CN105644176B - A kind of processing method of glitter powder bat printing film - Google Patents

A kind of processing method of glitter powder bat printing film Download PDF

Info

Publication number
CN105644176B
CN105644176B CN201610019451.9A CN201610019451A CN105644176B CN 105644176 B CN105644176 B CN 105644176B CN 201610019451 A CN201610019451 A CN 201610019451A CN 105644176 B CN105644176 B CN 105644176B
Authority
CN
China
Prior art keywords
glitter powder
silicon oil
primer
membranes
pet silicon
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201610019451.9A
Other languages
Chinese (zh)
Other versions
CN105644176A (en
Inventor
罗广桃
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ningbo Chuangyuan Cultural Development Co Ltd
Original Assignee
Ningbo Chuangyuan Cultural Development Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ningbo Chuangyuan Cultural Development Co Ltd filed Critical Ningbo Chuangyuan Cultural Development Co Ltd
Priority to CN201610019451.9A priority Critical patent/CN105644176B/en
Publication of CN105644176A publication Critical patent/CN105644176A/en
Application granted granted Critical
Publication of CN105644176B publication Critical patent/CN105644176B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of processing method of glitter powder bat printing film, feature is first to modulate base oil, then by base oil and open profit in mass ratio be 3:2 ratio uniform mixing, obtain primer, then tune machine is carried out to screen process press, primer is coated by screen process press to one side PET silicon oil membranes again, after the completion of coating, passed through toward the one side with primer artificial or tremble powder machine and uniformly spread glitter powder, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces, finally dries the one side PET silicon oil membranes of one side dusting, obtains glitter powder bat printing film;It is covered in as long as advantage is the glitter powder bat printing film for processing to obtain by this method on the printing surface of printed article, can be by glitter powder bat printing to printed article by heating pressurization, make printed article that there is stronger visual effect, particularly suitable for the glitter powder bat printing for the printing paper printed to non-aqueous inks, it is easy to operate and pad printing method is simple, without special equipment, it is adapted to a small amount of processing such as personalized customization, and cost is relatively low.

