CN106758287A - A kind of glycols water soluble polyurethane resin artificial leather manufacture method - Google Patents

A kind of glycols water soluble polyurethane resin artificial leather manufacture method Download PDF

Info

Publication number
CN106758287A
CN106758287A CN201510818020.4A CN201510818020A CN106758287A CN 106758287 A CN106758287 A CN 106758287A CN 201510818020 A CN201510818020 A CN 201510818020A CN 106758287 A CN106758287 A CN 106758287A
Authority
CN
China
Prior art keywords
artificial leather
paint
polyurethane resin
soluble polyurethane
glycols
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510818020.4A
Other languages
Chinese (zh)
Inventor
王东
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangyin Yonglong Plastics Co Ltd
Original Assignee
Jiangyin Yonglong Plastics Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangyin Yonglong Plastics Co Ltd filed Critical Jiangyin Yonglong Plastics Co Ltd
Priority to CN201510818020.4A priority Critical patent/CN106758287A/en
Publication of CN106758287A publication Critical patent/CN106758287A/en
Pending legal-status Critical Current

Abstract

The present invention relates to a kind of glycols water soluble polyurethane resin artificial leather manufacture method, it is to use glycols water soluble polyurethane resin to configure to cover with paint, lacquer, colour wash, etc. slurry, then slurry will be covered with paint, lacquer, colour wash, etc. to cover with paint, lacquer, colour wash, etc. in artificial leather base fabric surface, the polyurethane artificial leather for being dyeed by dyeing treatment again, covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:100 parts of glycols water soluble polyurethane resin, 20~120 parts of dimethylformamide, 20~120 parts of acetone.Glycols water soluble polyurethane resin is used as artificial leather top finishing material, dyeing process can be carried out with dyestuff, color effects by that can obtain dyestuff coloring after dyeing treatment, make product have the characteristics of bright-colored, coating permeability is good, surface color fastness is high, color animal migration is small.

