CN107245539A - A kind of persistent form fur feel improver and its preparation method and application - Google Patents

A kind of persistent form fur feel improver and its preparation method and application Download PDF

Info

Publication number
CN107245539A
CN107245539A CN201710607164.4A CN201710607164A CN107245539A CN 107245539 A CN107245539 A CN 107245539A CN 201710607164 A CN201710607164 A CN 201710607164A CN 107245539 A CN107245539 A CN 107245539A
Authority
CN
China
Prior art keywords
persistent form
feel improver
fur
skin
feel
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201710607164.4A
Other languages
Chinese (zh)
Inventor
段郑军
郑超斌
郑红超
康定国
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Fanbo Cleaning Technology Research Co Ltd
Original Assignee
Beijing Fanbo Cleaning Technology Research Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing Fanbo Cleaning Technology Research Co Ltd filed Critical Beijing Fanbo Cleaning Technology Research Co Ltd
Priority to CN201710607164.4A priority Critical patent/CN107245539A/en
Publication of CN107245539A publication Critical patent/CN107245539A/en
Pending legal-status Critical Current

Abstract

The invention provides a kind of persistent form fur feel improver and its preparation method and application, including according to the following component of mass percentage:Silicone oil 5%~30%, fatty alcohol 0.1%~5%, nonionic surfactant 1%~10%, preservative 0.1%~1% and deionized water 54%~93.8%.Persistent form fur feel improver provided herein, using the formula design concept of the scientific and feature of environmental protection, lasting under circumstances can keep bright, soft, the smooth performance of fur, significantly improve fur quality.The feel improvement processing of sheepskin hair, raw fox skin, recoon dog skin, standard mink skin and rabbit is may be used as, energy consumption is reduced, meets market demands.

Description

A kind of persistent form fur feel improver and its preparation method and application
Technical field
The present invention relates to fur manufacturing process Final finishing technical field, in particular to a kind of persistent form fur feel Improver and its preparation method and application.
Background technology
Fur in process, due to by degreasing, pickling, softening, tanning, drift color, the series of processes, hair such as dyeing Scale layer damage seriously, causes fleece tarnish, easily knot not fluffy, the easy electrostatic when weather is more dried, is unfavorable for Arrange, pursuit of the influence people to high-grade fur comfortableness.
Fur feel improver is as the additive in fur manufacturing manufacturing process, mainly to improve fur goods product Matter, improves fur feel, and assign fur remarkable soft, smooth and antistatic effect.
As domestic economy maintains sustained and rapid growth, people are further pulled on to domestic demand market, and quality is worn for fur It is also proposed that very high requirement, the also more and more higher of the requirement to fur material enterprise chemicals therewith.But current fur processing enterprise Used fur feel improver, effect can meet customer requirement in a short time, humid air and environmental pollution compared with In serious air, it is difficult to persistently keep feel and gloss, fleece feel can be astringent or even can cause adhesive hair, often because of hand Sense problem and influence subsequent production, due to repeatedly carrying out the use of hand feel finishing agent, serious dirt is will also result in environment Dye.
In view of this, it is special to propose the present invention.
The content of the invention
The first object of the present invention is to provide a kind of persistent form fur feel improver, described to solve the above problems Persistent form fur feel improver, using the formula design concept of the scientific and feature of environmental protection, there is provided a kind of persistent form fur hand Feel improver, can the lasting performance for keeping fur bright, soft, smooth under circumstances, fur can be significantly improved Quality, reduces energy consumption, meets market demands.
The second object of the present invention is to provide a kind of preparation method of described persistent form fur feel improver, the party Each material is dissolved, mixed by method successively, have the advantages that it is convenient, simple, be easy to large-scale production.
The third object of the present invention is to provide a kind of application of described persistent form fur feel improver, may be used as In sheepskin hair, raw fox skin, recoon dog skin, the feel improvement processing of standard mink skin and rabbit.
In order to realize the above-mentioned purpose of the present invention, spy uses following technical scheme:
A kind of persistent form fur feel improver, including according to the following component of mass percentage:
Silicone oil 5%~30%, fatty alcohol 0.1%~5%, nonionic surfactant 1%~10%, preservative 0.1% ~1% and deionized water 54%~93.8%.
