CN108251934A - A kind of production method of skin makeup fiber blended color yarn - Google Patents

A kind of production method of skin makeup fiber blended color yarn Download PDF

Info

Publication number
CN108251934A
CN108251934A CN201710980288.7A CN201710980288A CN108251934A CN 108251934 A CN108251934 A CN 108251934A CN 201710980288 A CN201710980288 A CN 201710980288A CN 108251934 A CN108251934 A CN 108251934A
Authority
CN
China
Prior art keywords
fiber
skin makeup
water
production method
minutes
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201710980288.7A
Other languages
Chinese (zh)
Inventor
吴炳华
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhuhai Li Lian Textile And Dyeing Industry Co Ltd
Original Assignee
Zhuhai Li Lian Textile And Dyeing Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Zhuhai Li Lian Textile And Dyeing Industry Co Ltd filed Critical Zhuhai Li Lian Textile And Dyeing Industry Co Ltd
Priority to CN201710980288.7A priority Critical patent/CN108251934A/en
Publication of CN108251934A publication Critical patent/CN108251934A/en
Pending legal-status Critical Current

Abstract

Production method more particularly to one kind the invention discloses a kind of skin makeup fiber blended color yarn is easy to process, is not required to device upgrade, the production method of economic and practical skin makeup fiber blended color yarn.The technological process of the present invention is stock-dye, weighing, batch mixing, cotton carding, drafting, rove, spun yarn, winder, doubling, double twisting.Present invention is mainly used for field of textiles.

Description

A kind of production method of skin makeup fiber blended color yarn
Technical field
The present invention relates to field of textiles more particularly to a kind of production methods of skin makeup fiber blended color yarn.
Background technology
Skin makeup fiber (UMORFIL) is the functional fiber that Taibei high-tech textile company Camangi was researched and developed in 2012, Its raw material is the collagen in fish scale, and is a kind of decomposable new machine using biotechnology by being bonded with viscose rayon It can environment-protection fiber.The natural collagen protein amino acid contained in fiber so that using skin makeup fiber as the textile pro-skin of raw material, have Conducive to health, skin can be made more smooth, more high resilience, and promote blood circulation, a crucial advantage is this original Collagen, amino acid can still keep activity after expecting multiple wash water, high-performance more than the functional characteristic Bi Xu of this expression skin makeup fiber Fiber and fabric are more longlasting, the day of the characteristic of the latter often by coating technology or substrate powder rather than fiber in itself What right ingredient was realized.There is another this fiber the moisture absorption of the gloss as silk, the soft lubrication, flaxen fiber as cashmere the spies such as to breathe freely Point, disclosure satisfy that people to dress ornament naturalization, comfortableization, personalization pursuit.But existing skin makeup fiber openpore dyeing yarn Color is single, if with the openpore yarn or fabric of the fiber blends such as cotton, wool or cashmere to cotton, wool or cashmere When other fibers carry out co-bathing dyeing processing, different performance raw material is also easy to produce in co-bathing dyeing paints irregular and causes fiber Dyeing defect, aberration, and co-bathing dyeing because the dyeing time it is long, easily the collagen in skin makeup fiber is damaged, makes U.S. Skin fiber hardens, is tendering, it is impossible to fully demonstrate skin makeup fiber softening, the characteristic that pro-skin, smooth, moisture absorption are breathed freely, and base yarn or Piece dyeing finishing cannot get abundant color.
Invention content
The invention discloses a kind of production method of skin makeup fiber blended color yarn, to solve the deficiencies in the prior art.
