CN108195838A - A kind of rapid detection method of woodcare paint glossiness - Google Patents
A kind of rapid detection method of woodcare paint glossiness Download PDFInfo
- Publication number
- CN108195838A CN108195838A CN201711417325.XA CN201711417325A CN108195838A CN 108195838 A CN108195838 A CN 108195838A CN 201711417325 A CN201711417325 A CN 201711417325A CN 108195838 A CN108195838 A CN 108195838A
- Authority
- CN
- China
- Prior art keywords
- woodcare paint
- detection method
- rapid detection
- sample
- dried
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Disclosed by the invention to belong to paint film detection technique field, specially a kind of rapid detection method of woodcare paint glossiness, the rapid detection method of the woodcare paint glossiness includes the following steps:S1:Feedstock processing:Woodcare paint sample to be measured is taken to be placed in 75 80 degrees Celsius of baking oven to be dried;S2:Sample making:Wooden model is taken, polishes flat to the surface of wooden model, then cleans out, dried woodcare paint is sprayed on to the surface of wooden model;S3:It is dry:The sample made is 45 hours dry in the environment of constant temperature and humidity;S4:Detection:Dried sample is measured 35 times using digital glossometer, finally take the average value of measurement, a kind of rapid detection method for woodcare paint glossiness that the invention proposes, it is rational to control drying time and dry humidity, detection accuracy is improved, and substantially reduces detection time, improves production efficiency, it is of low cost, it is easy to operation.
Description
Technical field
The present invention relates to paint film detection technique field, specially a kind of rapid detection method of woodcare paint glossiness.
Background technology
Woodcare paint refers to a kind of lacquer type organic coating on woodwork, there is polyester, polyurethane paint etc., can be divided into aqueous and oily
Property.It can be divided into bloom, semi-matte, dumb light by gloss.It can be divided into furniture lacquer, floor paint etc. by purposes.Natural woodcare paint is commonly called as greatly
Paint, and have the title of " state's paint ".The juice to get off is tapped from lacquer tree and is known as Chinese lacquer or former bucket paint, filtering off impurity with calico is known as
Raw lacquer.It in the production process of woodcare paint, needs to be detected the glossiness of woodcare paint, the inspection of existing woodcare paint glossiness
Time-consuming for survey method, and accuracy of detection is low, and cost is excessively high, it is proposed that a kind of rapid detection method of woodcare paint glossiness.
Invention content
The purpose of the present invention is to provide a kind of rapid detection method of woodcare paint glossiness, to solve above-mentioned background technology
The detection method of the existing woodcare paint glossiness of middle proposition the problem of time-consuming, and accuracy of detection is low, and cost is excessively high.
To achieve the above object, the present invention provides following technical solution:A kind of rapid detection method of woodcare paint glossiness,
The rapid detection method of the woodcare paint glossiness includes the following steps:
S1:Feedstock processing:Woodcare paint sample to be measured is taken to be placed in 75-80 degrees Celsius of baking oven to be dried;
S2:Sample making:Wooden model is taken, polishes flat to the surface of wooden model, then cleans out, after drying
Woodcare paint be sprayed on the surface of wooden model;
S3:It is dry:The sample made is 4-5 hours dry in the environment of constant temperature and humidity;
S4:Detection:Dried sample is measured 3-5 times using digital glossometer, finally takes the average value of measurement.
Preferably, the drying temperature time in the step S1 is 20-30 minutes.
Preferably, the spraying method of woodcare paint is brushing, has gas or airless spraying in the step S2.
Preferably, the quantity for spray of woodcare paint is 16-18 ㎡/L in the step S2.
Preferably, the specification of the wooden model in the step S2 is 100mm × 100mm × 3.2mm.
Preferably, the drying temperature in the step S3 is 20-25 degrees Celsius, and dry relative humidity is 45%-55%.
Preferably, in the step S3, when being dried, sample is placed in the white steel disk for be covered with gauze and done
It is dry.
Compared with prior art, the beneficial effects of the invention are as follows:The invention propose a kind of woodcare paint glossiness it is quick
Detection method reasonably controls drying time and dry humidity, improves detection accuracy, and substantially reduce detection time,
Production efficiency is improved, it is of low cost, it is easy to operation.
Description of the drawings
Fig. 1 is detection method flow chart.
Specific embodiment
Below in conjunction with the attached drawing in the embodiment of the present invention, the technical solution in the embodiment of the present invention is carried out clear, complete
Site preparation describes, it is clear that described embodiment is only part of the embodiment of the present invention, instead of all the embodiments.It is based on
Embodiment in the present invention, those of ordinary skill in the art are obtained every other without making creative work
Embodiment shall fall within the protection scope of the present invention.