It is preferred that, described persistent form fur feel improver, including according to the following component of mass percentage:
Organosilicon 5%~25%, fatty alcohol 0.5%~3%, nonionic surfactant 3%~8%, preservative 0.1% ~0.5% and deionized water 63.5%~91.4%.
It is preferred that, the silicone oil is one or more of in dimethicone, amido silicon oil and polyether modified silicon oil Combination.
It is preferred that, the fatty alcohol is selected from C12-14Alcohol and C16-18Alcohol;
Preferred one or several kinds of combinations of the fatty alcohol in lauryl alcohol, tetradecyl alchohol, hexadecanol and octadecyl alcolol.
It is preferred that, the nonionic surfactant be selected from peregal, polyethylene glycol, isomerous tridecanol polyoxyethylene ether and One or more of combinations in lanolin isohexadecyl ether;
It is furthermore preferred that it is described it is average add as peregal o-9, the polyethylene glycol is polyethylene glycol 1500, the isomery ten Triol APEO is isomerous tridecanol polyoxyethylene ether 1307.
It is preferred that, state preservative and be selected from sodium benzoate, MIT, the different thiophenes of 5- chloro-2-methyls -4- One or more of combinations in oxazoline -3- ketone and p-hydroxybenzoate.
The preparation method of described persistent form fur feel improver, comprises the following steps:
(1), nonionic surfactant is added in portions of de-ionized water, stirring, heating obtain non-ionic surface work The aqueous solution of property agent, it is standby;
It is preferred that described be heated to 50~60 DEG C;
(2), fatty alcohol is put into reactor, 50~70 DEG C are heated to, it is to be dissolved after add silicone oil while stirring, mix The aqueous solution of the nonionic surfactant added afterwards in step (1);
It is preferred that, in step (2), solution is maintained at 50~70 DEG C;
(3) stirring is completely dissolved nonionic surfactant, is then cooled to 25~30 DEG C, adds remaining deionization Water and preservative, obtain the persistent form fur feel improver;
It is preferred that mixing time be 30~50 minutes.
The application of described persistent form fur feel improver, including processing sheepskin hair and thin miscellaneous skin, the thin miscellaneous suitcase Include raw fox skin, recoon dog skin, standard mink skin and rabbit.
It is preferred that, the feel processing method of the sheepskin hair comprises the following steps:
(1) configuration sheepskin hair treatment fluid:Including 80~120 parts of 80~120 parts of formic acid, alcohol according to mass fraction meter and 800~1000 parts of water, the addition of the persistent form fur feel improver is 40~70ml/L, and the treatment fluid configured is stirred It is stand-by after mixing uniformly;
(2) the sheepskin treatment fluid that step (1) has been configured uniformly is brushed on wool with long hairbrush, rolled repeatedly on ironing machine Scald, until wool drying, not moist, processing completion.
It is preferred that, the feel processing method of the thin miscellaneous skin comprises the following steps:
Every 40 kilograms wooden chaffs add long type fur feel improver described in 500~700mL, add appropriate antistatic additive, Rotary drum carries out wooden chaff and adds light, completion processing.
Compared with prior art, beneficial effects of the present invention are:
(1) persistent form fur feel improver provided herein, is designed using the formula of the scientific and feature of environmental protection and managed Read, can the lasting performance for keeping fur bright, soft, smooth under circumstances, significantly improve fur quality.
(2) persistent form fur feel improver provided herein is used, sheepskin hair, raw fox skin, recoon dog is may be used as The feel improvement processing of skin, standard mink skin and rabbit, reduces energy consumption, meets market demands.
Embodiment
Technical scheme is clearly and completely described below in conjunction with embodiment, but ability Field technique personnel will be understood that following described embodiment is a part of embodiment of the invention, rather than whole embodiments, The present invention is merely to illustrate, and is not construed as limiting the scope of the present invention.Based on the embodiment in the present invention, the common skill in this area The every other embodiment that art personnel are obtained under the premise of creative work is not made, belongs to the model that the present invention is protected Enclose.Unreceipted actual conditions person in embodiment, the condition advised according to normal condition or manufacturer is carried out.Agents useful for same or instrument Unreceipted production firm person, is the conventional products that can be obtained by commercially available purchase.
A kind of persistent form fur feel improver, including according to the following component of mass percentage:
Silicone oil 5%~30%, fatty alcohol 0.1%-5%, nonionic surfactant 1%~10%, preservative 0.1%~ 1% and deionized water 54%~93.8%.
