CN109732726A - A kind of surface lacquer support wax Coating technology for outdoor desk-chair - Google Patents

A kind of surface lacquer support wax Coating technology for outdoor desk-chair Download PDF

Info

Publication number
CN109732726A
CN109732726A CN201910052124.7A CN201910052124A CN109732726A CN 109732726 A CN109732726 A CN 109732726A CN 201910052124 A CN201910052124 A CN 201910052124A CN 109732726 A CN109732726 A CN 109732726A
Authority
CN
China
Prior art keywords
chair
outdoor desk
parts
lacquer
outdoor
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910052124.7A
Other languages
Chinese (zh)
Inventor
金戟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Yuyao Rongda Plastic Industry Co Ltd
Original Assignee
Yuyao Rongda Plastic Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Yuyao Rongda Plastic Industry Co Ltd filed Critical Yuyao Rongda Plastic Industry Co Ltd
Priority to CN201910052124.7A priority Critical patent/CN109732726A/en
Publication of CN109732726A publication Critical patent/CN109732726A/en
Pending legal-status Critical Current

Abstract

The present invention relates to tables and chairs technical field of surface; more particularly to a kind of surface lacquer support wax Coating technology for outdoor desk-chair; solve the protectiveness existing in the prior art that cannot take into account technique of waxing and its excellent decorative disadvantage, comprising the following steps: S1 surface cleaning;S2 drains drying;S3 substrate sanding;S4 prime treatment;Bis- sandings of S5;The processing of S6 finishing coat;The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively carries out along the grain sanding to outdoor desk-chair;S8 waxes;The end S9 reason: repeating to uniformly spray processing solvent to the surface of outdoor desk-chair, and guarantees that the quantity for spray of single side is 10g/m2‑15g/m2, the present invention to outdoor desk-chair carry out three times sanding handle, and it is per treatment after carry out coast of paint processing; processing of waxing finally is carried out, compensates for the disadvantage of traditional coating protective difference of waxing, and remains preferable dicoration simultaneously; technique is convenient and simple, and production cost is low.

