CN109021828A - A kind of environmental protection steel component heat expansion-proof coating and preparation method thereof - Google Patents

A kind of environmental protection steel component heat expansion-proof coating and preparation method thereof Download PDF

Info

Publication number
CN109021828A
CN109021828A CN201810938247.6A CN201810938247A CN109021828A CN 109021828 A CN109021828 A CN 109021828A CN 201810938247 A CN201810938247 A CN 201810938247A CN 109021828 A CN109021828 A CN 109021828A
Authority
CN
China
Prior art keywords
parts
calgon
paraffin
butyl ether
thickener
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201810938247.6A
Other languages
Chinese (zh)
Inventor
童庆军
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nanjing Li Tong Heavy Machinery Co Ltd
Original Assignee
Nanjing Li Tong Heavy Machinery Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nanjing Li Tong Heavy Machinery Co Ltd filed Critical Nanjing Li Tong Heavy Machinery Co Ltd
Priority to CN201810938247.6A priority Critical patent/CN109021828A/en
Publication of CN109021828A publication Critical patent/CN109021828A/en
Withdrawn legal-status Critical Current

Abstract

The invention discloses a kind of Thermal expansion coating for environment-friendly anti-steel member, each component including following mass fraction: 6-10 parts of propylene glycol n-butyl ether;0.1-0.8 parts of calgon;0.3-0.9 parts of sodium tripolyphosphate;12-22 parts of paraffin;0.1-0.5 parts of thickener;18-28 parts of water.Meanwhile the invention discloses the preparation methods of the coating.Coating of the present invention has the characteristics that property stabilization, asepsis environment-protecting.

Description

A kind of environmental protection steel component heat expansion-proof coating and preparation method thereof
Technical field
The present invention relates to steel member field more particularly to a kind of Thermal expansion coating for environment-friendly anti-steel member and its preparation sides Method.
Background technique
At high temperature, steel anchoring piece is easy expansion, and overcoat fusing there are gaps, is not easy steel because dilation is pre- Refractory material processed destroys.When heated, because steel expand, prefabricated component cracks most of preform products, peels off, steel construction It is burned, makes scrap of the product, cause to waste.
Traditional steel construction coating process: it one is with plastic film, swathes in steel structure surface;Another kind is to use pitch It is brushed on one layer.It is wherein swathed with plastic film, time-consuming, laborious, when casting is also easy to fall off;It is smeared with pitch, when baking has Special odor was heated to 260 DEG C after 5 hours, contained by the ingredients such as anthracene, phenanthrene, pyrene will evaporate, these ingredients are Toxic, air is polluted, the body of injury people is easy.
Currently, also lacking environmentally friendly effective steel member heat expansion-proof coating.
Summary of the invention
Goal of the invention: in view of the deficiencies of the prior art with defect, the present invention provides a kind of environment-friendly type anti-steel member thermal expansion Coating and preparation method thereof, the coating of preparation have the characteristics that property stabilization, asepsis environment-protecting.
A kind of technical solution: Thermal expansion coating for environment-friendly anti-steel member of the invention, it is characterised in that: including following quality The each component of number: 6-10 parts of propylene glycol n-butyl ether;0.1-0.8 parts of calgon;0.3-0.9 parts of sodium tripolyphosphate;Paraffin 12-22 parts;0.1-0.5 parts of thickener;18-28 parts of water.
Preferably, each component including following mass fraction: 6 parts of propylene glycol n-butyl ether;0.1 part of calgon;Trimerization 0.3 part of sodium phosphate;12 parts of paraffin;0.1 part of thickener;18 parts of water.
Preferably, each component including following mass fraction: 10 parts of propylene glycol n-butyl ether;0.8 part of calgon;Trimerization 0.9 part of sodium phosphate;22 parts of paraffin;0.5 part of thickener;28 parts of water.
Preferably, each component including following mass fraction: 8 parts of propylene glycol n-butyl ether;0.5 part of calgon;Trimerization 0.6 part of sodium phosphate;16 parts of paraffin;0.3 part of thickener;24 parts of water.
A kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member, it is characterised in that: include the following steps:
(1) according to 6-10 parts of propylene glycol n-butyl ether;0.1-0.8 parts of calgon;0.3-0.9 parts of sodium tripolyphosphate;Stone 12-22 parts of wax;0.1-0.5 parts of thickener;The mass fraction that 18-28 parts of water prepares each component;
(2) dispersion liquid is added propylene glycol n-butyl ether, paraffin, thickening in agitator after stirring 800rpm-1000rpm Agent, water are added in agitator, and adjusting viscosity is 160-200 unit, obtain the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.
The utility model has the advantages that compared with prior art, the present invention has a kind of following remarkable advantage: environment-friendly type provided by the invention Anti- steel member thermally expands coating and provides the preparation method of the coating, which has the characteristics that property stabilization, asepsis environment-protecting; This method has the characteristics that easy to operate, at low cost.
Specific embodiment
Technical solution of the present invention is further described With reference to embodiment.
Embodiment 1:
A kind of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, each component including following mass fraction: the third two 6 parts of alcohol n-butyl ether;0.1 part of calgon;0.3 part of sodium tripolyphosphate;12 parts of paraffin;0.1 part of thickener;18 parts of water.
A kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, includes the following steps:
(1) according to 6 parts of propylene glycol n-butyl ether;0.1 part of calgon;0.3 part of sodium tripolyphosphate;12 parts of paraffin;Thickening 0.1 part of agent;The mass fraction that 18 parts of water prepares each component;
(2) dispersion liquid is added in agitator after stirring 800rpm and propylene glycol n-butyl ether, paraffin, thickener, water is added In agitator, adjusting viscosity is 160 units, obtains the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.
Embodiment 2:
A kind of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, each component including following mass fraction: the third two 10 parts of alcohol n-butyl ether;0.8 part of calgon;0.9 part of sodium tripolyphosphate;22 parts of paraffin;0.5 part of thickener;28 parts of water.
A kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, includes the following steps:
(1) according to 10 parts of propylene glycol n-butyl ether;0.8 part of calgon;0.9 part of sodium tripolyphosphate;22 parts of paraffin;Thickening 0.5 part of agent;The mass fraction that 28 parts of water prepares each component;
(2) dispersion liquid is added in agitator after stirring 1000rpm and propylene glycol n-butyl ether, paraffin, thickener, water is added In agitator, adjusting viscosity is 200 units, obtains the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.
Embodiment 3:
A kind of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, each component including following mass fraction: the third two 8 parts of alcohol n-butyl ether;0.5 part of calgon;0.6 part of sodium tripolyphosphate;16 parts of paraffin;0.3 part of thickener;24 parts of water.
A kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, includes the following steps:
(1) according to 8 parts of propylene glycol n-butyl ether;0.5 part of calgon;0.6 part of sodium tripolyphosphate;16 parts of paraffin;Thickening 0.3 part of agent;The mass fraction that 24 parts of water prepares each component;
(2) dispersion liquid is added in agitator after stirring 900rpm and propylene glycol n-butyl ether, paraffin, thickener, water is added In agitator, adjusting viscosity is 180 units, obtains the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.
Embodiment 4:
A kind of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, each component including following mass fraction: the third two 7 parts of alcohol n-butyl ether;0.3 part of calgon;0.4 part of sodium tripolyphosphate;15 parts of paraffin;0.2 part of thickener;20 parts of water.
A kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, includes the following steps:
(1) according to 7 parts of propylene glycol n-butyl ether;0.3 part of calgon;0.4 part of sodium tripolyphosphate;15 parts of paraffin;Thickening 0.2 part of agent;The mass fraction that 20 parts of water prepares each component;
(2) dispersion liquid is added in agitator after stirring 850rpm and propylene glycol n-butyl ether, paraffin, thickener, water is added In agitator, adjusting viscosity is 165 units, obtains the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.
Embodiment 5:
A kind of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, each component including following mass fraction: the third two 9 parts of alcohol n-butyl ether;0.7 part of calgon;0.8 part of sodium tripolyphosphate;20 parts of paraffin;0.4 part of thickener;26 parts of water.
A kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member of the present embodiment, includes the following steps:
(1) according to 9 parts of propylene glycol n-butyl ether;0.7 part of calgon;0.8 part of sodium tripolyphosphate;20 parts of paraffin;Thickening 0.4 part of agent;The mass fraction that 26 parts of water prepares each component;
(2) dispersion liquid is added in agitator after stirring 950rpm and propylene glycol n-butyl ether, paraffin, thickener, water is added In agitator, adjusting viscosity is 190 units, obtains the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.

