CN115558382A - Simple and rapid construction floor paint and preparation method thereof - Google Patents
Simple and rapid construction floor paint and preparation method thereof Download PDFInfo
- Publication number
- CN115558382A CN115558382A CN202211278691.2A CN202211278691A CN115558382A CN 115558382 A CN115558382 A CN 115558382A CN 202211278691 A CN202211278691 A CN 202211278691A CN 115558382 A CN115558382 A CN 115558382A
- Authority
- CN
- China
- Prior art keywords
- component
- agent
- resin
- viscosity
- floor paint
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention relates to a simple and rapid construction floor paint and a preparation method thereof, wherein the simple and rapid construction floor paint comprises a component A and a component B in parts by weight: the component A comprises: 15-25% of solvent-free low-viscosity resin bisphenol F epoxy resin, 15-25% of medium-viscosity resin bisphenol A epoxy resin, 5-15% of reactive diluent, 0.3-0.7% of viscosity-reducing dispersing wetting agent, 0.15-0.25% of flatting agent, 0.2-0.4% of quick defoaming agent, 34-44% of low-oil-absorption filler, 0.4-0.8% of anti-settling additive, 8-10% of resin color paste and 0.2-0.6% of anti-scratching additive; and B component: 20 to 28 percent of modified fatty amine curing agent and 0.5 to 1.5 percent of curing accelerator. The floor paint solves the problems that the existing floor paint is complicated in construction process, consumes working hours, consumes financial resources and consumes labor, is efficient in construction, simplifies working procedures, and reduces or does not increase cost.
Description
Technical Field
The invention relates to the technical field of floor paint, in particular to simple and rapid construction floor paint and a preparation method thereof.
Background
The prior epoxy floor paint, polyurethane floor paint and other types of resin paints comprise three materials of priming paint, intermediate coat and finishing paint in the construction process, wherein the priming paint plays roles in permeating and reinforcing a foundation, sealing sand holes, cracks and the like of the foundation, and a common concrete foundation generally needs to be constructed for 2-3 times. The floating coat has the functions of increasing the thickness, repairing pot holes, leveling the ground and increasing the compressive strength, and the common concrete foundation generally needs to be constructed for 2-4 times after the floating coat is mixed with quartz sand or powder.
The finish paint has the functions of color decoration effect, surface purification, water and oil resistance and the like, and the common foundation construction 2 is more than the whole. Therefore, the existing floor paint construction process is complicated, consumes working hours, consumes financial resources and labor, is efficient in construction, simplifies the working procedures, reduces or does not increase the cost of the construction process, and needs a simple and rapid floor paint.
Disclosure of Invention
Aiming at the defects in the prior art, the invention aims to provide a simple and rapid floor paint and a preparation method thereof, which solve the problems of complicated construction process, time consumption, financial consumption and labor consumption of the traditional floor paint, realize efficient construction, simplify the working procedures and reduce or not increase the cost.
The above object of the present invention is achieved by the following technical solutions:
the utility model provides a simple and easy quick construction floor paint, includes A component and B component according to the part by weight, its characterized in that:
the component A comprises: 15-25% of solvent-free low-viscosity resin bisphenol F epoxy resin, 15-25% of medium-viscosity resin bisphenol A epoxy resin, 5-15% of active diluent, 0.3-0.7% of viscosity-reducing dispersing wetting agent, 0.15-0.25% of flatting agent, 0.2-0.4% of quick defoaming agent, 34-44% of low-oil-absorption filler, 0.4-0.8% of anti-settling auxiliary agent, 8-10% of resin color paste and 0.2-0.6% of anti-scratching auxiliary agent;
and B component: 20 to 28 percent of modified fatty amine curing agent and 0.5 to 1.5 percent of curing accelerator.
