CN107673684A - A kind of ink and painting day sanded brick production technology - Google Patents
A kind of ink and painting day sanded brick production technology Download PDFInfo
- Publication number
- CN107673684A CN107673684A CN201710987112.4A CN201710987112A CN107673684A CN 107673684 A CN107673684 A CN 107673684A CN 201710987112 A CN201710987112 A CN 201710987112A CN 107673684 A CN107673684 A CN 107673684A
- Authority
- CN
- China
- Prior art keywords
- basic unit
- ink
- pressure head
- mold frame
- natural sand
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material includes cement, meter Shi and flour;The composition of capstock includes red natural sand, black natural sand, white natural sand and binder materials;Specific make step:Red natural sand, black natural sand, white natural sand and binder materials are proportionally mixed into capstock by S1;Cement, meter Shi and flour are stirred into basic unit with mixer in proportion and expected by S2;S3 pours into basic unit's material in low mold frame, is gently pressed with pressure head, and pressure head depression distance is between 5 10mm, and after light pressure, pressure head leaves low mold frame;Precoat uniform distribution is pushed down low mold frame by S4 above basic unit's material, then with pressure head, and entirely through excitational equipment, so as to exclude air, the moisture in basic unit's material and capstock, obtains ink and painting day sanded brick;After S5 obtains ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, maintenance ink and painting day sanded brick is stood, packs, dispatches from the factory.
Description
Technical field
The present invention relates to the technical field of construction material, specifically, refers to a kind of ink and painting day sanded brick production technology.
Background technology
With the increasingly raising of the continuous development of construction industry, particularly living standards of the people, people are to living environment requirement
Increasingly stricter, people, for the needs of brick, will not change from ancient times to the present in building construction, traditional azulejo,
Out-of-flatness, water permeability resistance can be bad, and water absorbing properties are higher.
In existing building, use sanded brick surface layer it is basic will be based on grey, while the often face in decoration process
The intensity of layer is not high, and surface is easy to rugged place occur, and its influences whole shape, client is caused greatly
Hidden danger.
It is therefore desirable to design a kind of to improve sanded brick surface layer intensity and sanded brick surface layer technical scheme attractive in appearance.
The content of the invention
The present invention provides a kind of ink and painting day sanded brick production technology, for solving to exist in the prior art:In existing skill
In art, the surface layer of brick often insufficient strength, easily drop, especially influence the technical problem of brick bulk strength.
In order to solve the above-mentioned technical problem, reach and improve sanded brick surface layer intensity and sanded brick surface layer beneficial effect attractive in appearance, this
Invention is achieved through the following technical solutions:Including basic unit's material and capstock, the composition of basic unit material includes cement, meter Shi and broken
Powder;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:Red natural sand, black natural sand, white natural sand and binder materials are proportionally mixed into capstock;
S2:Cement, meter Shi and flour are stirred into basic unit with mixer in proportion to expect;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 5-10mm, after light pressure, pressure
Head leaves low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtaining ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance curing water
Black painting day sanded brick and then packaging, dispatch from the factory.
The red natural sand crosses 20~40 mesh sieves, and black natural sand crosses 20~40 mesh sieves, and white natural sand crosses 20~40
Mesh, the binder materials are cement.
In order to preferably realize the present invention, further, the S3:Basic unit's material is poured into low mold frame, gently pressed with pressure head,
Pressure head depression distance is between 8-10mm, and after light pressure, pressure head leaves low mold frame.
In order to preferably realize the present invention, further, the S3:Basic unit's material is poured into low mold frame, gently pressed with pressure head,
Pressure head depression distance is between 9mm, and after light pressure, pressure head leaves low mold frame.
In order to preferably realize the present invention, further, the composition of basic unit material include cement, meter Shi and flour according to
Ratio is 3~9:1~6:1~11.
In order to preferably realize the present invention, further, the composition of the capstock is natural including red natural sand, black
Sand, white natural sand and binder materials are proportionally 1~10:1~12:1~10:5~15.
In order to preferably realize the present invention, further, the binder materials is cement.
The present invention is passed through by the way that the composition of surface layer is arranged into black natural sand, red natural sand and white natural sand
The combination of the free deal of these three compositions so that the color showed the variation of surface layer, what is be particular about very much for face paving
Place, by the proportioning of these three compositions, entirety can be made to show a width landscape painting, while because adding gelling in composition
Material, the material are preferably cement, there is fine cohesive force so that the natural sand of three different colors, can firmly glue
It is connected on basic unit's material, so as to strengthen the intensity of capstock of the present invention, relative in the prior art, capstock is substantially painting one
For the azulejo of layer color, structure of the invention is more stable, and applicability is stronger.
The present invention compared with prior art, has advantages below and beneficial effect:
(1) present invention is by setting basic unit's material and capstock to prepare the sanded brick with chromatic colour, the surface layer of this sanded brick, not only
With color, while also have the advantages that anti-flammability is high, intensity is high;
(2) present invention can make sanded brick surface layer that the mixing of different color be presented by the regulation and control to capstock formula rate
Surface layer, make sanded brick surface layer color diversified;
(3) preparation process of the present invention is simple, and novel in design, product face brick is rich in color, durability, so that enterprise
Market efficiency is good.
Embodiment
The present invention is described in further detail with reference to embodiment, but the implementation of the present invention is not limited to this.
