CN110625714A - One-time forming wood veneer bending process - Google Patents

One-time forming wood veneer bending process Download PDF

Info

Publication number
CN110625714A
CN110625714A CN201910917772.4A CN201910917772A CN110625714A CN 110625714 A CN110625714 A CN 110625714A CN 201910917772 A CN201910917772 A CN 201910917772A CN 110625714 A CN110625714 A CN 110625714A
Authority
CN
China
Prior art keywords
wood veneer
shaped groove
bending
bending process
bent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910917772.4A
Other languages
Chinese (zh)
Inventor
杨劲松
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dongguan Zhongjin Furniture Co ltd
Original Assignee
Dongguan Zhongjin Furniture Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dongguan Zhongjin Furniture Co ltd filed Critical Dongguan Zhongjin Furniture Co ltd
Priority to CN201910917772.4A priority Critical patent/CN110625714A/en
Publication of CN110625714A publication Critical patent/CN110625714A/en
Priority to PCT/CN2020/115979 priority patent/WO2021057604A1/en
Pending legal-status Critical Current

Abstract

The invention belongs to the technical field of wood veneer bending, and particularly relates to a one-time forming wood veneer bending process, which comprises the following steps: s1: firstly, polishing and grinding the wood veneer, then performing paint spraying operation on the polished wood veneer, and then performing protective layer coating operation on the wood veneer after finishing the paint spraying operation, S2: firstly, determining a bending line at a position where a wood veneer needs to be bent, and forming a V-shaped groove by taking the bending line at the bending position as a central line according to the bending angle of the wood veneer; the method comprises the steps of firstly determining a bending line of a wood veneer to be bent, setting a V-shaped groove by taking the bending line of the bending position as a central line according to the bending angle of the wood veneer, enabling the bottom end of the V-shaped groove to be 0.5-0.7mm away from the bottom surface of the wood veneer, not cutting off the wood veneer, and rotatably bending along the V-shaped groove, so that the plate cannot be broken, and the integrity of the plate is ensured while the bending is realized, so that the surface of the bent wood veneer is more attractive.

Description

一次性成型木饰面折弯工艺One-time molding wood veneer bending process

技术领域technical field

本发明属于木饰面折弯技术领域,具体涉及一次性成型木饰面折弯工艺。The invention belongs to the technical field of wood veneer bending, in particular to a one-time molding wood veneer bending process.

背景技术Background technique

木饰面是用各种名贵木材如红榉、樱桃木等0.6MM厚进口实木单板做为木饰面,经过复杂的设备流程、160T压力、250度高温将单板牢固定在模板基层上,将原本在现场装修项目木工工程和木器漆工程中凡是要做油漆的饰面部分在工厂内通过精加工作业进行生产(如:房门、门套、窗套、踢脚线、墙面木饰造型、衣柜、橱柜等),然后到现场进行组装。The wood veneer is made of various precious woods such as red beech, cherry wood and other 0.6MM thick imported solid wood veneers as the wood veneer. After complex equipment process, 160T pressure, and 250 degree high temperature, the veneer is firmly fixed on the formwork base In the factory, the decorative parts that are to be painted in the carpentry engineering and wood paint engineering of the on-site decoration project are produced in the factory through finishing operations (such as: doors, door covers, window covers, baseboards, wall wood moldings, wardrobes, cabinets, etc.), and then assembled on site.

在对拐角处的贴附面进行贴附木饰面时,现有的工艺大多将木饰面进行切割,然后进行贴附,最后进行封边,采用此工艺需要将木饰面进行切割,在连接处会有接缝,即使采用封边胶进行封边,但是破坏了木饰面的表面完整性,影响整体美观。When attaching the wood veneer to the attached surface at the corner, most of the existing processes cut the wood veneer, then attach it, and finally seal the edge. Using this process, the wood veneer needs to be cut. There will be seams at the joints. Even if edge sealing is used for edge sealing, it will destroy the surface integrity of the wood veneer and affect the overall appearance.