The present invention in a preferred example may be further configured to: the component A comprises: 20% of solvent-free low-viscosity resin bisphenol F epoxy resin, 20% of medium-viscosity resin bisphenol A epoxy resin, 10% of active diluent, 0.5% of viscosity-reducing dispersing wetting agent, 0.2% of flatting agent, 0.3% of quick defoaming agent, 39% of low-oil-absorption filler, 0.6% of anti-settling auxiliary agent, 9% of resin color paste and 0.4% of scratch-resistant auxiliary agent;
and B component: 24 percent of modified fatty amine curing agent and 1 percent of curing accelerator.
The invention in a preferred example may be further configured to: the weight part ratio of the component A to the component B is A: b = 4.
The present invention in a preferred example may be further configured to: the filler is one or more of barium sulfate and silicon micropowder.
The present invention in a preferred example may be further configured to: the resin color paste contains 50% of resin by weight.
A preparation method of simple and rapid construction floor paint comprises the following steps:
step S1, preparation of a component A: adding solvent-free low-viscosity resin bisphenol F epoxy resin, medium-viscosity resin bisphenol A epoxy resin, an active diluent, a viscosity-reducing dispersing wetting agent, a leveling agent, a quick defoaming agent, a low-oil-absorption filler, an anti-settling auxiliary agent, a resin color paste and a scratch-resistant auxiliary agent into a reaction kettle according to a proportion, fully mixing and stirring, and filtering for later use after uniformly stirring;
step S2, preparation of a component B: mixing the modified aliphatic amine curing agent and the curing accelerator together according to a proportion, uniformly stirring, and standing for 10min;
step S3, when in use, the component A and the component B are mixed according to the proportion A: and B =4, the simple and rapid construction floor paint can be obtained after uniformly mixing and stirring the components in the ratio of 1.
In summary, the present invention includes at least one of the following beneficial effects:
the simple and rapid-construction floor paint disclosed by the invention can be directly coated on the common ground, still has a glossy surface effect, and is high in bonding strength and compressive strength. The film-forming paint surface obtained after the curing of the modified aliphatic amine curing agent reaches the national standard of the terrace, has the characteristics of high hardness, scratch resistance, high leveling degree and the like, and is manufactured by adopting non-toxic ingredients.
Detailed Description
The technical scheme in the embodiment of the application will be clearly and completely described below; it is obvious that the described embodiments are only a part of the embodiments of the present application, and not all embodiments, and all other embodiments obtained by those of ordinary skill in the art without any inventive work based on the embodiments in the present application belong to the protection scope of the present application.
The solvent-free low-viscosity resin bisphenol F epoxy resin and the medium-viscosity resin bisphenol A epoxy resin are bisphenol F epoxy resin and bisphenol A epoxy resin disclosed in the invention patent with the application number of CN201610671139.8, belong to the prior art, are not described herein, and improve the high temperature resistance, the corrosion resistance and the mechanical property of the two-component epoxy resin coating.
The modified aliphatic amine curing agent plays a role in curing the solvent-free low-viscosity resin bisphenol F epoxy resin and the medium-viscosity resin bisphenol A epoxy resin, improves the mechanical properties, heat resistance, water resistance, corrosion resistance and the like of the coating, belongs to the prior art, and is not described herein any more.
The resin color paste disclosed in the invention patent with the application number of CN201610344718.1 belongs to the prior art, and is not described herein, and isooctanol in the resin color paste has a boiling point as high as 185-189 ℃, and has a boiling point much higher than that of other solvents. In the production process of the resin color paste, the reaction temperature is about 100 ℃ generally. Isooctanol is selected as a solvent, and the characteristic of high boiling point of the isooctanol is utilized, so that the isooctanol is not easy to volatilize in the production process, the loss is reduced, and the isooctanol is safe and environment-friendly; meanwhile, isooctanol also has the function of anticorrosion, and the anticorrosion effect of the coating is improved.
