CN108165138A - Insulation rust-proof anti-corrosive paint - Google Patents
Insulation rust-proof anti-corrosive paint Download PDFInfo
- Publication number
- CN108165138A CN108165138A CN201711469434.6A CN201711469434A CN108165138A CN 108165138 A CN108165138 A CN 108165138A CN 201711469434 A CN201711469434 A CN 201711469434A CN 108165138 A CN108165138 A CN 108165138A
- Authority
- CN
- China
- Prior art keywords
- proof anti
- insulation
- corrosive paint
- rust
- corrosive
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses insulation rust-proof anti-corrosive paints, are related to building coating field, and the mass ratio of the insulation rust-proof anti-corrosive paint is:5.25 7.25% adhesive, 0.5 2.5% photocuring prepolymer, 2.75 4.75% sodium metasilicate, 0.25 2.25% polyoxyethylene enzyme, 3.5 5.5% wax ester, 24 26% basis material, 0.5 1.5% curing agent, 0.5 2.5% surfactant, 1 3% polyurethane, 7 9% thermal resistance separated material, 1.5 3.5% solvent, 4 6% filler and 0.25 2.25% pigment, rest part are deionized water.The present invention makes this coating preferably fitting and metope by being added with Ludox and sodium metasilicate, epoxy acrylate can be faster by the paint solidification of liquid, the effect of insulation can be played simultaneously, polyurethane can be with antirust, anti-corrosive, wax ester has good lubricity, each material is made preferably to merge, insulation and antirust, anti-corrosive of this coating for exterior wall are allow by the fusion of this each material.
Description
Technical field
The present invention relates to building coating fields, and in particular to insulation rust-proof anti-corrosive paint.
Background technology
Existing external wall is generally all with insulating mold coating brushing, but existing heat insulating effect is general, Gu
Change is slower, but also without antirust, anti-corrosive and other effects.Therefore, the present invention proposes insulation rust-proof anti-corrosive paint.
Invention content
In view of the above-mentioned problems, the present invention proposes insulation rust-proof anti-corrosive paint, the insulation rust-proof anti-corrosive paint
Mass ratio be:The adhesive of 5.25-7.25%, the photocuring prepolymer of 0.5-2.5%, 2.75-4.75% sodium metasilicate,
The polyoxyethylene enzyme of 0.25-2.25%, the wax ester of 3.5-5.5%, the basis material of 24-26%, 0.5-1.5% curing agent,
The surfactant of 0.5-2.5%, the polyurethane of 1-3%, the thermal resistance separated material of 7-9%, the solvent of 1.5-3.5%, 4-6% are filled out
The pigment of material and 0.25-2.25%, rest part is deionized water.
Further improvement lies in that:Described adhesive is Ludox.
Further improvement lies in that:Described matrix material for epoxy resin, one kind in saturated polyester resin lattice polyurethane or
Multiple combinations.
Further improvement lies in that:The surfactant is one kind of carboxylic acid, sulfonic acid, sulfuric acid, amino or amido.
Further improvement lies in that:The thermal resistance separated material is ceramic particle or hollow glass micropearl.
Further improvement lies in that:It is 3.62g/cc that the granularity of the ceramic particle, which is density, 30-60 microns of grain size.
Further improvement lies in that:The solvent is arbitrary in toluene, dimethylbenzene, butyl glycol ether and butyl
One or more combinations.
Further improvement lies in that:The filler is any one or more combination in talcum powder, mica powder or barium sulfate.
Further improvement lies in that:The pigment is titanium dioxide or barium sulfate.
Further improvement lies in that:The density of the titanium dioxide or barium sulfate be 4.26g/cc, 30-60 microns of grain size.
Beneficial effects of the present invention:The present invention makes this coating preferably fitting and wall by being added with Ludox and sodium metasilicate
Face, epoxy acrylate can be faster by the paint solidification of liquid, while can play the effect of insulation, and polyurethane can be with
Antirust, anti-corrosive, wax ester have good lubricity, and each material is made preferably to merge, and make this coating by the fusion of this each material
The insulation and antirust, anti-corrosive of exterior wall can be directed to.
Specific embodiment
In order to deepen the understanding of the present invention, the present invention is further described below in conjunction with embodiment, the present embodiment
It is only used for explaining the present invention, be not intended to limit the scope of the present invention..