Silicone oil, silicone oil refers to keeping the linear polysiloxanes product of liquid condition at room temperature.Be divided into methyl-silicone oil and The class of modified silicon oil two.The most frequently used silicone oil --- methyl-silicone oil, also referred to as common silicone oil, all methyl of its organic group, first Base silicone oil has good chemical stability, insulating properties, and hydrophobic performance is good.It is waterproof after leather is handled through silicone oil, but do not influence Gas permeability and penetrability, can extend leather service life.Upper leather its tensile strength after processing can improve 11% to 14%, wear-resisting Property is also significantly improved, and can also improve dressing.
Fatty alcohol, fatty alcohol is the aliphatic alcohols with 8 to 22 carbon atom chains.Fatty alcohol generally has the carbon of even number Atom and a hydroxyl for being connected to carbochain end.Formula is ROH.Using fatty alcohol as raw material, make a variety of with various excellent The surfactant of different in nature energy.
Silicone oil is usually cation, is used alone to processing leather and fur effect and bad, adds fatty alcohol and non-ionic surface Activating agent is more conducive to make fur become soft as surface conditioning agent.In addition, fatty alcohol also has certain degreasing power.
It is preferred that, described persistent form fur feel improver, including according to the following component of mass percentage:
Organosilicon 5%~25%, fatty alcohol 0.5%~3%, nonionic surfactant 3%~8%, preservative 0.1% ~0.5% and deionized water 63.5%~91.4%.
The component of persistent form fur feel improver can be carried out preferred.
It is preferred that, the silicone oil is one or more of in dimethicone, amido silicon oil and polyether modified silicon oil Combination.
It is furthermore preferred that the silicone oil is selected from dimethyl silicone polymer, dimethyl silicone polymer, amido silicon oil, amido silicon oil With one or several kinds of combinations in polyether modified siloxane.
Still more preferably, the viscosity of the dimethyl silicone polymer is 12500cs, the dimethyl silicone polymer Viscosity is 1000cs, and the ammonia value of the amido silicon oil is 0.5~0.9.
It is preferred that, the fatty alcohol is selected from C12-14Alcohol and C16-18Alcohol;
Preferred one or several kinds of combinations of the fatty alcohol in lauryl alcohol, tetradecyl alchohol, hexadecanol and octadecyl alcolol.
It is preferred that, the nonionic surfactant be selected from peregal, polyethylene glycol, isomerous tridecanol polyoxyethylene ether and One or more of combinations in lanolin isohexadecyl ether;
It is furthermore preferred that it is described it is average add as peregal o-9, the polyethylene glycol is polyethylene glycol 1500, the isomery ten Triol APEO is isomerous tridecanol polyoxyethylene ether 1307.
Nonionic surfactant, the surfactant of ion is not produced in aqueous.Nonionic surfactant exists Solubility in water is due to have the functional group of strongly hydrophilic in molecule, nonionic surfactant be quantitatively only second to it is cloudy from Sub- surfactant.It is average to add as fatty alcohol and ethylene oxide condensate, milky decorating film.Wherein, peregal o-9 color and lusters Pt-Co≤20, hydrocarbon 86 ± 3mgKOH/g of value, moisture content≤1.0, pH value (1% aqueous solution) 5.0~7.0, HLB value 12~12.5.It is poly- The structural formula of ethylene glycol is HO (CH2CH2O)nH, by oxirane and water or ethylene glycol, progressively addition polymerization is formed.Polyethylene glycol 1500 be the mixture of oxirane and water polycondensation, is white waxy solid thin slice or particulate powder;Slightly special smell. It is readily soluble in water or ethanol, it is insoluble in ether.Condensation point is 41~46 DEG C, and the dynamic viscosity at 40 DEG C is 3.0~4.0mm2/S。
Isomerous tridecanol polyoxyethylene ether, is easily dispersed or dissolved in water, with excellent wetability, permeability and emulsibility. There is special emulsifying effectiveness to amido silicon oil and dimethicone, and effect after use can be improved, than general silicone oil emulsification agent Consumption is less, and emulsion is more stable, and has extremely strong penetration, may penetrate into the inside of fiber, so as to obtain more satisfied softness Feel.Wherein, No. CAS is 9043-30-5, and pH-5.5-7.5, cloud point is 60.0-62.0, and HBL values are 10.5, condensation point < 5 DEG C, wetting power 80, foam height 50, surface tension 27, viscosity 85.
