CN106976142A - A kind of production handling process of solid wood furniture - Google Patents

A kind of production handling process of solid wood furniture Download PDF

Info

Publication number
CN106976142A
CN106976142A CN201710259535.4A CN201710259535A CN106976142A CN 106976142 A CN106976142 A CN 106976142A CN 201710259535 A CN201710259535 A CN 201710259535A CN 106976142 A CN106976142 A CN 106976142A
Authority
CN
China
Prior art keywords
assembled
woollen
mould proof
parts
furniture
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201710259535.4A
Other languages
Chinese (zh)
Inventor
张强
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201710259535.4A priority Critical patent/CN106976142A/en
Publication of CN106976142A publication Critical patent/CN106976142A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of production handling process of solid wood furniture, including sawing sheet, mould proof processing, boiled in wax, fine grinding, japanning assembly and post processing;Furniture log is divided into multiple assembled blocks by sawing sheet according to furniture shape and construction;Mould proof processing is that assembled woollen is used into mould proof PROCESS FOR TREATMENT, dries to water content and is less than 10%;Thicknesser mortise is will to dry woollen using thicknessing machine to scrape and make joinery and its construction, and turns into cool drying after fine fodder, fine fodder surface spraying priming paint after polishing, is assembled into product.The rational technology of the present invention, the solid wood furniture good product quality of production department, not craze and transfiguration, enhances mould proof ability, and performance is stable, service life is long.

