CN106583058A - Collophanite reverse flotation collecting agent and preparing method thereof - Google Patents

Collophanite reverse flotation collecting agent and preparing method thereof Download PDF

Info

Publication number
CN106583058A
CN106583058A CN201611240728.7A CN201611240728A CN106583058A CN 106583058 A CN106583058 A CN 106583058A CN 201611240728 A CN201611240728 A CN 201611240728A CN 106583058 A CN106583058 A CN 106583058A
Authority
CN
China
Prior art keywords
parts
collecting agent
tween
polyoxyethylene ether
fatty alcohol
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201611240728.7A
Other languages
Chinese (zh)
Inventor
张晖
周琼波
何宾宾
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Yunnan Phosphate Chemical Group Corp Ltd
Original Assignee
Yunnan Phosphate Chemical Group Corp Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Yunnan Phosphate Chemical Group Corp Ltd filed Critical Yunnan Phosphate Chemical Group Corp Ltd
Priority to CN201611240728.7A priority Critical patent/CN106583058A/en
Publication of CN106583058A publication Critical patent/CN106583058A/en
Pending legal-status Critical Current

Abstract

The invention discloses a collophanite reverse flotation collecting agent and a preparing method thereof. The collecting agent is prepared from the following raw materials including, by weight, 30-40 parts of industrial grade animal oil fatty acid, 5-10 parts of inorganic base, 3-5 parts of dodecyl dimethyl betaine, 1-3 parts of aliphatic amine, 2-4 parts of tween, 3-5 parts of fatty alcohol-polyoxyethylene ether, 1-3 parts of foaming agents and 33-55 parts of water. The collecting agent is good in disperse performance, low in work temperature, high in efficiency and the like, and compared with a conventional collophanite reverse flotation magnesium removal collecting agent, the dosage of the collecting agent can be reduced by about 10%.

