CN105919193B - The production method of easy to operate pure cotton plucking colour bright adhesive lining - Google Patents
The production method of easy to operate pure cotton plucking colour bright adhesive lining Download PDFInfo
- Publication number
- CN105919193B CN105919193B CN201610355018.2A CN201610355018A CN105919193B CN 105919193 B CN105919193 B CN 105919193B CN 201610355018 A CN201610355018 A CN 201610355018A CN 105919193 B CN105919193 B CN 105919193B
- Authority
- CN
- China
- Prior art keywords
- plucking
- dyeing
- fabric
- point coating
- powder point
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The invention discloses a kind of production method of easy to operate pure cotton plucking colour bright adhesive lining, production procedure includes turning over seam, plucking, concise, bleaching, dyeing, shiinkproof finish, bright powder point coating, machine shrunk step;Present invention process is easy to operate, saves water and energy and subtracts dirt, excellent product performance, coating surface light, and coating backside has one layer of pluffy hair, and color jail degree≤4 grade are dissociated and hydrolysis formaldehyde≤35mg/kg, are 1.0%~+0.5% through broadwise washing size changing rate;After plucking adhesive lining is bonded with garment material so that the good hand feeling of fabric is abundant.
Description
The application is application number " 201510614737.7 ", the applying date " 2015.9.24 ", title " pure cotton plucking colourama
The divisional application of bright adhesive lining and its production method ".
Technical field
The present invention relates to a kind of pure cotton plucking colour bright adhesive lining and its production method.
Background technology
After surface smooth adhesive lining is bonded with garment material, typically all compare consolidation, there is no fluffy feel.High-grade slim coloured silk
If using achromaticity adhesive lining, adhesive lining color can be caused not matched with fabric color in color garment production, clothes product are influenceed
Matter.If coloured adhesive lining poor color fastness, also to influence high-grade clothing quality, in addition the high-grade adhesive lining of influence performance and
Using effect.In addition, conventional production adhesive lining, surface dimness, during appearance test, the fault such as leak source, holiday is not easy entirely sometimes
Portion verifies, garment enterprise can produce the loss such as drop using not detecting fault adhesive lining and be made dress-goods.
The content of the invention
It is an object of the invention to provide a kind of coating surface light, coating backside has one layer of pluffy hair;Se Lao Du≤4
Level;Free and hydrolysis formaldehyde≤35mg/kg;Through the pure cotton plucking colourama that broadwise washing size changing rate is -1.0%~+0.5%
Bright adhesive lining and its production method.
Technical solution of the invention is:
A kind of pure cotton plucking colour bright adhesive lining, it is characterized in that:Coating surface light, coating backside has one layer of fluffy suede
Hair;Se Lao Du≤4 grade;Free and hydrolysis formaldehyde≤35mg/kg;It is -1.0%~+0.5% through broadwise washing size changing rate.
The fabric specification of lining cloth is the one kind in following two kinds:The first width is 48.5 inches, yarn count is 60s×
60s, density be 68 × 52 pieces/inch, second width is 48.5 inches, yarn count is 80 s×80s, density be 80 × 60/
Inch.
A kind of production method of pure cotton plucking colour bright adhesive lining, successively including turning over seam, plucking, concise, bleaching, dye
Color, shiinkproof finish, bright powder point coating, machine shrunk step;Brushing process is that lifting by one side is secondary, and cylinder rotating speed 75 rpm is suitable
Porcupine roller rotating speed 700rpm, along porcupine roller cylinder pressure 0.20Mpa, inverse porcupine roller cylinder pressure 0.25Mpa, inverse porcupine roller rotating speed 800rpm;
Upper fabric guide roll tension force 1.8%, preceding fabric guide roll tension force 2.8%, rear fabric guide roll tension force 1.9% enters 14~16m/min of cloth speed.Plucking
Afterwards, fabric face covers one layer of uniform fine hair.