Embodiment one
The mass ratio of insulation rust-proof anti-corrosive paint is:5.25% Ludox, 2.5% photocuring prepolymer,
2.75% sodium metasilicate, 2.25% polyoxyethylene enzyme, 3.5% wax ester, 26% epoxy resin, 0.5% curing agent,
2.5% carboxylic acid, 1% polyurethane, 9% ceramic particle, 1.5% toluene, 6% talcum powder and 0.25% titanium white
Powder, rest part are deionized water.
Embodiment two
The mass ratio of insulation rust-proof anti-corrosive paint is:6.25% Ludox, 1.5% photocuring prepolymer,
3.75% sodium metasilicate, 1.25% polyoxyethylene enzyme, 4.5% wax ester, 25% epoxy resin, 1% curing agent,
1.5% carboxylic acid, 2% polyurethane, 8% ceramic particle, 2.5% toluene, 5% talcum powder and 1.25% titanium white
Powder, rest part are deionized water.
Embodiment three
The mass ratio of insulation rust-proof anti-corrosive paint is:7.25% Ludox, 0.5% photocuring prepolymer,
4.75% sodium metasilicate, 0.25% polyoxyethylene enzyme, 5.5% wax ester, 24% epoxy resin, 1.5% curing agent,
0.5% carboxylic acid, the polyurethane of 1-3%, 7% ceramic particle, 3.5% toluene, 4% talcum powder and 2.25% titanium white
Powder, rest part are deionized water.
It is obtained according to above three groups of embodiments, when the mass ratio of insulation rust-proof anti-corrosive paint is:5.25-7.25%'s
Ludox, the photocuring prepolymer of 0.5-2.5%, the sodium metasilicate of 2.75-4.75%, 0.25-2.25% polyoxyethylene enzyme,
The wax ester of 3.5-5.5%, the epoxy acrylate of 24-26%, the curing agent of 0.5-1.5%, 0.5-2.5% surface-active
Agent, the polyurethane of 1-3%, the ceramic particle of 7-9%, the color stuffing of 1.5-3.5%, 4-6% exterior wall paint and 0.25-
2.25% mill base, when remaining is water, heat preservation, heat-insulated, antirust and corrosion-resistant effect are best.
The present invention makes the better fitting of this coating and metope, epoxy acrylate can by being added with Ludox and sodium metasilicate
With faster by the paint solidification of liquid, while the effect of insulation can be played, polyurethane can have very with antirust, anti-corrosive, wax ester
Good lubricity, makes each material preferably merge, and allows guarantor of this coating for exterior wall by the fusion of this each material
Warm heat-insulated and antirust, anti-corrosive.
Claims (10)
1. insulation rust-proof anti-corrosive paint, it is characterised in that:The mass ratio of the insulation rust-proof anti-corrosive paint is:
The adhesive of 5.25-7.25%, the photocuring prepolymer of 0.5-2.5%, the sodium metasilicate of 2.75-4.75%, 0.25-2.25%
Polyoxyethylene enzyme, the wax ester of 3.5-5.5%, the basis material of 24-26%, the curing agent of 0.5-1.5%, 0.5-2.5% table
Face activating agent, the polyurethane of 1-3%, the thermal resistance separated material of 7-9%, the solvent of 1.5-3.5%, 4-6% filler and 0.25-
2.25% pigment, rest part are deionized water.
2. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:Described adhesive is Ludox.
3. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:Described matrix material is asphalt mixtures modified by epoxy resin
One or more combinations in fat, saturated polyester resin lattice polyurethane.
4. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:The surfactant isCarboxylic Acid、Sulfonic acid、Sulfuric acid、AminoOr one kind of amido.
5. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:The thermal resistance separated material is micro- for ceramics
Grain or hollow glass micropearl.
6. insulation rust-proof anti-corrosive paint according to claim 5, it is characterised in that:The granularity of the ceramic particle is
Density is 3.62g/cc, 30-60 microns of grain size.
7. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:The solvent is toluene, diformazan
Any one or more combination in benzene, butyl glycol ether and butyl.
8. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:The filler is talcum powder, cloud
Any one or more combination in female powder or barium sulfate.
9. insulation rust-proof anti-corrosive paint according to claim 1, it is characterised in that:The pigment is titanium dioxide or sulphur
Sour barium.
10. insulation rust-proof anti-corrosive paint according to claim 9, it is characterised in that:The titanium dioxide or barium sulfate
Density for 4.26g/cc, 30-60 microns of grain size.