To solve the above problems, the technical solution of the present invention is:
A kind of production method of skin makeup fiber blended color yarn, production method are:A, stock-dye, first by skin makeup fibre Dimension carries out dyeing pre-treatment, then carries out dyeing process, color fixing process of followed by soaping, and it is complete finally to carry out soft finish technique Into stock-dye;
B, weighing needs to weigh fiber using dry ratio according to product;
The fiber weighed is carried out laying mixing, adds in 2%~6% water, mixed fiber is in closed-loop by c, batch mixing It is placed under border 12~36 hours and carries out health;
Raw material after batch mixing is combed into 15~22 grams/5 meters by d, cotton carding on flat top card, and doffing speed 18~ 26 revs/min of the carded sliver;
E, drafting carries out three on drawing frame and obtains 15~22 grams/5 meters with drawing-off, and with radical 6~8, drawing-off The ripe bar that 6~8 times of multiple;
Ripe bar draw twisting after drafting is wound into 5~8 grams/10 meters, drafting multiple 5~8 by f, rove on fly frame Times, the rove that 30~60 twists/m of the twist;
G, spun yarn twists roving-drafting into 1.67~3.57 grams/100 meters on spinning frame, 15~35 times of drafting multiple, The spun yarn that 500~1000 twists/m of the twist;
Spun yarn is coiled into cylinder yarn by h, winder on automatic winder using 600~1000 ms/min of winder speed;
I, doubling, on doubling frame using 500~1000 ms/min and linear velocity by two or more pieces single thread it is parallel and and Into strand;
J, double twisting twists the strand simultaneously with after into the twist on two-for-one twister:250~650 twists/m, ingot speed for 4000~ 8000 revs/min.
Further, in the step a by skin makeup fiber carry out dyeing pre-treatment be add at normal temperatures bath raio for 8~ In 15 water, 0.5 g/l of bleeding agent is added in, 1 g/l of soaping agent is warming up to 85~95 degree, keeps the temperature 10 minutes, discharged water Water.
Further, dyeing process is carried out in the step a to be added at normal temperatures in the water that bath raio is 8~15, is used Na2CO3The auxiliary agents such as dyestuff, anhydrous sodium sulphate are added in after adjusting PH to 8.0~8.5,30~80g/L of anhydrous sodium sulphate concentration plays cylinder in three times, with 1 DEG C/Warm to 60 degree of min liters, it protects Warm 60 minutes, then adds in 12~35g/L Na2CO3, it is desirable that cylinder is played in three times, continues heat preservation 60 Minute, then acetic acid tune PH to 5.5~6.0, heat preservation discharges water for 10 minutes.
Further, color fixing process of soaping in the step a is 1~2 g/l of soaping agent of addition under room temperature, is warming up to 85 ~95 degree, 10~20 minutes are kept the temperature, discharged water water, and color fixing agent is added at 45 DEG C~50 DEG C, keeps the temperature 15~20 minutes.
Further, soft finish technique is to add in hydrophilic softener at 45 DEG C~50 DEG C in the step a, heat preservation It 10~15 minutes, discharges water.
Further, when skin makeup fiber is mixed with cotton in the step c, add in 3.5% soft water, 0.5% it is anti- Electrostatic agent, mixed fiber is placed under enclosed environment carries out health for 12~36 hours, and holding workshop humid control is:60% ~80%.
Further, when skin makeup fiber is mixed with wool or cashmere fibres in the step c, 3.0%~6.0% is added in Soft water, 0.5% antistatic agent, 0.5~1.0 non-ionic and crude oil, mixed fiber places under enclosed environment It carries out health within 12~36 hours, makes in finish and water fully penetrated to fiber, holding workshop humid control is:60%~80%.
Further, speed is controlled in 150~250m/min in the step e.
Further, ingot speed is 500~800 revs/min in the step f.
Further, ingot speed is 7000~12000 revs/min in the step g.
The beneficial effects of the invention are as follows:Skin makeup fiber blended color yarn is produced using the above method, yarn strength is high, item Dry uniform, filoplume is few, and physical index reaches high-class product standard, and the fabric being made by it, soft, pro-skin, smooth, moisture absorption is saturating Gas, pro-skin is comfortable, uvioresistant, and technological process is simple, and being not required to upgrading existing equipment can put into production, and save manpower, object Power, financial resources enhance the competitiveness of enterprise.
