CN108088983A - A kind of automobile water paint and the mating lower cracking detection method of fluid sealant - Google Patents
A kind of automobile water paint and the mating lower cracking detection method of fluid sealant Download PDFInfo
- Publication number
- CN108088983A CN108088983A CN201711277643.0A CN201711277643A CN108088983A CN 108088983 A CN108088983 A CN 108088983A CN 201711277643 A CN201711277643 A CN 201711277643A CN 108088983 A CN108088983 A CN 108088983A
- Authority
- CN
- China
- Prior art keywords
- paint
- fluid sealant
- panel
- test plate
- cracking
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of automobile water paints and the mating lower cracking detection method of fluid sealant, mainly include the following steps that:Glued membrane is coated on test plate (panel), allotment paint by the paint spraying on the glued membrane, controls the test plate (panel) to carry out cracking simulation experiment, detects and analyze the result of the cracking simulation experiment;The automobile water paint of the present invention and the mating lower split test method of fluid sealant, the cracking situation of detection different type water paint and scene fluid sealant can quickly be carried out, and testing result is evaluated, quickly determine whether the matching of the water paint and corresponding fluid sealant is excellent, the water paint lower cracking detection method mating with fluid sealant and evaluation method developed of the present invention are easy to operate, controllability is good, favorable reproducibility, can quickly detect and judge, can provide reference frame with the mating application of fluid sealant at the scene for water paint.
Description
Technical field
The present invention relates to a kind of automobile lacker crack determining technical field, a kind of particularly automobile water paint is matched somebody with somebody with fluid sealant
The lower cracking detection method of set.
Background technology
With the country in environmental protection to the strict demand in auto industry, water paint is as a kind of environmental protection, high quality and low
Application of the paint of cost on vehicle coating process is constantly expanded.Domestic automobile main engine plants are in aqueous lacquer craftwork upslide at present
Enter extensive application and research.
Water paint is inevitable that other auxiliary materials with painting dressing automobiles is needed to carry out mating application during automobile production,
In it is particularly important with the mating application of automobile sealant.And fluid sealant often occurs with water paint in mating application in production
The problem of problem of Cracking after drying influences plates of automobile sealing, is further also easy to produce inner cavity corrosion, therefore water paint and fluid sealant
Matching verification just it is particularly important.
But it there is no related matching examination criteria and method to automobile water paint and fluid sealant under mating application at present
Cracking situation be detected and evaluate.
The content of the invention
It is existing to solve the object of the present invention is to provide a kind of automobile water paint and the mating lower cracking detection method of fluid sealant
It there is no related matching examination criteria and method to automobile water paint and fluid sealant in the mating lower cracking situation used in technology
The deficiency for being detected and evaluating, the present invention can be quickly and effectively in production scene to the matching performance of water paint and fluid sealant
It is used for quickly detecting, reference frame is provided for automobile water paint and matching for fluid sealant.
To achieve these goals, invention broadly provides following technical solutions:
A kind of automobile water paint and the mating lower cracking detection method of fluid sealant, comprise the following steps:The coating adhesive on test plate (panel)
Film;Allotment paint;By the paint spraying on the glued membrane;The test plate (panel) is controlled to carry out cracking simulation experiment;It detects and divides
Analyse the result of the cracking simulation experiment.
Preferably, further included before the glued membrane being coated on the test plate (panel):Pre-process the test plate (panel);Select the glued membrane
Coating method.Pre-processing the test plate (panel) is specially:Clear up the impurity on test plate (panel) surface, polishing test plate (panel) surface.
Preferably, coat on the test plate (panel) and further included between the glued membrane and the allotment paint:Dry the glued membrane;
Be sticked thickness datum strip on the glued membrane.
Preferably, allocate it is described paint and by the paint spraying on the glued membrane between further include:Described in selection
The spraying method of paint.
Preferably, the paint is allocated to specifically include:The temperature of the paint is adjusted to 20 ± 1 DEG C.
Preferably, the paint spraying is specifically included on the glued membrane:Water colour paint is pressed into thickness along gradient uniformity
The mode of variation is sprayed on the glued membrane;Dry the water colour paint;Varnish equal thickness is sprayed on to the water colour paint
On;Dry the varnish.
Preferably, the test plate (panel) is controlled to carry out the cracking simulation experiment to specifically include:The test plate (panel) is protected at 165 DEG C
Hold 35min;The test plate (panel) is carried out quick strong cold.
Preferably, the result for detecting and analyzing the cracking simulation experiment specifically includes:Detect whether the paint occurs
Cracking, if it is, record cracking situation, if it is not, then detection of end and recording mating good.