Embodiment 1:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:50kg red natural sands are crossed into 20 mesh sieves, 50kg black natural sands cross 40 mesh sieves, 50kg white natural sands cross 80
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 5mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 1.
Embodiment 2:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:30kg red natural sands are crossed into 40 mesh sieves, 60kg black natural sands cross 40 mesh sieves, 50kg white natural sands cross 40
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 5mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 2.
Embodiment 3:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:50kg red natural sands are crossed into 30 mesh sieves, 40kg black natural sands cross 60 mesh sieves, 60kg white natural sands cross 40
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 6mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 3.
Embodiment 4:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:40kg red natural sands are crossed into 20 mesh sieves, 80kg black natural sands cross 60 mesh sieves, 60kg white natural sands cross 40
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 7mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 4.
Embodiment 5:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:20kg red natural sands are crossed into 40 mesh sieves, 50kg black natural sands cross 80 mesh sieves, 60kg white natural sands cross 60
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 8mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 5.
Embodiment 6:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:50kg red natural sands are crossed into 60 mesh sieves, 20kg black natural sands cross 40 mesh sieves, 40kg white natural sands cross 20
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 9mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 6.
Embodiment 7:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:40kg red natural sands are crossed into 30 mesh sieves, 40kg black natural sands cross 40 mesh sieves, 90kg white natural sands cross 20
Mesh sieve and 20kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 10mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 7.
Comparative example 1:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:80kg red natural sands are crossed into 20 mesh sieves, 80kg black natural sands cross 10 mesh sieves, 80kg white natural sands cross 10
Mesh sieve is mixed into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 1mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 8.
Comparative example 2:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:80kg red natural sands are crossed into 20 mesh sieves, 80kg black natural sands cross 20 mesh sieves, 80kg white natural sands cross 10
Mesh sieve and 2kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 2mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 9.
Comparative example 3:
A kind of ink and painting day sanded brick production technology, including basic unit's material and capstock, the composition of basic unit's material include water
Mud, meter Shi and flour;The composition of the capstock includes red natural sand, black natural sand, white natural sand and binder materials;
Specific make step:
S1:80kg red natural sands are crossed into 20 mesh sieves, 50kg black natural sands cross 10 mesh sieves, 80kg white natural sands cross 10
Mesh sieve and 10kg cement mixings are into capstock;
S2:By 300kg cement, 600kg rice stone and 110kg flours, it is stirred into basic unit with mixer and expects;
S3:Basic unit's material to be poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 4mm, after light pressure, pressure head
Leave low mold frame;
S4:By precoat uniform distribution above basic unit's material, then with pressure head low mold frame is pushed down, and set entirely through exciting
It is standby, so as to exclude air, the moisture in basic unit's material and capstock, obtain ink and painting day sanded brick;
S5:After obtained ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink
Painting day sanded brick and then packaging, dispatch from the factory, that is, obtain finished product 10.
The contrast of experimental data:Finished product 1~7 can comply with the national standard requirements, and the crushing resistance of the surface layer of finished product 8~10
Energy, and tensile property do not meet requirements of the national standard.
Although an embodiment of the present invention has been shown and described, it will be understood by those skilled in the art that being:
A variety of change, modification, replacement and modification, the present invention can be carried out to these embodiments by not departing under the principle and objective of the present invention
Scope limited by claim and its equivalent.
Claims (5)
- A kind of 1. ink and painting day sanded brick production technology, it is characterised in that:Including basic unit's material and capstock, basic unit material into Dividing includes cement, meter Shi and flour;The composition of the capstock include red natural sand, black natural sand, white natural sand and Binder materials;Specific make step:S1:Red natural sand, black natural sand, white natural sand and binder materials are proportionally mixed into capstock;S2:Cement, meter Shi and flour are stirred into basic unit with mixer in proportion to expect;S3:Basic unit's material is poured into low mold frame, gently pressed with pressure head, pressure head depression distance is between 5-10mm, after light pressure, pressure head from Open low mold frame;S4:By precoat uniform distribution above basic unit's material, then with pressure head push down low mold frame, and entirely through excitational equipment, from And basic unit's material and air, moisture in capstock are excluded, obtain ink and painting day sanded brick;S5:After obtaining ink and painting day sanded brick, ink and painting day sanded brick is released from low mold frame, stands maintenance ink and painting day Sanded brick and then packaging, dispatch from the factory.
- 2. ink and painting day sanded brick production technology according to claim 1, it is characterised in that:The S3:Basic unit's material is fallen Enter in low mold frame, gently pressed with pressure head, pressure head depression distance is between 8-10mm, and after light pressure, pressure head leaves low mold frame.
- 3. ink and painting day sanded brick production technology according to claim 1, it is characterised in that:The S3:Basic unit's material is fallen Enter in low mold frame, gently pressed with pressure head, pressure head depression distance is between 9mm, and after light pressure, pressure head leaves low mold frame.
- 4. ink and painting day sanded brick production technology according to claim 1, it is characterised in that:Basic unit material into subpackage It is proportionally 3~9 to include cement, meter Shi and flour:1~6:1~11.
- 5. ink and painting day sanded brick production technology according to claim 1, it is characterised in that:The capstock into subpackage It is proportionally 1~10 to include red natural sand, black natural sand, white natural sand and binder materials:1~12:1~10:5~ 15。