Description

A kind of surface lacquer support wax Coating technology for outdoor desk-chair
Technical field
The present invention relates to tables and chairs technical field of surface more particularly to a kind of surface lacquer support wax paintings for outdoor desk-chair Decorations technique.
Background technique
Outdoor desk-chair, which refers to, can be arranged multiple outdoor desk-chairs in gardens for outdoor tables and chairs, to facilitate the person of visiting a park to stop It has a rest, for outdoor desk-chair, it is easy to be influenced by extraneous wind and rain, therefore the surface performance of outdoor desk-chair is particularly important, family Outer tables and chairs when leaving the factory, mostly will do it the various processing of carry out on surface layer.
Although modern varnish Coating technology is good to the protectiveness of furniture surface, for having covered wooden original on hardwood furniture The excellent material having, in addition, hardwood furniture has the carved pattern of larger area more, common varnish covers with paint, lacquer, colour wash, etc. the life for hindering carved pattern Dynamic to show, technique of today cannot take into account the protectiveness and its excellent dicoration of technique of waxing, so that the technique of script can not Suitable for production requirement now.
Therefore, we have proposed a kind of surface lacquer support wax Coating technologies for outdoor desk-chair for solving the above problems.
Summary of the invention
The purpose of the present invention is to solve the protectiveness existing in the prior art that cannot take into account technique of waxing and its excellent Good decorative disadvantage, and a kind of surface lacquer support wax Coating technology for outdoor desk-chair proposed.
To achieve the goals above, present invention employs following technical solutions:
A method of the surface lacquer support wax for outdoor desk-chair is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: outdoor desk-chair is subjected to spray washing, washing times 2-3 times, and every 5- using deionized water 10min carries out a spray washing, and outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, the environment that intensity of illumination is 1.0*105lx-1.2*105lx is placed on Under, 40-60min is drained, drying to surface moisture is 5%-10%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 15g/m2-20g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 10g/m2-15g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
S8 waxes: taking beeswax to be put into heater and heats fusing, and rapidly uniformly puts the beeswax of fusing with suede brush and be coated in Then outdoor desk-chair surface is heated on one side with heat gun and keeps beeswax state, with suede brush, along the grain direction is uniform by beeswax on one side It smears out, guarantees that the applying amount of single side is 10g/m2-15g/m2, then use cold air blasting gun instead, brush outdoor desk-chair surface, cool down rapidly Beeswax state is condensed, wipes outdoor desk-chair surface with clean cotton yarn after the completion, the beeswax on outdoor desk-chair surface is received net;
The end S9 reason: repeating the surface of outdoor desk-chair to uniformly spray processing solvent, and guarantees that the quantity for spray of single side is 10g/m2-15g/m2
Preferably, in the S1, by outdoor desk-chair using deionized water carry out spray washing, washing times 2 times, and every 8min carries out a spray washing, and outdoor desk-chair surface clean is clean.
Preferably, in the S2, outdoor desk-chair is taken out, being placed on intensity of illumination is 1.1*105In the environment of lx, drain 50min, drying to surface moisture are 8%.
Preferably, in the S4, the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees final single side Quantity for spray is 18g/m2
Preferably, in the S6, the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees final single side Quantity for spray is 13g/m2
Preferably, the priming paint is PU paint, and the finishing coat is NC paint.
Preferably, it in the S8, takes beeswax to be put into heater and heats fusing, and is rapidly that the beeswax of fusing is equal with suede brush Then the beeswax state that keeps is heated on even spot printing tables and chairs surface outdoors with heat gun on one side, temperature is maintained at 30-45 DEG C, on one side With suede brush, along the grain direction uniformly smears out beeswax, guarantees that the applying amount of single side is 13g/m2, then use cold air blasting gun instead, brush family Outer tables and chairs surface is cooled to rapidly 5-15 DEG C of condensation beeswax state, outdoor desk-chair surface is wiped with clean cotton yarn after the completion, by family The beeswax on outer tables and chairs surface is received net.
Preferably, in the S9, the surface of outdoor desk-chair is repeated to uniformly spray processing solvent, and guarantee the spray of single side Painting amount is 13g/m2
Preferably, in the S9, processing solvent includes following component in parts by weight: 15-20 parts of potassium chlorate, methylol are fine Tie up plain 10-12 parts of sodium, 8-12 parts of boric acid, 8-10 parts of citric acid, 4-7 parts of polyvinyl alcohol, 5-9 parts of furfuryl alcohol, aqueous polyurethane emulsion 10-14 parts, 5-8 parts of fennel oil, 60-80 parts of water.
Preferably, in the S9, processing solvent includes following component in parts by weight: 18 parts of potassium chlorate, hydroxylmethyl cellulose 11 parts of plain sodium, 10 parts of boric acid, 9 parts of citric acid, 5 parts of polyvinyl alcohol, 7 parts of furfuryl alcohol, 12 parts of aqueous polyurethane emulsion, 6 parts of fennel oil, 70 parts of water.
Compared with prior art, the beneficial effects of the present invention are:
1, the present invention has carried out comprehensive cleaning to outdoor desk-chair, has avoided the table of the outdoor desk-chair of script at the beginning of processing Layer situation has an impact processing, and final effect is improved from source.
2, the present invention to outdoor desk-chair carry out three times sanding handle, and it is per treatment after carry out coast of paint processing, finally Processing of waxing is carried out, the disadvantage of traditional coating protective difference of waxing is compensated for, and remains preferable dicoration, technique side simultaneously Just simple, production cost is low.