Specific embodiment
The specific embodiment of the present invention is described in further detail below.
The present invention production method be:Skin makeup fiber is carried out dyeing pre-treatment first, is then contaminated by a, stock-dye Color is processed, color fixing process of followed by soaping, and is finally carried out soft finish technique and is completed stock-dye;
B, weighing needs to weigh fiber using dry ratio according to product;
The fiber weighed is carried out laying mixing, adds in 2%~6% water, mixed fiber is in closed-loop by c, batch mixing It is placed under border 12~36 hours and carries out health;
Raw material after batch mixing is combed into 15~22 grams/5 meters by d, cotton carding on flat top card, and doffing speed 18~ 26 revs/min of the carded sliver;
E, drafting carries out three on drawing frame and obtains 15~22 grams/5 meters with drawing-off, and with radical 6~8, drawing-off The ripe bar that 6~8 times of multiple;
Ripe bar draw twisting after drafting is wound into 5~8 grams/10 meters, drafting multiple 5~8 by f, rove on fly frame Times, the rove that 30~60 twists/m of the twist;
G, spun yarn twists roving-drafting into 1.67~3.57 grams/100 meters on spinning frame, 15~35 times of drafting multiple, The spun yarn that 500~1000 twists/m of the twist;
Spun yarn is coiled into cylinder yarn by h, winder on automatic winder using 600~1000 ms/min of winder speed;
I, doubling, on doubling frame using 500~1000 ms/min and linear velocity by two or more pieces single thread it is parallel and and Into strand;
J, double twisting twists the strand simultaneously with after into the twist on two-for-one twister:250~650 twists/m, ingot speed for 4000~ 8000 revs/min.
Further, in the step a by skin makeup fiber carry out dyeing pre-treatment be add at normal temperatures bath raio for 8~ In 15 water, 0.5 g/l of bleeding agent is added in, 1 g/l of soaping agent is warming up to 85~95 degree, keeps the temperature 10 minutes, discharged water Water.
Further, dyeing process is carried out in the step a to be added at normal temperatures in the water that bath raio is 8~15, is used Na2CO3The auxiliary agents such as dyestuff, anhydrous sodium sulphate are added in after adjusting PH to 8.0~8.5,30~80g/L of anhydrous sodium sulphate concentration plays cylinder in three times, with 1 DEG C/Warm to 60 degree of min liters, it protects Warm 60 minutes, then adds in 12~35g/L Na2CO3, it is desirable that play cylinder in three times, continue to keep the temperature 60 minutes, then acetic acid tune PH to 5.5~6.0, heat preservation discharged water for 10 minutes.
Further, color fixing process of soaping in the step a is 1~2 g/l of soaping agent of addition under room temperature, is warming up to 85 ~95 degree, 10~20 minutes are kept the temperature, discharged water water, and color fixing agent is added at 45 DEG C~50 DEG C, keeps the temperature 15~20 minutes.
Further, soft finish technique is to add in hydrophilic softener at 45 DEG C~50 DEG C in the step a, heat preservation It 10~15 minutes, discharges water.
Further, when skin makeup fiber is mixed with cotton in the step c, add in 3.5% soft water, 0.5% it is anti- Electrostatic agent, mixed fiber is placed under enclosed environment carries out health for 12~36 hours, and holding workshop humid control is:60% ~80%.
Further, when skin makeup fiber is mixed with wool or cashmere fibres in the step c, 3.0%~6.0% is added in Soft water, 0.5% antistatic agent, 0.5~1.0 non-ionic and crude oil, mixed fiber places under enclosed environment It carries out health within 12~36 hours, makes in finish and water fully penetrated to fiber, holding workshop humid control is:60%~80%.
Further, speed is controlled in 150~250m/min in the step e.
Further, ingot speed is 500~800 revs/min in the step f.