Referring to Fig. 1, the present invention provides a kind of rapid detection method of woodcare paint glossiness:
Embodiment 1
The rapid detection method of the woodcare paint glossiness includes the following steps:
S1:Feedstock processing:Woodcare paint sample to be measured is taken to be placed in 77.5 degrees Celsius of baking oven to be dried, drying temperature
Time is 24 minutes;
S2:Sample making:Wooden model is taken, polishes flat to the surface of wooden model, then cleans out, after drying
Woodcare paint be sprayed on the surface of wooden model, the spraying method of woodcare paint is brushes, has gas or airless spraying, the spray of woodcare paint
Painting amount is 17 ㎡/L, and the specification of wooden model is 100mm × 100mm × 3.2mm;
S3:It is dry:The sample made is placed in the white steel disk for being covered with gauze, it is dry in the environment of constant temperature and humidity
4.5 hours, drying temperature was 23 degrees Celsius, and dry relative humidity is 50%;
S4:Detection:Dried sample is measured 4 times using digital glossometer, finally takes the average value of measurement.
Embodiment 2
The rapid detection method of the woodcare paint glossiness includes the following steps:
S1:Feedstock processing:Woodcare paint sample to be measured is taken to be placed in 75 degrees Celsius of baking oven to be dried, during drying temperature
Between be 20 minutes;
S2:Sample making:Wooden model is taken, polishes flat to the surface of wooden model, then cleans out, after drying
Woodcare paint be sprayed on the surface of wooden model, the spraying method of woodcare paint is brushes, has gas or airless spraying, the spray of woodcare paint
Painting amount is 16 ㎡/L, and the specification of wooden model is 100mm × 100mm × 3.2mm;
S3:It is dry:The sample made is placed in the white steel disk for being covered with gauze, dry 4 in the environment of constant temperature and humidity
Hour, drying temperature is 20 degrees Celsius, and dry relative humidity is 45%;
S4:Detection:Dried sample is measured 3 times using digital glossometer, finally takes the average value of measurement.
Embodiment 3
The rapid detection method of the woodcare paint glossiness includes the following steps:
S1:Feedstock processing:Woodcare paint sample to be measured is taken to be placed in 80 degrees Celsius of baking oven to be dried, during drying temperature
Between be 30 minutes;
S2:Sample making:Wooden model is taken, polishes flat to the surface of wooden model, then cleans out, after drying
Woodcare paint be sprayed on the surface of wooden model, the spraying method of woodcare paint is brushes, has gas or airless spraying, the spray of woodcare paint
Painting amount is 18 ㎡/L, and the specification of wooden model is 100mm × 100mm × 3.2mm;
S3:It is dry:The sample made is placed in the white steel disk for being covered with gauze, dry 5 in the environment of constant temperature and humidity
Hour, drying temperature is 25 degrees Celsius, and dry relative humidity is 55%;
S4:Detection:Dried sample is measured 5 times using digital glossometer, finally takes the average value of measurement.
It although an embodiment of the present invention has been shown and described, for the ordinary skill in the art, can be with
Understanding without departing from the principles and spirit of the present invention can carry out these embodiments a variety of variations, modification, replace
And modification, the scope of the present invention is defined by the appended.
Claims (7)
1. a kind of rapid detection method of woodcare paint glossiness, it is characterised in that:The rapid detection method of the woodcare paint glossiness
Include the following steps:
S1:Feedstock processing:Woodcare paint sample to be measured is taken to be placed in 75-80 degrees Celsius of baking oven to be dried;
S2:Sample making:Wooden model is taken, polishes flat to the surface of wooden model, then cleans out, by dried wood
Device paint is sprayed on the surface of wooden model;
S3:It is dry:The sample made is 4-5 hours dry in the environment of constant temperature and humidity;
S4:Detection:Dried sample is measured 3-5 times using digital glossometer, finally takes the average value of measurement.
2. a kind of rapid detection method of woodcare paint glossiness according to claim 1, it is characterised in that:The step S1
In the drying temperature time be 20-30 minutes.
3. a kind of rapid detection method of woodcare paint glossiness according to claim 1, it is characterised in that:The step S2
The spraying method of middle woodcare paint is brushes, has gas or airless spraying.
4. a kind of rapid detection method of woodcare paint glossiness according to claim 1, it is characterised in that:The step S2
The quantity for spray of middle woodcare paint is 16-18 ㎡/L.
5. a kind of rapid detection method of woodcare paint glossiness according to claim 1, it is characterised in that:The step S2
In wooden model specification be 100mm × 100mm × 3.2mm.
6. a kind of rapid detection method of woodcare paint glossiness according to claim 1, it is characterised in that:The step S3
In drying temperature for 20-25 degrees Celsius, dry relative humidity is 45%-55%.
7. a kind of rapid detection method of woodcare paint glossiness according to claim 1, it is characterised in that:The step S3
In, when being dried, sample is placed in the white steel disk for be covered with gauze and be dried.