CN108381372A - A kind of medium temperature pearl polishing method - Google Patents

A kind of medium temperature pearl polishing method Download PDF

Info

Publication number
CN108381372A
CN108381372A CN201810262302.4A CN201810262302A CN108381372A CN 108381372 A CN108381372 A CN 108381372A CN 201810262302 A CN201810262302 A CN 201810262302A CN 108381372 A CN108381372 A CN 108381372A
Authority
CN
China
Prior art keywords
polishing
stir
pearl
degree
frying
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201810262302.4A
Other languages
Chinese (zh)
Other versions
CN108381372B (en
Inventor
戚鸟定
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhejiang Tears Of Angels Pearl Co ltd
Original Assignee
Zhejiang Tears Of Angels Pearl Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Zhejiang Tears Of Angels Pearl Co ltd filed Critical Zhejiang Tears Of Angels Pearl Co ltd
Priority to CN201810262302.4A priority Critical patent/CN108381372B/en
Publication of CN108381372A publication Critical patent/CN108381372A/en
Application granted granted Critical
Publication of CN108381372B publication Critical patent/CN108381372B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of medium temperature pearl polishing methods, include the following steps:A) by pearl by heating devices heat, heating temperature is:60~70 degree, heating time is:20~30 minutes;B) polishing material is poured into burnishing device, and starts burnishing device operation, burnishing device operating temperature is made to reach 60~70 degree;C) pearl heated is poured into burnishing device and is polished, and ensure 60~70 degree of operating temperature until polishing is completed;Compared with prior art, can polishing effect it is good, work efficiency is high.