Further, ingot speed is 7000~12000 revs/min in the step g.
In practical applications:
First, using 100% skin makeup fiber blended color yarn, skin makeup fiber is subjected to dyeing pre-treatment at normal temperatures first It adds in the water that bath raio is 8~15, adds in 0.5 g/l of bleeding agent, 1 g/l of soaping agent is warming up to 85~95 degree, heat preservation 10 Minute, discharged water water.Secondly carrying out dyeing process is added at normal temperatures in the water that bath raio is 8~15, uses Na2CO3Adjust PH extremely Auxiliary agents, the 30~80g/L of anhydrous sodium sulphate concentration such as dyestuff, anhydrous sodium sulphate are added in after 8.0~8.5 and plays cylinder in three times, rising Warm with 1 DEG C/min arrives It 60 degree, protects Warm 60 minutes, then adds in 12~35g/L Na2CO3, it is desirable that cylinder is played in three times, continues heat preservation 60 minutes, then vinegar Acid adjusts PH to 5.5~6.0, and heat preservation discharges water for 10 minutes.The color fixing process that carries out soaping again is to add in 1~2 g/l under room temperature to soap Agent is warming up to 85~95 degree, keeps the temperature 10~20 minutes, and discharged water water, and color fixing agent, heat preservation 15~20 are added at 45 DEG C~50 DEG C Minute.Then it is that hydrophilic softener is added at 45 DEG C~50 DEG C to carry out soft finish technique, keeps the temperature 10~15 minutes, puts Water.In next step, the Mobil fiber laying weighed is mixed, adds in 4% soft water, 1% antistatic agent, mixed fiber It is placed under enclosed environment and carries out within 30 hours health, holding workshop humid control is:60%~80%.In next step, in cover-plate type The raw material after batch mixing is combed into 15.6 grams/5 meters on carding machine, the carded sliver that 19.5 revs/min of doffing speed keeps the regain to be 14%;In next step, three are carried out on drawing frame and obtains 15.6 grams/5 meters with drawing-off, and with radical 8,8 times of drafting multiple Ripe bar, speed control in 180m/min;In next step, the ripe bar draw twisting after drafting is wound into 5.18 on fly frame Gram/10 meters, 6 times of drafting multiple, 36 twists/m of the twist, ingot speed is 600 revs/min of rove;In next step, by rove on spinning frame Draw twisting is into 1.85 grams/100 meters, and 28 times of drafting multiple, 884 twists/m of the twist, ingot speed is 9000 revs/min of spun yarn;It is next Step, cylinder yarn is coiled on automatic winder using 600 ms/min of winder speed by spun yarn;In next step, it is used on doubling frame 600 ms/min and linear velocity two single thread are parallel and and into strand;In next step, the strand simultaneously with after is added on two-for-one twister It is twisted the twist:884 twists/m, ingot speed is 6500 revs/min.