The first embodiment is as follows:
the invention discloses a simple and rapid construction floor paint which comprises a component A and a component B in parts by weight:
the component A comprises: 15-25% of solvent-free low-viscosity resin bisphenol F epoxy resin, 15-25% of medium-viscosity resin bisphenol A epoxy resin, 5-15% of active diluent, 0.3-0.7% of viscosity-reducing dispersing wetting agent, 0.15-0.25% of flatting agent, 0.2-0.4% of quick defoaming agent, 34-44% of low-oil-absorption filler, 0.4-0.8% of anti-settling auxiliary agent, 8-10% of resin color paste and 0.2-0.6% of anti-scratching auxiliary agent; and the component B comprises: 20 to 28 percent of modified fatty amine curing agent and 0.5 to 1.5 percent of curing accelerator.
The weight portion ratio of the component A to the component B is A: b =4, the filler is one or more of barium sulfate and silicon micropowder, and the resin color paste contains 50% of resin by weight.
Example two:
the invention discloses a preparation method of simple and rapid construction floor paint, which comprises the following steps:
step S1, preparation of a component A: 5% of solvent-free low-viscosity resin bisphenol F epoxy resin, 15% of medium-viscosity resin bisphenol A epoxy resin, 5% of active diluent, 0.3% of viscosity-reducing dispersing wetting agent, 0.15% of flatting agent, 0.2% of quick defoaming agent, 34% of low-oil-absorption filler, 0.4% of anti-settling auxiliary agent, 8% of resin color paste and 0.2% of scratch-resistant auxiliary agent are added into a reaction kettle according to a proportion, fully mixed and stirred, and filtered for later use after being uniformly stirred;
step S2, preparation of a component B: mixing 20% of modified fatty amine curing agent and 0.5% of curing accelerator together according to a proportion, uniformly stirring, and standing for 10min;
step S3, when in use, the component A and the component B are mixed according to the proportion A: b =4, after being mixed and stirred uniformly, the simple and rapid construction floor paint coating can be obtained. Wherein, the filling material is one or more of barium sulfate and silicon micropowder, and the resin color paste contains 50 percent of resin by weight.
Example three:
the invention discloses a preparation method of simple and rapid construction floor paint, which comprises the following steps:
step S1, preparation of a component A: 25 percent of solvent-free low-viscosity resin bisphenol F epoxy resin, 25 percent of medium-viscosity resin bisphenol A epoxy resin, 15 percent of active diluent, 0.7 percent of viscosity-reducing dispersing wetting agent, 0.25 percent of flatting agent, 0.4 percent of quick defoaming agent, 44 percent of low-oil-absorption filler, 0.8 percent of anti-settling auxiliary agent, 10 percent of resin color paste and 0.6 percent of scratch-resistant auxiliary agent are added into a reaction kettle according to the proportion and are fully mixed and stirred, and the mixture is filtered for standby application after being uniformly stirred;
step S2, preparation of a component B: mixing 28% of modified fatty amine curing agent and 1.5% of curing accelerator according to a proportion, uniformly stirring, and standing for 10min;
step S3, when in use, the component A and the component B are mixed according to the proportion A: and B =4, the simple and rapid construction floor paint can be obtained after uniformly mixing and stirring the components in the ratio of 1. Wherein, the filling material is one or more of barium sulfate and silicon micropowder, and the resin color paste contains 50 percent of resin by weight.
Example four:
the invention discloses a preparation method of simple and rapid construction floor paint, which comprises the following steps:
step S1, preparation of a component A: 20 percent of solvent-free low-viscosity resin bisphenol F epoxy resin, 20 percent of medium-viscosity resin bisphenol A epoxy resin, 10 percent of active diluent, 0.5 percent of viscosity-reducing dispersing wetting agent, 0.2 percent of flatting agent, 0.3 percent of quick defoaming agent, 39 percent of low-oil-absorption filler, 0.6 percent of anti-settling auxiliary agent, 9 percent of resin color paste and 0.4 percent of scratch-resistant auxiliary agent are added into a reaction kettle according to the proportion and are fully mixed and stirred, and the mixture is filtered for standby after being uniformly stirred;
step S2, preparation of a component B: mixing 24% of modified aliphatic amine curing agent and 1% of curing accelerator together according to a proportion, uniformly stirring and standing for 10min;
step S3, when in use, the component A and the component B are mixed according to the proportion A: and B =4, the simple and rapid construction floor paint can be obtained after uniformly mixing and stirring the components in the ratio of 1. Wherein, the filling material is one or more of barium sulfate and silicon micropowder, and the resin color paste contains 50 percent of resin by weight.