Description

A kind of medium temperature pearl polishing method
【Technical field】
The present invention relates to a kind of medium temperature pearl polishing methods, belong to pearl processing technique field.
【Background technology】
Pearl is a kind of organic gemstone, and from the point of view of the principle of polishing, pearl is different from other gem and jades.Other class gem and jades It is mechanism (levigate), chemical action (formation surface plasticity if the polishing process of diamond, jade is a kind of process of grinding Layer or deliquescent layer and molecular layer are spread again) and physics chemical action (materialization between polishing agent, water and jewel entry material is anti- Answer) process.And pearl polishing is a kind of process for being ground and replenishing.On the one hand, polishing carrier can be ground the recessed of pearl surface Convex injustice keeps pearl surface more smooth;On the other hand, by bright substance (i.e. wax) replenish pearl surface micro-pore and In surface defect so that light is kept when pearl surface is propagated successively, to improve the intensity of light reflection of pearl surface.With Society's continuous development, the polishing of traditional pearl can no longer meet needs, good, work effect that therefore, it is necessary to a kind of polishing effects The high medium temperature pearl polishing method of rate.
【Invention content】
The purpose of the present invention is exactly to solve the problems of the prior art, proposes that a kind of polishing effect is good, work efficiency is high Medium temperature pearl polishing method.
To achieve the above object, the present invention proposes a kind of medium temperature pearl polishing method, includes the following steps:
A) by pearl by heating devices heat, heating temperature is:60~70 degree, heating time is:20~30 minutes;
B) polishing material is poured into burnishing device, and starts burnishing device operation, burnishing device operating temperature is made to reach 60~70 degree;
C) pearl heated is poured into burnishing device and is polished, and ensure 60~70 degree of operating temperature until throwing Light is completed;
The polishing material is formed after being dried by the polishing carrier particle after polishing fluid immersion treatment, and soaking temperature is:60 ~70 degree, soaking time is:1~2 hour, the polishing carrier particle was walnut shell or is made of cork oak and cork oak shell Vegetable cork be made, the quality proportioning of the cork oak and cork oak shell is 5:3;
The quality proportioning of each component of the polishing fluid is:Paraffin:3~5 parts, ethyl alcohol:80~90 parts, glycerine:1~3 part, Stearic acid:1~2 part;
The burnishing device includes lower bottom base, several springs, vibrating motor, vibrating disk, several stir-frying devices and upper bed-plate, The upper end of the pedestal is equipped with the circumferentially equally distributed spring of shape, and the upper end of the spring is equipped with upper bed-plate, the upper bed-plate It is equipped with vibrating motor and vibrating disk, the vibrating motor is located at the centre of vibrating disk, stir-frying device is equipped in the vibrating disk, Cavity is formed in the vibrating disk, the rear and front end of the vibrating disk is respectively equipped with the inlet and outlet being connected to cavity, institute It includes motor, mounting base and stir-frying mechanism to state stir-frying device, and the mounting base is fixed on the upper end of the charge slot of vibrating disk, described Mounting base is equipped with motor, and the rotation axis of the motor is equipped with stir-frying mechanism, if the stir-frying mechanism includes connecting seat, involvement The circumferential surface of junctor, several stir-frying plates and several hairbrush, the connecting seat is equipped with equally distributed connector, the connector Free end is equipped with stir-frying plate, and the free end of the stir-frying plate is equipped with hairbrush.
Preferably, the heating temperature in a) step is:65 degree, heating time is:25 minutes.
Preferably, the soaking temperature is:65 degree, soaking time is:1.5 hour.
Preferably, the quality proportioning of each component of the polishing fluid is:Paraffin:4 parts, ethyl alcohol:85 parts, glycerine:2 parts, Stearic acid:1.5 part.
Preferably, b) the step and c) operating temperature in step is:65 degree.
Beneficial effects of the present invention:The present invention is by using walnut shell or the cork being made of cork oak and cork oak shell Polishing carrier particle is made in material, and is impregnated in 60~70 degree of polishing fluid, ensures to improve processing speed while adsorbance, Pearl is not damaged and ensures polishing effect, and the formula of polishing fluid can increase the lubricity of polishing material, increase the light of pearl It spends, burnishing device ensures the dispersion effect of pearl and polishing material, further increases polishing effect and working efficiency at work, Compared with prior art, can polishing effect it is good, work efficiency is high.
The feature and advantage of the present invention will be described in detail by embodiment combination attached drawing.
【Description of the drawings】
Fig. 1 is the structural schematic diagram of burnishing device.
In figure:1- lower bottom bases, 2- springs, 3- vibrating motors, 4- vibrating disks, 5- stir-frying device, 6- upper bed-plates, 7- cavitys, 8- imports, the outlets 9-.
【Specific implementation mode】
Embodiment 1
A) by pearl by heating devices heat, heating temperature is:65 degree, heating time is:25 minutes;
B) polishing material is poured into burnishing device, and starts burnishing device operation, burnishing device operating temperature is made to reach 65 degree;
C) pearl heated is poured into burnishing device and is polished, and ensure 65 degree of operating temperature until having polished At;
The polishing material is formed after being dried by the polishing carrier particle after polishing fluid immersion treatment, and soaking temperature is:65 Degree, soaking time are:1.5 hours, the polishing carrier particle was walnut shell;
The quality proportioning of each component of the polishing fluid is:Paraffin:4 parts, ethyl alcohol:85 parts, glycerine:2 parts, stearic acid:1.5 Part;
Paraffin, ethyl alcohol, glycerine and stearic acid are added in mixing vessel according to above-mentioned quality proportioning for the preparation of polishing fluid, Then heating is uniformly mixed, and heating mixing temperature is 50 degree.
Embodiment 2
A) by pearl by heating devices heat, heating temperature is:65 degree, heating time is:25 minutes;
B) polishing material is poured into burnishing device, and starts burnishing device operation, burnishing device operating temperature is made to reach 65 degree;
C) pearl heated is poured into burnishing device and is polished, and ensure 65 degree of operating temperature until having polished At;
The polishing material is formed after being dried by the polishing carrier particle after polishing fluid immersion treatment, and soaking temperature is:65 Degree, soaking time are:1.5 hours, the vegetable cork that the polishing carrier particle is made of cork oak and cork oak shell was made, The quality proportioning of the cork oak and cork oak shell is 5:3;
The quality proportioning of each component of the polishing fluid is:Paraffin:4 parts, ethyl alcohol:85 parts, glycerine:2 parts, stearic acid:1.5 Part;
Paraffin, ethyl alcohol, glycerine and stearic acid are added in mixing vessel according to above-mentioned quality proportioning for the preparation of polishing fluid, Then heating is uniformly mixed, and heating mixing temperature is 50 degree.
Refering to fig. 1, the burnishing device includes lower bottom base 1, several springs 2, vibrating motor 3, vibrating disk 4, several stir-fryings Device 5 and upper bed-plate 6, the upper end of the pedestal 1 is equipped with circumferentially the equally distributed spring 2 of shape, the upper end of the spring 2 are equipped with Upper bed-plate 6, the upper bed-plate 6 are equipped with vibrating motor 3 and vibrating disk 4, and the vibrating motor 3 is located at the centre of vibrating disk 4, institute It states and is equipped with stir-frying device 5 in vibrating disk 4, be formed with cavity 7 in the vibrating disk 4, the rear and front end of the vibrating disk 4 is set respectively There are the import 8 being connected to cavity 7 and outlet 9, the stir-frying device 5 includes motor 51, mounting base 52 and stir-frying mechanism 53, described Mounting base 52 is fixed on the upper end of the charge slot of vibrating disk 4, and the mounting base 52 is equipped with motor 51, the rotation of the motor 51 Axis is equipped with stir-frying mechanism 53, and the stir-frying mechanism 53 includes connecting seat 531, several connectors 532, several 533 and of stir-frying plate The circumferential surface of several hairbrush 534, the connecting seat 531 is equipped with equally distributed connector 532, the freedom of the connector 532 End is equipped with stir-frying plate 533, and the free end of the stir-frying plate 533 is equipped with hairbrush 534.
In the burnishing device course of work, polishing material is poured into burnishing device, and starts burnishing device operation, heating is situated between Matter flows into cavity 7 from import 8 and is heated to vibrating disk 4, then after 9 outflow of outlet, operating temperature to be achieved, after heating Pearl pour into vibrating disk 4, then start motor 51 drive stir-frying mechanism 53 rotate, through stir-frying plate 533 pearl and polishing Material is stir-fried by the plate 533 that stir-fries, and improves the dispersion effect of pearl and polishing material.
Above-described embodiment is the description of the invention, is not limitation of the invention, it is any to simple transformation of the present invention after Scheme all belong to the scope of protection of the present invention.