Second, using 40% skin makeup fiber and 60% cotton blended color spinning yarn, before skin makeup fiber is dyed first Processing is added at normal temperatures in the water that bath raio is 8~15, adds in 0.5 g/l of bleeding agent, and 1 g/l of soaping agent is warming up to 85 ~95 degree, 10 minutes are kept the temperature, discharged water water.Secondly carrying out dyeing process is added at normal temperatures in the water that bath raio is 8~15, is used Na2CO3The auxiliary agents such as dyestuff, anhydrous sodium sulphate are added in after adjusting PH to 8.0~8.5,30~80g/L of anhydrous sodium sulphate concentration plays cylinder in three times, with 1 DEG C/Warm to 60 degree of min liters, it protects Warm 60 minutes, then adds in 12~35g/L Na2CO3, it is desirable that play cylinder in three times, continue to keep the temperature 60 minutes, then acetic acid tune PH to 5.5~6.0, heat preservation discharged water for 10 minutes.The color fixing process that carries out soaping again is added under room temperature 1~2 g/l of soaping agent is warming up to 85~95 degree, keeps the temperature 10~20 minutes, discharged water water, and fixation is added at 45 DEG C~50 DEG C Agent keeps the temperature 15~20 minutes.Then it is that hydrophilic softener is added at 45 DEG C~50 DEG C to carry out soft finish technique, heat preservation 10 It~15 minutes, discharges water.In next step, the Mobil fiber weighed with cotton laying is mixed, adds in 3.5% soft water, 0.5% Antistatic agent, mixed fiber is placed under enclosed environment carries out health for 18 hours, and holding workshop humid control is:60%~ 80%.In next step, the raw material after batch mixing is combed into 18.8 grams/5 meters on flat top card, 23 revs/min of doffing speed The carded sliver, it is 12% to keep regain;In next step, three are carried out on drawing frame and obtains 18.8 grams/5 meters, and and root with drawing-off Number 8, the ripe bar that 8 times of drafting multiple, speed are controlled in 200m/min;In next step, the ripe bar after drafting is led on fly frame Twisting winding is stretched into 6.27 grams/10 meters, and 6 times of drafting multiple, 45 twists/m of the twist, ingot speed is 750 revs/min of rove;In next step, Roving-drafting is twisted into 2.08 grams/100 meters on spinning frame, 30 times of drafting multiple, 772 twists/m of the twist, ingot speed 10000 Rev/min spun yarn;In next step, spun yarn is coiled into cylinder yarn using 800 ms/min of winder speed on automatic winder;In next step, On doubling frame using 800 ms/min and linear velocity two single thread are parallel and and into strand;It in next step, will on two-for-one twister And the strand with after is twisted into the twist:772 twists/m, ingot speed is 8000 revs/min.
Third, using 40% skin makeup fiber and 60% 70S mercerized wool blended color spinning yarns, first by skin makeup fiber into Row dyeing pre-treatment is added at normal temperatures in the water that bath raio is 8~15, the bleeding agent of 0.5 g/l of addition, 1 g/l of soaping agent, 85~95 degree are warming up to, keeps the temperature 10 minutes, discharged water water.Secondly it is that addition bath raio is 8~15 at normal temperatures to carry out dyeing process Water in, use Na2CO3The auxiliary agents such as dyestuff, anhydrous sodium sulphate are added in after adjusting PH to 8.0~8.5,30~80g/L of anhydrous sodium sulphate concentration is in three times Lower cylinder rises Warm to 60 degree with 1 DEG C/min, protects Warm 60 minutes, then adds in 12~35g/L Na2CO3, it is desirable that cylinder is played in three times, Continue heat preservation 60 minutes, then acetic acid tune PH to 5.5~6.0, heat preservation discharges water for 10 minutes.The color fixing process that carries out soaping again is normal Temperature is lower to add in 1~2 g/l of soaping agent, is warming up to 85~95 degree, keeps the temperature 10~20 minutes, discharged water water, at 45 DEG C~50 DEG C Color fixing agent is added in, keeps the temperature 15~20 minutes.Then it is that hydrophily softness is added at 45 DEG C~50 DEG C to carry out soft finish technique Agent keeps the temperature 10~15 minutes, discharges water.In next step, the Mobil fiber weighed is mixed with cotton laying, add in 4.5% it is soft Water, 0.5% antistatic agent, 1% non-ionic and crude oil, mixed fiber are placed 24 hours under enclosed environment and are carried out Health, holding workshop humid control are:60%~80%.In next step, the raw material after batch mixing is combed on flat top card Into 18 grams/5 meters, the carded sliver that 22 revs/min of doffing speed, it is 18% to keep regain;In next step, three are carried out on drawing frame simultaneously 18 grams/5 meters are obtained, and with radical 8 with drawing-off, the ripe bar that 8 times of drafting multiple, speed is controlled in 220m/min;In next step, exist The ripe bar draw twisting after drafting is wound into 7.14 grams/10 meters on fly frame, 5.02 times of drafting multiple, 45 twists/m of the twist, ingot Speed is 700 revs/min of rove;In next step, roving-drafting is twisted into 3.57 grams/100 meters on spinning frame, drafting multiple 20 Times, 660 twists/m of the twist, ingot speed is 9500 revs/min of spun yarn;In next step, 800 ms/min of winder is used on automatic winder Spun yarn is coiled into cylinder yarn by speed;In next step, on doubling frame using 800 ms/min and linear velocity by two single thread it is parallel and and Into strand;In next step, the strand simultaneously with after is twisted into the twist on two-for-one twister:660 twists/m, ingot speed is 6000 revs/min.
