CN110116445A - The degreasing method on secondary degreasing floor - Google Patents

The degreasing method on secondary degreasing floor Download PDF

Info

Publication number
CN110116445A
CN110116445A CN201910375037.5A CN201910375037A CN110116445A CN 110116445 A CN110116445 A CN 110116445A CN 201910375037 A CN201910375037 A CN 201910375037A CN 110116445 A CN110116445 A CN 110116445A
Authority
CN
China
Prior art keywords
floor
temperature
humidity
steam boiler
degreasing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910375037.5A
Other languages
Chinese (zh)
Inventor
董敦喜
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Home To Shanghai Industrial Co Ltd
Original Assignee
Home To Shanghai Industrial Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Home To Shanghai Industrial Co Ltd filed Critical Home To Shanghai Industrial Co Ltd
Priority to CN201910375037.5A priority Critical patent/CN110116445A/en
Publication of CN110116445A publication Critical patent/CN110116445A/en
Pending legal-status Critical Current

Abstract

The invention discloses the degreasing methods on secondary degreasing floor, it is related to solid wooden floor board field, floor is put into the constant steam boiler of humidity and is heated up to predetermined temperature, heating duration continues 12-24h, later floor is continued to be placed in steam boiler and dries 8h, and keep temperature in boiler, humidity is constant, floor is cooled down again, hydrofuge, after so that its temperature and humidity is reached predetermined temperature and predetermined moisture, floor is set to keep 8h in the temperature and humidity, operation to floor spray water steam and before repeating later, floor is placed on 12h in steam boiler again, and keep relative humidity in steam boiler.Floor is placed in steam boiler and carries out repeatedly heating drying repeatedly by the present invention, heating temperature in steam boiler can step by step bake out the moisture of ground intralamellar part with heating humidity, without being damaged to the wood-fibred on floor, so that floor be made to reach, toughness is higher, and color is more preferable.The on-deformable purpose of shape.