发明内容Contents of the invention

为解决上述背景技术中提出的问题。本发明提供了一次性成型木饰面折弯工艺。In order to solve the problems raised in the above-mentioned background technology. The invention provides a one-time molding wood veneer bending process.

为实现上述目的,本发明提供如下技术方案:一次性成型木饰面折弯工艺,包括以下步骤:In order to achieve the above object, the present invention provides the following technical solution: a one-time forming wood veneer bending process, comprising the following steps:

S1:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业;S1: First, polish and polish the wood veneer, then spray and paint the polished and polished wood veneer, and then apply a protective layer to the wood veneer after the painting operation;

S2:首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”;S2: First determine the bending line where the wood veneer needs to be bent, and according to the angle of bending the wood veneer, open a "V-shaped groove" with the bending line at the bend as the center line;

S3:向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合;S3: Apply adhesive glue to the "V-shaped groove" at the bend, and use a laminating machine to bond the adhesive glue;

S4:将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,然后对折弯后的木饰面进行保压;S4: Rotate and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and then press the bent wood veneer;

S5:在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理。S5: After the pressure holding is completed, use edge sealing glue for the bonded "V-shaped groove" for edge sealing.

优选的,木饰面与装配体上插槽相对应的一侧开设有若干个倒角。Preferably, several chamfers are provided on the side of the wood veneer corresponding to the slot on the assembly.

优选的,若干个倒角为等距间隔布置且相互平行。Preferably, several chamfers are arranged at equidistant intervals and parallel to each other.

优选的,所述倒角的斜面方向与木饰面插接的方向相同。Preferably, the direction of the slope of the chamfer is the same as the insertion direction of the wood veneer.

优选的,S2中的“V形槽”的角度与需要折弯的角度相同。Preferably, the angle of the "V-shaped groove" in S2 is the same as the angle to be bent.

优选的,S2中的“V形槽”的底端距离木饰面的底面为0.5-0.7mm。Preferably, the bottom end of the "V-shaped groove" in S2 is 0.5-0.7mm away from the bottom surface of the wood veneer.

优选的,S3中的粘接胶为拼板胶,且施胶量为150g-250g/㎡。Preferably, the bonding glue in S3 is jigsaw glue, and the amount of glue applied is 150g-250g/㎡.

优选的,S4中的保压时间为2-5min。Preferably, the holding time in S4 is 2-5min.

优选的,S5中的封边胶为玻璃胶。Preferably, the edge sealant in S5 is glass glue.

与现有技术相比,本发明的有益效果是:Compared with prior art, the beneficial effect of the present invention is:

首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”,且“V形槽”的底端距离木饰面的底面为0.5-0.7mm,并未将木饰面切断,在进行折弯时,可沿“V形槽”进行转动折弯,不会造成板材断裂,实现折弯的同时,保证板材的完整性,使得折弯后的木饰面表面较为美观。First determine the bending line where the wood veneer needs to be bent, and according to the angle of bending the wood veneer, set up a "V-shaped groove" with the bending line at the bend as the center line, and the "V-shaped groove" The bottom end is 0.5-0.7mm away from the bottom surface of the wood veneer, and the wood veneer is not cut off. When bending, it can be rotated and bent along the "V-shaped groove", which will not cause the plate to break and realize the perfect bending. At the same time, the integrity of the board is guaranteed, so that the bent wood veneer surface is more beautiful.

附图说明Description of drawings

附图用来提供对本发明的进一步理解,并且构成说明书的一部分,与本发明的实施例一起用于解释本发明,并不构成对本发明的限制。在附图中:The accompanying drawings are used to provide a further understanding of the present invention, and constitute a part of the description, and are used together with the embodiments of the present invention to explain the present invention, and do not constitute a limitation to the present invention. In the attached picture:

图1为本发明中的“V形槽”结构示意图;Fig. 1 is the structural representation of " V-shaped groove " among the present invention;

图2为本发明中的倒角结构示意图。Fig. 2 is a schematic diagram of the chamfering structure in the present invention.

