse section operation is, earlier thread vacuum metallization processes polyester film is tied up bunchy, lie in a horizontal plane in again on the platform that is provided with the cutter sweep of the vertical lift pressing plate of cylinder interlock and accurate knife rest feeding Control Component, then, adjusting crosscut silk width equates with rip cutting silk width, also be the micron number magnitude, carry out the crosscut silk, make foursquare sheet-like particle.
Above-mentioned operation of sieving is, Manufactured foursquare sheet-like particle sieved, and promptly be even-grained goods, sieve mesh is 20~60.
The preparation method's of this polyester sequin further feature is:
In the pretreatment of raw material operation according to the percentage by weight of setting 35: 10: 1: 35 are mixed with oil-soluble chromium coating with paint composite blending oil, yellow powder, rouge and powder and the three-in-one stirring solvent of toluene-ethyl ester-butanols, standby.
The vacuum coating operation is vacuum aluminum-coated.
Sequin is that the length of side is 1~100 micron a square.
The sequin color is gold, silver color, orange, rose-colored, large red, aubergine, purple sieve blueness, royal blue, coffee color, green, grey, black and white.
The present invention's beneficial effect against existing technologies is, it is few to have a preparation section, and quality of item is good, production efficiency height, the advantage that input cost is low.The present invention adopts high temperature fixation operation, make the vacuum metallization processes polyester film under the high temperature of setting near fusion modification, oil-soluble chromium coating can fully permeate, acidproof especially, alkaline-resisting, sun-proof, and in preparation process, needn't add the lubricating oil and the water of White Mineral Oil one class, also correspondingly remove the operation of hyperthermia drying lubricating oil and water, both reduced energy resource consumption, shortened preparation time again.The polyester sequin cutter sweep that the inventive method adopts, being provided with vertical lift pressing plate and accurate knife rest feeding Control Component with cylinder interlock, can be 15~75 microns vacuum metallization processes polyester film precision with thickness, to cut into the length of side equably be 1~100 micron square reliably.
The preparation method of a kind of polyester sequin of the specific embodiment
The preparation method of this polyester sequin has pretreatment of raw material, vacuum coating, printing coating, high temperature fixation, rip cutting silk, transverse section and the operation of sieving successively:
The above-mentioned raw materials pretreatment process is, with the thickness of rolling be 50 microns polyester film to cut into width be 75 centimetres rolling polyester film, standby; Also according to the percentage by weight of setting 35: 10: 1: 35 are mixed with oil-soluble chromium coating with blending oil, yellow powder, rouge and powder and the three-in-one stirring solvent of toluene-ethyl ester-butanols, standby.
Above-mentioned vacuum coating operation is, earlier the rolling polyester film inserted vacuum film coating chamber, and the limit is around film again, the limit evaporation, under vacuum condition with the even evaporation of metallic aluminium set on polyester film is two-sided, make the polyester film vacuum metallization processes.
Above-mentioned printing painting process is the vacuum metallization processes polyester film to be delivered to printing machine, even coating 8 gram oil-soluble chromium coating every square metre vacuum metallization processes polyester film is two-sided.
Above-mentioned high temperature fixation operation is, with the vacuum metallization processes polyester film of dope dissolubility chromium coating, insert and carry out fixation treatment in the high temperature color-fixing device, high temperature color-fixing device temperature is 200 ℃, vacuum metallization processes polyester film fltting speed is 4 meters/minute, promptly the high temperature fixation treatment time of 4 meters vacuum metallization processes polyester films is 1 minute, the whole volume of last harvest.
Above-mentioned rip cutting wire process is, to put in order the vacuum metallization processes polyester film of volume earlier repairs around film on membrane coiler, lie in a horizontal plane in again that pressurization makes it closely knit on the platform that is provided with the cutter sweep of the vertical lift pressing plate of cylinder interlock and accurate knife rest feeding Control Component, then, adjusting rip cutting silk width is 10 microns, carry out the rip cutting silk, the whole vacuum metallization processes polyester film of rolling up is cut into thread vacuum metallization processes polyester film.
