CN105906210A - Jianshui pottery manufacture method based on fusion of blue-and-white processing, glazing, engraving and filling - Google Patents
Jianshui pottery manufacture method based on fusion of blue-and-white processing, glazing, engraving and filling Download PDFInfo
- Publication number
- CN105906210A CN105906210A CN201610288716.5A CN201610288716A CN105906210A CN 105906210 A CN105906210 A CN 105906210A CN 201610288716 A CN201610288716 A CN 201610288716A CN 105906210 A CN105906210 A CN 105906210A
- Authority
- CN
- China
- Prior art keywords
- blue
- white
- glazing
- engraving
- filling
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention discloses a Jianshui pottery manufacture method based on fusion of blue-and-white processing, glazing, engraving and filling. The Jianshui pottery manufacture method includes step 1, performing blue-and-white processing and glazing, and step 2, performing engraving, filling and manual polishing. According to the step 1, a glazing material comprises 40% of clay-wash, 35% of calcite powder and 25% of white mortar, and the temperature for sintering is decreased to 1195 DEG C; according to the step 2, 10% of blue earth is added into a white mud material to increase the sintering temperature to 1195 DEG C, so that the sintering temperatures in the step 1 and the step 2 are unified, and a process-infused product is formed. The Jianshui pottery manufacture method has the advantages that the ratios of ingredients of the glaze material and raw materials for engraving and filling are redistributed, and the sintering temperatures for the glaze material and the raw materials for engraving and filling are unified to 1195 DEG C, and the processes are fused into one product successfully, so that the problem of generation of inferior-quality products caused by insufficient temperatures for blue-and-white processing and glazing, dark glazes or ultrahigh temperatures for engraving and filling during sintering is solved effectively.
Description
Technical field
The present invention relates to ceramic making field, build the water blue and white glazing of pottery particularly to one and inscribe fusion system of fillering
Make method.
Background technology
Build water ceramics, of long standing and well established, with a long history, it with its " sound such as single sonorous stone, bright such as water, bright such as mirror,
Light mirror is according to people, simple and tasteful " artistic beauty, attracted the sight of most people.1980, in former
Professor Yang great Shen of centre arts and crafts college waits and builds water conservancy project skill artistic pottery factory and combine, to north of the city two km
Wan Yao village Gu kiln site has carried out examining or check research in earnest, it is believed that " it is blue and white, bright that Song has celadon, unit to have to build water kiln
There is crude pottery, have purple to make pottery clearly ".In recent years, pour down in the care of governments at all levels and the pass of each mainstream media, " build
Water purple is made pottery " rank among the ranks of " national non-material cultural heritage ", " building water purple pottery " and " building water to make pottery "
The most successfully declare as " the national geography certification mark ".
Build water pottery to produce so far, blue and white, glazing;Inscribe the single development of skill fillered, polish by hand, build
Make pottery frush glazing integration technology of banketing blue and white quarter of water uses and builds water this locality white clay base, merges and builds water kilneye history and send out
The quarter occurred since Song Yuanqing glaze and blue and white manufacture craft have again clear late period concurrently in exhibition fills out technique, and difficulty exists
The compatible burning of blue or green glaze, blue and white glaze proportioning and spackle at quarter is made, and oxidation kiln flame burns after making, and quarter fills out part and uses
Manual polishing, makes every effort to one integral piece implements and covers and build the ripe skill occurred in water kilneye development history.
On same implements, in traditional technology, blue and white glazing part needs temperature 1250 DEG C during burning is made,
Inscribe part of fillering to burn the temperature made and not can exceed that 1175 DEG C, both temperature difference 75 DEG C, meeting during firing
Occurring that blue and white glazing portion temperature is inadequate, glaze does not works or inscribes portion temperature of fillering too high one-tenth substandard products.
Summary of the invention
The invention provides one build water make pottery blue and white glazing inscribe fusion preparation method of fillering, to solve existing skill
It is inadequate that art there will be blue and white glazing portion temperature during firing, and glaze does not works or inscribes part temperature of fillering
The problem spending high one-tenth substandard products.
For solving the problems referred to above, as one aspect of the present invention, it is provided that one builds water pottery blue and white glazing periodical
Filler quarter fusion preparation method, including:
Step 1, makes blue and white glazing: at glaze containing clay wash 40%, gingival cyst of mucous gland in the newborn stone flour 35%, white sand slurry 25%,
Thus burning is made the temperature of needs and is reduced to 1195 DEG C;
Step 2, inscribe filler, manual polishing: in white clay thin material, add the blue clay of 10% to strengthen sintering temperature
Degree, makes burning make temperature and brings up to 1195 DEG C, so that the burning of step 1 and step 2 is made temperature and is reached unified,
The implements that formation process merges.
By technique scheme, present invention proportioning glaze again and inscribing fillers required raw-material composition,
Make both burnings make required temperature and form unified 1195 DEG C, make technique successful fusion on implements, from
And efficiently solve and during firing, there will be blue and white glazing portion temperature not, glaze does not works or inscribes
Portion temperature of fillering too high one-tenth substandard products.
Detailed description of the invention
Hereinafter embodiments of the invention are described in detail, but the present invention can be defined by the claims and
The multitude of different ways covered is implemented.
The invention provides one build water make pottery blue and white glazing inscribe fusion preparation method of fillering, including:
Step 1, makes blue and white glazing: at glaze containing clay wash 40%, gingival cyst of mucous gland in the newborn stone flour 35%, white sand slurry 25%,
Thus burning is made the temperature of needs and is reduced to 1195 DEG C, and clay wash 50% in traditional raw material, gingival cyst of mucous gland in the newborn stone flour 30%,
White sand slurry 20%, the temperature that its burning makes needs is 1250 DEG C.
Step 2, inscribe filler, manual polishing: in white clay thin material, add the blue clay of 10% to strengthen sintering temperature
Degree, makes burning make temperature and brings up to 1195 DEG C from 1175 DEG C, reach so that the burning of step 1 and step 2 makes temperature
To unified, that formation process merges implements.
By technique scheme, present invention proportioning glaze again and inscribing fillers required raw-material composition,
Make both burnings make required temperature and form unified 1195 DEG C, make technique successful fusion on implements, from
And efficiently solve and during firing, there will be blue and white glazing portion temperature not, glaze does not works or inscribes
Portion temperature of fillering too high one-tenth substandard products.
The present invention is fused to a device by building water pottery single technique of appearance from evolution so far at the beginning of the unit of Song end
On thing, it is the innovation during water purple pottery traditional culture is built in succession, by the fusion of single technique,
Abundant build water pottery product while, explore the development building water Tao Xin.
The foregoing is only the preferred embodiments of the present invention, be not limited to the present invention, for ability
For the technical staff in territory, the present invention can have various modifications and variations.All in the spirit and principles in the present invention
Within, any modification, equivalent substitution and improvement etc. made, should be included in protection scope of the present invention it
In.
Claims (1)
1. one kind build water make pottery blue and white glazing inscribe fusion preparation method of fillering, it is characterised in that including:
Step 1, makes blue and white glazing: described glaze containing described clay wash 40%, gingival cyst of mucous gland in the newborn stone flour 35%,
White sand slurry 25%, thus burning is made the temperature of needs and is reduced to 1195 DEG C;
Step 2, inscribe filler, manual polishing: in white clay thin material, add the blue clay of 10% to strengthen burning
Junction temperature, makes burning make temperature and brings up to 1195 DEG C, reach so that the burning of step 1 and step 2 makes temperature
To unified, that formation process merges implements.