具体实施方式Detailed ways

下面将结合本发明实施例中的附图,对本发明实施例中的技术方案进行清楚、完整地描述,显然,所描述的实施例仅仅是本发明一部分实施例,而不是全部的实施例。基于本发明中的实施例,本领域普通技术人员在没有做出创造性劳动前提下所获得的所有其他实施例,都属于本发明保护的范围。The following will clearly and completely describe the technical solutions in the embodiments of the present invention with reference to the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only some, not all, embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by persons of ordinary skill in the art without making creative efforts belong to the protection scope of the present invention.

实施例1Example 1

请参阅图1-2,本发明提供以下技术方案:一次性成型木饰面折弯工艺,包括以下步骤,Please refer to Fig. 1-2, the present invention provides the following technical solutions: one-time forming wood veneer bending process, including the following steps,

S1:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业;S1: First, polish and polish the wood veneer, then spray and paint the polished and polished wood veneer, and then apply a protective layer to the wood veneer after the painting operation;

S2:首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”;S2: First determine the bending line where the wood veneer needs to be bent, and according to the angle of bending the wood veneer, open a "V-shaped groove" with the bending line at the bend as the center line;

S3:向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合;S3: Apply adhesive glue to the "V-shaped groove" at the bend, and use a laminating machine to bond the adhesive glue;

S4:将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,然后对折弯后的木饰面进行保压;S4: Rotate and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and then press the bent wood veneer;

S5:在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理。S5: After the pressure holding is completed, use edge sealing glue for the bonded "V-shaped groove" for edge sealing.

本实施方案中:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业,先对木饰面进行处理,便于后续的加工,首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,参照图1,以折弯处的折弯线为中线开设“V形槽”,且“V形槽”的底端距离木饰面的底面为0.5-0.7mm,并未将木饰面切断,在进行折弯时,可沿“V形槽”进行转动折弯,不会造成板材断裂,实现折弯的同时,保证板材的完整性,使得折弯后的木饰面表面较为美观,向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合,将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,将折弯后的木饰面进行粘接,使其稳固成型,然后对折弯后的木饰面进行保压,使得粘接胶凝固,保证折弯后的木饰面不会发生回弹,在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理,对“V形槽”进行密封,参照图2,木饰面与装配体上插槽相对应的一侧开设有若干个倒角,若干个倒角为等距间隔布置且相互平行,倒角的斜面方向与木饰面插接的方向相同,在进行装配时,以倒角的斜面方向向前推动,使得木饰面上的倒角与装配体上的插槽插接,在若干个倒角的作用下,木饰面上的倒角插入插槽较为容易,将木饰面与插槽脱离时较为费力,从增加木饰面的安装稳定性。In this embodiment: firstly, the wood veneer is polished and polished, then the polished and polished wood veneer is sprayed with paint, and then the wood veneer after the painting operation is finished is coated with a protective layer. For processing, it is convenient for subsequent processing. First, determine the bending line where the wood veneer needs to be bent. According to the required bending angle for the wood veneer, refer to Figure 1, and use the bending line at the bend as the center line to open " V-shaped groove", and the bottom of the "V-shaped groove" is 0.5-0.7mm away from the bottom surface of the wood veneer, and the wood veneer is not cut off. When bending, it can be rotated and folded along the "V-shaped groove" Bending will not cause the board to break, and at the same time to realize the bending, ensure the integrity of the board, so that the surface of the wood veneer after bending is more beautiful, apply adhesive glue to the "V-shaped groove" at the bending place, and Use a laminating machine to bond the adhesive glue, turn and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and carry out the bending of the wood veneer Bonding to make it stable and forming, and then pressurize the bent wood veneer to make the adhesive solidify, so as to ensure that the bent wood veneer will not rebound. The "V-shaped groove" of the "V-shaped groove" is edge-sealed with edge sealing glue to seal the "V-shaped groove". Referring to Figure 2, there are several chamfers on the side of the wood veneer corresponding to the groove on the assembly. The two chamfers are arranged at equal intervals and parallel to each other. The direction of the chamfer is the same as that of the wood veneer. When assembling, push forward in the direction of the chamfer to make the chamfer on the wood veneer It is plugged into the slot on the assembly. Under the action of several chamfers, it is easier to insert the chamfer on the wood veneer into the slot, but it is more laborious to separate the wood veneer from the slot. Installation stability.

