CN106914395A - The water paint coating process of Russian birch door-plate Transparent color - Google Patents

The water paint coating process of Russian birch door-plate Transparent color Download PDF

Info

Publication number
CN106914395A
CN106914395A CN201710333819.3A CN201710333819A CN106914395A CN 106914395 A CN106914395 A CN 106914395A CN 201710333819 A CN201710333819 A CN 201710333819A CN 106914395 A CN106914395 A CN 106914395A
Authority
CN
China
Prior art keywords
spray
color
sand paper
sand
coating process
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201710333819.3A
Other languages
Chinese (zh)
Inventor
陈照友
陈杰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ningbo Phoenix Jie Lun Wood Ltd By Share Ltd
Original Assignee
Ningbo Phoenix Jie Lun Wood Ltd By Share Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ningbo Phoenix Jie Lun Wood Ltd By Share Ltd filed Critical Ningbo Phoenix Jie Lun Wood Ltd By Share Ltd
Priority to CN201710333819.3A priority Critical patent/CN106914395A/en
Publication of CN106914395A publication Critical patent/CN106914395A/en
Pending legal-status Critical Current

Abstract

A kind of water paint coating process of Russian birch door-plate Transparent color, it is characterised in that comprise the following steps that material is repaired;Spray aqueous attachment bottom;Spraying UV spray attachments bottom spraying UV transparent primings;Repeatedly fill up polishing;Repeatedly spray water paint.Due to not using oil paint, and water paint is used, product safety environmental protection, VOC content declines 20 times than oil paint, and product odorlessness, case hardness is strong, be difficult to scratch, uvioresistant intensity is stronger, and application Rear Door surface gloss is superpower.