The test is carried out according to a floor paint test method GB/T22374-2008 floor coating material floor part, and the experimental result of the invention is as follows:
the implementation principle of the embodiment is as follows: the simple and rapid-construction floor paint disclosed by the invention can be directly coated on the common ground, still has a glossy surface effect, and is high in bonding strength and compressive strength. The film-forming paint surface after being cured by the modified aliphatic amine curing agent reaches the national standard of a floor, has the characteristics of high hardness, scratch resistance, high leveling degree and the like, and is manufactured by adopting non-toxic ingredients.
The embodiments of the present invention are all preferred embodiments of the present invention, and the scope of the present invention is not limited thereby, so: all equivalent changes made according to the structure, shape and principle of the invention are covered by the protection scope of the invention.
Claims (6)
1. The utility model provides a floor paint simply constructs fast, includes A component and B component according to the part by weight, its characterized in that:
the component A comprises: 15-25% of solvent-free low-viscosity resin bisphenol F epoxy resin, 15-25% of medium-viscosity resin bisphenol A epoxy resin, 5-15% of reactive diluent, 0.3-0.7% of viscosity-reducing dispersing wetting agent, 0.15-0.25% of flatting agent, 0.2-0.4% of quick defoaming agent, 34-44% of low-oil-absorption filler, 0.4-0.8% of anti-settling additive, 8-10% of resin color paste and 0.2-0.6% of anti-scratching additive;
and B component: 20 to 28 percent of modified fatty amine curing agent and 0.5 to 1.5 percent of curing accelerator.
2. The simple and rapid construction floor paint according to claim 1, characterized in that the component A: 20% of solvent-free low-viscosity resin bisphenol F epoxy resin, 20% of medium-viscosity resin bisphenol A epoxy resin, 10% of active diluent, 0.5% of viscosity-reducing dispersing wetting agent, 0.2% of flatting agent, 0.3% of quick defoaming agent, 39% of low-oil-absorption filler, 0.6% of anti-settling auxiliary agent, 9% of resin color paste and 0.4% of scratch-resistant auxiliary agent;
and the component B comprises: 24 percent of modified fatty amine curing agent and 1 percent of curing accelerator.
3. The simple and rapid construction floor paint as claimed in any one of claims 1 or 2, wherein the weight part ratio of the component A to the component B is A: b = 4.
4. The simple and rapid construction floor paint according to claim 1, wherein the filler is one or more of barium sulfate and silica micropowder.
5. The simple and rapid construction floor paint and the preparation method thereof as claimed in claim 1, wherein the resin color paste contains 50% by weight of resin.
6. The preparation method of the simple and rapid construction floor paint according to any one of claims 1 to 5, characterized by comprising the following steps:
step S1, preparation of a component A: adding solvent-free low-viscosity resin bisphenol F epoxy resin, medium-viscosity resin bisphenol A epoxy resin, an active diluent, a viscosity-reducing dispersing wetting agent, a leveling agent, a quick defoaming agent, a low-oil-absorption filler, an anti-settling auxiliary agent, a resin color paste and a scratch-resistant auxiliary agent into a reaction kettle according to a proportion, fully mixing and stirring, and filtering for later use after uniformly stirring;
step S2, preparation of a component B: mixing the modified aliphatic amine curing agent and the curing accelerator together according to a proportion, uniformly stirring, and standing for 10min;
step S3, when in use, the component A and the component B are mixed according to the proportion A: b =4, after being mixed and stirred uniformly, the simple and rapid construction floor paint coating can be obtained.