Description

A kind of production handling process of solid wood furniture
Technical field
The present invention relates to Furniture manufacturing technical field, and in particular to a kind of production handling process of solid wood furniture.
Background technology
Solid wood furniture is made using solid sawn lumber or solid wood board as base material, surface is through covering with paint, lacquer, colour wash, etc. the furniture handled;Or herein Used on class base material after plates of solid wood or veneer overlay, then cover with paint, lacquer, colour wash, etc. the furniture of processing;Solid wood furniture is made in existing life It is widely loved by the people for a kind of luxury goods.In the production process of solid wood furniture, in order to the full extent Production and processing sale is carried out, in process for easy process, many processing steps are using machining, and screw is solid Fixed, although such method has a preferable integral benefit, but the quality of single product can not ensure, hold after a long time use Easily there is the phenomenon damaged.And existing sheet material uses drying technology mostly, although can play and a certain degree of remove water work( Can, but can not be fully effective remove moisture removal, craze and transfiguration easily occurs for sheet material after a long time use.
The water content direct relation furniture of furniture timber does not carry out the timber dried to the adaptability of seasonal variations General moisture content brings production into and the phenomenons such as mouldy, deformation, cracking easily occurs, efficiently control moisture content more than 50% It is an important ring during Furniture manufacturing.
Natural trees pass through sawing, turn into the timber of manufacture furniture after drying, and timber leaves after drying oven its Moisture content is not constant, its meeting constantly moisture absorption and desorption in transport, storage, manufacturing process, or even by perfect Oil paint coating turns into a piece of furniture moisture absorption and the behavior of desorption and still will not stopped, only because the iris action of paint so that Moisture absorption and desorption become relatively slow, no longer so consumingly cause furniture size to change, cause structure and wood quality and surface Coating cracking.
The manufacture method of existing solid wood furniture, has as a drawback that:Timber wax is lost in big, mechanical property variation, toughness Reduction;Joinery and its construction is not ideal enough;It is not easy to recognize the fineness of the manufacture crafts such as carver, polishing;The natural line of furniture material Reason, color and luster, breath can not be preserved effectively;It can not effectively reduce and swollen, cracking etc. is taken out caused by wood change.
The content of the invention
It is an object of the invention to provide a kind of production handling process of solid wood furniture.
For up to above-mentioned purpose, a kind of production department's science and engineering of solid wood furniture is provided in one embodiment of the present of invention Skill, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet, obtains assembled woollen;
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature control At 40 DEG C ~ 60 DEG C, dry to water content and be less than 10%, dry and obtain mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 2h ~ 5h is boiled in beeswax, boiled in wax removes the unnecessary honeybee of woollen surface attachment after finishing Wax, obtains and dries woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into;
7), post processing:Waxing polishing processing is carried out in product surface.
One of prioritization scheme of the present invention, being additionally included on mould proof woollen needs the part carved to be carved The step of processing.
One of prioritization scheme of the present invention, in last handling process, the junction for being additionally included in joinery and its construction is uniform Smear Environment-friendlyglue glue.
One of prioritization scheme of the present invention, mould proof handling process includes:Assembled woollen is sent into drying shed and heated 12h is handled, it is 60 DEG C to control temperature in drying shed, and humidity is 60%RH;And 5 DEG C of temperature is reduced every 3h, humidity 5% is reduced; Heat after 12h in feeding constant-temperature house natural storage 2 ~ 5 days in the environment of 20 DEG C ~ 25 DEG C of room temperature, relative humidity 30%RH.
One of prioritization scheme of the present invention, reinforcing is continuously sprayed on the assembled block surface that sawing sheet technique is additionally included in segmentation The step of liquid is soaked;The temperature of forced fluid is 60 DEG C ~ 80 DEG C during sprinkling, is dried every time after sprinkling 1h to dry tack free, weight It is multiple to handle at least 2 times;Contain calcium chloride 1mol/L, the mol/L of D-sorbite 0.5 and sodium carboxymethylcellulose in forced fluid 0.5mol/L。
One of prioritization scheme of the present invention, priming paint includes 40 ~ 70 parts of short oil alkyd resin, 10 ~ 15 parts of talcum powder, stone 1 ~ 5 part of English powder, 0.1 ~ 0.5 part of levelling agent, 0.5 ~ 1 part of bentonite, 5 ~ 10 parts of zinc stearate, 2 ~ 4 parts of butyl acetate, polyethylene pyrrole 2 ~ 3 parts of pyrrolidone, 2 ~ 3 parts of sodium alginate, 2 ~ 3 parts of Aspartame.
One of prioritization scheme of the present invention, levelling agent is polyether-modified dimethyl silicone polymer.
In summary, the present invention has advantages below:
1st, rational technology of the invention, the solid wood furniture good product quality of production department, not craze and transfiguration, enhances mould proof ability, Performance is stable, service life is long.
2nd, the present invention also optimizes mould proof handling process, and more preferable mould proof effect is obtained by the method for stage cooling Really so that solid wood is difficult to absorb moisture in the later stage, improves water resistance.
3rd, the present invention allows forced fluid to enter inside solid wood and wooden fibre by spraying forced fluid in sawing sheet technical process Dimension contact so that the moisture inside solid wood is difficult to lose, also causing the affinity of the solid wood after processing and outside moisture reduces, from And moisture protection is improved, it can also reduce the probability of cracking.
4th, present invention optimizes the formula of priming paint, it can solve the problem that middle priming paint can not reduce solid wood cracking in the prior art Problem, while also improving closed performance, water-fast moisture effect is more preferable.
Embodiment
A kind of production handling process of solid wood furniture is disclosed in one embodiment of the present of invention, is comprised the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet, obtains assembled woollen.
Moulding that can be according to drawing and furniture during sawing sheet and the furniture log of the suitable size of size selection, furniture is former Wood cuts into multiple timber, and each timber is a part of solid wood furniture;These assembled woollen rough surface, it is necessary to by Subsequent treatment can obtain smooth surface, while better performance can be obtained.
In the optimal enforcement example of the present invention, reinforcing is continuously sprayed on the assembled block surface that sawing sheet technique is additionally included in segmentation The step of liquid is soaked;Moistening step for example can be carried out after log cutting.The temperature of forced fluid is 60 DEG C ~ 80 during sprinkling DEG C, dry to dry tack free, reprocess at least 2 times after sprinkling 1h every time;Contain calcium chloride 1mol/L, sorbose in forced fluid Alcohol 0.5mol/L and sodium carboxymethylcellulose 0.5mol/L, solvent can be water.The water content of assembled woollen in itself is higher, hair Hole open state;The present invention makes it infiltrate woollen woollen sprinkling forced fluid so that the surface part of woollen is reinforced liquid parcel, Forced fluid is gradually infiltrated into inside woollen, and moisture evaporation after drying, hardening agent still has wood fibre in wood fibre Moisture be wrapped and be difficult dehydration, and reduced with the adhesion of outside moisture, improve water resistance.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is dried to water content at 40 DEG C ~ 60 DEG C and is less than 10%, dries and obtains mould proof woollen after finishing.