During dyeing, cold-rolling heap staining is carried out using reactive dye, the technical recipe for contaminating light green color product is:
Dye liquor:Active yellow 3 R S 0.06g/L, activity gorgeous yellow 4GL 0.2g/L, reactive brilliant bule BB 0.2g/L, bleeding agent
1g/L。
Alkali lye:Caustic soda(36 ° of B é) 30g/L, sodium metasilicate(38-40°Bé) 30-40g/L.
Dyeing is:
Dye liquor and alkali lye 4:1 ratio mixes, pick-up rate 65%, speed 60-65m/min, stacking at room temperature 15-16h.
Dyeing aftertreatment technology is:
Enter cloth → normal temperature and wash → fourth, fifth lattice soap boiling through reductive steam box vapour → first, second and third lattice flowing cool water(Soap boiling
Liquid 2~3g/L, 80-90 DEG C)→ the six lattice(70~80 DEG C)The → the seven lattice of washing(50~60 DEG C)Washing the → the eight lattice flowing is cold
Washing → drying → cropping.Speed:60~65m/min.
Shallow khaki product is contaminated, dye liquor composition is:
The g/L of active yellow 3 R S 0.08, active red RB 0.12g/L, reactive brilliant bule BB 0.07g/L, bleeding agent 1g/L
Alkali lye:Caustic soda(36 ° of B é) 30g/L, sodium metasilicate(38-40°Bé) 30-40g/L.
Dyeing and dyeing aftertreatment technology are identical with dye light green color product.
When bright powder point coating is arranged, by open width enter cloth, 220 ~ 255 DEG C of preheatings of No. 1 oily hot-rolling, No. 2 oily hot-rollings 210 ~
260 DEG C of preheatings, engraved roll PE PURs powder point coating, No. 3 220 ~ 260 DEG C of oily hot-rollings are heated, use power to be 1000 ~ 3000W
Infrared tube carry out infrared baking melt, mirror roller calendering, tentering setting, temperature≤25 DEG C water cooling, package step;Engraved roll mesh
Number:30th, 33 mesh/inch;30 ± 2g/m of fabric powder point coating amount2, prevent reverse side from permeating;During powder point coating, it is impossible to occur
Jump powder, leak source, half head;During powder point coating, the 100 DEG C of hot water circuits in engraved roll inside;65 ~ 85 DEG C of heat of engraved roll roller interior circulation
Water;Enter cloth speed for 18 ~ 22m/min.
Present invention process is easy to operate, saves water and energy and subtracts dirt, excellent product performance, and coating surface light, coating backside has
One layer of pluffy hair;Se Lao Du≤4 grade;Free and hydrolysis formaldehyde≤35mg/kg;It is -1.0% through broadwise washing size changing rate
~+0.5%
With reference to embodiment, the invention will be further described.
Specific embodiment
Embodiment 1:
Lining cloth fabric door width is 48.5 inches, yarn count is 60s×60s, density be 68 × 52 pieces/inch;
A kind of production method of pure cotton plucking colour bright adhesive lining, including turn over seam, plucking, concise, bleaching, dyeing, anti-
Contracting is arranged, bright powder point coating, machine shrunk step;
During wharf's pavement quality, lifting by one side is secondary, the rpm of cylinder rotating speed 75, along porcupine roller rotating speed 700rpm, along porcupine roller cylinder pressure
0.20Mpa, inverse porcupine roller cylinder pressure 0.25Mpa, inverse porcupine roller rotating speed 800rpm;Upper fabric guide roll tension force 1.8%, preceding fabric guide roll tension force
2.8%, rear fabric guide roll tension force 1.9% enters 14~16m/min of cloth speed.After plucking, fabric face covers one layer of uniform fine hair.Draw
After hair adhesive lining is bonded with garment material so that the good hand feeling of fabric is abundant.