Claims (5)

1. a kind of medium temperature pearl polishing method, it is characterised in that:Include the following steps:
A) by pearl by heating devices heat, heating temperature is:60~70 degree, heating time is:20~30 minutes;
B) polishing material is poured into burnishing device, and starts burnishing device operation, make burnishing device operating temperature reach 60~ 70 degree;
C) pearl heated is poured into burnishing device and is polished, and ensure 60~70 degree of operating temperature until having polished At;
The polishing material is formed after being dried by the polishing carrier particle after polishing fluid immersion treatment, and soaking temperature is:60~70 Degree, soaking time are:1~2 hour, the polishing carrier particle was walnut shell or is made of cork oak and cork oak shell soft Wood material is made, and the quality proportioning of the cork oak and cork oak shell is 5:3;
The quality proportioning of each component of the polishing fluid is:Paraffin:3~5 parts, ethyl alcohol:80~90 parts, glycerine:1~3 part, tristearin Acid:1~2 part;
The burnishing device includes lower bottom base (1), several springs (2), vibrating motor (3), vibrating disk (4), several stir-frying devices (5) and upper bed-plate (6), the upper end of the pedestal (1) is equipped with the circumferentially equally distributed spring of shape (2), the spring (2) it is upper End is equipped with upper bed-plate (6), and the upper bed-plate (6) is equipped with vibrating motor (3) and vibrating disk (4), and the vibrating motor (3) is located at The centre of vibrating disk (4), the vibrating disk (4) is interior to be equipped with stir-frying device (5), and cavity (7) is formed in the vibrating disk (4), The rear and front end of the vibrating disk (4) is respectively equipped with the import (8) being connected to cavity (7) and outlet (9), the stir-frying device (5) include motor (51), mounting base (52) and stir-frying mechanism (53), the mounting base (52) is fixed on the charge of vibrating disk (4) The upper end of slot, the mounting base (52) are equipped with motor (51), and the rotation axis of the motor (51) is equipped with stir-frying mechanism (53), The stir-frying mechanism (53) includes connecting seat (531), several connectors (532), several stir-frying plates (533) and several hairbrush (534), the circumferential surface of the connecting seat (531) is equipped with equally distributed connector (532), the freedom of the connector (532) End is equipped with stir-frying plate (533), and the free end of the stir-frying plate (533) is equipped with hairbrush (534).
2. a kind of medium temperature pearl polishing method as described in claim 1, it is characterised in that:Heating temperature in a) step For:65 degree, heating time is:25 minutes.
3. a kind of medium temperature pearl polishing method as described in claim 1, it is characterised in that:The soaking temperature is:65 degree, leaching Bubble the time be:1.5 hour.
4. a kind of medium temperature pearl polishing method as described in claim 1, it is characterised in that:The matter of each component of the polishing fluid Amount matches:Paraffin:4 parts, ethyl alcohol:85 parts, glycerine:2 parts, stearic acid:1.5 part.
5. a kind of medium temperature pearl polishing method according to any one of claims 1 to 4, it is characterised in that:B) the step And c) operating temperature in step is:65 degree.
CN201810262302.4A 2018-03-28 2018-03-28 Medium-temperature pearl polishing method Expired - Fee Related CN108381372B (en)