Description

The water paint coating process of Russian birch door-plate Transparent color
Technical field
The present invention relates to a kind of coating process of door-plate, more particularly to the coating process that a kind of washing of door-plate is painted.
Background technology
The timber of existing birch is filbert to bronzing, with glittering surface and smooth mechanism.Yellow-white is slightly brown, Substantially, wooden body is pure thin for annual ring, slightly weighs hard, and structure is thin, and mechanical strength is big, high resilience, and hygroscopicity is big, drying warpage easy to crack. It is very not durable under the environment for being easy to rotten, it is more to be used in clamping plate form.Birch be generally used for special plywood, floor, Furniture, paper pulp, interior material, car and boat equipment, glued board etc..Made furniture smooth abrasion-proof, decorative pattern is apparent.Nowadays it is used to tie The making of structure, parquetry and inner frame.Russian domestic birch is originated in be commonly referred to as (Russian birch).
Furniture is made of birch has easy processing, and tangent plane is smooth, paints and the good advantage of glue performance, but exist simultaneously Fiber shearing resistance is poor, easily " neat stubble breaks ", not corrosion resistant, not wear-resisting, the deficiency such as easy to crack after drying and warpage.Due to Russian birch Procurement price is more cheap, is used as door-plate now also more and more, how to carry out application, makes it have good environmental protection Type, ultraviolet-resistent property and wearability, are always the content of those skilled in the art's research, but public there is presently no the document of this respect Open.
The content of the invention
The technical problems to be solved by the invention are directed to the above-mentioned state of the art and provide a kind of environment-friendly type, ultraviolet-resistent property And the water paint coating process of all good Russian birch door-plate Transparent color of wearability.
The present invention solve the technical scheme that is used of above-mentioned technical problem for:A kind of water of Russian birch door-plate Transparent color Property paint coating process, it is characterised in that comprise the following steps:
A, material repairing, using putty, and with 320# sand paper sandings, having pit to damage for former material is carried out, and 502 glue enter Row repairing, to without horizontal sand print and surfacing it is smooth, then under the conditions of 28~32 DEG C, drying 3~5 hours;
B, once spray, spray aqueous adhesion primer, 85~105g/m of quantity for spray2, then under the conditions of 28~32 DEG C, do Dry 2~3 hours;
C, secondary spraying, UV transparent primings, 120~180cmj/m of mercury lamp are sprayed using reciprocating spraying machine2, quantity for spray is 296.5~306.5g/m2, under thermostatic control, drying 5~8 minutes, temperature control is at 25~35 DEG C;
D, once fill up polishing, polished using putty, with 240# sand paper or 320# sand paper, it is ensured that flat smooth, without pit, Worn without sand, without bright spot;
E, three sprayings, continue to spray UV transparent primings using reciprocating spraying machine, and quantity for spray is 296.5~306.5g/ m2, under thermostatic control, dry 5~8 minutes, temperature control at 25~35 DEG C, using photo solidification machine;
F, it is secondary fill up polishing, using putty polish, with 400# sand paper or 600# sand paper, it is ensured that flat smooth, without pit, Worn without sand, without bright spot;
G, chromatography, chromatography is carried out with reference to colour table, and corner does not show money or valuables one carries unintentionally side, 20~30g/m of chromatography2, then at 28~32 DEG C Under the conditions of, dry 0.5~1 hour;
H, solid color, are processed with reference to colour table with scouring pad solid color, and the color long position that chromatography covers is cleaned out;
I, color is repaiied, with reference to colour table, color essence is added to repair and carry out spraying in color liquid and repair color;
J, four sprayings, with reference to the brightness of colour table, aqueous finish paint are sprayed, and quantity for spray is 211.63~231.63g/m2, Dry 6~8 hours, temperature control is at 28~32 DEG C;
K, sanding, using the sanding of 800# sand paper or 1000# sand paper sandings, it is ensured that impulse- free robustness, particle and worn without sand;
L, five sprayings, with reference to the brightness of colour table, continuation is sprayed with aqueous finish paint, and quantity for spray is 297~317g/m2, do Dry 8~12 hours, temperature control was at 30~34 DEG C.
Preferably, the aqueous adhesion primer described in step b is the type of Shanghai Ahmedabad scholar's new material Co., Ltd production Number for 1115D aqueous adhesion primer.
Preferably, the UV transparent primings described in step c and e are the type of Shanghai Ahmedabad scholar's new material Co., Ltd production Number for 1221D UV transparent primings.
Preferably, the aqueous finish paint described in step j and l is the model of Hebei Chenyang IndustrialL&trade Group Co., Ltd.'s production It is the morning yang edema paint of aqueous clear finish.
Compared with prior art, the advantage of the invention is that:The present invention does not use oil paint, and uses water paint, produces Product safety and environmental protection, VOC (dimethylbenzene) contents decline 20 times than oil paint, and product odorlessness, case hardness is strong, are difficult to scratch, and resist Uitraviolet intensity is stronger, and application Rear Door surface gloss is superpower.
Specific embodiment
The present invention is described in further detail with reference to embodiments.
Embodiment 1, the water paint coating process of the Russian birch door-plate Transparent color in the present embodiment, it is characterised in that bag Include following steps:
A, material repairing, using putty, and with 320# sand paper sandings, having pit to damage for former material is carried out, and 502 glue enter Row repairing, to without horizontal sand print and surfacing it is smooth, then under the conditions of 30 DEG C, drying 4 hours;
B, once spray, spray aqueous adhesion primer, quantity for spray 95g/m2, then under the conditions of 30 DEG C, dry 2~3 small When, make the UV transparent primings of sequent surface stronger with timber adhesive force;
C, secondary spraying, UV transparent primings, mercury lamp 150cmj/m are sprayed using reciprocating spraying machine2, quantity for spray is 301.5g/m2, under thermostatic control, drying 5~8 minutes, at 25~35 DEG C, the effect of UV transparent primings is filling timber to temperature control Line, increases paint film, makes product more smooth, and feel is more preferable;
D, once fill up polishing, polished using putty, with 240# sand paper or 320# sand paper, it is ensured that flat smooth, without pit, Worn without sand, without bright spot, its effect is the defect of product fill, makes product appearance fuller more smooth;
E, three sprayings, continue to spray UV transparent primings using reciprocating spraying machine, and quantity for spray is 301.5g/m2, in perseverance Temperature regulation under, dry 5~8 minutes, temperature control at 25~35 DEG C, using photo solidification machine;
F, it is secondary fill up polishing, using putty polish, with 400# sand paper or 600# sand paper, it is ensured that flat smooth, without pit, Worn without sand, without bright spot;
G, chromatography, chromatography is carried out with reference to colour table, and corner does not show money or valuables one carries unintentionally side, chromatography 25g/m2, then under the conditions of 30 DEG C, do Dry 0.5~1 hour, it is possible to achieve imitative American Style, product does old treatment;
H, reference colour table are processed with scouring pad solid color, and the color long position that chromatography covers is cleaned out, and make next procedure Surface after color is repaiied more to have levels sense;
I, color is repaiied, with reference to colour table, color essence is added to repair and carry out spraying in color liquid and repair color;
J, four sprayings, with reference to the brightness of colour table, aqueous finish paint are sprayed, and quantity for spray is 221.63g/m2, dry 6~8 Hour, at 30 DEG C, its effect is the plumpness that cover surface sand paper print increases surface lacquer to temperature control;
K, sanding, using the sanding of 800# sand paper or 1000# sand paper sandings, it is ensured that impulse- free robustness, particle and worn without sand;
L, five sprayings, with reference to the brightness of colour table, continuation is sprayed with aqueous finish paint, and quantity for spray is 307g/m2, dry 8~ 12 hours, at 32 DEG C, its effect was to increase plumpness and light flexibility to temperature control.
Aqueous adhesion primer is the model of Shanghai Ahmedabad scholar's new material Co., Ltd production in step b in the present embodiment The aqueous adhesion primer of 1115D;The UV of the model 1221D of Shanghai Ahmedabad scholar's new material Co., Ltd production is saturating in step c and e Bright priming paint;Aqueous finish paint is the morning of the aqueous clear finish of model of Hebei Chenyang IndustrialL&trade Group Co., Ltd.'s production in step j and l Yang edema paint.
Oil paint is not used, and uses water paint, product safety environmental protection, VOC (dimethylbenzene) contents decline than oil paint 20 times, product odorlessness, case hardness is strong, is difficult to scratch, and uvioresistant intensity is stronger, and application Rear Door surface gloss surpasses By force.

