China
Prior art keywords
quartz sand
treatment
magnetic separation
sand
meshes
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201911073472.9A
Other languages
Chinese (zh)
Other versions
CN110976071B (en
Inventor
钟森林
梁焘茂
吴城材
张超达
谢宝华
徐晓衣
王丰雨
王丽娟
许丽敏
陈俊明
陈龙
王威
周庆红
蔡绍波
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangzhou Yueyou Academy Mineral Resource Technology Co ltd
Institute Of Resources Comprehensive Utilization Guangdong Academy Of Sciences
Institute of Resource Utilization and Rare Earth Development of Guangdong Academy of Sciences
Original Assignee
Guangzhou Yueyou Academy Mineral Resource Technology Co ltd
Guangdong Institute of Resources Comprehensive Utilization
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangzhou Yueyou Academy Mineral Resource Technology Co ltd, Guangdong Institute of Resources Comprehensive Utilization filed Critical Guangzhou Yueyou Academy Mineral Resource Technology Co ltd
Priority to CN201911073472.9A priority Critical patent/CN110976071B/en
Publication of CN110976071A publication Critical patent/CN110976071A/en
Application granted granted Critical
Publication of CN110976071B publication Critical patent/CN110976071B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Links

Images

Classifications

    • BPERFORMING OPERATIONS; TRANSPORTING
    • B03SEPARATION OF SOLID MATERIALS USING LIQUIDS OR USING PNEUMATIC TABLES OR JIGS; MAGNETIC OR ELECTROSTATIC SEPARATION OF SOLID MATERIALS FROM SOLID MATERIALS OR FLUIDS; SEPARATION BY HIGH-VOLTAGE ELECTRIC FIELDS
    • B03BSEPARATING SOLID MATERIALS USING LIQUIDS OR USING PNEUMATIC TABLES OR JIGS
    • B03B9/00General arrangement of separating plant, e.g. flow sheets

Abstract

The invention discloses a method for purifying and processing quartz sand for a petroleum fracturing propping agent, which comprises the following steps: s100, carrying out classified screening and impurity filtering treatment on the natural quartz sand raw material to obtain a natural quartz sand crude product; s200, scrubbing the natural quartz sand coarse product subjected to classified screening and impurity filtering treatment; s300, carrying out graded desliming treatment on the natural quartz sand coarse product after scrubbing treatment; s400, reselecting the natural quartz sand crude product subjected to graded desliming treatment to obtain quartz refined sand; s500, carrying out magnetic separation and impurity removal on the quartz refined sand obtained after the gravity separation to obtain quartz sand high-intensity magnetic separation tailings; s600, carrying out color separation or flotation treatment on the quartz sand high-intensity magnetic separation tailings obtained after the impurities are removed through magnetic separation, so that various impurities in the quartz sand can be completely and completely removed, and the service performance of the quartz sand as a fracturing propping agent is ensured. And screening the product to obtain quartz sand finished products for qualified fracturing propping agents with different grain sizes.