It is preferred that, state preservative and be selected from sodium benzoate, MIT, the different thiophenes of 5- chloro-2-methyls -4- One or more of combinations in oxazoline -3- ketone and p-hydroxybenzoate.
Preservative can prevent reagent from going bad, and improve the service life of improver.
The preparation method of described persistent form fur feel improver, comprises the following steps:
(1), nonionic surfactant is added in portions of de-ionized water, stirring, heating obtain non-ionic surface work The aqueous solution of property agent, it is standby;
It is preferred that described be heated to 50~60 DEG C;
(2), fatty alcohol is put into reactor, 50~70 DEG C are heated to, it is to be dissolved after add silicone oil while stirring, mix The aqueous solution of the nonionic surfactant added afterwards in step (1);
It is preferred that, in step (2), solution is maintained at 50~70 DEG C;
(3) stirring is completely dissolved nonionic surfactant, is then cooled to 25~30 DEG C, adds remaining deionization Water and preservative, obtain the persistent form fur feel improver;
It is preferred that mixing time be 30~50 minutes.
The preparation method of persistent form fur feel improver provided herein, each material is dissolved successively, mixed, tool Have the advantages that conveniently, it is simple, be easy to large-scale production.
The application of described persistent form fur feel improver, including processing sheepskin hair and thin miscellaneous skin, the thin miscellaneous suitcase Include raw fox skin, recoon dog skin, standard mink skin and rabbit.
It is preferred that, the feel processing method of the sheepskin hair comprises the following steps:
(1) configuration sheepskin hair treatment fluid:Including 80~120 parts of 80~120 parts of formic acid, alcohol according to mass fraction meter and 800~1000 parts of water, the addition of the persistent form fur feel improver is 40~70ml/L, and the treatment fluid configured is stirred It is stand-by after mixing uniformly;
(2) the sheepskin treatment fluid that step (1) has been configured uniformly is brushed on wool with long hairbrush, rolled repeatedly on ironing machine Scald, until wool drying, not moist, processing completion.
It is preferred that, the feel processing method of the thin miscellaneous skin comprises the following steps:
Every 40 kilograms wooden chaffs add long type fur feel improver described in 500~700mL, add appropriate antistatic additive, Rotary drum carries out wooden chaff and adds light, completion processing.
The application process of persistent form fur feel improver provided herein is simple, holding fur light that can be lasting Bright, soft, smooth performance, significantly improves fur quality.It may be used as sheepskin hair, raw fox skin, recoon dog skin, standard mink skin and rabbit Feel improvement processing, reduce energy consumption, meet market demands.
Embodiment 1
The persistent form fur feel improver that the present embodiment is provided, the weight/mass percentage composition table of its component is as shown in table 1.
The component content of the embodiment 1 of table 1
The persistent form fur feel improver preparation method, its step is as follows:
(1) nonionic surfactant is dissolved with 40g deionized waters, and be heated to 50 degree it is stand-by;
(2), fatty alcohol is put into reactor, 50 DEG C are begun heat to, it is to be dissolved after add organosilicon while stirring, stir Mix uniform;Nonionic surfactant input reactor in, and be heated to 5 DEG C degree, it is to be dissolved after stir;
(3) 40g nonionic surfactant water-soluble liquid is slowly added in reactor, after being well mixed, stirred 30 minutes Afterwards, cooling is started;
(4) material is cooled to 25~30 DEG C of room temperature, adds remaining deionized water and preservative, produced after stirring Described persistent form fur feel improver composition.
Embodiment 2
The persistent form fur feel improver that the present embodiment is provided, the weight/mass percentage composition table of its component is as shown in table 2.
The component content of the embodiment 2 of table 2
The persistent form fur feel improver preparation method, its step is as follows:
(1) nonionic surfactant is dissolved with 40g deionized waters, and be heated to 50 degree it is stand-by;
(2), fatty alcohol is put into reactor, 70 DEG C are begun heat to, it is to be dissolved after add organosilicon while stirring, stir Mix uniform;In nonionic surfactant input reactor, and be heated to 70 DEG C, it is to be dissolved after stir;
(3) 40g nonionic surfactant water-soluble liquid is slowly added in reactor, after being well mixed, stirred 30 minutes Afterwards, cooling is started;
(4) material is cooled to 25~30 DEG C of room temperature, adds remaining deionized water and preservative, produced after stirring Described persistent form fur feel improver composition.