Claims (4)

1. a kind of water paint coating process of Russian birch door-plate Transparent color, it is characterised in that comprise the following steps:
A, material repairing, using putty, and with 320# sand paper sandings, having pit to damage for former material is carried out, and 502 glue are repaiied Mend, to without horizontal sand print and surfacing it is smooth, then under the conditions of 28~32 DEG C, drying 3~5 hours;
B, once spray, spray aqueous adhesion primer, 85~105g/m of quantity for spray2, then under the conditions of 28~32 DEG C, dry 2~ 3 hours;
C, secondary spraying, UV transparent primings, 120~180cmj/m of mercury lamp are sprayed using reciprocating spraying machine2, quantity for spray is 296.5 ~306.5g/m2, under thermostatic control, drying 5~8 minutes, temperature control is at 25~35 DEG C;
D, polishing is once filled up, polished using putty, with 240# sand paper or 320# sand paper, it is ensured that flat smooth, without pit, without sand Wear, without bright spot;
E, three sprayings, continue to spray UV transparent primings using reciprocating spraying machine, and quantity for spray is 296.5~306.5g/m2, Under thermostatic control, dry 5~8 minutes, temperature control at 25~35 DEG C, using photo solidification machine;
F, it is secondary fill up polishing, using putty polish, with 400# sand paper or 600# sand paper, it is ensured that flat smooth, without pit, without sand Wear, without bright spot;
G, chromatography, chromatography is carried out with reference to colour table, and corner does not show money or valuables one carries unintentionally side, 20~30g/m of chromatography2, then in 28~32 DEG C of conditions Under, dry 0.5~1 hour;
H, solid color, are processed with reference to colour table with scouring pad solid color, and the color long position that chromatography covers is cleaned out;
I, color is repaiied, with reference to colour table, color essence is added to repair and carry out spraying in color liquid and repair color;
J, four sprayings, with reference to the brightness of colour table, aqueous finish paint are sprayed, and quantity for spray is 211.63~231.63g/m2, dry 6 ~8 hours, temperature control was at 28~32 DEG C;
K, sanding, using the sanding of 800# sand paper or 1000# sand paper sandings, it is ensured that impulse- free robustness, particle and worn without sand;
L, five sprayings, with reference to the brightness of colour table, continuation is sprayed with aqueous finish paint, and quantity for spray is 297~317g/m2, dry 8~ 12 hours, temperature control was at 30~34 DEG C.
2. the water paint coating process of Russian birch door-plate Transparent color according to claim 1, it is characterised in that step b Described in aqueous adhesion primer for Shanghai Ahmedabad scholar's new material Co., Ltd production model 1115D aqueous attachment bottom Paint.
3. the water paint coating process of Russian birch door-plate Transparent color according to claim 1, it is characterised in that step c With the UV transparent primings that the UV transparent primings described in e are the model 1221D that Shanghai Ahmedabad scholar's new material Co., Ltd produces.
4. the water paint coating process of Russian birch door-plate Transparent color according to claim 1, it is characterised in that step j With the morning yang edema that the aqueous finish paint described in l is the aqueous clear finish of model that Hebei Chenyang IndustrialL&trade Group Co., Ltd. produces Paint.
CN201710333819.3A 2017-05-12 2017-05-12 The water paint coating process of Russian birch door-plate Transparent color Pending CN106914395A (en)