Description

Quartz sand purification processing method for petroleum fracturing propping agent
Technical Field
The invention relates to the technical field of mineral purification, in particular to a method for purifying and processing quartz sand for a petroleum fracturing propping agent.
Background
With the rapid development of national economy, the demand of various industries on petroleum is increasing day by day, and for low-permeability oil fields, the water conservancy fracturing technology becomes an important technical measure for promoting permeability and increasing yield. In the operation of using the hydraulic fracturing technology, the fracturing propping agent plays an important role because of the functions of enhancing the oil guiding capacity of the stratum, increasing the oil drainage area, improving the permeability of the stratum and the like.
At present, the main types of fracturing propping agents are roughly classified into quartz sand, resin sand, ceramsite and the like, and the quartz sand is widely used due to high quality and low price, and becomes the fracturing propping agent material with the largest use amount. The quartz sand for fracturing propping agents is usually prepared by screening and purifying natural quartz sand, and the natural quartz sand raw material often contains various impurities, such as fine mud, iron ore, feldspar, mica, rock debris and the like, which can affect the service performance of the quartz sand, so that the impurities need to be removed. However, the existing purification and impurity removal methods still stay in the simple washing treatment process, and various impurities mixed in the quartz sand cannot be effectively removed, so that the quartz sand product cannot meet the use performance index requirements of the fracturing propping agent.
Disclosure of Invention
Therefore, the invention needs to provide a method for purifying and processing quartz sand for a petroleum fracturing propping agent, and aims to solve the problem that impurities in the quartz sand cannot be effectively removed in the prior art, so that the service performance of the quartz sand as the fracturing propping agent is poor.
The technical scheme is as follows:
a method for purifying and processing quartz sand for petroleum fracturing propping agent comprises the following steps:
s100, carrying out classified screening and impurity filtering treatment on the natural quartz sand raw material to obtain a natural quartz sand crude product;
s200, scrubbing the natural quartz sand coarse product subjected to classified screening and impurity filtering treatment;
s300, carrying out graded desliming treatment on the natural quartz sand coarse product after scrubbing treatment;
s400, reselecting the natural quartz sand crude product subjected to graded desliming treatment to obtain quartz refined sand;
s500, carrying out magnetic separation and impurity removal on the quartz refined sand obtained after the gravity separation to obtain quartz sand high-intensity magnetic separation tailings;
s600, carrying out color separation or flotation treatment on the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal to obtain a quartz sand finished product for the petroleum fracturing propping agent.
The method for purifying and processing the quartz sand for the petroleum fracturing propping agent is mainly used for removing impurities and purifying the quartz sand serving as the fracturing propping agent so as to remove various impurities in the quartz sand. Specifically, firstly, natural quartz sand raw materials are subjected to classified screening and impurity filtering treatment to remove large gravels, fine sand and soil; then, scrubbing the crude product of the natural quartz sand, and further dissociating to remove fine mud and iron impurities adhered to the surface of the quartz sand; then, carrying out graded desliming treatment on the crude product of the natural quartz sand, and further removing fine mud and wastewater mixed in the crude product of the natural quartz sand to obtain cleaner quartz sand; and then reselecting the quartz sand, thereby removing the heavy mineral impurities, and obtaining the quartz refined sand. Then, carrying out magnetic separation and impurity removal treatment on the quartz refined sand, thereby further removing the included strong magnetic minerals and weak magnetic minerals and obtaining the quartz sand strong magnetic tailings; and finally, performing color separation or flotation treatment on the quartz sand high-intensity magnetic separation tailings, so that low-intensity mineral impurities such as feldspar, rock debris and the like which are mixed can be removed, thus obtaining a quartz sand finished product with the breakage rate meeting the requirements of the fracturing propping agent, ensuring that all impurities in the quartz sand are removed cleanly and thoroughly, ensuring the service performance of the quartz sand as the fracturing propping agent, and improving the permeability and yield increasing capability of the hydraulic fracturing technology in a low-permeability oil field.
The technical solution of the present application is further described below:
