CN107805394A - A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent and preparation method thereof - Google Patents

A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent and preparation method thereof Download PDF

Info

Publication number
CN107805394A
CN107805394A CN201711295292.6A CN201711295292A CN107805394A CN 107805394 A CN107805394 A CN 107805394A CN 201711295292 A CN201711295292 A CN 201711295292A CN 107805394 A CN107805394 A CN 107805394A
Authority
CN
China
Prior art keywords
parts
swelling agent
oil
table tennis
environment
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201711295292.6A
Other languages
Chinese (zh)
Inventor
刘海文
李海强
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Huizhou Free Sports Sports Science And Technology Service Co Ltd
Original Assignee
Huizhou Free Sports Sports Science And Technology Service Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Huizhou Free Sports Sports Science And Technology Service Co Ltd filed Critical Huizhou Free Sports Sports Science And Technology Service Co Ltd
Priority to CN201711295292.6A priority Critical patent/CN107805394A/en
Publication of CN107805394A publication Critical patent/CN107805394A/en
Pending legal-status Critical Current

Abstract

The present invention relates to one kind to be related to polymeric material field, discloses a kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent, including following parts by weight component:0.02 0.1 parts of antioxidant;0.2 0.5 parts of sodium acid carbonate;35 parts of wax class;8 15 parts of grease.The swelling agent excellent performance, it is friendly to human body environment.The invention also discloses the preparation method of two kinds of formulations of its solid and liquid, and its application is convenient, is adapted to various motion occasions.