具体的,木饰面与装配体上插槽相对应的一侧开设有若干个倒角。Specifically, several chamfers are provided on the side of the wood veneer corresponding to the slot on the assembly.

具体的,若干个倒角为等距间隔布置且相互平行。Specifically, several chamfers are arranged at equidistant intervals and parallel to each other.

具体的,倒角的斜面方向与木饰面插接的方向相同。Specifically, the direction of the bevel of the chamfer is the same as the direction of insertion of the wood veneer.

具体的,S2中的“V形槽”的角度与需要折弯的角度相同。Specifically, the angle of the "V-shaped groove" in S2 is the same as the angle that needs to be bent.

具体的,S2中的“V形槽”的底端距离木饰面的底面为0.5mm。Specifically, the distance between the bottom end of the "V-shaped groove" in S2 and the bottom surface of the wood veneer is 0.5mm.

具体的,S3中的粘接胶为拼板胶,且施胶量为150g/㎡。Specifically, the bonding glue in S3 is jigsaw glue, and the amount of glue applied is 150g/㎡.

具体的,S4中的保压时间为2min。Specifically, the holding time in S4 is 2 minutes.

具体的,S5中的封边胶为玻璃胶。Specifically, the edge sealant in S5 is glass glue.

实施例2Example 2

请参阅图1-2,本发明提供以下技术方案:一次性成型木饰面折弯工艺,包括以下步骤,Please refer to Fig. 1-2, the present invention provides the following technical solutions: one-time forming wood veneer bending process, including the following steps,

S1:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业;S1: First, polish and polish the wood veneer, then spray and paint the polished and polished wood veneer, and then apply a protective layer to the wood veneer after the painting operation;

S2:首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”;S2: First determine the bending line where the wood veneer needs to be bent, and according to the angle of bending the wood veneer, open a "V-shaped groove" with the bending line at the bend as the center line;

S3:向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合;S3: Apply adhesive glue to the "V-shaped groove" at the bend, and use a laminating machine to bond the adhesive glue;

S4:将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,然后对折弯后的木饰面进行保压;S4: Rotate and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and then press the bent wood veneer;

S5:在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理。S5: After the pressure holding is completed, use edge sealing glue for the bonded "V-shaped groove" for edge sealing.