Third, using 45% skin makeup fiber and 55% cashmere blended color spinning yarn, skin makeup fiber is dyed first Pre-treatment is added at normal temperatures in the water that bath raio is 8~15, adds in 0.5 g/l of bleeding agent, and 1 g/l of soaping agent is warming up to 85~95 degree, 10 minutes are kept the temperature, discharged water water.Secondly carrying out dyeing process is added at normal temperatures in the water that bath raio is 8~15, Use Na2CO3Auxiliary agents, the 30~80g/L of anhydrous sodium sulphate concentration such as dyestuff, anhydrous sodium sulphate, which are added in, after tune PH to 8.0~8.5 plays cylinder in three times, with 1 DEG C/min rises Warm to 60 degree, protects Warm 60 minutes, then adds in 12~35g/L Na2CO3, it is desirable that play cylinder in three times, continue to keep the temperature 60 minutes, then acetic acid tune PH to 5.5~6.0, heat preservation discharged water for 10 minutes.The color fixing process that carries out soaping again is added under room temperature 1~2 g/l of soaping agent is warming up to 85~95 degree, keeps the temperature 10~20 minutes, discharged water water, and fixation is added at 45 DEG C~50 DEG C Agent keeps the temperature 15~20 minutes.Then it is that hydrophilic softener is added at 45 DEG C~50 DEG C to carry out soft finish technique, heat preservation 10 It~15 minutes, discharges water.In next step, the Mobil fiber weighed with cotton laying is mixed, adds in 4% soft water, 0.5% it is anti- Electrostatic agent, 0.5% non-ionic and crude oil, mixed fiber are placed 24 hours under enclosed environment and carry out health, keep Workshop humid control is:60%~80%.In next step, the raw material after batch mixing is combed into 15 grams/5 on flat top card Rice, the carded sliver that 20 revs/min of doffing speed, it is 18% to keep regain;In next step, three are carried out on drawing frame and is obtained with drawing-off To 15 grams/5 meters, and with radical 8, the ripe bar that 8 times of drafting multiple, speed is controlled in 200m/min;In next step, on fly frame Ripe bar draw twisting after drafting is wound into 5 grams/10 meters, 6 times of drafting multiple, 35 twists/m of the twist, ingot speed is 600 revs/min Rove;In next step, roving-drafting is twisted into 2.08 grams/100 meters on spinning frame, 24 times of drafting multiple, 832 twists/m of the twist, Ingot speed is 8000 revs/min of spun yarn;In next step, spun yarn is coiled into cylinder using 600 ms/min of winder speed on automatic winder Yarn;In next step, on doubling frame using 800 ms/min and linear velocity two single thread are parallel and and into strand;In next step, exist The strand simultaneously with after is twisted into the twist on two-for-one twister:832 twists/m, ingot speed is 7200 revs/min.
Above-mentioned specific embodiment is the preferred embodiment of the present invention, can not be limited the invention, and others are appointed The change or other equivalent substitute modes what is made without departing from technical scheme of the present invention, are included in the protection of the present invention Within the scope of.