Description

A kind of processing method of glitter powder bat printing film
Technical field
The present invention relates to glitter powder printing, more particularly to a kind of processing method of glitter powder bat printing film.
Background technology
Glitter powder is also gold and silver piece, diamante, flashlight powder etc., is passed through by the plating material of the high different-thickness of smart brightness Accurate cutting forms.The treatment material unique as a kind of effect, glitter powder are widely used in christmas crafts product, candle work Skill, cosmetics, silk-screen printing industry, ornament materials etc., for strengthening the visual effect of product, decorative parts bumps are made to have layer It is secondary, more third dimension.At present, glitter powder is printed on the materials such as paper, cloth, metal and generally required by special equipment, and must Batch production that need be certain, and for some draw a design making or personalized customization, then cost is very high, causes its application by very Big limitation.
The content of the invention
The technical problems to be solved by the invention be to provide one kind can meet personalized customization etc. on a small quantity processing and cost compared with The processing method of glitter powder bat printing film low, without special equipment.
Technical scheme is used by the present invention solves above-mentioned technical problem:A kind of processing method of glitter powder bat printing film, Including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 30~37%, polyvinyl chloride 20~ 23%th, calcium carbonate 17~18%, unsaturated oleic acid 5~10%, phthalic anhydride 7~8%, antimony oxide 6~8%, O-phthalic Sour didecyl 0.4~0.6%, dibasic calcium stearate 0.6~0.9%, trioctyl phosphate 0.4~0.8%, Tissuemat E 0.6~ 1.2%th, tristerin 0.2~0.3%, alkyl phthalates 0.5~0.7%, carbon black 0.5~0.6%, acrylic acid copolymer The above each component of thing 4~6% uniformly mixes at normal temperatures, obtains base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The net of 250~300 mesh, 3 layers of photosensitive layer is installed on screen process press Version, take the soft-slab that hardness is 75HRC or 90HRC to be used as scraper plate, during installation, control the gradient of scraper plate and tool rest as 35~40 °;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >= 230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen Printed edge is retracted 3~7mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into list by screen process press On the silicone oil face of face PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
Compared with prior art, as long as it is an advantage of the invention that the glitter powder bat printing film for processing to obtain by this method covers On the printing surface of printed article, it on glitter powder bat printing to printed article, can will make printed article with stronger by heating pressurization Visual effect, particularly suitable for the glitter powder bat printing for the printing paper printed to non-aqueous inks, and pad printing method is simple, It is easy to operate, without special equipment, it is adapted to a small amount of processing such as personalized customization, and cost is relatively low.
Embodiment
The present invention is described in further detail with reference to embodiments.
Embodiment one:A kind of processing method of glitter powder bat printing film, including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 30%, polyvinyl chloride 23%, calcium carbonate 17%th, unsaturated oleic acid 8%, phthalic anhydride 7.5%, antimony oxide 6%, didecyl phthalate 0.4%, dibasic are hard Resin acid calcium 0.6%, trioctyl phosphate 0.8%, Tissuemat E 1.2%, tristerin 0.3%, alkyl phthalates 0.7%, Carbon black 0.5%, the above each component of acrylic copolymer 4% uniformly mix at normal temperatures, obtain base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The half tone of 300 mesh, 3 layers of photosensitive layer is installed on screen process press, taken hard Soft-slab for 75HRC is spent as scraper plate, and during installation, it is 35 ° to control the gradient of scraper plate and tool rest;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >= 230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen Printed edge is retracted 5mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side by screen process press On the silicone oil face of PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
Embodiment two:A kind of processing method of glitter powder bat printing film, including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 35%, polyvinyl chloride 20%, calcium carbonate 17.8%th, unsaturated oleic acid 5%, phthalic anhydride 7.5%, antimony oxide 6.5%, didecyl phthalate 0.6%, disalt Base calcium stearate 0.9%, trioctyl phosphate 0.4%, Tissuemat E 1.0%, tristerin 0.2%, alkyl phthalates 0.5%th, carbon black 0.6%, the above each component of acrylic copolymer 4% uniformly mix at normal temperatures, obtain base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The half tone of 250 mesh, 3 layers of photosensitive layer is installed on screen process press, taken hard Soft-slab for 90HRC is spent as scraper plate, and during installation, it is 35 ° to control the gradient of scraper plate and tool rest;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >= 230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen Printed edge is retracted 7mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side by screen process press On the silicone oil face of PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
Embodiment three:A kind of processing method of glitter powder bat printing film, including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 32%, polyvinyl chloride 20.5%, carbonic acid Calcium 17.5%, unsaturated oleic acid 6.2%, phthalic anhydride 8%, antimony oxide 7%, didecyl phthalate 0.5%, disalt Base calcium stearate 0.7%, trioctyl phosphate 0.6%, Tissuemat E 0.7%, tristerin 0.2%, alkyl phthalates 0.6%th, carbon black 0.5%, the above each component of acrylic copolymer 5% uniformly mix at normal temperatures, obtain base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The half tone of 300 mesh, 3 layers of photosensitive layer is installed on screen process press, taken hard Soft-slab for 75HRC is spent as scraper plate, and during installation, it is 40 ° to control the gradient of scraper plate and tool rest;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >= 230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen Printed edge is retracted 3mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side by screen process press On the silicone oil face of PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
The glitter powder bat printing film for processing to obtain by the above method, golden green onion is carried out to the printing paper of non-aqueous inks printing The concrete operations of powder bat printing are:Glitter powder bat printing film is covered on the printing surface of printing paper, passes through roller or other simple Equipment is heated to glitter powder bat printing film and pressurizeed, and heating-up temperature is 120~150 DEG C, and pressure is 5~10MPa, heating pressurization 2~3 seconds Afterwards, glitter powder bat printing film is taken away, printing paper, which moves up, is printed on glitter powder pattern.

Claims (1)

1. a kind of processing method of glitter powder bat printing film, it is characterised in that including step in detail below:
(1) base oil, is modulated:It is by weight/mass percentage composition:Cyclomethicone 30~37%, polyvinyl chloride 20~23%, Calcium carbonate 17~18%, unsaturated oleic acid 5~10%, phthalic anhydride 7~8%, antimony oxide 6~8%, O-phthalic Sour didecyl 0.4~0.6%, dibasic calcium stearate 0.6~0.9%, trioctyl phosphate 0.4~0.8%, Tissuemat E 0.6 ~1.2%, tristerin 0.2~0.3%, alkyl phthalates 0.5~0.7%, carbon black 0.5~0.6%, propylene The above each component of acid copolymer 4~6% uniformly mixes at normal temperatures, obtains base oil;
(2) it is, 3 in mass ratio with opening profit by the above-mentioned base oil modulated:2 ratio uniform mixing, obtains primer;
(3) tune machine, is carried out to screen process press:The half tone of 250~300 mesh, 3 layers of photosensitive layer is installed on screen process press, taken The soft-slab that hardness is 75HRC or 90HRC is used as scraper plate, during installation, controls the gradient of scraper plate and tool rest as 35~40 °;
(4) PET silicon oil membranes, are chosen:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >=230N/ m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk-screen printing Edge is retracted 3~7mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side PET by screen process press On the silicone oil face of silicon oil membrane;
(6), after the completion of primer coating, one side PET silicon oil membranes are removed, are passed through toward the one side with primer artificial or to tremble powder machine uniform Glitter powder is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
CN201610019451.9A 2016-01-13 2016-01-13 A kind of processing method of glitter powder bat printing film Active CN105644176B (en)