Description

A kind of Collophane anti-floatation collector and preparation method thereof
Technical field
The invention belongs to collophane reverse flotation technical field, more particularly to a kind of Collophane anti-floatation collector and its preparation Method.
Background technology
Phosphorus ore is important industrial chemicals, is widely used in agricultural, medicine, military affairs, food energy industry.Although China's phosphorus ore storage Amount is larger, but with Morocco, the U.S. can compared with, China's rock phosphate in powder grade is relatively low and flotability can be relatively poor.Additionally, China The many rich ores of lean ore are few, and rock phosphate in powder has to pass through the production requirement that phosphoric acid by wet process could be met after beneficiation enrichment.
Generally speaking phosphorus ore is divided into carbonate-type, silicate-type and mixed type, carbonate-type in the form of its stone-like pulse is present Collophane, its stone-like pulse mainly exists with the form of dolomite, calcite.It is by anti-floating to exclude dolomite, the method for calcite Choosing, its technology characteristics meet the principle of " floating few suppression is more ", and energy consumption is relatively low, is the prevailing technology of currently processed carbonate-type phosphorus ore. Collecting agent in reverse floatation mainly utilizes fatty acid prepared by Oleum Brassicae campestriss, soybean oil based on vegetable fatty acids, such as.These plants Oil price lattice are higher, do not only exist the problem that grain is striven with people, and because synergist selects improper, cause that low-temperature solubility is poor, disperse Ability is low, causes its consumption to remain high.Additionally, the Ca in ore pulp2+、Mg2+Unavoidable ion can consume fatty-acid collector, make It is further up into collector dosage.
The Chinese patent application of Application No. CN201310029412.3 discloses one kind to turn waste into wealth waste oil and carries out The method for preparing collophane reverse flotation carbonate mineral collecting agent.It is made up of waste oil, alkali and water, by its mass parts trench is compared Oil:Alkali:Water=1:0.15~0.3:400 ratio mixing, reacts 1~1.5 hour under 40~80 DEG C of constant temperature, that is, make Collophane reverse flotation carbonate mineral collecting agent is obtained, its step is:A. waste oil is heated to into 40~80 DEG C, filters, precipitates and remove Solid waste is gone, then is dehydrated to waste oil moisture content less than 1%;B. waste oil composition is detected, according to testing result, is adjusted Site preparation ditch line of oils part, the content for making C12~C18 in waste oil component reaches required index;C. waste oil is pressed:Alkali:Water=1: 0.15~0.3:400 ratio mixing, in 40~80 DEG C of constant temperature saponification 1~1.5 hour, adjusts pH value to 11, that is, obtain Obtain collophane reverse flotation carbonate mineral collecting agent.Because waste oil source is complicated, different batches material component is changed greatly, must Single fat acid (or purity higher fatty acid) must be added according to index, not only increased technological process, and be improve into This.
The Chinese patent application of Application No. CN201410622082.3 discloses a kind of phosphate reverse flotation collecting agent, and this is caught Receive agent to be made up of the component of following mass percent:Aliphatic acid polyethenoxy base ester salt 40~80%, alkyl polyoxyethylene base Ether phosphoric acid monoester salt 14~50%, aliphatic alcohol polyethenoxy base ether 5~20%, Arlacel-20 1~10%.The collecting agent is applied to Phosphate reverse flotation calcite.Although collecting agent is compared with fatty acid collecting agent, with very strong collecting ability and high selectivity; Compared with the collecting agent of α-amido aryl phosphoric acids class, cheap, consumption is little, draws materials conveniently.But, due to the collecting agent with Nonionic surfactant is raw material, and these raw materials have to pass through chemical industry synthesis and just can obtain, and its unit price is significantly larger than originated The fatty acid collecting agent of nature, not with wide variety of prospect.
The content of the invention
The present invention is directed to the deficiencies in the prior art, there is provided a kind of Collophane anti-floatation collector and preparation method thereof.This It is bright to be matched somebody with somebody by cationic surfactant, chelating agen and fatty acid complex, dispersive property of the fatty acid in phosphate ore pulp is improved, so as to have Effect improves its collecting performance, eliminates Ca in ore pulp2+、Mg2+Deng the impact of unavoidable ion.
Technical scheme is as follows:A kind of Collophane anti-floatation collector, the collecting agent is by following weight portion Raw material is made:Technical grade animal oil fatty acid 30-40 parts, inorganic base 5-10 parts, empgen BB 3-5 parts, fatty amine 1-3 Part, tween 2-4 parts, fatty alcohol-polyoxyethylene ether 3-5 parts, foaming agent 1-3 parts and water 33-55 parts.
One or more of the inorganic base in sodium carbonate, sodium hydroxide and sodium bicarbonate.
The one kind or several of the fatty amine in lauryl amine, octadecylamine and N, N- dimethyl dodecylamine Kind.
One or more of the tween in tween 20, Tween-40, Tween-60 and tween 80.
The fatty alcohol-polyoxyethylene ether (AEO) is selected from fatty alcohol-polyoxyethylene ether -10, fatty alcohol-polyoxyethylene ether -15 With one or more in fatty alcohol-polyoxyethylene ether -20.
The foaming agent is selected from cocoanut fatty acid diethanolamide (6501), dodecylbenzene sodium sulfonate and dodecyl One or more in sodium sulfate.