3, the present invention has carried out the spraying of processing solvent in the tail end of processing, by handling solvent, carries out to outermost layer Processing, so that the outermost layer of outdoor desk-chair has the function of fungus-proof antisepsis, improves the quality of finally obtained outdoor desk-chair.
Detailed description of the invention
Fig. 1 is a kind of flow chart of the surface lacquer support wax Coating technology for outdoor desk-chair proposed by the present invention.
Specific embodiment
Unless otherwise defined, all technologies used herein and scientific term have and the common skill of fields of the present invention The normally understood identical meaning of art personnel.When there is a conflict, the definition in this specification shall prevail." quality, concentration, temperature What degree, time or other values or parameter were limited with range, preferred scope or a series of upper limit preferred values and lower preferable values When Range Representation, this be should be understood as specifically disclosing by any range limit or preferred value and any range lower limit or preferably Any pairing of value is formed by all ranges, regardless of whether the range separately discloses.For example, the range of 1-50 should be understood that Be include selected from 1,2,3,4,5,6,7,8,9,10,11,12,13,14,15,16,17,18,19,20,21,22,23,24,25, 26,27,28,29,30,31,32,33,34,35,36,37,38,39,40,41,42,43,44,45,46,47,48,49 or 50 Any number, number combinatorics on words or subrange and all fractional values between above-mentioned integer, for example, 1.1,1.2, 1.3,1.4,1.5,1.6,1.7,1.8 and 1.9.It is specific to consider the extension since any endpoint in range about subrange " nested subrange ".For example, the nested subrange of exemplary range 1-50 may include 1-10,1-20 on a direction, 1-30 and 1-40, or 50-40,50-30,50-20 and 50-10 in another direction."
Combined with specific embodiments below the present invention is made further to explain.
Embodiment one
The method that a kind of surface lacquer support wax for outdoor desk-chair proposed by the present invention is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: carrying out spray washing using deionized water for outdoor desk-chair, and washing times 2 times, and every 5min A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.0*105In the environment of lx, drain 40min, drying to surface moisture are 5%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 15g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 10g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
S8 waxes: taking beeswax to be put into heater and heats fusing, and rapidly uniformly puts the beeswax of fusing with suede brush and be coated in Then outdoor desk-chair surface is heated on one side with heat gun and keeps beeswax state, temperature is maintained at 30 DEG C, on one side along the grain with suede brush Direction uniformly smears out beeswax, guarantees that the applying amount of single side is 10g/m2, it then uses cold air blasting gun instead, brushes outdoor desk-chair surface, 5 DEG C of condensation beeswax states are cooled to rapidly, outdoor desk-chair surface are wiped with clean cotton yarn after the completion, by the bee on outdoor desk-chair surface Wax is received net;
The end S9 reason: repeating the surface of outdoor desk-chair to uniformly spray processing solvent, and guarantees that the quantity for spray of single side is 10g/m2
Further, processing solvent includes following component in parts by weight: 15 parts of potassium chlorate, sodium cellulose glycolate 10 Part, 8 parts of boric acid, 8 parts of citric acid, 4 parts of polyvinyl alcohol, 5 parts of furfuryl alcohol, 10 parts of aqueous polyurethane emulsion, 5 parts of fennel oil, 60 parts of water.
Embodiment two
The method that a kind of surface lacquer support wax for outdoor desk-chair proposed by the present invention is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: carrying out spray washing using deionized water for outdoor desk-chair, and washing times 2 times, and every 6min A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.1*105In the environment of lx, drain 45min, drying to surface moisture are 6%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 17g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 12g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
S8 waxes: taking beeswax to be put into heater and heats fusing, and rapidly uniformly puts the beeswax of fusing with suede brush and be coated in Then outdoor desk-chair surface is heated on one side with heat gun and keeps beeswax state, temperature is maintained at 35 DEG C, on one side along the grain with suede brush Direction uniformly smears out beeswax, guarantees that the applying amount of single side is 12g/m2, it then uses cold air blasting gun instead, brushes outdoor desk-chair surface, 7 DEG C of condensation beeswax states are cooled to rapidly, outdoor desk-chair surface are wiped with clean cotton yarn after the completion, by the bee on outdoor desk-chair surface Wax is received net;
The end S9 reason: repeating the surface of outdoor desk-chair to uniformly spray processing solvent, and guarantees that the quantity for spray of single side is 12g/m2
Further, processing solvent includes following component in parts by weight: 16 parts of potassium chlorate, sodium cellulose glycolate 11 Part, 9 parts of boric acid, 9 parts of citric acid, 5 parts of polyvinyl alcohol, 6 parts of furfuryl alcohol, 12 parts of aqueous polyurethane emulsion, 6 parts of fennel oil, 70 parts of water.
Embodiment three
The method that a kind of surface lacquer support wax for outdoor desk-chair proposed by the present invention is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: carrying out spray washing using deionized water for outdoor desk-chair, and washing times 2 times, and every 8min A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.1*105In the environment of lx, drain 50min, drying to surface moisture are 8%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 18g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 14g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