The beneficial effects of the present invention are:
The present invention provides a kind of automobile water paint and the mating lower cracking detection method of fluid sealant, mainly including following step
Suddenly:Glued membrane is coated on test plate (panel);Allotment paint;By the paint spraying on the glued membrane;The test plate (panel) is controlled to crack
Simulation test;Detect and analyze the result of the cracking simulation experiment;It is opened under automobile water paint and the fluid sealant of the present invention are mating
Test method is split, can quickly carry out the cracking situation of detection different type water paint and scene fluid sealant, and detection is tied
Fruit is evaluated, and quickly determines the water paint that whether matching of the water paint and corresponding fluid sealant is excellent, and the present invention is developed
Lower cracking detection method mating with fluid sealant and evaluation method are easy to operate, controllability is good, favorable reproducibility, can quickly realize detection and
Judge, reference frame can be provided for water paint and the mating application of fluid sealant at the scene.
Description of the drawings
Fig. 1 is flow chart of the automobile water paint with the mating lower cracking detection method of fluid sealant of the present invention.
Specific embodiment
The embodiments described below with reference to the accompanying drawings are exemplary, is only used for explaining the present invention, and cannot be construed to
Limitation of the present invention.
For the method that detection water paint there is no to match effect with fluid sealant in the prior art, the present invention provides a kind of
Automobile water paint and the mating lower cracking detection method of fluid sealant can be directed to automobile water paint and match situation development with fluid sealant
Detection and evaluation, the cracking situation of detection different type water paint and scene fluid sealant are evaluated testing result, quickly
It determines whether the water paint is mating excellent with fluid sealant, reliable foundation and reference is provided for subsequent production.
Automobile water paint provided in an embodiment of the present invention and the mating lower cracking detection method of fluid sealant, as shown in Figure 1, including
Following steps:
Glued membrane is coated on test plate (panel);
It can also comprise the following steps before coating glued membrane on test plate (panel):Pre-process the test plate (panel);Select glued membrane coating side
Formula.
It is specially the dust and impurity for clearing up test plate (panel) surface, polishing test plate (panel) surface etc. to pre-process test plate (panel), is applied with improving
Overlay on the flatness of the glued membrane on test plate (panel).
It is specially to select by the way of manual brush coating or machine brush coating to select glued membrane coating method.
Manual glue brush may be employed, fluid sealant can also be coated uniformly on test plate (panel) by apparatus control glue rifle.In order to
Convenient for later observations, when by fluid sealant coated on test plate (panel), it can be coated and be in strip glued membrane, for the number of guarantee test
According to more sufficient, the larger rectangular-shaped glued membrane of width is preferably applied as.
Being coated on test plate (panel) further preferably includes between glued membrane and allotment paint:Dry the glued membrane;It is sticked on the glued membrane
Thickness datum strip.
Coated on test plate (panel), after forming glued membrane, in order to which fluid sealant is promoted to dry, preventing fluid sealant not dry fluid sealant
It deforms or drips when dry, test plate (panel) can be placed in baking oven and toasted, test plate (panel) is preferably toasted 10 at 110 DEG C
Minute, so fluid sealant can be dried and baking was caused to fluid sealant.
The thickness of the water paint sprayed on glued membrane, the coating thickness benchmark preferably on glued membrane are subsequently read out for convenience
Item, the thickness datum strip can be sealing strip or other easy strip tapes being close on glued membrane.
If the shape of the glued membrane coated out early period is not regular enough, spreading knife or Frictioning device subsequently may be employed, it is right
Glued membrane that is coated and having dried carries out frictioning adjustment, glued membrane is spread to more regular shape, in order to subsequent behaviour
Make and observe.
Allotment paint;
Allotment paint specifically includes:
The temperature of the paint is adjusted to 20 ± 1 DEG C;The viscosity of the paint is adjusted to the first setting viscosity.Herein
In experiment, the paint of use mainly includes water colour paint and varnish.According to the condition of the product description defined of paint to oil
Paint is adjusted, wherein first sets viscosity of the viscosity as corresponding paint spraying state.
It is further included in allotment paint and by the paint spraying between the glued membrane:Select the spraying method of paint.
Paint spraying mode can be to be sprayed using robot, or using gas spray gun hand spray, incite somebody to action
Deployed paint spraying can also carry out spraying simulation before glued membrane using other test plate (panel)s, according to spraying analog result ratio
Compared with Control During Paint Spraying by Robot effect and gas spray gun hand spray effect, subsequent operation is carried out in a manner which kind of confirmation uses.
After spraying method is determined, deployed paint is placed in Shi Pen robots or in gas spray gun, it is ensured that
The supply gas pressure and stable working state of Shi Pen robots or gas spray gun meet and stablize spraying conditions, and standard is carried out for spraying
It is standby.
By the paint spraying on the glued membrane;
The paint spraying is specifically included on the glued membrane:
Water colour paint is sprayed in a manner that thickness changes along gradient uniformity on the glued membrane;
It is raw for follow-up batch in order to guarantee definitely to know the thickness of the water paint to crack when cracking
Foundation is provided in production and practical application, water colour paint is preferably sprayed on the glue in a manner that thickness changes along gradient uniformity
On film.The thickness range of paint film after water colour paint spraying is preferably 0~15 μm.And the scope of water colour paint spraying is preferred
More than the scope of glued membrane, glued membrane is made full use of with realizing.