本实施方案中:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业,先对木饰面进行处理,便于后续的加工,首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,参照图1,以折弯处的折弯线为中线开设“V形槽”,且“V形槽”的底端距离木饰面的底面为0.5-0.7mm,并未将木饰面切断,在进行折弯时,可沿“V形槽”进行转动折弯,不会造成板材断裂,实现折弯的同时,保证板材的完整性,使得折弯后的木饰面表面较为美观,向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合,将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,将折弯后的木饰面进行粘接,使其稳固成型,然后对折弯后的木饰面进行保压,使得粘接胶凝固,保证折弯后的木饰面不会发生回弹,在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理,对“V形槽”进行密封,参照图2,木饰面与装配体上插槽相对应的一侧开设有若干个倒角,若干个倒角为等距间隔布置且相互平行,倒角的斜面方向与木饰面插接的方向相同,在进行装配时,以倒角的斜面方向向前推动,使得木饰面上的倒角与装配体上的插槽插接,在若干个倒角的作用下,木饰面上的倒角插入插槽较为容易,将木饰面与插槽脱离时较为费力,从增加木饰面的安装稳定性。In this embodiment: firstly, the wood veneer is polished and polished, then the polished and polished wood veneer is sprayed with paint, and then the wood veneer after the painting operation is finished is coated with a protective layer. For processing, it is convenient for subsequent processing. First, determine the bending line where the wood veneer needs to be bent. According to the required bending angle for the wood veneer, refer to Figure 1, and use the bending line at the bend as the center line to open " V-shaped groove", and the bottom of the "V-shaped groove" is 0.5-0.7mm away from the bottom surface of the wood veneer, and the wood veneer is not cut off. When bending, it can be rotated and folded along the "V-shaped groove" Bending will not cause the board to break, and at the same time to realize the bending, ensure the integrity of the board, so that the surface of the wood veneer after bending is more beautiful, apply adhesive glue to the "V-shaped groove" at the bending place, and Use a laminating machine to bond the adhesive glue, turn and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and carry out the bending of the wood veneer Bonding to make it stable and forming, and then pressurize the bent wood veneer to make the adhesive solidify, so as to ensure that the bent wood veneer will not rebound. The "V-shaped groove" of the "V-shaped groove" is edge-sealed with edge sealing glue to seal the "V-shaped groove". Referring to Figure 2, there are several chamfers on the side of the wood veneer corresponding to the groove on the assembly. The two chamfers are arranged at equal intervals and parallel to each other. The direction of the chamfer is the same as that of the wood veneer. When assembling, push forward in the direction of the chamfer to make the chamfer on the wood veneer It is plugged into the slot on the assembly. Under the action of several chamfers, it is easier to insert the chamfer on the wood veneer into the slot, but it is more laborious to separate the wood veneer from the slot. Installation stability.

具体的,木饰面与装配体上插槽相对应的一侧开设有若干个倒角。Specifically, several chamfers are provided on the side of the wood veneer corresponding to the slot on the assembly.

具体的,若干个倒角为等距间隔布置且相互平行。Specifically, several chamfers are arranged at equidistant intervals and parallel to each other.

具体的,倒角的斜面方向与木饰面插接的方向相同。Specifically, the direction of the bevel of the chamfer is the same as the direction of insertion of the wood veneer.

具体的,S2中的“V形槽”的角度与需要折弯的角度相同。Specifically, the angle of the "V-shaped groove" in S2 is the same as the angle that needs to be bent.

具体的,S2中的“V形槽”的底端距离木饰面的底面为0.6mm。Specifically, the distance between the bottom end of the "V-shaped groove" in S2 and the bottom surface of the wood veneer is 0.6mm.

具体的,S3中的粘接胶为拼板胶,且施胶量为200g/㎡。Specifically, the bonding glue in S3 is jigsaw glue, and the amount of glue applied is 200g/㎡.

具体的,S4中的保压时间为3min。Specifically, the holding time in S4 is 3 minutes.

具体的,S5中的封边胶为玻璃胶。Specifically, the edge sealant in S5 is glass glue.

实施例3Example 3

请参阅图1-2,本发明提供以下技术方案:一次性成型木饰面折弯工艺,包括以下步骤,Please refer to Fig. 1-2, the present invention provides the following technical solutions: one-time forming wood veneer bending process, including the following steps,

S1:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业;S1: First, polish and polish the wood veneer, then spray and paint the polished and polished wood veneer, and then apply a protective layer to the wood veneer after the painting operation;

S2:首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”;S2: First determine the bending line where the wood veneer needs to be bent, and according to the angle of bending the wood veneer, open a "V-shaped groove" with the bending line at the bend as the center line;

S3:向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合;S3: Apply adhesive glue to the "V-shaped groove" at the bend, and use a laminating machine to bond the adhesive glue;

S4:将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,然后对折弯后的木饰面进行保压;S4: Rotate and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and then press the bent wood veneer;

S5:在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理。S5: After the pressure holding is completed, use edge sealing glue for the bonded "V-shaped groove" for edge sealing.