Description

A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent and preparation method thereof
Technical field
The present invention relates to polymeric material field, and in particular to a kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer expansion Agent and preparation method thereof.
Background technology
The technological innovation relevant with table tennis device therefor and the change of rule generate great shadow to this motion Ring, have impact on the result of many lofty tones match including World Championships.Particularly table tennis bat and two main portion Part-rubber and bottom plate-has had many technical improvement, because International Table Tennis Federation(ITTF)Nineteen twenty-six just This motion of formula tissue(International Table Tennis Federation is still management organization of the world).Modern table tennis bat has a kind of " inversion rubber "(Also referred to as For " rubber "), its top-sheet made of vulcanization rubber is adhered on the internal layer of expanded rubber sponge or foam.Rubber adheres to On the timber or Wood composite material blade of optimization.The motion feature of modern table tennis bat is made with nineteen twenties Racket or the racket even used in nineteen fifties almost do not have any similarity.
One world-class sportsman can be using the equipment of modernization, so that up to 100 miles of ball is fast per hour and is up to 9000 turns per minute of ball speed rotation.
In later stage nineteen seventies, many paddler have found that certain form of solvent can influence rubber Kinetic characteristic.These sportsmen use the short time before match will based on the adhesive of solvent such as trichloro ethylene and 1,2- dichloroethylene " rubber "(The usually used term in table tennis)It is bonded on veneer.To lift rubber performance, however it is such molten Agent volatility is big, and VOC is exceeded, unfavorable to human body and environment.
The content of the invention
The technical problems to be solved by the invention are to provide a kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent, Environmentally friendly using food grade raw material, VOC emission is extremely low, on the sponge applied to table tennis case glue, can absorb rapidly swollen It is swollen, and viscosity is good.
The technical problems to be solved by the invention are achieved by the following technical programs:
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent, is paste or liquid, the preparing raw material of paste swelling agent Including following parts by weight component:
Antioxidant 0.02-0.1 parts;
Sodium acid carbonate 0.2-0.5 parts;
Wax class 3-5 parts;
Grease 8-15 parts;
The preparing raw material of liquid swelling agent includes following parts by weight component:
Antioxidant 0.2-0.5 parts;
Sodium acid carbonate 1-5 parts;
Wax class 3-8 parts;
Grease 70-80 parts.
Further, described grease includes:Seabuckthorm Seed Oil, soybean oil, grape-kernel oil, Queensland nut seed oil, Jojoba Seed is oily, shepherd's purse seed is saved at white pond flower seed oil, Butyrospermum parkii fruit fat, olive oil, sweet almond oil, avocado oil, hemp-seed oil, deep-sea two At least one of oil, camellia seed oil, hydrogenated coco-glyceride class, hydrogenated sunflower oil, cocoa seed fat or a variety of arbitrary proportions Mixing.
Further, described wax class includes:Beeswax, candelila wax, Brazil wax, beeswax, sunflower seeds wax, Jojoba The mixing of at least one of seed wax or a variety of arbitrary proportions.
Further, described antioxidant includes:Vitamin E, tert-butylhydroquinone one of which or two kinds are any The mixing of ratio.
A kind of preparation method of described environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent, comprises the following steps:
a:By antioxidant, sodium acid carbonate, grease homogenizer homogeneous 20 minutes, then stir 20 minutes, sealing and standing 3 days, Filtered using 300-400 mesh oil filter paper, it is stand-by;
b:Wax class, remaining grease are heated into 90 DEG C in heating cylinder to be uniformly dissolved, 50 DEG C is cooled to and adds obtained by step a Material dissolution is uniform;
c:Mould molding is injected, obtains paste finished product.
A kind of preparation method of described environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent, comprises the following steps:
a:By antioxidant, sodium acid carbonate, amount of grease homogenizer homogeneous 20 minutes, then stir 20 minutes, sealing and standing 3 My god, filtered using 300-400 mesh oil filter paper, it is stand-by;
b:Wax class, remaining grease are heated into 90 DEG C in heating cylinder to be uniformly dissolved, 50 DEG C is cooled to and adds obtained by step a Material dissolution stirs, and is cooled to room temperature and obtains liquid finished product.
The present invention has the advantages that:
Swelling agent is mainly used on the sponge of film table tennis bat series glue, can be rapidly permeated into using grease among sponge, formed compared with Good faying face, the wax class of outer layer form outer membrane sodium acid carbonate and slowly decompose aerogenesis, and formation bubble is expanded in wax class, makes set Glue is molded rapidly.
Embodiment
With reference to embodiment, the present invention will be described in detail, and embodiment is only the preferred embodiment of the present invention, It is not limitation of the invention.
Raw material used in embodiment 1-6 is conventional commercial product.
Embodiment 1
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer paste swelling agent, preparing raw material include following parts by weight component:
0.02 part of vitamin E;
0.5 part of sodium acid carbonate;
5 parts of beeswax;
13 parts of olive oil.
Embodiment 2
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer paste swelling agent, preparing raw material include following parts by weight component:
0.1 part of vitamin E;
0.2 part of sodium acid carbonate;
3 parts of beeswax;
8 parts of olive oil.
Embodiment 3
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer paste swelling agent, preparing raw material include following parts by weight component:
0.05 part of vitamin E;
0.3 part of sodium acid carbonate;
4 parts of beeswax;
15 parts of olive oil.
Embodiment 1-3 preparation method comprises the following steps:
a:By the vitamin E, sodium acid carbonate, olive oil of aforementioned proportion homogenizer homogeneous 20 minutes, 20 points are then stirred Clock, sealing and standing 3 days, filtered using 300 mesh oil filter papers, it is stand-by;
b:Beeswax, remaining olive oil are heated into 90 DEG C in heating cylinder to be uniformly dissolved, 50 DEG C is cooled to and adds step A resulting materials are uniformly dissolved;
c:Mould molding is injected, obtains paste finished product.
Embodiment 4
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer liquid swelling agent, preparing raw material include following parts by weight component:
0.3 part of vitamin E;
1 part of sodium acid carbonate;
8 parts of beeswax;
70 parts of olive oil.
Embodiment 5
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer liquid swelling agent, preparing raw material include following parts by weight component:
0.5 part of vitamin E;
5 parts of sodium acid carbonate;
5 parts of beeswax;
80 parts of olive oil.
Embodiment 6
A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer liquid swelling agent, preparing raw material include following parts by weight component: 0.2 part of vitamin E;
4 parts of sodium acid carbonate;
3 parts of beeswax;
73 parts of olive oil.
Embodiment 4-6 preparation method comprises the following steps:
a:By the vitamin E, sodium acid carbonate, olive oil of aforementioned proportion homogenizer homogeneous 20 minutes, 20 points are then stirred Clock, sealing and standing 3 days, filtered using 400 mesh oil filter papers, it is stand-by;
b:Beeswax, remaining olive oil are heated into 90 DEG C in heating cylinder to be uniformly dissolved, 50 DEG C is cooled to and adds step The dissolving of a resulting materials stirs, and is cooled to room temperature and obtains liquid finished product.
In order to further illustrate the present invention, embodiment 1-6 is accordingly tested below:
Paste swelling agent obtained by embodiment 1-3 is uniformly applied on the sponge of certain commercially available set glue, placement treats that sponge inhales completely After receiving swelling agent(That is sponge surface dry oil free), glue warp to be covered into tubular, hold by test consumed time, and rolled state The continuous time(The time required to not rolled up completely to set glue).
Liquid swelling agent obtained by embodiment 4-6 is uniformly painted on the sponge of certain commercially available set glue, placement treats that sponge is complete After hypersorption swelling agent(That is sponge surface dry oil free), glue warp to be covered is into tubular, test the consumed time, and curly The state duration(The time required to not rolled up completely to set glue).
Test result is as follows:
Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Embodiment 6
Spent time (h) 3 3.5 3 4 5 4.5
Duration (d) 17 20 19 18 15 21
Curling set obtained by set the glue comparative example 1-2 and embodiment 1-6 of unused swelling agent is gluing on bottom plate, choose 10 National second grade sportsman carries out table tennis impact test, and set glue used and bottom plate are the commercially available conventional products of same model, Compared with comparative example 1-2, the racket impact sense obtained by embodiment 1-6 is more preferable, and the power of ball, rotation are stronger.