Mould proof handling process includes:Assembled woollen is sent into drying shed and heats 12h, controls the temperature in drying shed to be 60 DEG C, humidity is 60%RH;And 5 DEG C of temperature is reduced every 3h, humidity 5% is reduced;Heat 12h after feeding constant-temperature house in Natural storage 2 ~ 5 days in the environment of 20 DEG C ~ 25 DEG C of room temperature, relative humidity 30%RH.
The water content of mould proof woollen is relatively low, and with good engraving performance, present invention additionally comprises needed on mould proof woollen The part carved carries out Carving Machining, for example, can carve out various decorative patterns.
3), boiled in wax:Mould proof woollen is inserted 2h ~ 5h is boiled in beeswax, boiled in wax removes many of woollen surface attachment after finishing Remaining beeswax, obtains and dries woollen.
Mould proof timber water content is relatively low, is placed in beeswax and is conducive to the appearance formation beeswax layer of woollen, further improves hair Smoothness, sanding property energy and the water resistance of material.
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more smart Really, joinery and its construction is then made according to the connection of each assembled block.
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, Obtain fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling after spraying solidifies after finishing through Overheating Treatment has been sprayed Fine fodder after finishing, which is immediately fed into hot drying room, to be solidified, and solidification temperature can select 50 DEG C.Then again after being polished for a plurality of times The joinery and its construction of each assembled block is connected, product is assembled into.
Priming paint includes 40 ~ 70 parts of short oil alkyd resin, 10 ~ 15 parts of talcum powder, 1 ~ 5 part of silica flour, levelling agent 0.1 ~ 0.5 Part, 0.5 ~ 1 part of bentonite, 5 ~ 10 parts of zinc stearate, 2 ~ 4 parts of butyl acetate, 2 ~ 3 parts of polyvinylpyrrolidone, sodium alginate 2 ~ 3 Part, 2 ~ 3 parts of Aspartame;Levelling agent is polyether-modified dimethyl silicone polymer.
7), post processing:In product surface carries out waxing polishing processing, last handling process, in the junction of joinery and its construction It is uniform to smear Environment-friendlyglue glue, further improve water-protected enclosure performance.
Embodiment 1
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain calcium chloride 1mol/L, D-sorbite 0.5 in forced fluid Mol/L and sodium carboxymethylcellulose 0.5mol/L.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of polyvinylpyrrolidone, 2 parts of sodium alginate, 3 parts of Aspartame.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 2
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain the mol/L of D-sorbite 0.5 and carboxymethyl in forced fluid Sodium cellulosate 0.5mol/L.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of polyvinylpyrrolidone, 2 parts of sodium alginate, 3 parts of Aspartame.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 3
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain calcium chloride 1mol/L, sodium carboxymethylcellulose in forced fluid 0.5mol/L。
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of polyvinylpyrrolidone, 2 parts of sodium alginate, 3 parts of Aspartame.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 4
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain calcium chloride 1mol/L, D-sorbite 0.5 in forced fluid mol/L。
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of polyvinylpyrrolidone, 2 parts of sodium alginate, 3 parts of Aspartame.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 5
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain calcium chloride 1mol/L, D-sorbite 0.5 in forced fluid Mol/L and sodium carboxymethylcellulose 0.5mol/L.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of sodium alginate, 3 parts of Aspartame.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 6
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain calcium chloride 1mol/L, D-sorbite 0.5 in forced fluid Mol/L and sodium carboxymethylcellulose 0.5mol/L.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of polyvinylpyrrolidone, 3 parts of Aspartame.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 7
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
Forced fluid is continuously sprayed on the assembled block surface of segmentation to be soaked;The temperature of forced fluid is 70 DEG C during sprinkling, often Dry to dry tack free, reprocess 3 times after secondary sprinkling 1h;Contain calcium chloride 1mol/L, D-sorbite 0.5 in forced fluid Mol/L and sodium carboxymethylcellulose 0.5mol/L.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
Priming paint include 50 parts of short oil alkyd resin, 10 parts of talcum powder, 2 parts of silica flour, 0.3 part of levelling agent, 1 part of bentonite, 6 parts of zinc stearate, 2 parts of butyl acetate, 2 parts of polyvinylpyrrolidone, 2 parts of sodium alginate.
7), post processing:Waxing polishing processing is carried out in product surface.
Embodiment 8
A kind of production handling process of solid wood furniture, comprises the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet.
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature Control is at 50 DEG C, and it is 8% to dry to water content, dries and obtains mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 3h is boiled in beeswax, boiled in wax removes the unnecessary beeswax of woollen surface attachment after finishing, Obtain and dry woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into.
7), post processing:Waxing polishing processing is carried out in product surface.
The product or sheet material that are obtained after method processing in 1 ~ embodiment of embodiment 8 are subjected to moistureproof experiment;Experimental method For:Solid wood furniture or sheet material are exposed in atomized steam, the temperature of atomized steam is 50 DEG C, each product or sheet material Open-assembly time is 10 days.The Unit Weight that the front and rear solid wood furniture of exposure or sheet material are measured after 10 days is poor, i.e., every kilogram solid wood board Material absorb moisture weight, unit for gram, the experimental results are shown inthe following table for it.
Table 1:The moistureproof experimental result of 1 ~ embodiment of embodiment 8
Embodiment Unit Weight is poor Embodiment Unit Weight is poor
Embodiment 1 42 Embodiment 5 58
Embodiment 2 48 Embodiment 6 62
Embodiment 3 50 Embodiment 7 60
Embodiment 4 52 Embodiment 8 124
From table 1 it follows that embodiment 8 is compared with Example 1, the timber water absorption of embodiment 8 is far longer than embodiment 1, Illustrate that the moisture effect of embodiment 1 is optimal.Embodiment 2 and embodiment 3 reduce calcium chloride and sorb respectively compared with Example 1 Sugar alcohol, its moisture effect slightly has reduction, but equally has the moisture effect of conspicuousness compared to embodiment 8;Embodiment 4 and embodiment 5 reduce sodium carboxymethylcellulose and polyvinylpyrrolidone compared with Example 1, and its moisture effect has compared to embodiment 8 Notable moisture effect, but it is somewhat below 1 ~ embodiment of embodiment 3;Embodiment 6 and embodiment 7 reduce sodium alginate and A Si Ba Tian, its moisture effect has notable moisture effect compared to embodiment 8, but is somewhat below 1 ~ embodiment of embodiment 5.As can be seen here, The present invention is after forced fluid process step and optimization priming paint is added, and its humidity resistance is further increased, and illustrates above-mentioned reality Facilitation can be played to the moisture effect of solid wood by applying increased material in example.