S8 waxes: taking beeswax to be put into heater and heats fusing, and rapidly uniformly puts the beeswax of fusing with suede brush and be coated in Then outdoor desk-chair surface is heated on one side with heat gun and keeps beeswax state, temperature is maintained at 40 DEG C, on one side along the grain with suede brush Direction uniformly smears out beeswax, guarantees that the applying amount of single side is 14g/m2, it then uses cold air blasting gun instead, brushes outdoor desk-chair surface, 10 DEG C of condensation beeswax states are cooled to rapidly, outdoor desk-chair surface are wiped with clean cotton yarn after the completion, by outdoor desk-chair surface Beeswax is received net;
The end S9 reason: repeating the surface of outdoor desk-chair to uniformly spray processing solvent, and guarantees that the quantity for spray of single side is 14g/m2
Further, processing solvent includes following component in parts by weight: 18 parts of potassium chlorate, sodium cellulose glycolate 11 Part, 11 parts of boric acid, 9 parts of citric acid, 6 parts of polyvinyl alcohol, 8 parts of furfuryl alcohol, 13 parts of aqueous polyurethane emulsion, 7 parts of fennel oil, water 75 Part.
Example IV
The method that a kind of surface lacquer support wax for outdoor desk-chair proposed by the present invention is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: carrying out spray washing using deionized water for outdoor desk-chair, and washing times 3 times, and every 10min A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.2*105In the environment of lx, drain 60min, drying to surface moisture are 10%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 20g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 15g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
S8 waxes: taking beeswax to be put into heater and heats fusing, and rapidly uniformly puts the beeswax of fusing with suede brush and be coated in Then outdoor desk-chair surface is heated on one side with heat gun and keeps beeswax state, temperature is maintained at 45 DEG C, on one side along the grain with suede brush Direction uniformly smears out beeswax, guarantees that the applying amount of single side is 15g/m2, it then uses cold air blasting gun instead, brushes outdoor desk-chair surface, 15 DEG C of condensation beeswax states are cooled to rapidly, outdoor desk-chair surface are wiped with clean cotton yarn after the completion, by outdoor desk-chair surface Beeswax is received net;
The end S9 reason: repeating the surface of outdoor desk-chair to uniformly spray processing solvent, and guarantees that the quantity for spray of single side is 15g/m2
Further, processing solvent includes following component in parts by weight: 20 parts of potassium chlorate, sodium cellulose glycolate 12 Part, 12 parts of boric acid, 10 parts of citric acid, 7 parts of polyvinyl alcohol, 9 parts of furfuryl alcohol, 14 parts of aqueous polyurethane emulsion, 8 parts of fennel oil, water 80 Part.
Comparative example one
A method of the surface lacquer support wax for outdoor desk-chair is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: carrying out spray washing using deionized water for outdoor desk-chair, and washing times 3 times, and every 10min A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.2*105In the environment of lx, drain 60min, drying to surface moisture are 10%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 20g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 15g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
The end S8 reason: repeating the surface of outdoor desk-chair to uniformly spray processing solvent, and guarantees that the quantity for spray of single side is 15g/m2
Further, processing solvent includes following component in parts by weight: 20 parts of potassium chlorate, sodium cellulose glycolate 12 Part, 12 parts of boric acid, 10 parts of citric acid, 7 parts of polyvinyl alcohol, 9 parts of furfuryl alcohol, 14 parts of aqueous polyurethane emulsion, 8 parts of fennel oil, water 80 Part.
Comparative example two
A method of the surface lacquer support wax for outdoor desk-chair is covered with paint, lacquer, colour wash, etc., comprising the following steps:
S1 surface cleaning: carrying out spray washing using deionized water for outdoor desk-chair, and washing times 3 times, and every 10min A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.2*105In the environment of lx, drain 60min, drying to surface moisture are 10%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sand successively is carried out to outdoor desk-chair Light;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees the spraying of final single side Amount is 20g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees the spraying of final single side Amount is 15g/m2
The sanding of the end S7: carrying out sanding again, and using the sand paper of 300#, 250#, 200# model, successively to outdoor desk-chair into Row along the grain sanding;
S8 waxes: taking beeswax to be put into heater and heats fusing, and rapidly uniformly puts the beeswax of fusing with suede brush and be coated in Then outdoor desk-chair surface is heated on one side with heat gun and keeps beeswax state, temperature is maintained at 45 DEG C, on one side along the grain with suede brush Direction uniformly smears out beeswax, guarantees that the applying amount of single side is 15g/m2, it then uses cold air blasting gun instead, brushes outdoor desk-chair surface, 15 DEG C of condensation beeswax states are cooled to rapidly, outdoor desk-chair surface are wiped with clean cotton yarn after the completion, by outdoor desk-chair surface Beeswax is received net.
Above-described embodiment one to example IV, comparative example one and comparative example two are detected, as a result as follows:
The foregoing is only a preferred embodiment of the present invention, but scope of protection of the present invention is not limited thereto, Anyone skilled in the art in the technical scope disclosed by the present invention, according to the technique and scheme of the present invention and its Inventive concept is subject to equivalent substitution or change, should be covered by the protection scope of the present invention.