Embodiment 3
The persistent form fur feel improver that the present embodiment is provided, the weight/mass percentage composition table of its component is as shown in table 3.
The component content of the embodiment 3 of table 3
The preparation method of the persistent form fur feel improver preparation method be the same as Example 1.
Embodiment 4
The persistent form fur feel improver that the present embodiment is provided, the weight/mass percentage composition table of its component is as shown in table 4.
The component content of the embodiment 4 of table 4
The preparation method of the persistent form fur feel improver preparation method be the same as Example 2.
Embodiment 5
The persistent form fur feel improver that the present embodiment is provided, the weight/mass percentage composition table of its component is as shown in table 5.
The component content of the embodiment 5 of table 5
The preparation method of the persistent form fur feel improver preparation method be the same as Example 1.
Embodiment 6
The weight/mass percentage composition table of its component of the persistent form fur feel improver of the present embodiment offer is as shown in table 6.
The component content of the embodiment 6 of table 6
The preparation method of the persistent form fur feel improver preparation method be the same as Example 2.
The sheepskin feel processing method of experimental example 1
(1) configuration sheepskin hair treatment fluid:Including 80~120 parts of 80~120 parts of formic acid, alcohol according to mass fraction meter and 800~1000 parts of water, the addition of the persistent form fur feel improver is 40~70ml/L, and the treatment fluid configured is stirred It is stand-by after mixing uniformly;
(2) the sheepskin treatment fluid that step (1) has been configured uniformly is brushed on wool with long hairbrush, rolled repeatedly on ironing machine Scald, until wool drying, not moist, processing completion.
(3) test judgment criteria, mainly by experienced technical staff by observing, hand the mode such as touch and distinguished, can There can be certain error, but all in controlled range, content mainly includes the wool non yellowing after processing, not adhesive hair and dirty hair shows As, feel it is smooth it is soft, rich in gloss.
Using the above method, the feel improver provided using the embodiment of the present application 1-6 is handled, and result is such as Shown in table 7.
The sheepskin feel result of table 7
Product Color inhibition/dirt hair Soft slipping Glossiness Bulkiness
Embodiment 1 Nothing ++++ +++ +++
Embodiment 2 Nothing +++++ ++++ +++
Embodiment 3 Nothing +++++ +++++ ++++
Embodiment 4 Nothing ++++ +++++ ++++
Embodiment 5 Nothing +++++ ++++ +++++
Embodiment 6 Nothing +++++ +++ +++
Market like product Discoloration, flavescence ++++ +++ +++
Wherein "+" represents properties of product, and "+" is more, illustrates that performance is better.
Test result indicates that, feel improver provided herein, compared with commodity similar with market, to sheepskin processing There is more preferable effect.
The feel processing method of the thin miscellaneous skin of experimental example 2
(1), every 40 kilograms wooden chaffs add long type fur feel improver described in 500~700mL, add appropriate antistatic Agent, carries out wooden chaff in rotary drum and adds light, completion processing.
(2), test judgment criteria, mainly by experienced technical staff by observing, hand the mode such as touch and distinguished, comment Certain error is there may be during estimating, but all in technical staff's controlled range, the main wool non yellowing included after processing, Not adhesive hair and dirty hair phenomenon, feel it is smooth it is soft, rich in gloss.
Using the above method, the feel improver provided using the embodiment of the present application 1-6 is handled, and result is such as Shown in table 8.
The feel result of the thin miscellaneous skin of table 8
Product Color inhibition/dirt hair Soft slipping Glossiness Bulkiness
1 Nothing +++ ++ +++
2 Nothing +++++ +++ ++++
3 Nothing +++++ +++ +++++
4 Nothing ++++ ++++ ++++
5 Nothing ++++ +++++ +++++
6 Nothing +++++ +++ +++++
Market like product Discoloration, flavescence ++++ ++++ +++
Wherein "+" represents properties of product, and "+" is more, illustrates that performance is better.
Test result indicates that, feel improver provided herein, compared with commodity similar with market, at thin miscellaneous skin Reason has more preferable effect.