During dyeing, cold-rolling heap staining is carried out using reactive dye, the technical recipe of light green color product is:
Dye liquor:Active yellow 3 R S 0.06g/L, activity gorgeous yellow 4GL 0.2g/L, reactive brilliant bule BB 0.2g/L, bleeding agent
1g/L。
Alkali lye:Caustic soda(36 ° of B é) 30g/L, sodium metasilicate(38-40°Bé) 30-40g/L.
Dyeing is:
Dye liquor and alkali lye 4:1 ratio mixes, pick-up rate 65%, 60~65m/min of speed, 15~16h of stacking at room temperature.
Dyeing aftertreatment technology is:
Enter cloth → normal temperature and wash → fourth, fifth lattice soap boiling through reductive steam box vapour → first, second and third lattice flowing cool water(Soap boiling
Liquid 2~3g/L, 80~90 DEG C)→ the six lattice(70-80℃)The → the seven lattice of washing(50-60℃)The → the eight lattice flowing cool water of washing
Wash → dry → cropping.Speed:60-65m/min.
When bright powder point coating is arranged, by open width enter cloth, 220 ~ 255 DEG C of preheatings of No. 1 oily hot-rolling, No. 2 oily hot-rollings 210 ~
260 DEG C of preheatings, engraved roll PE PURs powder point coating, 220 ~ 260 DEG C of heating of No. 3 oily hot-rollings, use power infrared for 3000W
Pipe carry out infrared baking melt, mirror roller calendering, tentering setting, temperature≤25 DEG C water cooling, package step;Engraved roll mesh number:30、33
Mesh/inch;30 ± 2g/m of fabric powder point coating amount2, prevent reverse side from permeating;During powder point coating, it is impossible to occur jumping powder, leakage
Point, half head;During powder point coating, the 100 DEG C of hot water circuits in engraved roll inside;65 ~ 85 DEG C of hot water of engraved roll roller interior circulation;Enter cloth speed
It is 18 ~ 22m/min to spend.
Embodiment 2:
Lining cloth fabric door width is 48.5 inches, yarn count is 80 s×80s, density be 80 × 60 pieces/inch;
A kind of production method of pure cotton plucking colour bright adhesive lining, including turn over seam, plucking, concise, bleaching, dyeing, anti-
Contracting is arranged, bright powder point coating, machine shrunk step;
During wharf's pavement quality, lifting by one side is secondary, the rpm of cylinder rotating speed 75, along porcupine roller rotating speed 700rpm, along porcupine roller cylinder pressure
0.20Mpa, inverse porcupine roller cylinder pressure 0.25Mpa, inverse porcupine roller rotating speed 800rpm;Upper fabric guide roll tension force 1.8%, preceding fabric guide roll tension force
2.8%, rear fabric guide roll tension force 1.9% enters 14~16m/min of cloth speed.After plucking, fabric face covers one layer of uniform fine hair.Draw
After hair adhesive lining is bonded with garment material so that the good hand feeling of fabric is abundant.
During dyeing, cold-rolling heap staining is carried out using reactive dye, shallow khaki product dye liquor composition is:
The g/L of active yellow 3 R S 0.08, active red RB 0.12g/L, reactive brilliant bule BB 0.07g/L, bleeding agent 1g/L
Alkali lye:Caustic soda(36 ° of B é) 30g/L, sodium metasilicate(38-40°Bé) 30-40g/L.
Dyeing and dyeing aftertreatment technology are same as Example 1.
When bright powder point coating is arranged, by open width enter cloth, 220 ~ 255 DEG C of preheatings of No. 1 oily hot-rolling, No. 2 oily hot-rollings 210 ~
260 DEG C of preheatings, engraved roll PE PURs powder point coating, 220 ~ 260 DEG C of heating of No. 3 oily hot-rollings, use power infrared for 2000W
Pipe carry out infrared baking melt, mirror roller calendering, tentering setting, temperature≤25 DEG C water cooling, package step;Engraved roll mesh number:30、33
Mesh/inch;29 ± 1g/m of fabric powder point coating amount2, prevent reverse side from permeating;During powder point coating, it is impossible to occur jumping powder, leakage
Point, half head;During powder point coating, the 100 DEG C of hot water circuits in engraved roll inside;65 ~ 85 DEG C of hot water of engraved roll roller interior circulation;Enter cloth speed
It is 18 ~ 22m/min to spend.