Claims (7)

1. the production handling process of a kind of solid wood furniture, it is characterised in that comprise the following steps:
1)Sawing sheet:Furniture log is divided into by multiple assembled blocks according to furniture shape and construction, and according to the chi of each assembled block Very little selection log sawing sheet, obtains assembled woollen;
2)Mould proof processing:Assembled woollen is used into mould proof PROCESS FOR TREATMENT, is put into drying box and dries after processing, temperature control At 40 DEG C ~ 60 DEG C, dry to water content and be less than 10%, dry and obtain mould proof woollen after finishing;
3), boiled in wax:Mould proof woollen is inserted 2h ~ 5h is boiled in beeswax, boiled in wax removes the unnecessary honeybee of woollen surface attachment after finishing Wax, obtains and dries woollen;
4), thicknesser mortise:Scraped using thicknessing machine by woollen is dried, make the size at each position of assembled block more accurate, so Joinery and its construction is made according to the connection of each assembled block afterwards;
5), fine grinding:Grinding process is carried out to each assembled block surface after mortise, makes the surface of each assembled block smooth, obtains Fine fodder;
6), japanning it is assembled:In fine fodder surface spraying priming paint, natural cooling, Ran Houzai after spraying solidifies after finishing through Overheating Treatment The joinery and its construction of each assembled block is connected after being polished for a plurality of times, product is assembled into;
7), post processing:Waxing polishing processing is carried out in product surface.
2. the production handling process of solid wood furniture as claimed in claim 1, it is characterised in that:Being additionally included on mould proof woollen needs The step of part carved carries out Carving Machining.
3. the production handling process of solid wood furniture as claimed in claim 1, it is characterised in that:In the last handling process, also Uniformly smear Environment-friendlyglue glue in the junction for being included in joinery and its construction.
4. the production handling process of solid wood furniture as claimed in claim 1, it is characterised in that:The mould proof handling process bag Include:Assembled woollen is sent into drying shed and heats 12h, it is 60 DEG C to control temperature in drying shed, and humidity is 60%RH;And 5 DEG C of temperature is reduced every 3h, humidity 5% is reduced;Heat after 12h in feeding constant-temperature house in 20 DEG C ~ 25 DEG C of room temperature, it is relatively wet Natural storage 2 ~ 5 days in the environment of degree 30%RH.
5. the production handling process of solid wood furniture as claimed in claim 1, it is characterised in that:The sawing sheet technique also includes The step of forced fluid is soaked continuously is sprayed on the assembled block surface of segmentation;The temperature of forced fluid is 60 DEG C ~ 80 DEG C during sprinkling, Dry to dry tack free, reprocess at least 2 times after sprinkling 1h every time;Contain calcium chloride 1mol/L, sorb in the forced fluid The mol/L of sugar alcohol 0.5 and sodium carboxymethylcellulose 0.5mol/L.
6. the production handling process of solid wood furniture as claimed in claim 1, it is characterised in that:The priming paint includes short oil alkyd 40 ~ 70 parts of resin, 10 ~ 15 parts of talcum powder, 1 ~ 5 part of silica flour, 0.1 ~ 0.5 part of levelling agent, 0.5 ~ 1 part of bentonite, zinc stearate 5 ~ 10 parts, 2 ~ 4 parts of butyl acetate, 2 ~ 3 parts of polyvinylpyrrolidone, 2 ~ 3 parts of sodium alginate, 2 ~ 3 parts of Aspartame.
7. the production handling process of solid wood furniture as claimed in claim 6, it is characterised in that:The levelling agent is polyether-modified Dimethyl silicone polymer.
CN201710259535.4A 2017-04-20 2017-04-20 A kind of production handling process of solid wood furniture Pending CN106976142A (en)