本实施方案中:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业,先对木饰面进行处理,便于后续的加工,首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,参照图1,以折弯处的折弯线为中线开设“V形槽”,且“V形槽”的底端距离木饰面的底面为0.5-0.7mm,并未将木饰面切断,在进行折弯时,可沿“V形槽”进行转动折弯,不会造成板材断裂,实现折弯的同时,保证板材的完整性,使得折弯后的木饰面表面较为美观,向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合,将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,将折弯后的木饰面进行粘接,使其稳固成型,然后对折弯后的木饰面进行保压,使得粘接胶凝固,保证折弯后的木饰面不会发生回弹,在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理,对“V形槽”进行密封,参照图2,木饰面与装配体上插槽相对应的一侧开设有若干个倒角,若干个倒角为等距间隔布置且相互平行,倒角的斜面方向与木饰面插接的方向相同,在进行装配时,以倒角的斜面方向向前推动,使得木饰面上的倒角与装配体上的插槽插接,在若干个倒角的作用下,木饰面上的倒角插入插槽较为容易,将木饰面与插槽脱离时较为费力,从增加木饰面的安装稳定性。In this embodiment: firstly, the wood veneer is polished and polished, then the polished and polished wood veneer is sprayed with paint, and then the wood veneer after the painting operation is finished is coated with a protective layer. For processing, it is convenient for subsequent processing. First, determine the bending line where the wood veneer needs to be bent. According to the required bending angle for the wood veneer, refer to Figure 1, and use the bending line at the bend as the center line to open " V-shaped groove", and the bottom of the "V-shaped groove" is 0.5-0.7mm away from the bottom surface of the wood veneer, and the wood veneer is not cut off. When bending, it can be rotated and folded along the "V-shaped groove" Bending will not cause the board to break, and at the same time to realize the bending, ensure the integrity of the board, so that the surface of the wood veneer after bending is more beautiful, apply adhesive glue to the "V-shaped groove" at the bending place, and Use a laminating machine to bond the adhesive glue, turn and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and carry out the bending of the wood veneer Bonding to make it stable and forming, and then pressurize the bent wood veneer to make the adhesive solidify, so as to ensure that the bent wood veneer will not rebound. The "V-shaped groove" of the "V-shaped groove" is edge-sealed with edge sealing glue to seal the "V-shaped groove". Referring to Figure 2, there are several chamfers on the side of the wood veneer corresponding to the groove on the assembly. The two chamfers are arranged at equal intervals and parallel to each other. The direction of the chamfer is the same as that of the wood veneer. When assembling, push forward in the direction of the chamfer to make the chamfer on the wood veneer It is plugged into the slot on the assembly. Under the action of several chamfers, it is easier to insert the chamfer on the wood veneer into the slot, but it is more laborious to separate the wood veneer from the slot. Installation stability.

具体的,木饰面与装配体上插槽相对应的一侧开设有若干个倒角。Specifically, several chamfers are provided on the side of the wood veneer corresponding to the slot on the assembly.

具体的,若干个倒角为等距间隔布置且相互平行。Specifically, several chamfers are arranged at equidistant intervals and parallel to each other.

具体的,倒角的斜面方向与木饰面插接的方向相同。Specifically, the direction of the bevel of the chamfer is the same as the direction of insertion of the wood veneer.

具体的,S2中的“V形槽”的角度与需要折弯的角度相同。Specifically, the angle of the "V-shaped groove" in S2 is the same as the angle that needs to be bent.

具体的,S2中的“V形槽”的底端距离木饰面的底面为0.7mm。Specifically, the distance between the bottom end of the "V-shaped groove" in S2 and the bottom surface of the wood veneer is 0.7mm.