in one embodiment, in the step S100 of performing classified screening and impurity filtering on the natural quartz sand raw material, the natural quartz sand raw material is firstly passed through a 10-mesh sieve to filter out large gravels, so as to complete primary filtration; and then, fine sand and soil are further filtered by a sieve of 20 meshes to 140 meshes, and secondary filtration is completed.
In one embodiment, in the step S200, in the scrubbing treatment of the coarse natural quartz sand product after the classifying, screening and impurity filtering treatment, the raw natural quartz sand material is put into a scrubbing machine for pulping and scrubbing, so that fine mud and iron impurities on the surface of the raw natural quartz sand material are dissociated; wherein the scrubbing concentration is 50-70%, and the scrubbing time is 5-20 min.
In one embodiment, in the step S400, the natural quartz sand coarse product after the graded desliming treatment is reselected, specifically, the natural quartz sand coarse product is put into a spiral chute, heavy minerals are separated from quartz sand by the action of gravity and centrifugal force of a rotational flow, and the heavy minerals are directly discharged to obtain quartz concentrate.
In one embodiment, in the step S500, magnetic separation and impurity removal are performed on the quartz refined sand obtained after heavy separation, specifically, a low-intensity magnetic separator is firstly used to perform a first separation treatment on the quartz refined sand to remove strong magnetic minerals; and then, carrying out secondary sorting treatment on the quartz refined sand by using a strong magnetic separator to remove weakly magnetic minerals so as to obtain the quartz sand strong magnetic separation tailings.
In one embodiment, in the step S600, in the flotation treatment of the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal, the quartz sand high-intensity magnetic separation tailings are put into a flotation machine, and meanwhile, a collecting agent and an inhibitor are added into ore pulp, and low-intensity impurity minerals such as feldspar and rock debris are removed by a reverse flotation method, so that a quartz sand finished product with qualified breakage rate is obtained; the collector is prepared from a collector A and a collector B according to the mass ratio of 1.0: 0.5-3.0, and the amount is 500-2000 g/t; the collector A can be at least one of lauryl amine and coconut alkyl primary amine, and the collector B can be at least one of sodium petroleum sulfonate, sodium dodecyl sulfonate and sodium oleate; the inhibitor is sodium hexametaphosphate, and the amount of the inhibitor is 0-100 g/t; the pH value of the ore pulp is 2-3.
In one embodiment, in the step S600, in the color separation treatment of the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal, the quartz sand high-intensity magnetic separation tailings are firstly dehydrated and dried, and then the dried quartz sand high-intensity magnetic separation tailings are put into a color separator for separation treatment.
In one embodiment, in the step S600, after the quartz sand high-intensity magnetic separation tailings subjected to magnetic separation and impurity removal are subjected to color separation treatment to obtain a finished quartz sand product, the method further comprises screening the finished quartz sand product to obtain products with different particle sizes, such as 10-20 meshes, 20-40 meshes, 30-50 meshes, 40-60 meshes, 50-70 meshes, 70-140 meshes, and the like; or, after the step S600, performing flotation treatment on the quartz sand high-intensity magnetic separation tailings subjected to magnetic separation and impurity removal to obtain a quartz sand finished product, and then screening, dehydrating and drying the quartz sand finished product to obtain products with different particle sizes of 10-20 meshes, 20-40 meshes, 30-50 meshes, 40-60 meshes, 50-70 meshes, 70-140 meshes and the like.
Drawings
Fig. 1 is a flow chart of process steps of a method for purifying and processing quartz sand for a petroleum fracturing proppant according to an embodiment of the invention.
Detailed Description
In order to make the objects, technical solutions and advantages of the present invention more apparent, the present invention is further described in detail below with reference to the accompanying drawings and the detailed description. It should be understood that the detailed description and specific examples, while indicating the scope of the invention, are intended for purposes of illustration only and are not intended to limit the scope of the invention.
It will be understood that when an element is referred to as being "secured to," "disposed on" or "disposed on" another element, it can be directly on the other element or intervening elements may also be present. When an element is referred to as being "connected" to another element, it can be directly connected to the other element or intervening elements may also be present; the specific manner of fixedly connecting one element to another element can be implemented by the prior art, and will not be described herein, and preferably, a screw-threaded connection is used.
Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. As used herein, the term "and/or" includes any and all combinations of one or more of the associated listed items.