Claims (1)
1. a kind of production method of easy to operate pure cotton plucking colour bright adhesive lining, successively including turn over seam, plucking, it is concise,
Bleaching, dyeing, shiinkproof finish, bright powder point coating, machine shrunk step;It is characterized in that:Brushing process is that lifting by one side is secondary, tin
Woods rotating speed 75rpm, along porcupine roller rotating speed 700rpm, along porcupine roller cylinder pressure 0.20Mpa, inverse porcupine roller cylinder pressure 0.25Mpa, inverse pin
Roller rotating speed 800rpm;Upper fabric guide roll tension force 1.8%, preceding fabric guide roll tension force 2.8%, rear fabric guide roll tension force 1.9% enters cloth speed 14
~16m/min;After plucking, fabric face covers one layer of uniform fine hair;After plucking adhesive lining is bonded with garment material so that fabric
Good hand feeling it is abundant;
During dyeing, cold-rolling heap staining is carried out using reactive dye;
Contaminate light green color product technical recipe be:
Dye liquor:Active yellow 3 R S 0.06g/L, activity gorgeous yellow 4GL 0.2g/L, reactive brilliant bule BB0.2g/L, bleeding agent 1g/L;
Alkali lye:36 ° of B é caustic soda 30g/L, 38-40 ° of B é sodium metasilicate 30-40g/L;
Dyeing is:
Dye liquor and alkali lye 4:1 ratio mixes, pick-up rate 65%, 60~65m/min of speed, 15~16h of stacking at room temperature;
Dyeing aftertreatment technology is:
Enter cloth → normal temperature and wash → fourth, fifth lattice soap boiling through reductive steam box → first, second and third lattice flowing cool water, soap boiling liquid 2~
3g/L, 80~90 DEG C, the → the six 70~80 DEG C of lattice wash 50~60 DEG C of → the eight lattice flowing cool waters of washing of the → the seven lattice and wash → dry
Dry → cropping;Speed:60~65m/min;
Shallow khaki product is contaminated, dye liquor composition is:
Active yellow 3 R S 0.08g/L, active red RB 0.12g/L, reactive brilliant bule BB 0.07g/L, bleeding agent 1g/L
Alkali lye:36 ° of B é caustic soda 30g/L, 38-40 ° of B é sodium metasilicate 30-40g/L;
Dyeing and dyeing aftertreatment technology are identical with dye light green color product;
The treatment of bright powder point coating successively including open width enter cloth, 220~255 DEG C of preheatings of No. 1 oily hot-rolling, No. 2 oily hot-rollings 210~
260 DEG C of preheatings, engraved roll PE PURs powder point coating, 220~260 DEG C of heating of No. 3 oily hot-rollings, use power for 1000~
The infrared tube of 3000W carry out infrared baking melt, mirror roller calendering, tentering setting, temperature≤25 DEG C water cooling, package step;Engraving
Roller mesh number:30th, 33 mesh/inch;30 ± 2g/m of fabric powder point coating amount2, prevent reverse side from permeating;During powder point coating, it is impossible to
Occur jumping powder, leak source, half head;During powder point coating, the 100 DEG C of hot water circuits in engraved roll inside;Engraved roll roller interior circulation 65~85
DEG C hot water;Enter cloth speed for 18~22m/min;
The fabric specification of lining cloth is:Door width is 48.5 inches, yarn count is 80s×80s, density be 80 × 60 pieces/inch.