Description

The degreasing method on secondary degreasing floor
Technical field
The present invention relates to solid wooden floor board fields, the specially degreasing method on secondary degreasing floor.
Background technique
Solid wooden floor board is the floor decorative material also known as raw wood floor formed after natural timber drying, processing, is with real The floor that wood is directly processed into, the texture that there is timber to grow naturally for it are the non-conductors of heat, can play work cool in summer and warm in winter With comfortable foot feeling is the ideal material of the ground surface finishings such as bedroom, parlor, study using safe feature.
But solid wooden floor board currently on the market be in process of production 180 degrees Celsius at a temperature of thoroughly dried Dry, the wood-fibred that will lead to ground intralamellar part is withered, and discoloration, the later period can change the color on floor, and floor does not have toughness, uses the longevity It orders short;And the good and bad jumbled together for existing repairs profession, after agent takes product away from manufacturer, it may occur that adulterate, flicker disappears The case where person of expense, and consumer has little understanding for floor situation, is merely able to accept others' introduction, can not understand the true of floor Positive value leads to not purchase floor according to self-demand.
Summary of the invention
It is an object of the invention to: be to solve solid wooden floor board in process of production 180 degrees Celsius at a temperature of into What row was thoroughly dried, the wood-fibred that will lead to ground intralamellar part is withered, and discoloration, the later period can change the color on floor, and floor is not tough Property, service life is short;And the good and bad jumbled together for existing repairs profession, after agent takes product away from manufacturer, it may occur that filled with secondary Well, the case where flicker consumer, and consumer has little understanding for floor situation, is merely able to accept others' introduction, Wu Faliao The true value for solving floor leads to not the problem of purchasing floor according to self-demand, provides the degreasing side on secondary degreasing floor Method.
To achieve the above object, the invention provides the following technical scheme: the degreasing method on secondary degreasing floor, including it is following Step:
Step 1: floor being put into the constant steam boiler of humidity and is heated up to predetermined temperature, and heating duration continues 12- For 24 hours, floor A is obtained;
Step 2: floor A being continued to be placed in steam boiler and dries 8h, and keeps temperature, humidity in boiler constant, Obtain floor B;
Step 3: cooling down to floor B, hydrofuge, after so that its temperature and humidity is reached predetermined temperature and predetermined moisture, makes Floor B keeps 8h in the temperature and humidity, obtains floor C;
Step 4: water vapour is sprayed to floor C, obtains floor D;
Step 5: floor D is repeated Step 1: step 2 and step 3, obtain floor E;
Step 6: being placed on 12h in steam boiler for floor E, and keep the relative humidity in steam boiler, obtain half at Product A;
Step 7: semi-finished product A is laid in steam boiler, and dry 12-24h obtains finished product.
Preferably, the humidity in the step 1 and step 2 is 85%, and the predetermined temperature in step 1 is 120 Celsius Degree.
Preferably, the predetermined temperature in the step 3 is 60 degrees Celsius, predetermined moisture 40%.
Preferably, the steam boiler temperature in the step 6 is 50-60 degrees Celsius, and the water content on floor is 10- at this time 12%.
Preferably, the temperature of steam boiler is 50-55 degrees Celsius in the step 7.
Compared with prior art, the beneficial effects of the present invention are: the present invention by floor be placed in steam boiler carry out it is more Secondary heating repeatedly is dried, and the heating temperature in steam boiler can step by step bake out the moisture of ground intralamellar part with heating humidity, and It will not be damaged to the wood-fibred on floor, toughness is higher, and color is more preferable so that floor be made to reach.The on-deformable purpose of shape
Specific embodiment
Below in conjunction with the embodiment of the present invention, technical scheme in the embodiment of the invention is clearly and completely described, Obviously, described embodiments are only a part of the embodiments of the present invention, instead of all the embodiments.Based in the present invention Embodiment, every other embodiment obtained by those of ordinary skill in the art without making creative efforts, all Belong to the scope of protection of the invention.
The degreasing method on secondary degreasing floor, including the following steps:
Step 1: floor being put into the constant steam boiler of humidity and is heated up to predetermined temperature, and heating duration continues 12- For 24 hours, floor A is obtained;
Step 2: floor A being continued to be placed in steam boiler and dries 8h, and keeps temperature, humidity in boiler constant, Obtain floor B;
Step 3: cooling down to floor B, hydrofuge, after so that its temperature and humidity is reached predetermined temperature and predetermined moisture, makes Floor B keeps 8h in the temperature and humidity, obtains floor C;
Step 4: water vapour is sprayed to floor C, obtains floor D;
Step 5: floor D is repeated Step 1: step 2 and step 3, obtain floor E;
Step 6: being placed on 12h in steam boiler for floor E, and keep the relative humidity in steam boiler, obtain half at Product A;
Step 7: semi-finished product A is laid in steam boiler, and dry 12-24h obtains finished product.
Embodiment 1
As the preferred embodiment of the present invention: the humidity in step 1 and step 2 is 85%, and predetermined in step 1 Temperature is 120 degrees Celsius, and step 1 high temperature boiler reaches 120 degrees Celsius by 12-24h continuous heating, is added to floor Heat drying, is distilled out of floor internal moisture, and 85% humidity can prevent floor from occurring during the drying process in high-temperature boiler Depth carbonization, so as to cause the wood fibre in floor, withered, discoloration, without carrying out secondary operation after the drying, can make ground Plate color is more natural, beautiful, and when the floor in step 2 is dried, floor carries out in 120 degrees Celsius of steam boiler The drying of 8h is processed, and the moisture of floor deep layer can be baked out, the aridity of floor each section is made to reach similar state.
Embodiment 2
As the preferred embodiment of the present invention: the predetermined temperature in step 3 is 60 degrees Celsius, predetermined moisture 40%, step Cooling hydrofuge in rapid three is the purpose dried again to floor, prevents floor from occurring in the event of high temperatures for a long time Dry excessive problem, 60 degrees Celsius of temperature will not make floor occur deep layer carbonization, and preceding drying twice is by floor deep layer Moisture is dried to outer layer, and when drying again, in the state of relative low temperature, outer layer moisture is baked out, and reaches and does not damage ground intralamellar part Wood-fibred, and the purpose that moisture is dried as far as possible, and 40% humidity can be effectively prevented floor outer layer and be carbonized at this time, together When be also possible to prevent that outer moisture is excessively high to enter ground intralamellar part, the case where leading to moisture adverse current generation.
Embodiment 3
As the preferred embodiment of the present invention: the steam boiler temperature in step 6 is 50-60 degrees Celsius, and relative humidity is 10-12%, floor is at 50-60 degrees Celsius, and the water content on floor is in the environment of 10-12% at this time, and inside disperses extra Moisture is evaporated again, and external relative humidity can keep the humidity in floor to be not less than 10%, to keep floor Toughness and floor inside wood-fibred activity, up to 12h drying course in, the excessive moisture in floor is filled Divide drying, floor after drying repeatedly at this time, and the activity of wood-fibred having finalized the design almost inside floor toughness, color and floor, Floor deep layer moisture content is substantially equal with floor outer layer moisture content, so that the performance on floor be stablized, will not occur Form or otherwise physical change.
Embodiment 4
As the preferred embodiment of the present invention: the temperature of steam boiler is 50-55 degrees Celsius in step 7, and floor is in 50- When carrying out air-dried in 55 degrees Celsius of dry and ventilated room, it is that its outer layer moisture is subjected to last time drying, prevents outer layer moisture Excessively, floor is caused to be easy to happen mildew or damage, Improving The Quality of Products, if without 50-55 degrees Celsius of natural air drying, The remaining moisture of floor outer layer, after contacting with the air, so as to cause floor outer layer mildew, corrosion occur for mould easy to breed, If floor outer layer does not contain excessive moisture, at such a temperature, the moisture in floor will not be oven-dried, and not will lead to floor Nei Shui The problem for dividing content very few.
It is obvious to a person skilled in the art that invention is not limited to the details of the above exemplary embodiments, Er Qie In the case where without departing substantially from spirit or essential attributes of the invention, the present invention can be realized in other specific forms.Therefore, no matter From the point of view of which point, the present embodiments are to be considered as illustrative and not restrictive, and the scope of the present invention is by appended power Benefit requires rather than above description limits, it is intended that all by what is fallen within the meaning and scope of the equivalent elements of the claims Variation is included within the present invention.Any label in claim should not be construed as limiting the claims involved.