Description

A kind of glycols water soluble polyurethane resin artificial leather manufacture method
Technical field
The invention belongs to polyurethane resin artificial leather preparation method technical field, and in particular to a kind of glycol for being easy to dye The manufacture method of class water soluble polyurethane resin artificial leather.
Background technology
Surface has the artificial leather of dyestuff coloring effect, and its bright in luster, transparency is high, is applied to the fashion such as case and bag women's shoes It is loved by people on product, but conventional synthesis leather generally uses pigment coloring mode, it is impossible to and reaching dyestuff coloring is had Effect, although dyestuff coloring effect can be obtained using the manufacture method that the coloring of dyestuff water colouring agent is added in coating material, But this manufacture method can bring serious colour migration to move, poor color fastness, the problems such as cost price is high, making for product is constrained With.
In traditional synthetic leather manufacturing process, mill base, toner and organic dyestuff, metal network need to be added in coating paste
The coloring materials such as dyestuff are closed, so that assign finished leather different colors, but coat colorization feel is partially hard, and coloring formula is once It is determined that after, coating is presented solid color, and gloss and color and luster are dull, without the stereovision such as the depth, light and shade, new and old.Exploitation is just In dyeing artificial leather be those skilled in the art need thinking problem.
The content of the invention
The technical problems to be solved by the invention are directed to above-mentioned prior art and provide a kind of polyurethane people be easy to and dye Fabricate-leather, can be dyeed with dyestuff, and product has the characteristics of bright-colored, coating permeability is good, surface color fastness is high.
The present invention the used technical scheme that solves the above problems is:A kind of glycols water soluble polyurethane resin artificial leather Manufacture method, is to use glycols water soluble polyurethane resin to configure to cover with paint, lacquer, colour wash, etc. slurry, then will cover with paint, lacquer, colour wash, etc. slurry and covers with paint, lacquer, colour wash, etc. in artificial leather Scrim surfaces, then the polyurethane artificial leather dyeed by dyeing treatment;
Covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:
100 parts of glycols water soluble polyurethane resin
20~60 parts of water.
Preferably, described covering with paint is to make surface technology by release liners dry method to fit to glycols soluble polyurethane surface layer In artificial leather wet half-finished product.
Preferably described covering with paint is that glycols soluble polyurethane is covered with paint, lacquer, colour wash, etc. into slurry with surface printing method to cover with paint, lacquer, colour wash, etc. in artificial leather Dry method surface of semi-finished.
Preferably, the covering with paint is that glycols soluble polyurethane is applied into finish coat with rolling method to be coated with to artificial leather base fabric Surface of semi-finished.
Described dyeing
Polyurethane resin artificial leather in the present invention is easy to dyeing, and dyeing processing mode includes pad dyeing, dye gigging, overflow dyeing or gas Stream dyeing.
Compared with prior art, the advantage of the invention is that:Using glycols water soluble polyurethane resin as artificial leather Top finishing material, can carry out dyeing process with dyestuff, the color effects by that can obtain dyestuff coloring after dyeing treatment, make Product has the characteristics of bright-colored, coating permeability is good, surface color fastness is high, color animal migration is small, is dyeed with common artificial leather Few compared to dyestuff usage amount, and dyeing time is very short, dyeing can be completed compared with low temperature, dyeing relatively simple, cost compared with Low, energy saving.
Specific embodiment
The present invention is described in further detail with reference to embodiments.
Embodiment 1
Glycols water soluble polyurethane resin artificial leather manufacture method, is to use glycols water soluble polyurethane resin to configure to cover with paint, lacquer, colour wash, etc. Slurry, then will cover with paint, lacquer, colour wash, etc. slurry and covers with paint, lacquer, colour wash, etc. in artificial leather base fabric surface, and foregoing covering with paint is to make surface technology by two by release liners dry method Alcohols soluble polyurethane surface layer is fitted in artificial leather wet half-finished product, then the polyurethane dyeed by pad dyeing treatment Artificial leather.
Covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:
100 parts of glycols water soluble polyurethane resin
20 parts of water.
Embodiment 2
Glycols water soluble polyurethane resin artificial leather manufacture method, is to use glycols water soluble polyurethane resin to configure to cover with paint, lacquer, colour wash, etc. Slurry, then will cover with paint, lacquer, colour wash, etc. slurry and covers with paint, lacquer, colour wash, etc. in artificial leather base fabric surface, and foregoing covering with paint is with surface printing method that glycols is water-soluble Polyurethane is covered with paint, lacquer, colour wash, etc. slurry and is covered with paint, lacquer, colour wash, etc. in artificial leather dry method surface of semi-finished, then the polyurethane artificial dyeed by dye gigging treatment Leather.
Covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:
100 parts of glycols water soluble polyurethane resin
60 parts of water.
Embodiment 3
Glycols water soluble polyurethane resin artificial leather manufacture method, is to use glycols water soluble polyurethane resin to configure to cover with paint, lacquer, colour wash, etc. Slurry, then will cover with paint, lacquer, colour wash, etc. slurry and cover with paint, lacquer, colour wash, etc. in artificial leather base fabric surface, and foregoing covering with paint is to use rolling method by glycols water-soluble poly Urethane applies finish coat coating and processes the polyurethane people for being dyeed to artificial leather base fabric's surface of semi-finished, then by airflow dyeing Fabricate-leather.
Covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:
100 parts of glycols water soluble polyurethane resin
40 parts of water.
Embodiment 4
Glycols water soluble polyurethane resin artificial leather manufacture method, is to use glycols water soluble polyurethane resin to configure to cover with paint, lacquer, colour wash, etc. Slurry, then will cover with paint, lacquer, colour wash, etc. slurry and covers with paint, lacquer, colour wash, etc. in artificial leather base fabric surface, and foregoing covering with paint is with surface printing method that glycols is water-soluble Polyurethane is covered with paint, lacquer, colour wash, etc. slurry and is covered with paint, lacquer, colour wash, etc. in artificial leather dry method surface of semi-finished, then processes the polyurethane for being dyeed by overflow dyeing Artificial leather.
Covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:
100 parts of glycols water soluble polyurethane resin
60 parts of water.

Claims (5)

1. a kind of glycols water soluble polyurethane resin artificial leather manufacture method, it is characterised in that:It is to use glycols water-soluble Slurry is covered with paint, lacquer, colour wash, etc. in polyurethane resin configuration, then will be covered with paint, lacquer, colour wash, etc. slurry and is covered with paint, lacquer, colour wash, etc. in artificial leather base fabric surface, then is obtained final product by dyeing treatment To the polyurethane artificial leather of dyeing,
Covering with paint, lacquer, colour wash, etc. slurry includes the component of following mass parts:
100 parts of glycols water soluble polyurethane resin
20~60 parts of water.
2. glycols water soluble polyurethane resin artificial leather manufacture method according to claim 1, it is characterised in that:It is described Covering with paint is to make surface technology by release liners dry method to fit in artificial leather wet half-finished product glycols soluble polyurethane surface layer.
3. glycols water soluble polyurethane resin artificial leather manufacture method according to claim 1, it is characterised in that:It is described Covering with paint is that glycols soluble polyurethane is covered with paint, lacquer, colour wash, etc. into slurry with surface printing method to cover with paint, lacquer, colour wash, etc. in artificial leather dry method surface of semi-finished.
4. glycols water soluble polyurethane resin artificial leather manufacture method according to claim 1, it is characterised in that:It is described Covering with paint is that glycols soluble polyurethane is applied into finish coat with rolling method to be coated with to artificial leather base fabric's surface of semi-finished.
5. glycols water soluble polyurethane resin artificial leather manufacture method according to claim 1, it is characterised in that:It is described Dyeing treatment is pad dyeing, dye gigging, overflow dyeing or airflow dyeing.
CN201510818020.4A 2015-11-24 2015-11-24 A kind of glycols water soluble polyurethane resin artificial leather manufacture method Pending CN106758287A (en)