Although illustrate and describing the present invention with specific embodiment, but it will be appreciated that various embodiments above is only used To illustrate technical scheme, rather than its limitations;It will be understood by those within the art that:Without departing substantially from this hair In the case of bright spirit and scope, the technical scheme described in foregoing embodiments can be modified, or to wherein Some or all of technical characteristic carries out equivalent substitution;And these modifications or replacement, do not make the essence of appropriate technical solution Depart from the scope of various embodiments of the present invention technical scheme;It is, therefore, intended that including belonging to the present invention in the following claims In the range of all these substitutions and modifications.

Claims (10)

1. a kind of persistent form fur feel improver, it is characterised in that including the following component according to mass percentage:
Silicone oil 5%~30%, fatty alcohol 0.1%~5%, nonionic surfactant 1%~10%, preservative 0.1%~1% With deionized water 54%~93.8%.
2. persistent form fur feel improver according to claim 1, it is characterised in that including according to mass percentage Following component:
Organosilicon 5%~25%, fatty alcohol 0.5%~3%, nonionic surfactant 3%~8%, preservative 0.1%~ 0.5% and deionized water 63.5%~91.4%.
3. persistent form fur feel improver according to claim 1 or 2, it is characterised in that the silicone oil is selected from diformazan One or more of combinations in base silicone oil, amido silicon oil and polyether modified silicon oil.
4. persistent form fur feel improver according to claim 1 or 2, it is characterised in that the fatty alcohol is selected from C12-14Alcohol and C16-18Alcohol;
It is preferred that one or several kinds of combinations of the fatty alcohol in lauryl alcohol, tetradecyl alchohol, hexadecanol and octadecyl alcolol.
5. persistent form fur feel improver according to claim 1 or 2, it is characterised in that the non-ionic surface is lived One or more of the property agent in peregal, polyethylene glycol, isomerous tridecanol polyoxyethylene ether and lanolin isohexadecyl ether Combination;
It is preferred that, it is described it is average add as peregal o-9, the polyethylene glycol is polyethylene glycol 1500, and the isomerous tridecanol gathers Oxygen vinethene is isomerous tridecanol polyoxyethylene ether 1307.
6. persistent form fur feel improver according to claim 1 or 2, it is characterised in that state preservative and be selected from benzene first One in sour sodium, MIT, CMIT and p-hydroxybenzoate Plant or several combinations.
7. the preparation method of the persistent form fur feel improver according to claim any one of 1-6, it is characterised in that bag Include following steps:
(1), nonionic surfactant is added in portions of de-ionized water, stirring, heating obtain nonionic surfactant The aqueous solution, it is standby;
It is preferred that described be heated to 50~60 DEG C;
(2), fatty alcohol is put into reactor, 50~70 DEG C are heated to, it is to be dissolved after add silicone oil while stirring, after mixing plus Enter the aqueous solution of the nonionic surfactant in step (1);
It is preferred that, in step (2), solution is maintained at 50~70 DEG C;
(3) stirring is completely dissolved nonionic surfactant, is then cooled to 25~30 DEG C, add remaining deionized water and Preservative, obtains the persistent form fur feel improver;
It is preferred that mixing time be 30~50 minutes.
8. the application of the persistent form fur feel improver according to claim any one of 1-6, it is characterised in that including place Sheepskin hair and thin miscellaneous skin are managed, the thin miscellaneous skin includes raw fox skin, recoon dog skin, standard mink skin and rabbit.
9. the application of persistent form fur feel improver according to claim 8, it is characterised in that the hand of the sheepskin hair Feel processing method, comprise the following steps:
(1) configuration sheepskin hair treatment fluid:Including 80~120 parts of 80~120 parts of formic acid, the alcohol and water according to mass fraction meter 800~1000 parts, the addition of the persistent form fur feel improver is 40~70ml/L, and the treatment fluid configured is stirred It is stand-by after uniform;
(2) the sheepskin treatment fluid that step (1) has been configured uniformly is brushed on wool with long hairbrush, it is repeatedly boiling hot on ironing machine, Until wool drying, not moist, processing completion.
10. the application of persistent form fur feel improver according to claim 8, it is characterised in that the thin miscellaneous skin Feel processing method, comprises the following steps:
Every 40 kilograms wooden chaffs add long type fur feel improver described in 500~700mL, appropriate antistatic additive are added, in rotary drum Carry out wooden chaff and add light, completion processing.
CN201710607164.4A 2017-07-24 2017-07-24 A kind of persistent form fur feel improver and its preparation method and application Pending CN107245539A (en)