As shown in fig. 1, a process flow chart of a method for purifying and processing quartz sand for a petroleum fracturing proppant shown in an embodiment of the present application specifically includes the following steps:
s100, carrying out classified screening and impurity filtering treatment on the natural quartz sand raw material to obtain a natural quartz sand crude product;
s200, scrubbing the natural quartz sand coarse product subjected to classified screening and impurity filtering treatment;
s300, carrying out graded desliming treatment on the natural quartz sand coarse product after scrubbing treatment;
s400, reselecting the natural quartz sand crude product subjected to graded desliming treatment to obtain quartz refined sand;
s500, carrying out magnetic separation and impurity removal on the quartz refined sand obtained after the gravity separation to obtain quartz sand high-intensity magnetic separation tailings;
s600, carrying out color separation or flotation treatment on the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal to obtain a qualified quartz sand finished product for the fracturing propping agent.
The method for purifying and processing the quartz sand for the petroleum fracturing propping agent is mainly used for removing impurities and purifying the quartz sand serving as the fracturing propping agent so as to remove various impurities in the quartz sand. Specifically, firstly, natural quartz sand raw materials are subjected to classified screening and impurity filtering treatment to remove large gravels, fine sand and soil; then, scrubbing the crude product of the natural quartz sand, and further dissociating to remove fine mud and iron impurities adhered to the surface of the quartz sand; then, carrying out graded desliming treatment on the crude product of the natural quartz sand, and further removing fine mud and wastewater mixed in the crude product of the natural quartz sand to obtain cleaner quartz sand; and then reselecting the quartz sand, thereby removing heavy mineral impurities and obtaining the quartz fine sand. Then, carrying out magnetic separation and impurity removal treatment on the quartz refined sand, thereby further removing the included strong magnetic minerals and weak magnetic minerals and obtaining the quartz sand strong magnetic tailings; and finally, performing color separation or flotation treatment on the quartz sand high-intensity magnetic separation tailings, so that low-intensity mineral impurities such as feldspar, rock debris and the like which are mixed can be removed, the clean and thorough removal of various impurities in the quartz sand can be ensured, the service performance of the quartz sand as a fracturing propping agent is ensured, a quartz sand finished product with the breakage rate meeting the requirement of the fracturing propping agent is obtained, and the capability of promoting the permeability and increasing the yield of a hydraulic fracturing technology in a low-permeability oil field is improved.
It should be noted that the raw material of the natural quartz sand of the present invention is a natural quartz sand formed through weathering, transportation, erosion, etc., wherein the particles of the natural quartz sand are round and have a smaller particle size than those of general quartz rock ores, and according to the geological conditions of the area, impurities such as large gravel, soil, iron impurities, feldspar, rock debris, etc. are included in the quartz sand, so that an effective filtering and purifying process method needs to be adopted to specifically remove the above-mentioned various impurities in the quartz sand to ensure the purifying effect.
Specifically, in one embodiment, in the step S100, the natural quartz sand raw material is subjected to classification screening and impurity filtering treatment to obtain a natural quartz sand crude product, and the natural quartz sand raw material is first filtered through a 10-mesh screen to remove large gravels, thereby completing primary filtration; and then, fine sand and soil are further filtered by a sieve of 20 meshes to 140 meshes, and secondary filtration is completed. Therefore, large gravels, small-particle-size gravels and soil in the natural quartz sand raw material can be removed in sequence in a grading and screening mode.
It should be noted that, depending on the structure and the particle size of the raw material of the natural quartz sand, other mesh screens may be used for the classified filtration in other embodiments, and all of them are within the protection scope of the present application.
In the step S200, in the scrubbing treatment of the coarse natural quartz sand product after the grading screening and impurity filtering treatment, the coarse natural quartz sand product is put into a scrubbing machine for pulping and scrubbing, so that fine mud and iron impurities on the surface of the coarse natural quartz sand product are dissociated; wherein the scrubbing concentration is 50-70%, and the scrubbing time is 5-20 min. It can be understood that the scrubbing machine has the effects that through stirring, the mutual friction among the quartz sand particles, the side wall of the machine body and the quartz sand particles can achieve high-frequency and multiple scrubbing, stubborn fine mud and iron impurities adhered to the surfaces of the quartz sand particles can be effectively scrubbed, fallen and removed, and further, a natural quartz sand coarse product with a clean appearance is obtained. Preferably, the scouring concentration of pulping and scouring the crude product of the natural quartz sand is 60%, and the scouring time is 10 min. Under the condition, the quartz sand is scrubbed, so that the scrubbing effect and the scrubbing efficiency can be considered, and the economic efficiency of the purification operation is improved.