Collecting agent operation principle of the present invention is as follows:The present invention is simultaneously matched somebody with somebody by cationic surfactant with fatty acid complex, is subtracted The intermolecular repulsive force that few fatty acid molecule is produced when mineral surfaces adsorb, so as to improve adsorbance, reaches raising fatty acid The purpose of collecting ability;The empgen BB that the present invention is used has stronger resistance to hard water, can be with Ca in ore pulp2+、 Mg2+Hardly possible forms coordination compound except (exempting from) ion, reduces its consumption to collecting agent, and tween and fatty alcohol-polyoxyethylene ether can be effectively Separate animals fatty acid oil, improves dispersive property of the fatty acid in phosphate ore pulp.Mutual synergism between each component promotes described Collophane anti-floatation collector is better than conventional collecting agent, with wider range of application.
The present invention also provides the preparation method of the Collophane anti-floatation collector, and methods described operation is as follows:By industry Level animal oil fatty acid, inorganic base and water are put in proportion in reactor, and stirring reaction completes saponification, according still further to ratio Input empgen BB, fatty amine, tween, fatty alcohol-polyoxyethylene ether and foaming agent, continue to stir, and mix homogeneously is obtained Collecting agent.
Saponification temperature is 70-90 DEG C in the preparation method, and the response time is 1-3 hours.
The collecting agent usage amount is 0.25~0.35kg/t raw ores, i.e., in pulp tank, by ore pulp and of the present invention Collecting agent is mixed in proportion 3min, and being subsequently sent to flotation device carries out flotation.
Compared with prior art, the invention has the advantages that:The collecting agent that the present invention is provided has dispersive property Well, the advantages of low operating temperature, efficiency high, compared with conventional collophane reverse flotation de-magging collector, collector dosage can decline 10% or so.The present invention solves technical grade for a long time with wide material sources, cheap technical grade animal oil as raw material The hidden danger of animal oil backflow dining table.
Specific embodiment
Technical scheme is described in further details with reference to specific embodiment.
Embodiment 1
Technical grade Adeps Sus domestica fatty acid 30Kg, sodium hydroxide 5Kg and water 55kg parts are put in reactor, in 80 DEG C of stirrings 3h, after saponification terminates, adds empgen BB 3Kg, lauryl amine 1Kg, tween 20 2Kg, aliphatic alcohol polyethenoxy Ether (AEO-10) 3Kg, cocoanut fatty acid diethanolamide (6501) 1Kg continue to stir, mix homogeneously.
It is that 0.25Kg/t is former that collecting agent in reverse floatation will be prepared by phosphate ore pulp agitator tank and ore pulp mineralising, addition is pumped into Ore deposit, after a flotation, phosphorus concentrate floatation indicators are 28.5%P2O5, 0.7%MgO, 1.56%, Fe2O31.65%Al2O3, P2O5The response rate reaches 87%, reaches the requirement of dihydrate wet-process phosphoric acid production ore deposit.
Embodiment 2
Technical grade Adeps Sus domestica fatty acid 30Kg, sodium hydroxide 5Kg and water 55kg parts are put in reactor, in 80 DEG C of stirrings 3h, after saponification terminates, adds empgen BB 3Kg, lauryl amine 2Kg, fatty alcohol-polyoxyethylene ether (AEO-10) 3Kg, tween 20 2Kg, cocoanut fatty acid diethanolamide (6501) 1Kg continue to stir, mix homogeneously.
It is that 0.25Kg/t is former that collecting agent in reverse floatation will be prepared by phosphate ore pulp agitator tank and ore pulp mineralising, addition is pumped into Ore deposit, after a flotation, phosphorus concentrate floatation indicators are 28.5%P2O5, 0.7%MgO, 1.56%Fe2O3, 1.65%Al2O3, P2O5The response rate reaches 87%, reaches the requirement of dihydrate wet-process phosphoric acid production ore deposit.
Embodiment 3
Technical grade Adeps Sus domestica fatty acid 30Kg, sodium hydroxide 5Kg and water 55kg parts are put in reactor, in 80 DEG C of stirrings 3h, after saponification terminates, adds empgen BB 3Kg, lauryl amine 1Kg, tween 20 2Kg, aliphatic alcohol polyethenoxy Ether (AEO-10) 3Kg, cocoanut fatty acid diethanolamide (6501) 1Kg continue to stir, mix homogeneously.
It is that 0.25Kg/t is former that collecting agent in reverse floatation will be prepared by phosphate ore pulp agitator tank and ore pulp mineralising, addition is pumped into Ore deposit, after a flotation, phosphorus concentrate floatation indicators are 28.5%P2O5, 0.7%MgO, 1.56%Fe2O3, 1.65%Al2O3, P2O5The response rate reaches 87%, reaches the requirement of dihydrate wet-process phosphoric acid production ore deposit.
Embodiment 4
Technical grade tallow acid 35Kg, sodium bicarbonate 8Kg and water 42Kg are put in reactor, at 80 DEG C 3h are stirred, After saponification terminates, empgen BB 4Kg, octadecylamine 2Kg, Tween-40 3Kg, fatty alcohol-polyoxyethylene ether are added (AEO-15) 4Kg, dodecylbenzene sodium sulfonate 2Kg continue to stir, mix homogeneously.
It is 0.3Kg/t raw ores that collecting agent in reverse floatation will be prepared by phosphate ore pulp agitator tank and ore pulp mineralising, addition is pumped into, After a flotation, phosphorus concentrate floatation indicators are 29.3%P2O5, 0.68%MgO, 1.49%Fe2O3, 1.55%Al2O3, P2O5 The response rate reaches 85%, reaches the requirement of dihydrate wet-process phosphoric acid production ore deposit.
Embodiment 5
Technical grade chicken oil fatty acid 40Kg, sodium carbonate 10Kg and water 33Kg are put in reactor, at 80 DEG C 3h, soap are stirred After change terminates, empgen BB 5Kg, N, N- dimethyl lauryl amine 3Kg, Tween-60 4Kg, aliphatic alcohol polyethenoxy are added Ether (AEO-20) 5Kg, sodium lauryl sulphate 3Kg continue to stir, mix homogeneously.
It is that 0.35Kg/t is former that collecting agent in reverse floatation will be prepared by phosphate ore pulp agitator tank and ore pulp mineralising, addition is pumped into Ore deposit, after a flotation, phosphorus concentrate floatation indicators are 29.7%P2O5, 0.68%MgO, 1.46%Fe2O3, 1.52%Al2O3, P2O5The response rate reaches 83%, reaches the requirement of dihydrate wet-process phosphoric acid production ore deposit.