具体的,S3中的粘接胶为拼板胶,且施胶量为250g/㎡。Specifically, the bonding glue in S3 is jigsaw glue, and the amount of glue applied is 250g/㎡.

具体的,S4中的保压时间为5min。Specifically, the holding time in S4 is 5 minutes.

具体的,S5中的封边胶为玻璃胶。Specifically, the edge sealant in S5 is glass glue.

本发明的工作原理及使用流程:本实施方案中:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业,先对木饰面进行处理,便于后续的加工,首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”,且“V形槽”的底端距离木饰面的底面为0.5-0.7mm,并未将木饰面切断,在进行折弯时,可沿“V形槽”进行转动折弯,不会造成板材断裂,实现折弯的同时,保证板材的完整性,使得折弯后的木饰面表面较为美观,向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合,将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,将折弯后的木饰面进行粘接,使其稳固成型,然后对折弯后的木饰面进行保压,使得粘接胶凝固,保证折弯后的木饰面不会发生回弹,在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理,对“V形槽”进行密封,木饰面与装配体上插槽相对应的一侧开设有若干个倒角,若干个倒角为等距间隔布置且相互平行,倒角的斜面方向与木饰面插接的方向相同,在进行装配时,以倒角的斜面方向向前推动,使得木饰面上的倒角与装配体上的插槽插接,在若干个倒角的作用下,木饰面上的倒角插入插槽较为容易,将木饰面与插槽脱离时较为费力,从增加木饰面的安装稳定性。The working principle and application process of the present invention: In this embodiment: first, the wood veneer is polished and polished, and then the polished and polished wood veneer is sprayed with paint, and then a protective layer is applied to the wood veneer after the painting operation is completed. For the coating operation, the wood veneer is processed first to facilitate subsequent processing. First, determine the bending line where the wood veneer needs to be bent. The line is the center line to open a "V-shaped groove", and the bottom of the "V-shaped groove" is 0.5-0.7mm away from the bottom surface of the wood veneer, and the wood veneer is not cut off. When bending, it can be bent along the "V-shaped The "groove" is rotated and bent without causing the plate to break. While realizing the bending, the integrity of the plate is ensured, so that the surface of the wood veneer after bending is more beautiful, and it is coated into the "V-shaped groove" at the bend. Adhesive glue, use a laminating machine to bond the adhesive glue, turn and bend the wood veneer along the "V-shaped groove", and make the two sides of the "V-shaped groove" fit together, after bending The wood veneer is bonded to make it stable and shaped, and then the bent wood veneer is kept under pressure to make the adhesive solidify, so as to ensure that the bent wood veneer will not rebound. , Use edge sealing glue to seal the "V-shaped groove" after bonding, and seal the "V-shaped groove". There are several chamfers on the side of the wood veneer corresponding to the slot on the assembly. Several chamfers are arranged at equidistant intervals and parallel to each other. The direction of the bevel of the chamfer is the same as that of the wood veneer. The corners are plugged into the slots on the assembly. Under the action of several chamfers, it is easier to insert the chamfers on the wood veneer into the slots, but it is more laborious to separate the wood veneer from the slots. installation stability.

最后应说明的是:以上仅为本发明的优选实施例而已,并不用于限制本发明,尽管参照前述实施例对本发明进行了详细的说明,对于本领域的技术人员来说,其依然可以对前述各实施例所记载的技术方案进行修改,或者对其中部分技术特征进行等同替换。凡在本发明的精神和原则之内,所作的任何修改、等同替换、改进等,均应包含在本发明的保护范围之内。Finally, it should be noted that the above are only preferred embodiments of the present invention, and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still understand The technical solutions recorded in the foregoing embodiments are modified, or some of the technical features are equivalently replaced. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention shall be included within the protection scope of the present invention.