In the step S400, the natural quartz sand coarse product after the graded desliming treatment is reselected, specifically, the natural quartz sand coarse product is put into a spiral chute, heavy minerals are separated from the quartz sand by the action of gravity and centrifugal force of a rotational flow, and the heavy minerals are directly discharged to obtain quartz refined sand. Through adopting the spiral chute to handle quartz sand, can effectively get rid of all kinds of heavy mineral impurity.
In addition, in the step S500, magnetic separation and impurity removal are performed on the quartz refined sand obtained after heavy separation, specifically, a low-intensity magnetic separator is firstly adopted to perform primary separation treatment on the quartz refined sand, so as to remove strong-magnetic minerals; and then, carrying out secondary sorting treatment on the quartz refined sand by using a strong magnetic separator to remove weakly magnetic minerals so as to obtain the quartz sand strong magnetic separation tailings. Therefore, the strong magnetic mineral impurities and the weak magnetic mineral impurities can be removed in a targeted manner through the weak magnetic separator and the strong magnetic separator, the impurity content in the quartz sand is greatly reduced, and the performance of the quartz sand as a fracturing propping agent is improved.
In the step S600, in the flotation treatment of the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal, the quartz sand high-intensity magnetic separation tailings are put into a flotation machine, a collecting combined agent and an inhibitor are added into ore pulp, and low-strength impurity minerals such as feldspar and rock debris are removed by a reverse flotation method to obtain a quartz sand finished product with qualified breakage rate; the collecting combined agent is prepared from a collecting agent A and a collecting agent B according to the mass ratio of 1.0: 0.5-3.0, and the amount is 500-2000 g/t; the collector A can be at least one of lauryl amine and coconut alkyl primary amine, and the collector B can be at least one of sodium petroleum sulfonate, sodium dodecyl sulfonate and sodium oleate; the inhibitor is sodium hexametaphosphate, and the amount of the inhibitor is 0-100 g/t; the PH of the ore pulp is 2-3.
In the step S600, in the color separation treatment of the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal, the quartz sand high-intensity magnetic separation tailings are firstly dehydrated and dried, and then the dried quartz sand high-intensity magnetic separation tailings are put into a color separator for separation treatment.
In addition, on the basis of any of the above embodiments, after the step S600, performing color separation treatment on the quartz sand high-intensity magnetic separation tailings subjected to magnetic separation and impurity removal to obtain a quartz sand finished product, screening the quartz sand finished product to obtain products with different particle sizes, such as 10-20 meshes, 20-40 meshes, 30-50 meshes, 40-60 meshes, 50-70 meshes, 70-140 meshes, and the like; or, in the step S600, after the quartz sand strong magnetic separation tailings subjected to the magnetic separation and impurity removal are subjected to flotation treatment to obtain a quartz sand finished product, the method further comprises the steps of screening and dehydrating the quartz sand finished product, and drying the quartz sand finished product to obtain products with different particle sizes, such as 10-20 meshes, 20-40 meshes, 30-50 meshes, 40-60 meshes, 50-70 meshes, 70-140 meshes and the like. Therefore, through sorting and screening, the qualified quartz sand for the fracturing propping agent with different grain sizes can be obtained, and the method is suitable for different markets and production requirements.
The technical features of the embodiments described above may be arbitrarily combined, and for the sake of brevity, all possible combinations of the technical features in the embodiments described above are not described, but should be considered as being within the scope of the present specification as long as there is no contradiction between the combinations of the technical features.
The above-mentioned embodiments only express several embodiments of the present invention, and the description thereof is more specific and detailed, but not construed as limiting the scope of the invention. It should be noted that, for a person skilled in the art, several variations and modifications can be made without departing from the inventive concept, which falls within the scope of the present invention. Therefore, the protection scope of the present patent shall be subject to the appended claims.