Claims (10)

1. a kind of method that the surface lacquer support wax for outdoor desk-chair is covered with paint, lacquer, colour wash, etc., which comprises the following steps:
S1 surface cleaning: outdoor desk-chair is subjected to spray washing, washing times 2-3 times, and every 5-10min using deionized water A spray washing is carried out, outdoor desk-chair surface clean is clean;
S2 drains drying: outdoor desk-chair being taken out, being placed on intensity of illumination is 1.0*105lx-1.2*105In the environment of lx, drain 40-60min, drying to surface moisture are 5%-10%;
S3 substrate sanding: using the sand paper of 1200#, 1000#, 800# model, along the grain sanding successively is carried out to outdoor desk-chair;
S4 prime treatment: the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees that the quantity for spray of final single side is 15g/m2-20g/m2
Bis- sandings of S5: using the sand paper of 600#, 500#, 400# model, along the grain sanding successively is carried out to outdoor desk-chair;
The processing of S6 finishing coat: the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees that the quantity for spray of final single side is 10g/m2-15g/m2
The sanding of the end S7: carrying out sanding, and using the sand paper of 300#, 250#, 200# model again, successively carries out to outdoor desk-chair suitable Wood grain sanding;
S8 waxes: take beeswax be put into heater heat fusing, and with suede brush rapidly by the uniform spot printing of the beeswax of fusing outdoors Then tables and chairs surface is heated on one side with heat gun and keeps beeswax state, with suede brush, along the grain direction uniformly smears out beeswax on one side, The applying amount for guaranteeing single side is 10g/m2-15g/m2, then use cold air blasting gun instead, brush outdoor desk-chair surface, rapidly cooling condensation bee Wax-like state wipes outdoor desk-chair surface with clean cotton yarn after the completion, the beeswax on outdoor desk-chair surface is received net;
The end S9 reason: repeating to uniformly spray processing solvent to the surface of outdoor desk-chair, and guarantees that the quantity for spray of single side is 10g/ m2-15g/m2
2. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S1, outdoor desk-chair is subjected to spray washing using deionized water, washing times 2 times, and once sprayed every 8min Washing, outdoor desk-chair surface clean is clean.
3. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S2, outdoor desk-chair is taken out, being placed on intensity of illumination is 1.1*105In the environment of lx, 50min is drained, it is dry to surface Water content is 8%.
4. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S4, the surface of tables and chairs carries out the spraying of priming paint manually outdoors, and guarantees that the quantity for spray of final single side is 18g/m2
5. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S6, the surface of tables and chairs carries out the spray painting of finishing coat manually outdoors, and guarantees that the quantity for spray of final single side is 13g/m2
6. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute Priming paint is stated as PU paint, the finishing coat is NC paint.
7. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S8, takes beeswax to be put into heater and heat fusing, and with suede brush rapidly by the uniform spot printing of the beeswax of fusing tables and chairs outdoors Then surface is heated on one side with heat gun and keeps beeswax state, temperature is maintained at 30-45 DEG C, on one side with suede brush along the grain direction Beeswax is uniformly smeared out, guarantees that the applying amount of single side is 13g/m2, then use cold air blasting gun instead, brush outdoor desk-chair surface, rapidly It is cooled to 5-15 DEG C of condensation beeswax state, wipes outdoor desk-chair surface with clean cotton yarn after the completion, by the bee on outdoor desk-chair surface Wax is received net.
8. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S9, the surface of outdoor desk-chair is repeated to uniformly spray processing solvent, and guarantee that the quantity for spray of single side is 13g/m2
9. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that institute It states in S9, processing solvent includes following component in parts by weight: 15-20 parts of potassium chlorate, 10-12 parts of sodium cellulose glycolate, boron 8-12 parts sour, 8-10 parts of citric acid, 4-7 parts of polyvinyl alcohol, 5-9 parts of furfuryl alcohol, 10-14 parts of aqueous polyurethane emulsion, fennel oil 5-8 Part, 60-80 parts of water.
10. the method that a kind of surface lacquer support wax for outdoor desk-chair according to claim 1 is covered with paint, lacquer, colour wash, etc., which is characterized in that In the S9, processing solvent includes following component in parts by weight: 18 parts of potassium chlorate, 11 parts of sodium cellulose glycolate, boric acid 10 Part, 9 parts of citric acid, 5 parts of polyvinyl alcohol, 7 parts of furfuryl alcohol, 12 parts of aqueous polyurethane emulsion, 6 parts of fennel oil, 70 parts of water.
CN201910052124.7A 2019-01-21 2019-01-21 A kind of surface lacquer support wax Coating technology for outdoor desk-chair Pending CN109732726A (en)