Above-mentioned transverse section operation is, earlier thread vacuum metallization processes polyester film is tied up bunchy, lie in a horizontal plane in again on the platform that is provided with the cutter sweep of the vertical lift pressing plate of cylinder interlock and accurate knife rest feeding Control Component, then, adjusting crosscut silk width equates with rip cutting silk width, also be 10 microns, carry out the crosscut silk, make foursquare sheet-like particle.
Above-mentioned operation of sieving is, Manufactured foursquare sheet-like particle sieved, and promptly be even-grained goods, sieve mesh is 60.
Sequin is that the length of side is 10 microns a square, and the sequin color is golden.

Claims (4)

1, a kind of preparation method of polyester sequin is characterized in that pretreatment of raw material is arranged successively, vacuum coating, printing coating, high temperature fixation, rip cutting silk, transverse section and the operation of sieving:
11 above-mentioned raw materials pretreatment process are, with the thickness of rolling is that to cut into width be 50~100 centimetres rolling polyester film for 15~75 microns polyester film, standby, also paint composite is stirred and be mixed with oil-soluble chromium coating according to the percentage by weight of setting, standby;
12 above-mentioned vacuum coating operations are, earlier the rolling polyester film are inserted vacuum film coating chamber, and the limit is around film again, the limit evaporation, under vacuum condition with the even evaporation of metal set on polyester film, make the polyester film vacuum metallization processes;
13 above-mentioned printing painting process are the vacuum metallization processes polyester film to be delivered to printing machine, even coating 1~10 gram oil-soluble chromium coating every square metre vacuum metallization processes polyester film is two-sided;
14 above-mentioned high temperature fixation operations are, with the vacuum metallization processes polyester film of dope dissolubility chromium coating, insert and carry out fixation treatment in the high temperature color-fixing device, high temperature color-fixing device temperature is 180~250 ℃, vacuum metallization processes polyester film fltting speed is 1~5 meter/minute, promptly the high temperature fixation treatment time of 1~5 meter vacuum metallization processes polyester film is 1 minute, the whole volume of last harvest;
15 above-mentioned rip cutting wire process are, to put in order the vacuum metallization processes polyester film of volume earlier repairs around film on membrane coiler, lie in a horizontal plane in again that pressurization makes it closely knit on the platform that is provided with the cutter sweep of the vertical lift pressing plate of cylinder interlock and accurate knife rest feeding Control Component, then, adjusting rip cutting silk width is the micron number magnitude, carry out the rip cutting silk, the whole vacuum metallization processes polyester film of rolling up is cut into thread vacuum metallization processes polyester film;
16 above-mentioned transverse section operations are, earlier thread vacuum metallization processes polyester film is tied up bunchy, lie in a horizontal plane in again on the platform that is provided with the cutter sweep of the vertical lift pressing plate of cylinder interlock and accurate knife rest feeding Control Component, then, adjusting crosscut silk width equates with rip cutting silk width, also be the micron number magnitude, carry out the crosscut silk, make foursquare sheet-like particle;
17 above-mentioned operations of sieving are, Manufactured foursquare sheet-like particle sieved, and promptly be even-grained goods, sieve mesh is 20~60.
2, the preparation method of polyester sequin as claimed in claim 1 is characterized in that in the pretreatment of raw material operation according to the percentage by weight of setting 35: 10: 1: 35 are mixed with oil-soluble chromium coating with paint composite blending oil, yellow powder, rouge and powder and the three-in-one stirring solvent of toluene-ethyl ester-butanols.
3, the preparation method of polyester sequin as claimed in claim 1 is characterized in that the vacuum coating operation is vacuum aluminum-coated.
4, the preparation method of polyester sequin as claimed in claim 1 is characterized in that sequin is that the length of side is 1~100 micron a square.
CNA031402267A 2003-08-18 2003-08-18 Preparing method for polyester sequin Pending CN1490152A (en)