Claims (8)

1. A method for purifying and processing quartz sand for a petroleum fracturing propping agent is characterized by comprising the following steps:
s100, carrying out classified screening and impurity filtering treatment on the natural quartz sand raw material to obtain a natural quartz sand crude product;
s200, scrubbing the natural quartz sand coarse product subjected to classified screening and impurity filtering treatment;
s300, carrying out graded desliming treatment on the natural quartz sand coarse product after scrubbing treatment;
s400, reselecting the natural quartz sand crude product subjected to graded desliming treatment to obtain quartz refined sand;
s500, carrying out magnetic separation and impurity removal on the quartz refined sand obtained after the gravity separation to obtain quartz sand high-intensity magnetic separation tailings;
s600, carrying out color separation or flotation treatment on the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal to obtain a quartz sand finished product for the petroleum fracturing propping agent.
2. The method for purifying and processing the quartz sand for the petroleum fracturing propping agent according to the claim 1, wherein in the step S100, the natural quartz sand raw material is subjected to classification screening and impurity filtering treatment to obtain a crude product of the natural quartz sand, and the crude product of the natural quartz sand is firstly filtered by a 10-mesh sieve to remove large gravels, so as to complete primary filtration; and then, fine sand and soil are further filtered by a sieve of 20 meshes to 140 meshes, and secondary filtration is completed.
3. The method for purifying and processing the quartz sand for the petroleum fracturing propping agent according to claim 1, wherein in the step S200 of scrubbing the crude product of the natural quartz sand after the grading screening and impurity filtering treatment, the crude product of the natural quartz sand is put into a scrubbing machine for pulping and scrubbing, so that fine mud and iron impurities on the surface of the crude product of the natural quartz sand are dissociated; wherein the scrubbing concentration is 50-70%, and the scrubbing time is 5-20 min.
4. The method for purifying and processing the quartz sand for the petroleum fracturing propping agent according to the claim 1, wherein in the step S400, the natural quartz sand crude product after the graded desliming treatment is reselected, specifically, the natural quartz sand crude product is put into a spiral chute, heavy minerals are separated from the quartz sand through the action of the gravity and the centrifugal force of the rotational flow, and the heavy minerals are directly discharged to obtain quartz refined sand.
5. The method for purifying and processing quartz sand for petroleum fracturing propping agent according to claim 1, wherein in said step S500, magnetic separation and impurity removal are performed on said quartz refined sand obtained after heavy separation, specifically, first separation treatment is performed on said quartz refined sand by using a low-intensity magnetic separator to remove strong magnetic minerals; and then, carrying out secondary sorting treatment on the quartz refined sand by using a strong magnetic separator to remove weakly magnetic minerals so as to obtain the quartz sand strong magnetic separation tailings.
6. The method for purifying and processing the quartz sand for the petroleum fracturing propping agent according to the claim 1, wherein in the step S600, the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal are subjected to flotation treatment, the quartz sand high-intensity magnetic separation tailings are put into a flotation machine, a collecting agent and an inhibitor are added into ore pulp, and low-intensity impurity minerals such as feldspar and rock debris are removed by a reverse flotation method to obtain a quartz sand finished product with qualified breakage rate; the collector is prepared from a collector A and a collector B according to the mass ratio of 1.0: 0.5-3.0, and the amount is 500-2000 g/t; the collector A can be at least one of lauryl amine and coconut alkyl primary amine, and the collector B can be at least one of sodium petroleum sulfonate, sodium dodecyl sulfonate and sodium oleate; the inhibitor is sodium hexametaphosphate, and the amount of the inhibitor is 0-100 g/t; the pH value of the ore pulp is 2-3.
7. The method for purifying and processing the quartz sand for the petroleum fracturing propping agent according to claim 1, wherein in the step S600, the quartz sand high-intensity magnetic separation tailings obtained after the magnetic separation and impurity removal are subjected to color separation treatment, the quartz sand high-intensity magnetic separation tailings are firstly subjected to dehydration and drying treatment, and then the dried quartz sand high-intensity magnetic separation tailings are put into a color separator for separation treatment.
8. The method for purifying and processing the quartz sand for the petroleum fracturing propping agent according to claim 1, wherein in the step S600, the quartz sand after magnetic separation and impurity removal is subjected to color separation treatment to obtain a quartz sand finished product, and then the quartz sand finished product is sieved to obtain products with different particle sizes of 10-20 meshes, 20-40 meshes, 30-50 meshes, 40-60 meshes, 50-70 meshes, 70-140 meshes and the like; or, after the step S600, performing flotation treatment on the quartz sand high-intensity magnetic separation tailings subjected to magnetic separation and impurity removal to obtain a quartz sand finished product, and then screening, dehydrating and drying the quartz sand finished product to obtain products with different particle sizes of 10-20 meshes, 20-40 meshes, 30-50 meshes, 40-60 meshes, 50-70 meshes, 70-140 meshes and the like.
CN201911073472.9A 2019-11-05 2019-11-05 Quartz sand purification processing method for petroleum fracturing propping agent Active CN110976071B (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN201911073472.9A CN110976071B (en) 2019-11-05 2019-11-05 Quartz sand purification processing method for petroleum fracturing propping agent