Claims (5)

1. a kind of Thermal expansion coating for environment-friendly anti-steel member, it is characterised in that: each component including following mass fraction: propylene glycol 6-10 parts of n-butyl ether;0.1-0.8 parts of calgon;0.3-0.9 parts of sodium tripolyphosphate;12-22 parts of paraffin;Thickener 0.1- 0.5 part;18-28 parts of water.
2. a kind of Thermal expansion coating for environment-friendly anti-steel member according to claim 1, it is characterised in that: including following quality The each component of number: 6 parts of propylene glycol n-butyl ether;0.1 part of calgon;0.3 part of sodium tripolyphosphate;12 parts of paraffin;Thickener 0.1 part;18 parts of water.
3. a kind of Thermal expansion coating for environment-friendly anti-steel member according to claim 1, it is characterised in that: including following quality The each component of number: 10 parts of propylene glycol n-butyl ether;0.8 part of calgon;0.9 part of sodium tripolyphosphate;22 parts of paraffin;Thickener 0.5 part;28 parts of water.
4. a kind of Thermal expansion coating for environment-friendly anti-steel member according to claim 1, it is characterised in that: including following quality The each component of number: 8 parts of propylene glycol n-butyl ether;0.5 part of calgon;0.6 part of sodium tripolyphosphate;16 parts of paraffin;Thickener 0.3 part;24 parts of water.
5. a kind of preparation method of Thermal expansion coating for environment-friendly anti-steel member, it is characterised in that: include the following steps:
(1) according to 6-10 parts of propylene glycol n-butyl ether;0.1-0.8 parts of calgon;0.3-0.9 parts of sodium tripolyphosphate;Paraffin 12- 22 parts;0.1-0.5 parts of thickener;The mass fraction that 18-28 parts of water prepares each component;
(2) dispersion liquid is added propylene glycol n-butyl ether, paraffin, thickener, water in agitator after stirring 800rpm-1000rpm It is added in agitator, adjusting viscosity is 160-200 unit, obtains the first mixture;
(3) calgon is added into the first mixture to be uniformly mixed with sodium tripolyphosphate, obtains coating products.
CN201810938247.6A 2018-08-17 2018-08-17 A kind of environmental protection steel component heat expansion-proof coating and preparation method thereof Withdrawn CN109021828A (en)