Claims (9)

1.一次性成型木饰面折弯工艺,包括以下步骤:1. One-time forming wood veneer bending process, including the following steps: S1:首先对木饰面进行抛光打磨,然后对抛光打磨后的木饰面进行喷涂油漆作业,然后对喷漆作业完毕后的木饰面进行保护层涂覆作业;S1: First, polish and polish the wood veneer, then spray and paint the polished and polished wood veneer, and then apply a protective layer to the wood veneer after the painting operation; S2:首先确定木饰面需要进行折弯处的折弯线,根据需要对木饰面折弯的角度,以折弯处的折弯线为中线开设“V形槽”;S2: First determine the bending line where the wood veneer needs to be bent, and according to the angle of bending the wood veneer, open a "V-shaped groove" with the bending line at the bend as the center line; S3:向折弯处的“V形槽”内涂覆粘接胶,在使用贴合机对粘接胶进行贴合;S3: Apply adhesive glue to the "V-shaped groove" at the bend, and use a laminating machine to bond the adhesive glue; S4:将木饰面沿“V形槽”进行转动折弯,并使得“V形槽”的两侧壁贴合,然后对折弯后的木饰面进行保压;S4: Rotate and bend the wood veneer along the "V-shaped groove", and make the two side walls of the "V-shaped groove" fit together, and then press the bent wood veneer; S5:在保压结束后,对贴合后的“V形槽”使用封边胶进行封边处理。S5: After the pressure holding is completed, use edge sealing glue for the bonded "V-shaped groove" for edge sealing. 2.根据权利要求1所述的一次性成型木饰面折弯工艺,其特征在于:木饰面与装配体上插槽相对应的一侧开设有若干个倒角。2. The one-time molding wood veneer bending process according to claim 1, characterized in that: there are several chamfers on the side of the wood veneer corresponding to the slot on the assembly. 3.根据权利要求2所述的一次性成型木饰面折弯工艺,其特征在于:若干个倒角为等距间隔布置且相互平行。3. The one-time molding wood veneer bending process according to claim 2, characterized in that: several chamfers are arranged at equal intervals and parallel to each other. 4.根据权利要求2所述的一次性成型木饰面折弯工艺,其特征在于:所述倒角的斜面方向与木饰面插接的方向相同。4. The one-time forming wood veneer bending process according to claim 2, characterized in that: the direction of the chamfered chamfer is the same as the direction in which the wood veneer is inserted. 5.根据权利要求1所述的一次性成型木饰面折弯工艺,其特征在于:S2中的“V形槽”的角度与需要折弯的角度相同。5. The one-time forming wood veneer bending process according to claim 1, characterized in that: the angle of the "V-shaped groove" in S2 is the same as the angle to be bent. 6.根据权利要求1所述的一次性成型木饰面折弯工艺,其特征在于:S2中的“V形槽”的底端距离木饰面的底面为0.5-0.7mm。6. The one-time molding wood veneer bending process according to claim 1, characterized in that: the bottom end of the "V-shaped groove" in S2 is 0.5-0.7 mm from the bottom surface of the wood veneer. 7.根据权利要求1所述的一次性成型木饰面折弯工艺,其特征在于:S3中的粘接胶为拼板胶,且施胶量为150g-250g/㎡。7. The one-time molded wood veneer bending process according to claim 1, characterized in that: the adhesive glue in S3 is jigsaw glue, and the amount of glue applied is 150g-250g/㎡. 8.根据权利要求1所述的一次性成型木饰面折弯工艺,其特征在于:S4中的保压时间为2-5min。8. The one-time molding wood veneer bending process according to claim 1, characterized in that: the holding time in S4 is 2-5 minutes. 9.根据权利要求1所述的一次性成型木饰面折弯工艺,其特征在于:S5中的封边胶为玻璃胶。9. The one-time molding wood veneer bending process according to claim 1, characterized in that: the edge sealant in S5 is glass glue.
CN201910917772.4A 2019-09-26 2019-09-26 One-time forming wood veneer bending process Pending CN110625714A (en)