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN201911073472.9A CN110976071B (en) 2019-11-05 2019-11-05 Quartz sand purification processing method for petroleum fracturing propping agent

Publications (2)

Publication Number Publication Date
CN110976071A true CN110976071A (en) 2020-04-10
CN110976071B CN110976071B (en) 2020-10-16

Family

ID=70083193

Family Applications (1)

Application Number Title Priority Date Filing Date
CN201911073472.9A Active CN110976071B (en) 2019-11-05 2019-11-05 Quartz sand purification processing method for petroleum fracturing propping agent

Country Status (1)

Country Link
CN (1) CN110976071B (en)

Cited By (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN111330731A (en) * 2020-04-30 2020-06-26 中建材通辽矽砂工业有限公司 Sorting device and sorting process for wet-method sorting of petroleum fracturing sand
CN112410016A (en) * 2020-10-22 2021-02-26 刘彬 Quartz sand for fracturing propping agent and preparation method and application thereof
CN112980423A (en) * 2021-02-23 2021-06-18 洲际海峡能源科技有限公司 Quartz sand proppant production method and system
CN113278410A (en) * 2021-04-29 2021-08-20 西南石油大学 Method for preparing proppant production raw material by using oil-based rock debris
CN113751187A (en) * 2021-08-27 2021-12-07 中铝郑州有色金属研究院有限公司 Quartz fine sand and preparation method and application thereof
CN114534905A (en) * 2022-02-17 2022-05-27 海南绿峰资源开发有限公司 Quartz sand tail mud recycling method

Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN101870474A (en) * 2010-06-30 2010-10-27 长沙矿冶研究院 Method for preparing quartz sand concentrate by mineral separation of desert aeolian sand
RU2431601C2 (en) * 2009-08-27 2011-10-20 Учреждение Российской академии наук Институт минералогии Уральского отделения РАН Method of producing highly pure concentrate from natural quartz
WO2014184523A1 (en) * 2013-05-13 2014-11-20 Heraeus Quartz Uk Limited Froth flotation separation for quartz purification and analysis of a quartz sample
CN104984818A (en) * 2015-07-16 2015-10-21 安徽东阳矿业科技有限公司 Method for purification of quartz sand ore in physical mode
CN105060299A (en) * 2015-07-16 2015-11-18 安徽东阳矿业科技有限公司 Quartz sand purification technology
CN108607679A (en) * 2018-04-28 2018-10-02 四川南联环资科技股份有限公司 A kind of quartz sand preparation process of high-efficiency environment friendly
CN109127110A (en) * 2018-08-10 2019-01-04 江苏凯达石英股份有限公司 Pyrite-type quartz sand flotation purifying technique

Patent Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
RU2431601C2 (en) * 2009-08-27 2011-10-20 Учреждение Российской академии наук Институт минералогии Уральского отделения РАН Method of producing highly pure concentrate from natural quartz
CN101870474A (en) * 2010-06-30 2010-10-27 长沙矿冶研究院 Method for preparing quartz sand concentrate by mineral separation of desert aeolian sand
WO2014184523A1 (en) * 2013-05-13 2014-11-20 Heraeus Quartz Uk Limited Froth flotation separation for quartz purification and analysis of a quartz sample
CN104984818A (en) * 2015-07-16 2015-10-21 安徽东阳矿业科技有限公司 Method for purification of quartz sand ore in physical mode
CN105060299A (en) * 2015-07-16 2015-11-18 安徽东阳矿业科技有限公司 Quartz sand purification technology
CN108607679A (en) * 2018-04-28 2018-10-02 四川南联环资科技股份有限公司 A kind of quartz sand preparation process of high-efficiency environment friendly
CN109127110A (en) * 2018-08-10 2019-01-04 江苏凯达石英股份有限公司 Pyrite-type quartz sand flotation purifying technique

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
范培强等: "国内高纯石英砂选矿与深加工研究现状", 《矿冶》 *

Cited By (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN111330731A (en) * 2020-04-30 2020-06-26 中建材通辽矽砂工业有限公司 Sorting device and sorting process for wet-method sorting of petroleum fracturing sand
CN111330731B (en) * 2020-04-30 2023-11-14 中建材通辽矽砂工业有限公司 Sorting device and sorting process for wet-sorting petroleum fracturing sand
CN112410016A (en) * 2020-10-22 2021-02-26 刘彬 Quartz sand for fracturing propping agent and preparation method and application thereof
CN112980423A (en) * 2021-02-23 2021-06-18 洲际海峡能源科技有限公司 Quartz sand proppant production method and system
CN113278410A (en) * 2021-04-29 2021-08-20 西南石油大学 Method for preparing proppant production raw material by using oil-based rock debris
CN113751187A (en) * 2021-08-27 2021-12-07 中铝郑州有色金属研究院有限公司 Quartz fine sand and preparation method and application thereof
CN113751187B (en) * 2021-08-27 2024-01-30 中铝郑州有色金属研究院有限公司 Quartz refined sand and preparation method and application thereof
CN114534905A (en) * 2022-02-17 2022-05-27 海南绿峰资源开发有限公司 Quartz sand tail mud recycling method
CN114534905B (en) * 2022-02-17 2024-01-09 海南绿峰资源开发有限公司 Quartz sand tail mud recycling method