Claims (10)

1. a kind of production method of skin makeup fiber blended color yarn, production method are:A, stock-dye, first by skin makeup fiber Dyeing pre-treatment is carried out, then carries out dyeing process, color fixing process of followed by soaping finally carries out soft finish technique completion Stock-dye;
B, weighing needs to weigh fiber using dry ratio according to product;
The fiber weighed is carried out laying mixing, adds in 2%~6% water, mixed fiber is under enclosed environment by c, batch mixing It places 12~36 hours and carries out health;
Raw material after batch mixing is combed into 15~22 grams/5 meters by d, cotton carding on flat top card, and 18~26 turns of doffing speed/ The carded sliver divided;
E, drafting carries out three on drawing frame and obtains 15~22 grams/5 meters with drawing-off, and with radical 6~8, drafting multiple 6~8 times of ripe bar;
Ripe bar draw twisting after drafting is wound into 5~8 grams/10 meters by f, rove on fly frame, 5~8 times of drafting multiple, The rove that 30~60 twists/m of the twist;
G, spun yarn twists roving-drafting into 1.67~3.57 grams/100 meters on spinning frame, 15~35 times of drafting multiple, the twist 500~1000 twists/m of spun yarn;
Spun yarn is coiled into cylinder yarn by h, winder on automatic winder using 600~1000 ms/min of winder speed;
I, doubling, on doubling frame using 500~1000 ms/min and linear velocity two or more pieces single thread is parallel and and into stock Line;
J, double twisting twists the strand simultaneously with after into the twist on two-for-one twister:250~650 twists/m, ingot speed is 4000~8000 Rev/min.
2. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step a Middle what skin makeup fiber was carried out dyeing pre-treatment added at normal temperatures in the water that bath raio is 8~15, is added in 0.5 g/l and is oozed Saturating agent, 1 g/l of soaping agent are warming up to 85~95 degree, keep the temperature 10 minutes, discharged water water.
3. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step a The middle dyeing process that carries out is added at normal temperatures in the water that bath raio is 8~15, uses Na2CO3Dye is added in after adjusting PH to 8.0~8.5 The auxiliary agents such as material, anhydrous sodium sulphate, 30~80g/L of anhydrous sodium sulphate concentration play cylinder in three times, rise Warm to 60 degree with 1 DEG C/min, protect Warm 60 minutes, Then 12~35g/L Na are added in2CO3, it is desirable that play cylinder in three times, continue heat preservation 60 minutes, then acetic acid tune PH to 5.5~ 6.0, heat preservation discharges water for 10 minutes.
4. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step a In color fixing process of soaping be 1~2 g/l of soaping agent of addition under room temperature, be warming up to 85~95 degree, heat preservation 10~20 minutes discharges water Water is crossed, color fixing agent is added at 45 DEG C~50 DEG C, keeps the temperature 15~20 minutes.
5. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step a Middle soft finish technique is that hydrophilic softener is added at 45 DEG C~50 DEG C, keeps the temperature 10~15 minutes, discharges water.
6. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step c It is middle when skin makeup fiber is mixed with cotton, 3.5% soft water is added in, 0.5% antistatic agent, mixed fiber is in closed-loop It is placed under border and carries out within 12~36 hours health, holding workshop humid control is:60%~80%.
7. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step c When middle skin makeup fiber is mixed with wool or cashmere fibres, the soft water of addition 3.0%~6.0%, 0.5% antistatic agent, 0.5 ~1.0 non-ionic and crude oil, mixed fiber placed under enclosed environment 12~36 hours carry out health, make finish with In water fully penetrated to fiber, holding workshop humid control is:60%~80%.
8. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step e It is middle to control speed in 150~250m/min.
9. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step f Middle ingot speed is 500~800 revs/min.
10. the production method of skin makeup fiber blended color yarn according to claim 1, it is characterised in that:The step g Middle ingot speed is 7000~12000 revs/min.
CN201710980288.7A 2017-10-19 2017-10-19 A kind of production method of skin makeup fiber blended color yarn Pending CN108251934A (en)