Claims (5)

1. the degreasing method on secondary degreasing floor, it is characterised in that: include the following steps:
Step 1: floor being put into the constant steam boiler of humidity and is heated up to predetermined temperature, and heating duration continues 12-24h, is obtained To floor A;
Step 2: floor A being continued to be placed in steam boiler and dries 8h, and keeps temperature, humidity in boiler constant, is obtained Floor B;
Step 3: cooling down to floor B, hydrofuge, after so that its temperature and humidity is reached predetermined temperature and predetermined moisture, makes floor B keeps 8h in the temperature and humidity, obtains floor C;
Step 4: water vapour is sprayed to floor C, obtains floor D;
Step 5: floor D is repeated Step 1: step 2 and step 3, obtain floor E;
Step 6: floor E is placed on 12h in steam boiler, and keeps the relative humidity in steam boiler, obtains semi-finished product A;
Step 7: semi-finished product A is laid in steam boiler, and dry 12-24h obtains finished product.
2. the degreasing method on secondary degreasing floor according to claim 1, it is characterised in that: the step 1 and step 2 Interior humidity is 85%, and the predetermined temperature in step 1 is 120 degrees Celsius.
3. the degreasing method on secondary degreasing floor according to claim 1, it is characterised in that: predetermined in the step 3 Temperature is 60 degrees Celsius, predetermined moisture 40%.
4. the degreasing method on secondary degreasing floor according to claim 1, it is characterised in that: the steam in the step 6 Boiler temperature is 50-60 degrees Celsius, and the water content on floor is 10-12% at this time.
5. the degreasing method on secondary degreasing floor according to claim 1, it is characterised in that: the steam in the step 7 The temperature of boiler is 50-55 degrees Celsius.
CN201910375037.5A 2019-05-07 2019-05-07 The degreasing method on secondary degreasing floor Pending CN110116445A (en)