Dry the water colour paint;
After water colour paint is sprayed, in order to improve water colour paint exsiccation speed, preferably to water colour paint film into
Row baking.The test plate (panel) for having sprayed water colour paint can be placed in an oven, be maintained at 55 DEG C and toast 8 minutes, it then will examination
Plate is cooled to room temperature, is ready for follow-up work.
Varnish equal thickness is sprayed on the water colour paint;
Dry the varnish.
In actual production application, when water colour paint is matched with fluid sealant, also the two is protected using varnish
Shield.In order to enable the present invention is further preferably coated with varnish closer to actual condition on water colour paint.Its specific spraying process
For:The varnish to match with water colour paint is sprayed on the water colour paint of test plate (panel), the preferred spraying of thickness of varnish is 25 μm, then
By varnish levelling 7 minutes, then test plate (panel) is put into baking oven and is toasted 20 minutes, promote varnish-drying.
The test plate (panel) is controlled to carry out cracking simulation experiment;
The test plate (panel) is controlled to carry out cracking simulation experiment to specifically include:
The test plate (panel) is kept into 35min at 165 DEG C;
The test plate (panel) is carried out quick strong cold.
The above process is:By the test plate (panel) Jing Guo above-mentioned processing, 165 DEG C of baking oven is put into, and keeps 35 at this temperature
Minute, after the completion of baking, the test plate (panel) is taken out, immediately after using the varnish table of gas spray gun compressed-air blows to the test plate (panel)
Face, the varnish, water colour paint and fluid sealant for making test plate (panel) are quick strong cold.
Detect and analyze the result of the cracking simulation experiment.
Detecting and analyze the result that the cracking simulation is tested is specially:Whether cracking detect the paint, if
It is then to record cracking situation, if it is not, then detection of end and recording mating good.
The result for detecting and analyzing the cracking simulation experiment specifically includes:The test plate (panel) for carrying out cracking simulation experiment is cold
But it is whether cracking to the varnish and water colour paint after room temperature, observed on test plate (panel), if there is cracking, then record cracking feelings
Condition, cracking situation specifically includes Size of Crack, crack quantity, the film thickness of corresponding water colour paint and cracking pole at cracking
Limit;It is if not cracking, then it represents that water colour paint is mating good with fluid sealant, it is possible to which that detection of end simultaneously records mating good
.
The structure, feature and effect of the present invention, more than institute are described in detail based on the embodiments shown in the drawings
Only presently preferred embodiments of the present invention is stated, but the present invention is not to limit practical range shown in drawing, it is every according to structure of the invention
Want made change or be revised as the equivalent embodiment of equivalent variations, when not going beyond the spirit of the description and the drawings,
It should all be within the scope of the present invention.
Claims (8)
1. a kind of automobile water paint and the mating lower cracking detection method of fluid sealant, which is characterized in that comprise the following steps:
Glued membrane is coated on test plate (panel);
Allotment paint;
By the paint spraying on the glued membrane;
The test plate (panel) is controlled to carry out cracking simulation experiment;
Detect and analyze the result of the cracking simulation experiment.
2. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that in institute
It states and is further included before the glued membrane is coated on test plate (panel):
Pre-process the test plate (panel);
Select the glued membrane coating method.
Pre-processing the test plate (panel) is specially:Clear up the impurity on test plate (panel) surface, polishing test plate (panel) surface.
3. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that in institute
It states to coat on test plate (panel) and be further included between the glued membrane and the allotment paint:
Dry the glued membrane;
Be sticked thickness datum strip on the glued membrane.
4. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that adjusting
With it is described paint and by the paint spraying on the glued membrane between further include:
Select the spraying method of the paint.
5. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that allotment
The paint specifically includes:
The temperature of the paint is adjusted to 20 ± 1 DEG C.
6. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that by institute
Paint spraying is stated to specifically include on the glued membrane:
Water colour paint is sprayed in a manner that thickness changes along gradient uniformity on the glued membrane;
Dry the water colour paint;
Varnish equal thickness is sprayed on the water colour paint;
Dry the varnish.
7. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that control
The test plate (panel) carries out the cracking simulation experiment and specifically includes:
The test plate (panel) is kept into 35min at 165 DEG C;
The test plate (panel) is carried out quick strong cold.
8. automobile water paint according to claim 1 and the mating lower cracking detection method of fluid sealant, which is characterized in that detection
It is specifically included with the result for analyzing the cracking simulation experiment:
Detect it is described paint it is whether cracking, if it is, record cracking situation, if it is not, then detection of end and record match somebody with somebody
Set is good.