Claims (6)

1. a kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent, it is characterised in that be paste or liquid, paste expands The preparing raw material of agent includes following parts by weight component:
Antioxidant 0.02-0.1 parts;
Sodium acid carbonate 0.2-0.5 parts;
Wax class 3-5 parts;
Grease 8-15 parts;
The preparing raw material of liquid swelling agent includes following parts by weight component:
Antioxidant 0.2-0.5 parts;
Sodium acid carbonate 1-5 parts;
Wax class 3-8 parts;
Grease 70-80 parts.
2. environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent according to claim 1, it is characterised in that described Grease includes:Seabuckthorm Seed Oil, soybean oil, grape-kernel oil, Queensland nut seed oil, jojoba seed oil, white pond flower seed oil, Butyrospermum parkii Shepherd's purse seed oil, camellia seed oil, hydrogenated coco glycerine are saved in fruit fat, olive oil, sweet almond oil, avocado oil, hemp-seed oil, deep-sea two The mixing of at least one of esters, hydrogenated sunflower oil, cocoa seed fat or a variety of arbitrary proportions.
3. environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent according to claim 1, it is characterised in that described Wax class includes:At least one of beeswax, candelila wax, Brazil wax, beeswax, sunflower seeds wax, Jojoba seed wax are a variety of The mixing of arbitrary proportion.
4. environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent according to claim 1, it is characterised in that described Antioxidant includes:The mixing of vitamin E, tert-butylhydroquinone one of which or two kinds of arbitrary proportions.
A kind of 5. preparation side of the environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent described in claim 1-4 any one Method, it is characterised in that comprise the following steps:
a:By antioxidant, sodium acid carbonate, grease homogenizer homogeneous 20 minutes, then stir 20 minutes, sealing and standing 3 days, Filtered using 300-400 mesh oil filter paper, it is stand-by;
b:Wax class, remaining grease are heated into 90 DEG C in heating cylinder to be uniformly dissolved, 50 DEG C is cooled to and adds obtained by step a Material dissolution is uniform;
c:Mould molding is injected, obtains paste finished product.
A kind of 6. preparation side of the environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent described in claim 1-4 any one Method, it is characterised in that comprise the following steps:
a:By antioxidant, sodium acid carbonate, grease homogenizer homogeneous 20 minutes, then stir 20 minutes, sealing and standing 3 days, Filtered using 300-400 mesh oil filter paper, it is stand-by;
b:Wax class, remaining grease are heated into 90 DEG C in heating cylinder to be uniformly dissolved, 50 DEG C is cooled to and adds obtained by step a Material dissolution stirs, and is cooled to room temperature and obtains liquid finished product.
CN201711295292.6A 2017-12-08 2017-12-08 A kind of environment-protecting and non-poisonous rubber on table tennis bat spongy layer swelling agent and preparation method thereof Pending CN107805394A (en)