Claims (8)

1. a kind of Collophane anti-floatation collector, it is characterised in that following weight portion meter, the collecting agent is by following raw materials according system Into:Technical grade animal oil fatty acid 30-40 parts, inorganic base 5-10 parts, empgen BB 3-5 parts, fatty amine 1-3 parts, tell Warm 2-4 parts, fatty alcohol-polyoxyethylene ether 3-5 parts, foaming agent 1-3 parts and water 33-55 parts.
2. Collophane anti-floatation collector as claimed in claim 1, it is characterised in that the inorganic base is selected from sodium carbonate, hydrogen One or more in sodium oxide and sodium bicarbonate.
3. Collophane anti-floatation collector as claimed in claim 1, it is characterised in that the fatty amine is selected from dodecyl One or more in amine, octadecylamine and N, N- dimethyl dodecylamine.
4. Collophane anti-floatation collector as claimed in claim 1, it is characterised in that the tween selected from tween 20, tell One or more in temperature -40, Tween-60 and tween 80.
5. Collophane anti-floatation collector as claimed in claim 1, it is characterised in that the fatty alcohol-polyoxyethylene ether is selected from One or more in fatty alcohol-polyoxyethylene ether -10, fatty alcohol-polyoxyethylene ether -15 and fatty alcohol-polyoxyethylene ether -20.
6. Collophane anti-floatation collector as claimed in claim 1, it is characterised in that the foaming agent is selected from coconut oil fat One or more in sour diglycollic amide, dodecylbenzene sodium sulfonate and sodium lauryl sulphate.
7. a kind of preparation method of the Collophane anti-floatation collector as described in claim 1~6 is arbitrary, it is characterised in that side Method operation is as follows:Technical grade animal oil fatty acid, inorganic base and water are put in proportion in reactor, stirring reaction completes soap Change reaction, according still further to ratio input empgen BB, fatty amine, tween, fatty alcohol-polyoxyethylene ether and foaming agent, continue Stirring, mix homogeneously obtains collecting agent.
8. the preparation method of Collophane anti-floatation collector as claimed in claim 7, it is characterised in that in the preparation method Saponification temperature is 70-90 DEG C, and the response time is 1-3 hours.
CN201611240728.7A 2016-12-28 2016-12-28 Collophanite reverse flotation collecting agent and preparing method thereof Pending CN106583058A (en)