Also Published As

Publication number Publication date
CN110976071B (en) 2020-10-16

Similar Documents

Publication Publication Date Title
CN110976071B (en) Quartz sand purification processing method for petroleum fracturing propping agent
CN103752401B (en) Potash feldspar iron removal process
CN103464272B (en) A kind of coarse slime two sections of water Jie method for separating
CN110201791B (en) Comprehensive utilization method of sandy kaolin tailings containing tourmaline, muscovite and quartz sand
CN101898168B (en) Beneficiation method for removing long quarry impurities by adopting strong magnetic flotation
CN101502819B (en) Pre-selection method of low-ore grade magnetic iron ore
CN109894259B (en) Comprehensive utilization method of gold tailings containing gold, iron and feldspar
CN110270432B (en) Method for removing non-calcareous mineral impurities in carbide slag
CN106733146A (en) Method for recovering rare earth minerals from rare earth tailings with heavy fine iron mud content
CN106829985A (en) A kind of method of the synthetical recovery of sandy kaoline containing mica
CN103769295A (en) Mineral dressing process for low-grade marble magnetic iron ore
CN203635312U (en) Mineral tailings grading and separating recovery system for middings magnetic separator in dense medium coal preparation plant
CN104475238B (en) A kind of enrichment method of appositional pattern navajoite
CN103230832A (en) Beneficiation method for recovering fine fraction iron from strong magnetic separation gangues of ferric oxide ores
CN105642431A (en) Method for gravity concentration and separation of sulfur concentrate in gangue containing sulfur
CN108993760A (en) A kind of low-grade difficulty of weathering selects manganese ore sorting process
CN105833987B (en) Shaping process in composite ore material screen
CN111375482B (en) Method for grading and sorting silico-calcic phosphate ore
CN112517234B (en) Beneficiation process for recovering garnet and rutile in limonite ore
CN213161291U (en) Equipment for sorting bauxite ore
CN109675711B (en) Mineral separation process for treating magnetite containing fine gold minerals
CN102527500A (en) Ultrasonic beneficiation method
CN111298960B (en) Echelon reduction process for flotation tailing coal slime
CN218654829U (en) Production line for processing building materials by using mine rubble
CN216936451U (en) Deep ash-reducing system for high-ash coarse coal slime

Legal Events

Date Code Title Description
PB01 Publication
PB01 Publication
SE01 Entry into force of request for substantive examination
SE01 Entry into force of request for substantive examination
GR01 Patent grant
GR01 Patent grant
CP01 Change in the name or title of a patent holder

Address after: 510651 Guangzhou Research Institute of nonferrous metals, no.363 Changxing Road, Tianhe District, Guangzhou City, Guangdong Province

Patentee after: GUANGZHOU YUEYOU ACADEMY MINERAL RESOURCE TECHNOLOGY CO.,LTD.

Patentee after: Institute of resources comprehensive utilization, Guangdong Academy of Sciences

Address before: 510651 Guangzhou Research Institute of nonferrous metals, no.363 Changxing Road, Tianhe District, Guangzhou City, Guangdong Province

Patentee before: GUANGZHOU YUEYOU ACADEMY MINERAL RESOURCE TECHNOLOGY CO.,LTD.

Patentee before: GUANGDONG INSTITUTE OF RESOURCES COMPREHENSIVE UTILIZATION

Address after: 510651 Guangzhou Research Institute of nonferrous metals, no.363 Changxing Road, Tianhe District, Guangzhou City, Guangdong Province

Patentee after: GUANGZHOU YUEYOU ACADEMY MINERAL RESOURCE TECHNOLOGY CO.,LTD.

Patentee after: Institute of resource utilization and rare earth development, Guangdong Academy of Sciences

Address before: 510651 Guangzhou Research Institute of nonferrous metals, no.363 Changxing Road, Tianhe District, Guangzhou City, Guangdong Province

Patentee before: GUANGZHOU YUEYOU ACADEMY MINERAL RESOURCE TECHNOLOGY CO.,LTD.

Patentee before: Institute of resources comprehensive utilization, Guangdong Academy of Sciences

CP01 Change in the name or title of a patent holder